Substrate processing device, substrate processing method, and semiconductor device manufacturing method

By performing Si spray treatment on dummy wafers in a substrate processing device, the problem of poor film thickness uniformity in large surface area wafer processing is solved, the yield and productivity are improved, and the surface-to-surface uniformity and film thickness uniformity are improved.

CN112823409BActive Publication Date: 2024-10-25KOKUSAI DENKI KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201880097988.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-09-25
Publication Date
2024-10-25
Estimated Expiration
2038-09-25

AI Technical Summary

Technical Problem

In the manufacturing process of semiconductor components, when large surface area wafers are processed, film thickness uniformity becomes poor, causing a loading effect that affects productivity and yield.

Method used

Using a substrate processing device, the dummy wafer is subjected to Si spray treatment to make its surface area greater than or equal to the surface area of ​​the product wafer to be processed, and the load effect is alleviated and the inter-surface uniformity is improved by adjusting the spray film thickness.

Benefits of technology

It effectively alleviates the problem of inter-surface unevenness when processing large surface area wafers, improves the yield and productivity, and ensures the uniformity of the film thickness of the wafer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112823409B_ABST
    Figure CN112823409B_ABST
Patent Text Reader

Abstract

The present invention provides a substrate processing device capable of alleviating the inter-surface non-uniformity (load effect) of multiple wafers when the multiple wafers are processed side by side. The substrate processing device is constructed to include: a substrate holder, which holds multiple substrates arranged at a specified interval; a reaction tube for accommodating the substrate holder, which has a top plate with an upper end closed and an opening at the bottom for allowing the substrate holder to enter and exit; a furnace body, which surrounds the top and sides of the reaction tube; a cover, which directly or indirectly holds the substrate holder and blocks the opening; and a gas supply mechanism, which provides a gas flow parallel to the surface of the surface side of each of the multiple substrates held on the substrate holder in the reaction tube. The substrate holder is constructed to hold a product substrate or a monitoring substrate with an integrated circuit pattern formed thereon and a dummy substrate with a Si spraying layer formed on the surface side, wherein the dummy substrate is located on both sides of the product substrate or the monitoring substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a substrate processing apparatus for processing a substrate in a manufacturing process of a semiconductor component and a method for manufacturing a semiconductor device. Background Art

[0002] In the heat treatment of substrates (wafers) in the manufacturing process of semiconductor components, for example, a vertical substrate processing apparatus is used. In the vertical substrate processing apparatus, a plurality of substrates are arranged and held in a vertical direction by a substrate holder, and the substrate holder is moved into a processing chamber. Thereafter, a processing gas is introduced into the processing chamber while the processing chamber is heated, and a thin film forming process is performed on the substrates.

[0003] Patent Document 1 describes a technique in which a gas distribution adjustment member having projections and depressions is provided above and below a placement area of ​​a plurality of substrates to be processed held by a substrate holder, and describes the use of two gas distribution adjustment members having different surface areas.

[0004] Patent Document 2 describes that a dummy wafer having the same surface area as that of a product wafer is used when a gate oxide film is deposited in a trench.

[0005] Patent document 3 discloses a vertical substrate processing device, which uses a gas distribution adjustment mechanism that increases the surface area of ​​the upper and lower peripheries of a substrate holder to make the consumption of processing gas consistent with the central part of the substrate holder in the vertical direction, thereby improving the uniformity of film thickness between substrates. As the gas distribution adjustment mechanism, the following examples are disclosed: (1) arranging a pattern dummy portion with a pattern magnification higher than that of a product substrate at the upper and lower parts of the substrate holder; (2) forming concavities and convexities in the upper and lower areas of the inner surface of a reaction tube by sandblasting; (3) forming concavities and convexities on the top plate and bottom plate of a substrate holder by sandblasting.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2017-22233

[0009] Patent Document 2: Japanese Patent Application Publication No. 2008-47785

[0010] Patent Document 3: Japanese Patent Application Publication No. 2015-173154 Summary of the invention

[0011] However, in the configurations described in Patent Documents 1 to 3, when a wafer with a very large processing surface area is processed, the uniformity of film thickness among multiple wafers may deteriorate. In particular, the situation where the uniformity deteriorates sharply at the upper and lower ends of the wafer arrangement area is called a loading effect. If this occurs, the number of wafers taken out as products decreases, and productivity decreases.

[0012] According to the present disclosure, a technology is provided that can alleviate the unevenness (loading effect) between the surfaces of a plurality of wafers when a plurality of wafers with large surface areas are processed side by side, thereby improving the processing yield and maintaining the productivity.

[0013] One scheme of the present disclosure provides a technology for constituting a substrate processing device, the substrate processing device comprising: a substrate holder, which holds a plurality of substrates arranged at a prescribed interval; a reaction tube for accommodating the substrate holder, the reaction tube having a top plate with an upper end closed and an opening at the bottom for allowing the substrate holder to enter and exit; a furnace body, which surrounds the top and sides of the reaction tube; a cover, which directly or indirectly holds the substrate holder and seals the opening; and a gas supply mechanism, which provides a gas flow parallel to the surface of the surface side of each of the plurality of substrates held on the substrate holder in the reaction tube, the substrate holder holding a product substrate or a monitoring substrate on which an integrated circuit pattern is formed and a dummy substrate on which a Si spraying layer is formed, wherein the dummy substrate is located on both sides of the product substrate or the monitoring substrate.

[0014] Effects of the Invention

[0015] According to the present disclosure, it is possible to alleviate the surface non-uniformity (loading effect) when processing a wafer having a large surface area, stably increase the number of wafers taken out as products compared to the related art, and maintain high productivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a longitudinal cross-sectional view showing a schematic structure of a vertical substrate processing apparatus according to Example 1 of the present disclosure.

[0017] Figure 2 This is a longitudinal cross-sectional view showing a schematic structure of a cleaning unit of a vertical substrate processing apparatus according to the first embodiment of the present disclosure.

[0018] Figure 3 It is a transverse cross-sectional view showing a schematic structure of a transfer chamber of a vertical substrate processing apparatus according to Example 1 of the present disclosure.

[0019] Figure 4 This is a longitudinal cross-sectional view showing a schematic structure of a processing furnace and a reaction tube of a vertical substrate processing apparatus according to Example 1 of the present disclosure.

[0020] Figure 5This is a block diagram showing the configuration of a controller of the vertical substrate processing apparatus according to the first embodiment of the present disclosure.

[0021] Figure 6 This is a graph showing the analysis results of the radical distribution between the surfaces of stacked wafers in the case of conventionally processing large surface area wafers.

[0022] Figure 7 This is a graph showing the cumulative pore volume distribution of the film of the Si dummy wafer in the vertical substrate processing apparatus according to Example 1 of the present disclosure.

[0023] Figure 8 This is a graph showing the analysis result of the radical distribution between the surfaces of stacked wafers in the vertical substrate processing apparatus according to Example 1 of the present disclosure.

[0024] Fig. 9 This is a flowchart showing a sequence example of a film forming process for forming a film on a batch of wafers using the vertical substrate processing apparatus according to the first embodiment of the present disclosure.

[0025] Fig.10 The figures are of a Si sputtering dummy wafer processed by the vertical substrate processing apparatus according to Example 1 of the present disclosure, wherein (a) is a top view and (b) is a front cross-sectional view.

[0026] Fig.11 This is a perspective view showing a tray in a state where a plurality of Si sputtering wafers having a smaller diameter than that of a dummy wafer are mounted on the tray in a vertical substrate processing apparatus according to a second embodiment of the present disclosure. DETAILED DESCRIPTION

[0027] The present disclosure relates to a substrate processing device, characterized in that when processing a large-consumption pattern wafer, Si spraying treatment is performed on upper and lower dummy wafers. As a result, the surface area of ​​the dummy wafer can be increased by tens to hundreds of times. In addition, by changing the spraying film thickness in the Si spraying treatment, the surface area of ​​the dummy wafer can be adjusted so that the surface area of ​​the dummy wafer is greater than or equal to the surface area of ​​the product wafer to be processed.

[0028] Therefore, the substrate processing apparatus disclosed in the present invention can be flexibly applied to processes with different film types and development stages. In addition, the load effect caused by the consumption difference between the pattern wafer and the dummy wafer can be alleviated, thereby improving the inter-surface uniformity.

[0029] In addition, the substrate processing device disclosed in the present invention is characterized in that a plurality of small-diameter wafers after Si spraying are mounted on a tray, and the sprayed film thickness is kept constant while changing the number of Si sprayed wafers mounted, thereby adjusting the surface area of ​​the tray.

[0030] According to the present disclosure, a technology is provided that can alleviate the unevenness (loading effect) between the surfaces of a plurality of wafers when a plurality of wafers with large surface areas are processed side by side, thereby improving the processing yield and maintaining the productivity.

[0031] The following is an explanation of the implementation of the present disclosure using the accompanying drawings. In addition, the present disclosure is not limited to the embodiments described below, and includes a variety of modified examples. The embodiments described below are detailed descriptions made to clearly and easily explain the present disclosure, and the present disclosure is not limited to having all the described structures. In addition, a part of the structure of a certain embodiment can be replaced by other embodiments, and other embodiments can be added to the structure of a certain embodiment. In addition, other structures can be added, deleted, or replaced with respect to a part of the structure of each embodiment.

[0032] Example 1

[0033] use Figures 1 to 10 , describing the substrate processing apparatus and the method for manufacturing a semiconductor device of Example 1.

[0034] <Overall Structure of Substrate Processing Equipment>

[0035] In this embodiment, the substrate processing apparatus is configured as a vertical substrate processing apparatus (hereinafter referred to as a processing apparatus) 1 that performs a substrate processing process such as heat treatment as one of the manufacturing processes in the manufacturing method of a semiconductor device (device). Figure 1 As shown, the processing apparatus 1 includes a transfer chamber 124 and a processing furnace 2 disposed above the transfer chamber 124 .

[0036] The processing furnace 2 includes: a cylindrical reaction tube 4 extending in the vertical direction; and a heater 3 of a first heating unit (furnace body) provided on the outer periphery of the reaction tube 4 (see Figure 4 The reaction tube 4 is made of, for example, quartz or SiC. A processing chamber 6 for processing a wafer 7 as a substrate is formed inside the reaction tube 4.

[0037] The cylindrical manifold 5 is connected to the lower end opening of the reaction tube 4 by means of a sealing member such as an O-ring, and supports the lower end of the reaction tube 4. The manifold 5 is formed of a metal such as stainless steel. The lower end opening of the manifold 5 is opened and closed by a disc-shaped gate or cover 122 not shown. The cover 122 is formed of a metal in a disc shape, for example. A sealing member such as an O-ring is provided on the upper surface of the gate and cover 122 not shown, thereby hermetically sealing the inside of the reaction tube 4 from the outside air.

[0038] A heat insulating portion 144 is placed on the cover 122. The heat insulating portion 144 is formed of, for example, quartz. The heat insulating portion 144 has a cover heater 144a as a second heating unit (heating unit) on the surface or inside. The cover heater 144a is configured to heat a substrate held below the processing chamber 6 and below a wafer boat 126 to be described later. A wafer boat 126 as a substrate holding portion is provided above the heat insulating portion 144. The wafer boat 126 is composed of a top plate 126a, a bottom plate 126c, and a plurality of columns 126b provided between the top plate 126a and the bottom plate 126c. The wafer boat 126 supports a plurality of wafers 7, for example, 25 to 150 wafers, in multiple layers in the vertical direction by placing the wafers 7 on multi-layer grooves formed on the columns 126b. The wafer boat 126 is formed of, for example, quartz or SiC. The substrate holding body 127 is composed of the heat insulating portion 144 and the wafer boat 126. During substrate processing, the substrate holder 127 is housed in the processing chamber 6 .

[0039] The heat insulating part 144 is connected to a rotating shaft 128 that penetrates the cover 122. The rotating shaft 128 is connected to a rotating mechanism 130 provided below the cover 122. By rotating the rotating shaft 128 by the rotating mechanism 130, the heat insulating part 144 and the wafer boat 126 can be rotated.

[0040] The transfer chamber 124 includes a substrate transfer machine 156, a wafer boat 126, and a wafer boat elevator 132 as a lifting mechanism. The substrate transfer machine 156 includes an arm (tweezers) 156a that can take out, for example, five wafers 7. The substrate transfer machine 156 is configured to transfer the wafers 7 between the wafer box 160 placed at the position of the wafer box opener 158 and the wafer boat 126 by rotating the arm 156a up and down using a drive mechanism (not shown). The wafer boat elevator 132 moves the wafer boat 126 in and out of the reaction tube 4 by lifting the cover 122 up and down. The configuration of the transfer chamber 124 will be described in detail later.

[0041] The processing apparatus 1 is provided with a gas supply mechanism 134 for supplying gas used for substrate processing into the processing chamber 6. The gas supplied by the gas supply mechanism 134 can be appropriately changed according to the type of film to be formed. The gas supply mechanism 134 includes a raw material gas supply unit (raw material gas supply system), a reaction gas supply unit (reaction gas supply system) and an inert gas supply unit (inert gas supply system).

[0042] The raw material gas supply system includes a gas supply pipe 9, on which a mass flow controller (MFC) 10 as a flow controller (flow control unit) and a valve 11 as an opening and closing valve are provided in order from the upstream direction. The gas supply pipe 9 is connected to a nozzle 8 that penetrates the side wall of the manifold 5. The nozzle 8 is vertically arranged in the reaction tube 4 in the up-down direction, and is formed with a plurality of supply holes that open toward the wafer 7 held in the wafer boat 126. The raw material gas is supplied to the wafer 7 through the supply holes of the nozzle 8.

[0043] Next, using the same configuration, the reactive gas is supplied from the reactive gas supply system via the gas supply pipe 9, MFC 10, valve 11 and nozzle 8 to the wafer 7. The reactive gas is supplied from the inert gas supply system via the gas supply pipe 12, MFC 13, valve 14 and nozzle 8 to the wafer 7.

[0044] An exhaust pipe 15 is installed on the manifold 5. A vacuum pump 18 as a vacuum exhaust device is connected to the exhaust pipe 15 via a pressure sensor 16 as a pressure detector (pressure detection unit) for detecting the pressure in the processing chamber 6 and an APC (Auto Pressure Controller) valve 17 as a pressure regulator (pressure regulation unit). With such a configuration, the pressure in the processing chamber 6 can be set to a processing pressure corresponding to the process.

[0045] Next, use Figures 1 to 3 The structure of the transfer chamber 124 of this embodiment will be described.

[0046] like Figure 2 , 3 As shown, the transfer chamber 124 is formed into a planar polygonal shape by a top plate, a bottom plate and a surrounding side wall 120, for example, a planar quadrilateral (rectangular parallelepiped). A cleaning unit 162 serving as a first air supply unit (first gas supply unit) is provided on one side of the transfer chamber 124. Gas serving as clean air (clean ambient gas) is supplied from the cleaning unit 162 to the transfer chamber 124. In addition, a circulation passage 174 for circulating the gas is formed in the space surrounding the transfer chamber 124. The gas supplied to the transfer chamber 124 is exhausted from the side exhaust portion 172a and is supplied again from the cleaning unit 162 to the transfer chamber 124 via the circulation passage 174. A radiator not shown is provided in the middle of the circulation passage 174, and the gas is cooled by passing through the radiator.

[0047] The cleaning unit 162 is arranged in a manner that an upper cleaning unit 162a and a lower cleaning unit 162b are adjacent to each other in the vertical direction. The upper cleaning unit 162a is configured to supply gas into the transfer chamber 124, especially the wafer boat 126. The lower cleaning unit 162b is configured to supply gas into the transfer chamber 124, especially the heat insulating portion 144. Hereinafter, the case of referring to the cleaning unit 162 includes the case of indicating the upper cleaning unit 162a, the case of indicating the lower cleaning unit 162b, or the case of indicating both of the above.

[0048] The cleaning unit 162 has a fan 164 as an air supply unit, a buffer zone 166 as a buffer chamber, a filter unit 168, and a gas supply port 170 in order from the upstream side. The buffer zone 166 is a diffusion space for blowing gas uniformly from the entire surface of the gas supply port 170. The filter unit 168 is configured to remove particles contained in the gas. The upper cleaning unit 162a and the lower cleaning unit 162b are both provided with a fan 164, a buffer zone 166, a filter unit 168, and a gas supply port 170.

[0049] A side exhaust portion 172a and a wafer boat elevator 132 are provided on a side surface opposite to the cleaning unit 162. The gas supplied from the upper cleaning unit 162a to the transfer chamber 124 is mainly exhausted from the side exhaust portion 172a, and is supplied from the cleaning unit 162 to the transfer chamber 124 again through the circulation path 174. Thus, a gas flow (side flow) in a horizontal direction (a direction parallel to the wafer 7) is formed in the upper region (wafer 7 region) in the transfer chamber 124.

[0050] like Figure 3 As shown, a pair of bottom exhaust parts 172b are provided on the bottom plate surface of the transfer chamber 124 across the wafer boat 126. The bottom exhaust part 172b is formed in a rectangular shape along one side of the transfer chamber 124. The gas supplied from the lower cleaning unit 162b to the transfer chamber 124 is mainly exhausted from the bottom exhaust part 172b, and is supplied from the cleaning unit 162 to the transfer chamber 124 again through the circulation passage 174. As a result, a vertical gas flow (downward flow) is formed in the lower area (heat insulation part 144 area) in the transfer chamber 124.

[0051] like Figure 2 and Figure 3As shown, a gas pipe 176 as a second air supply unit (second gas supply unit) is provided on a side other than the side opposite to the side where the cleaning unit 162 is provided. For example, the gas pipe 176 is provided on a side adjacent to the side where the cleaning unit 162 is provided. In the present embodiment, the gas pipe 176 is provided at a position opposite to the substrate transfer machine 156 in the transfer chamber 124 across the wafer boat 126 (a position between the side of the transfer chamber 124 and the wafer boat 126). The gas pipe 176 is configured to supply gas toward an area below the bottommost substrate placed on the wafer boat 126. Preferably, the gas pipe 176 is configured to supply gas toward an area between the bottommost substrate of the wafer boat 126 and the heat insulating portion 144.

[0052] like Figure 2 As shown, the gas pipe 176 is horizontally arranged in the transfer chamber 124, and is formed with a blow outlet 176a that opens toward the substrate holder 127. Gas is supplied to the transfer chamber 124, especially the substrate holder 127, through the blow outlet 176a of the gas pipe 176. As the gas, for example, an inert gas can be cited. The gas pipe 176 is connected to a transfer chamber gas supply mechanism 178 that supplies gas to the transfer chamber 124. The transfer chamber gas supply mechanism 178 includes a gas supply pipe 136c, and an MFC 138c and a valve 140c are sequentially provided on the gas supply pipe 136c from the upstream direction.

[0053] The gas pipe 176 is arranged so that the height position of the blowing port 176a is between the substrate at the bottom of the wafer boat 126 and the heat insulating portion 144. Figure 3 As shown, the blowing outlet 176a is formed by a plurality of openings. When the blowing outlet 176a is formed by an even number of openings, the same number of openings are formed on the left and right of the center line of the chip 7. When the blowing outlet 176b is formed by an odd number of openings, one opening is formed at the center line of the chip 7, and the same number of openings are formed on the left and right of the one opening. In the present embodiment, the blowing outlet 176a is formed with 5 openings, for example, with a diameter of less than 1 mm. When viewed from above, the blowing outlet 176a is formed in an area within the diameter range of the chip 7. In other words, it is formed in such a way that the opening (formation) range of the blowing outlet 176a falls within the diameter range of the chip 7. With such a configuration, the direction of the mainstream of the gas supplied from the blowing outlet 176a can be set to a horizontal direction. In this way, a gas barrier (gas curtain) can be formed in the space between the bottom substrate of the crystal boat 126 and the insulation part 144, and the gas curtain can be used to separate the upper ambient gas on the crystal boat 126 side (the ambient gas in the chip 7 area) from the lower ambient gas on the insulation part 144 side (the ambient gas in the insulation part 144 area).

[0054] like Figure 1As shown, the controller 29 for controlling the rotating mechanism 130, the wafer boat elevator 132, the substrate transfer machine 156, the gas supply mechanism 134 (MFC10, 13 and valves 11, 14), the APC valve 17, the cleaning unit 162, and the transfer chamber gas supply mechanism 178 (MFC138c and valve 140c) are connected. The controller 29 is composed of, for example, a microprocessor (computer) having a CPU, and is configured to control the operation of the processing device 1.

[0055] Treatment furnace 2 Figure 4 As shown, in order to heat the barrel of the reaction tube 4 described later, a heater 3 as a main heater is arranged in the up-down direction. The heater 3 is cylindrical and is arranged in the up-down direction around the barrel (the side in this embodiment) of the reaction tube 4 described later. The heater 3 is composed of a plurality of heater units divided into a plurality in the up-down direction. In this embodiment, the heater 3 includes an upper heater 3A, a central upper heater 3B, a central heater 3C, a central lower heater 3D, and a lower heater 3E from top to bottom. The heater 3 is supported by a heater base (not shown) as a retaining plate, so as to be vertically mounted on the installation base plate of the substrate processing device 1.

[0056] The upper heater 3A, the central upper heater 3B, the central heater 3C, the central lower heater 3D, and the lower heater 3E are electrically connected to the power conditioner 70, respectively. The power conditioner 70 is electrically connected to the controller 29. The controller 29 has a function as a temperature controller that controls the amount of power supplied to each heater using the power conditioner 70. By controlling the amount of power supplied to the power conditioner 70 using the controller 29, the temperature of each of the upper heater 3A, the central upper heater 3B, the central heater 3C, the central lower heater 3D, and the lower heater 3E is controlled. The heater 3 also functions as an activation mechanism (excitation unit) that activates (excites) the gas using heat as described later.

[0057] A reaction tube 4 constituting a reaction vessel (processing vessel) is arranged inside the heater 3. The reaction tube 4 is formed of a heat-resistant material such as quartz (SiO2) or silicon carbide (SiC), and is formed into a cylindrical shape with a closed upper end and an open lower end. The reaction tube 4 is a double tube structure having an outer tube 4A and an inner tube 4B that are mutually connected at a flange portion 4C at the lower end. In other words, the outer tube 4A and the inner tube 4B are respectively formed into a cylindrical shape, and the inner tube 4B is arranged inside the outer tube 4A. A top plate portion 72 that closes the upper end is provided on the outer tube 4A. In addition, a top plate 74 that closes the upper end is provided on the inner tube 4B, and the lower end of the inner tube 4B is open. The top plate 74 is formed into a shape with a flat inner surface. The outer tube 4A is arranged in a manner that surrounds the upper and side of the inner tube 4B.

[0058] A flange portion 4C is provided at the lower portion of the outer tube 4A. The flange portion 4C has an outer diameter larger than that of the outer tube 4A and protrudes outward. An exhaust port 4D communicating with the inner portion of the outer tube 4A is provided near the lower end of the reaction tube 4. The reaction tube 4 including the above parts is integrally formed of a single material. The outer tube 4A is formed to have a relatively thick wall thickness so as to be able to withstand the pressure difference when the inner side is made into a vacuum.

[0059] The processing furnace 2 includes a side heat insulator 76 and an upper heat insulator 78 disposed on the upper side of the heater 3 so as to cover the oblique upper side and the upper side of the ceiling plate portion 72 of the outer tube 4A. For example, the cylindrical side heat insulator 76 is provided on the upper part of the heater 3, and the upper heat insulator 78 is fixed to the side heat insulator 76 in a state of being bridged on the side heat insulator 76. Thus, the processing furnace 2 is configured to surround the upper and side sides of the reaction tube 4.

[0060] A top plate heater 80 is provided above the top plate 72 of the outer tube 4A and on the lower wall of the upper heat insulator 78 to heat the top plate 72 of the outer tube 4A and the top plate 74 of the inner tube 4B of the reaction tube 4. In the present embodiment, the top plate heater 80 is provided outside the outer tube 4A. The top plate heater 80 is electrically connected to the power conditioner 70. The controller 29 controls the amount of power supplied to the top plate heater 80 by using the power conditioner 70. Thus, the temperature of the top plate heater 80 is controlled independently of the temperature of the upper heater 3A, the central upper heater 3B, the central heater 3C, the central lower heater 3D, and the lower heater 3E.

[0061] The manifold 5 is cylindrical or truncated cone-shaped and is made of metal or quartz, and is provided so as to support the lower end of the reaction tube 4. The inner diameter of the manifold 5 is formed to be larger than the inner diameter of the reaction tube 4 (the inner diameter of the flange portion 4C). Thus, an annular space described later is formed between the lower end of the reaction tube 4 (the flange portion 4C) and the sealing cover 19 described later. This space or its peripheral components are collectively referred to as a furnace port.

[0062] The inner tube 4B has a main exhaust port 4E on its side and further inside the reaction tube than the exhaust port 4D, which communicates the inside and the outside, and a supply slit 4F at a position opposite to the main exhaust port 4E. The main exhaust port 4E may be a single longitudinal opening opened to the region where the wafer 7 as the substrate is arranged, or may be a plurality of slits extending in the circumferential direction (see FIG. Figure 1 The supply slits 4F are slits extending in the circumferential direction, and a plurality of supply slits 4F are arranged side by side in the vertical direction in a manner corresponding to the respective wafers 7 .

[0063] In the exhaust space S between the outer tube 4A and the inner tube 4B, one or more nozzles 8 for supplying a processing gas such as a raw material gas are provided corresponding to the position of the supply slit 4F. A gas supply pipe 9 for supplying a processing gas (raw material gas) passes through the manifold 5 and is connected to each of the nozzles 8. The processing gas discharged from the nozzle 8 flows parallel to the surface side of the wafer 7 in the gap between each wafer 7 (in the case of the uppermost wafer, the gap with the wafer boat top plate 21B) in a manner that crosses each wafer 7 from end to end.

[0064] On the flow path of each gas supply pipe 9, a mass flow controller (MFC) 10 as a flow controller and a valve 11 as an opening and closing valve are provided in order from the upstream direction. On the downstream side of the valve 11, a gas supply pipe 12 for supplying an inert gas is connected to the gas supply pipe 9. On the gas supply pipe 12, an MFC 13 and a valve 14 are provided in order from the upstream direction. The gas supply pipe 9, the MFC 10, and the valve 11 mainly constitute a gas supply mechanism as a processing gas supply system.

[0065] The nozzle 8 is disposed in the gas supply space S1 in a manner rising from the lower part of the reaction tube 4. One or more nozzle holes 8H for supplying gas are provided on the side and upper end of the nozzle 8. The plurality of nozzle holes 8H are opened in a manner corresponding to the openings of the respective supply slits 4F and toward the center of the reaction tube 4, so that the gas can be sprayed toward the wafer 7 through the inner tube 4B.

[0066] An exhaust pipe 15 for exhausting the atmosphere in the processing chamber 6 is connected to the exhaust port 4D. A vacuum pump 18 as a vacuum exhaust device is connected to the exhaust pipe 15 via a pressure sensor 16 as a pressure detector (pressure gauge) for detecting the pressure in the processing chamber 6 and an APC (Auto Pressure Controller) valve 17 as a pressure regulator (pressure regulating unit). The APC valve 17 can perform vacuum exhaust and stop vacuum exhaust in the processing chamber 6 by opening and closing the valve while the vacuum pump 18 is in operation. In addition, the APC valve 17 is configured to adjust the valve opening based on the pressure information detected by the pressure sensor 16 while the vacuum pump 18 is in operation, thereby adjusting the pressure in the processing chamber 6. The exhaust system is mainly composed of the exhaust pipe 15, the APC valve 17, and the pressure sensor 16. It is also conceivable to include the vacuum pump 18 in the exhaust system.

[0067] A sealing cap 19 is provided below the manifold 5 as a cover that can airtightly close the opening 90 at the lower end of the manifold 5. That is, the sealing cap 19 has a function as a cover (gate) that closes the outer tube 4A of the reaction tube 4. The sealing cap 19 is formed of a metal such as stainless steel or a nickel-based alloy and is formed in a disc shape. An O-ring 19A as a sealing member that abuts against the lower end of the manifold 5 is provided on the upper surface of the sealing cap 19.

[0068] In addition, on the upper surface of the sealing cover 19, a cover plate 20 for protecting the sealing cover 19 is provided for the portion of the manifold 5 that is closer to the inner side than the inner circumference of the lower end. The cover plate 20 is formed of a heat-resistant and corrosion-resistant material such as quartz, sapphire, or SiC, and is formed in the shape of a circular plate. The cover plate 20 does not require mechanical strength, so it can be formed with a thin wall. The cover plate 20 is not limited to a component prepared separately from the sealing cover 19, but may also be a thin film or layer of a nitride or the like coated on the inner surface of the sealing cover 19 or obtained by modifying the inner surface. In addition, the cover plate 20 may also have a wall that rises from the edge of the circumference along the inner surface of the manifold 5.

[0069] A wafer boat 21 (which is the same as the wafer boat 21) serving as a substrate holder is accommodated in the inner tube 4B of the reaction tube 4. Figure 1 The wafer boat 21 includes a plurality of upright pillars 21A and a circular wafer boat top plate 21B that fixes the upper ends of the plurality of pillars 21A to each other. Here, the wafer boat top plate 21B is an example of a top plate. In addition, in the present embodiment, the wafer boat 21 has an annular bottom plate 21C at the lower ends of the plurality of pillars 21A, but a circular bottom plate may be provided instead.

[0070] The wafer boat 21 supports, for example, 25 to 200 wafers 7 arranged in a horizontal posture and in a vertical direction in multiple layers with their centers aligned. Therefore, the wafers 7 are arranged at regular intervals. The wafer boat 21 is made of a heat-resistant material such as quartz or SiC.

[0071] It is preferred that the inner tube 4B of the reaction tube 4 has a minimum inner diameter that enables the wafer boat 21 to be safely carried in and out. In the present embodiment, for example, the diameter of the wafer boat top plate 21B is set to be 90% or more and 98% or less of the inner diameter of the inner tube 4B, or the interval between the wafers 7 held in the wafer boat 21 is set to be, for example, 6 mm or more and 16 mm or less. Here, it is preferred that the diameter of the wafer boat top plate 21B is 90% or more and 98% or less of the inner diameter of the inner tube 4B, more preferably 92% or more and 97% or less, and further preferably 94% or more and 96% or less.

[0072] By setting the diameter of the wafer boat top plate 21B to be 90% or more of the inner diameter of the inner tube 4B, the gap between the edge of the wafer boat top plate 21B and the inner tube 4B can be reduced, and the gas movement caused by diffusion (especially the flow of the excess radicals described later from the wafer boat top plate 21B to the wafer 7 side) can be suppressed. In addition, by setting the diameter of the wafer boat top plate 21B to be 98% or less of the inner diameter of the inner tube 4B, the wafer boat 21 can be safely moved in and out of the inner tube 4B.

[0073] In addition, the interval between the wafers 7 is preferably 6 mm or more and 16 mm or less, more preferably 7 mm or more and 14 mm or less, and further preferably 8 mm or more and 12 mm or less. By setting the interval between the wafers 7 to be 6 mm or more, the gas can flow smoothly between the adjacent wafers 7. In addition, by setting the interval between the wafers 7 to be 16 mm or less, more wafers 7 can be processed.

[0074] In addition, in this embodiment, the volume of the upper end space separated from other parts by the wafer boat top plate 21B and sandwiched by the top plate 74 and the wafer boat top plate 21B is set to, for example, be greater than 1 times and less than 3 times the volume of the space sandwiched by adjacent (neighboring) chips 7 held in the wafer boat 21.

[0075] Here, the volume of the upper end space sandwiched by the top plate 74 and the top plate 21B of the wafer boat is preferably 1 or more and 3 or less than the volume of the space sandwiched by the adjacent wafers 7, more preferably 1 or more and 2.5 or less, and further preferably 1 or more and 2 or less. That is, the volume of the upper end space sandwiched by the top plate 74 and the top plate 21B of the wafer boat is as small as possible. However, it is required that the gas flows smoothly to the main exhaust port 4E.

[0076] The absolute amount of excess gas is reduced by setting the volume of the upper end space sandwiched by the top plate 74 and the wafer boat top plate 21B to be less than three times the volume of the space sandwiched by the wafers 7 adjacent to each other held in the wafer boat 21. In addition, by setting the volume of the upper end space sandwiched by the top plate 74 and the wafer boat top plate 21B to be more than one times the volume of the space sandwiched by the wafers 7 adjacent to each other held in the wafer boat 21, the gas is allowed to flow smoothly toward the main exhaust port 4E.

[0077] A heat insulation assembly (heat insulation structure) 22 described later is arranged at the lower part of the wafer boat 21. The heat insulation assembly 22 has a structure that reduces heat conduction or heat transfer in the up and down directions, and usually has a cavity inside. The inside can be purged by an axial purge gas. In the reaction tube 4, the upper part where the wafer boat 21 is arranged is called the processing area A of the wafer 7, and the lower part where the heat insulation assembly 22 is arranged is called the heat insulation area B.

[0078] A rotating mechanism 23 (which rotates the wafer boat 21 ) is provided on the side of the sealing cover 19 opposite to the processing chamber 6 . Figure 1 The rotating mechanism 23 corresponds to the rotating mechanism 130. A gas supply pipe 24 for shaft purge gas is connected to the rotating mechanism 23. On the gas supply pipe 24, MFC 25 and valve 26 are provided in order from the upstream direction. One purpose of the purge gas is to protect the interior of the rotating mechanism 23 (for example, the bearings) from the corrosive gas used in the processing chamber 6. The purge gas is discharged from the rotating mechanism 23 along the rotating shaft 66 (corresponding to the rotating mechanism 130). Figure 1 corresponding to the rotating shaft 128) and is guided into the insulation assembly 22.

[0079] Crystal boat lift 27 (with Figure 1 132 of the embodiment) is vertically arranged at the lower part of the outside of the reaction tube 4, and acts as a lifting mechanism (transportation mechanism) for lifting and lowering the sealing cover 19. Thus, the wafer boat 21 and the wafer 7 supported by the sealing cover 19 are carried in and out of the processing chamber 6. In addition, a gate plate (not shown) for closing the lower end opening of the reaction tube 4 may be provided instead of the sealing cover 19 while the sealing cover 19 is lowered to the lowest position.

[0080] A temperature sensor (temperature detector) 28 as a processing space temperature sensor for detecting the temperature inside the reaction tube 4 is provided on the outer wall of the side of the outer tube 4A or the inner side of the inner tube 4B. The temperature sensor 28 is composed of, for example, a plurality of thermocouples arranged side by side up and down. Although not shown in the figure, the temperature sensor 28 is electrically connected to the controller 29. The controller 29 uses the power regulator 70 to adjust the amount of power supplied to the upper heater 3A, the central upper heater 3B, the central heater 3C, the central lower heater 3D, and the lower heater 3E, respectively, based on the temperature information detected by the temperature sensor 28, so that the temperature in the processing chamber 6 becomes the desired temperature distribution.

[0081] In addition, a temperature sensor (temperature detector) 82 as an upper space temperature sensor for detecting the temperature of the upper part of the reaction tube 4 is provided on the outer wall of the top plate portion 72 of the outer tube 4A. The temperature sensor 82 is composed of, for example, a plurality of thermocouples arranged side by side in the horizontal direction. Although not shown in the figure, the temperature sensor 82 is electrically connected to the controller 29. The controller 29 adjusts the amount of power supplied to the top plate heater 80 using the power regulator 70 based on the temperature information detected by the temperature sensor 82, so that the temperature of the upper part of the processing chamber 6 becomes a desired temperature distribution.

[0082] like Figure 1 As shown, a space particle measuring port (hereinafter referred to as a particle measuring port) 400 as a measuring port is provided in the transfer chamber 124. The particle measuring port 400 captures particles for measuring particles, and the particle measuring port 400 is connected to a space particle counter (hereinafter referred to as a particle counter) 402 as a counter for measuring particles in a tube 401. The particle measuring device as a measuring device for measuring particles floating in space is composed of the particle measuring port 400, the tube 401, and the particle counter 402. In addition, the particle counter 402 is connected to the controller 29 described later.

[0083] The particle counter 402 has a pump inside, which sucks the surrounding environmental gas from the particle measuring port 400. When the wafer boat 21 starts to descend from the processing furnace 2, that is, when the sealing cover 19 separates from the lower end of the processing furnace 2 and the furnace port 61 is opened, the controller 29 sends a "measurement start" signal to the particle counter 402. When the particle counter 402 receives the "measurement start" signal from the controller 29, it resets the number of particles stored before the start of the measurement to 0 (zero), detects the number of particles contained in the sucked-in environmental gas, counts the number cumulatively, and records it as the cumulative number of particles. In addition, the controller 29 can also display the number of particles sent from the particle counter 402 on the input and output device 222 (refer to Figure 5 ) on the display screen (hereinafter referred to as the screen).

[0084] The particle counter 402 is used to measure the particle size downstream of the cooling gas during the supply process. When the particle count measured by the particle counter 402 from the cooling gas passing through the dummy wafer stored in the wafer boat 21 and having the thermal spray coating formed thereon exceeds a predetermined value, the controller 29 performs a predetermined recording action, a reporting action, or an action of removing the corresponding dummy wafer from the wafer boat 21. In other words, the surface shape of the thermal spray coating is very random, so it is impossible to deny the possibility that the SiN film formed thereon has a specific local shape that is easy to peel off. Therefore, it is effective to actually perform film formation, find out the dummy wafer that is easy to generate particles, and remove it.

[0085] The controller 29 is as follows Figure 5 As shown, with MFC10, 13, 25, 138c, valves 11, 14, 26, 140c, pressure sensor 16, APC valve 17, vacuum pump 18, rotating mechanism 23, 130, wafer boat elevator 132 (with Figure 4 The controller 29 is electrically connected to the components such as the wafer boat elevator 27 and automatically controls them. In addition, the controller 29 is connected to the heaters 3 (upper heater 3A, central upper heater 3B, central heater 3C, central lower heater 3D, lower heater 3E), the top plate heater 80, the cover heater 34 ( Figure 1 The controller 29 is electrically connected to the heaters 3 (upper heater 3A, central upper heater 3B, central heater 3C, central lower heater 3D, lower heater 3E), the top plate heater 80, and the cover heater 34 through the power conditioner 70, although not shown in the figure.

[0086] The controller 29 is configured as a computer including a CPU (Central Processing Unit) 212, a RAM (Random Access Memory) 214, a storage device 216, and an I / O port 218. The RAM 214, the storage device 216, and the I / O port 218 are configured to be able to exchange data with the CPU 212 via an internal bus 220. The I / O port 218 is connected to each of the above-mentioned components. An input / output device 222 such as a touch panel and an external storage device 224 are connected to the controller 29.

[0087] The storage device 216 is composed of, for example, a flash memory, a HDD (Hard Disk Drive), etc. A control program for controlling the operation of the substrate processing apparatus 1, and a program (process recipe, cleaning recipe, etc.) for making each component of the substrate processing apparatus 1 perform film forming processing according to processing conditions are stored in the storage device 216 in a readable manner. The RAM 214 is configured as a memory area (work area) for temporarily holding programs, data, etc. read by the CPU 212.

[0088] The CPU 212 reads the control program from the storage device 216 and executes it, and reads the recipe from the storage device 216 in response to input of an operation command from the input / output device 222 or the like, and controls each component according to the recipe.

[0089] The controller 29 can be configured by installing the above-mentioned program continuously stored in an external storage device (e.g., a semiconductor memory such as a USB memory, a memory card, an optical disk such as a CD, a DVD, or a HDD) 224 into a computer. The storage device 216 and the external storage device 224 are configured as a tangible medium that can be read by a computer. Hereinafter, they are also referred to as recording media. In addition, the provision of the program to the computer can also be performed using a communication mechanism such as the Internet or a dedicated line instead of using the external storage device 224.

[0090] The controller 29 manages the use history of each dummy substrate. That is, for each dummy substrate, the history of being held on the substrate holder and processed together with the product wafer is maintained in the form of a cumulative value of film thickness. And, when the cumulative value exceeds a specified value, a specified recording action, a reporting action, or an action of removing the corresponding dummy wafer from the substrate holder is performed.

[0091] In such a configuration, the results of analyzing the distribution of free radicals between surfaces when a large surface area wafer (a surface area having a concavo-convex integrated circuit pattern formed on the front side, for example, 100 times that of a bare wafer having a flat surface) is processed using a conventional method as wafer 7 are shown in FIG. Figure 6. This is related to the film thickness distribution. In a vertical device, in addition to the wafer 7 (product wafer 610) used as a product, a process of loading several dummy wafers 620 that are not used as products at the upper and lower ends of the wafer boat 126 is usually performed. This is mainly to ensure the uniformity of the temperature of the product wafer 610. In this example, the product wafer 610 is loaded in the slits 8 to 107, and 7 to 8 dummy wafers 620 are loaded at both ends at the same interval as the product wafer 610.

[0092] Known in Figure 6 In the conventional method shown in FIG. 1 , the partial pressure of free radicals increases and the uniformity deteriorates at the upper and lower ends of the product wafer 610 (a wafer having a circuit pattern formed on its surface: hereinafter referred to as a pattern wafer). The reason for this is that the pattern wafer 610 has a large surface area and consumes a lot of free radicals, so the concentration of free radicals in the gas phase becomes low, while on the other hand, the consumption is small on the dummy wafer 620 with a small surface area, so the concentration of free radicals in the gas phase is high.

[0093] Furthermore, in the region where the pattern wafer 610 and the dummy wafer 620 are adjacent to each other and where such an extreme concentration difference is formed, the concentration in the gas phase diffuses, tending to ease the radical concentration difference. Therefore, the concentration at the upper and lower ends of the product wafer 610 inevitably becomes higher (film thickness becomes thicker), and uniformity deteriorates. In this way, a loading effect occurs due to the difference between the dummy wafer 620, which has almost no free radical consumption, and the pattern wafer 610, which has serious consumption (proportional to the surface area).

[0094] As a countermeasure to this, it is considered not to use the existing dummy wafer 620, but to perform Si spraying treatment on the dummy wafer to increase the surface area on the dummy wafer. By making the surface area of ​​the dummy wafer greater than or equal to the pattern wafer, the consumption difference between the two can be eliminated and the load effect can be alleviated. In addition, if, for example, only the surface of the dummy wafer is roughened, the surface area will only become several times that of the bare wafer, and it will not be able to cope with the pattern wafer with a large surface area. In this regard, if the Si spraying treatment of this method is used, the surface area can be increased to tens to hundreds of times that of the bare wafer.

[0095] [Method for fabricating Si dummy wafer by spraying]

[0096] In general, there are many cases where a defective wafer generated in a device manufacturing process is reground to prepare a dummy wafer. Fig.10 ) can also use such a dummy wafer (bare dummy) as a material. The Si spray dummy wafer of this embodiment first forms a Si spray coating 822 on the surface side of the bare dummy 821 as a single crystal Si wafer by Si spraying. Spraying is roughly divided into thermal spraying in which the raw material is melted into droplets (microparticles) and blown, and cold spraying in which solid powder is blown at a critical speed or above, and both can be used.

[0097] At this time, the pores in the Si spray coating 822 of the Si spray dummy wafer 820 become continuous pores, and in order to obtain a large surface area, it is necessary to stably spray under the condition of a moderately high porosity. In this regard, sometimes when spraying at low temperature, it is preferred that the splats after the particles are flattened by the impact of the substrate will not be too close. The porous film formed in this way has many continuous pores opened on the surface, and its surface area is proportional to the film thickness (volume), and this proportional constant is also called specific surface area.

[0098] After using Si spraying to form the Si spray film 822, the Si spraying dummy chip 820 is cleaned (for example, improved RCA cleaning) and dried similarly to the product chip 810 (equivalent to the pattern chip 610), and further inspected for foreign matter (particles) using a chip surface inspection device as needed.

[0099] In addition, in order to reproduce the free radical consumption during film formation on the product wafer 810 as faithfully as possible, it is preferable to make the diameter of the pores in the film of the Si sprayed dummy wafer 820 correspond to the size of the pattern of the product wafer 810 (the diameter of the via hole, the width of the groove). For example, the diameter of the via hole used in 3D NAND is less than 50nm. On the other hand, the diameter of the pores of the sprayed film formed by Si spraying can be controlled to a certain extent by the size of the particles to be sprayed.

[0100] Figure 7 An example of the cumulative pore volume distribution 701 of a preferred Si spray coating 822 formed on a Si spray dummy wafer 820 is shown in FIG. When the scale of the pattern of the product wafer 810 is set to 50 nm, the cumulative pore volume is about 40%. As such, the diameter of the via or the width of the groove of the preferred product wafer 810 falls within the range of pore diameters corresponding to 25% to 75% of the total volume in the cumulative pore volume distribution 701. If the pore diameter corresponding to 75% of the cumulative volume is smaller than the size of the pattern, the pores are too small, which may not only easily cause pore occlusion, but also cause other phenomena such as capillary condensation, and there is a possibility that the product wafer 810 cannot be simulated. On the other hand, if the pore diameter corresponding to 25% of the cumulative volume is larger than the size of the pattern, there is a possibility that the pores are too large and cannot be faithfully simulated.

[0101] Alternatively, the sprayed film produced by Si spraying may be made porous by anodic oxidation in a hydrofluoric acid aqueous solution to form mesopores of the same size as the pattern formed on the product wafer 810. In this case, the surface area S is expressed by the following formula:

[0102] S=S s0 ×t s×(1+S p0 ×t p ),

[0103] Here, t s is the spraying treatment time, S s0 is the surface area formed by spraying per unit time, t s is the anodizing time, S p0 S is the surface area increased by anodization in a short time. s0 and S p0 Gained through experience.

[0104] [Film Forming Simulation]

[0105] The results of the analysis of the free radical distribution between the surfaces of the Si sputtering dummy wafer 820 and the product wafer 810 on which the circuit pattern is formed are shown in FIG. Figure 8 . This calculation was performed with a model that is simpler than the actual device, but it shows that if there is no consumption difference between the Si spray dummy wafer 820 and the product wafer 810, both the upper and lower ends become flat, and the free radical distribution between the surfaces becomes uniform. By suppressing the free radical concentration difference, the loading effect can also be eliminated. Unless it is a CVD with controlled supply rate, the free radical partial pressure is not immediately proportional to the film thickness, but it is preferred that the concentration difference is within, for example, 5%.

[0106] In actual devices, the Si sprayed dummy wafer 820 , which has a surface area slightly larger than that of the product wafer 810 , may have good uniformity due to the presence of high concentrations of free radicals in the space between the wafer boat top plate and the reaction tube.

[0107] Since the Si spray layer of this method is roughly proportional to the surface area, the thicker the spray film is, the larger the surface area is. That is, the surface area can be freely adjusted by changing the spray film thickness. Therefore, even if the pattern formed on the surface side changes due to the film type and development stage, and thus the surface area of ​​the product wafer 810 changes, it can be flexibly dealt with in accordance with it.

[0108] [1 batch (batch) film forming process steps]

[0109] Next, mainly based on Figure 4 The composition shown, using Fig. 9 A sequence example of a process (hereinafter also referred to as a film forming process) of forming a film on one lot of wafers 7 as one process of a process of manufacturing a semiconductor device (device) using the above-described substrate processing apparatus 1 will be described.

[0110] (Wafer filling and wafer boat loading): S901

[0111] In Jingzhou 21( Figure 1On the wafer boat 126, a plurality of product wafers with patterns formed thereon are held at all positions capable of holding the wafers 7. When a plurality of wafers 7 are loaded into the wafer boat 21 (wafer filling), the wafer boat 21 is lifted by the wafer boat elevator 27 ( Figure 1 The wafer boat is moved into the processing chamber 6 by the wafer boat elevator 132 (wafer boat loading). At this time, the sealing cover 19 is in a state where the lower end of the manifold 5 is airtightly closed (sealed) by the O-ring 19A. The valve 26 can be opened from the standby state before wafer filling to supply a small amount of purge gas into the cylinder 39.

[0112] (Pressure regulation): S902

[0113] The vacuum pump 18 performs vacuum exhaust (decompression exhaust) so that the space in the processing chamber 6, that is, the space where the wafer 7 is located, reaches a predetermined pressure (vacuum degree). At this time, the pressure in the processing chamber 6 is measured by the pressure sensor 16, and the APC valve 17 performs feedback control based on the measured pressure information. The purge gas supply to the cylinder portion 39 and the operation of the vacuum pump 18 are maintained at least until the processing of the wafer 7 is completed.

[0114] (Heating process): S903

[0115] After oxygen and the like are fully exhausted from the processing chamber 6, the temperature in the processing chamber 6 starts to rise. Based on the temperature information detected by the temperature sensor 28, the amount of power supplied to the heaters 3 (upper heater 3A, central upper heater 3B, central heater 3C, central lower heater 3D, and lower heater 3E) is feedback-controlled so that the processing chamber 6 has a predetermined temperature distribution suitable for film formation. In addition, based on the temperature information detected by the temperature sensor 82, the amount of power supplied to the top plate heater 80 is feedback-controlled.

[0116] The heating in the processing chamber 6 by the heaters 3 (upper heater 3A, central upper heater 3B, central heater 3C, central lower heater 3D, lower heater 3E), the top plate heater 80 and the cover heater 34 is continuously performed at least until the processing (film formation) of the wafer 7 is completed. The power supply period to the cover heater 34 does not need to coincide with the heating period of the heater 3. It is preferred that the temperature of the cover heater 34 reaches the same temperature as the film formation temperature and the inner surface temperature of the manifold 5 reaches 180° C. or more (e.g., 260° C.) immediately before the film formation starts.

[0117] In addition, the rotation of the wafer boat 21 and the wafer 7 by the rotation mechanism 23 is started. By rotating the wafer boat 21 by the rotation mechanism 23 through the rotation shaft 66, the rotation table 37, and the cylindrical portion 39, the wafer 7 is rotated without rotating the cover heater 34. Thus, the uneven heating is reduced. The rotation of the wafer boat 21 and the wafer 7 by the rotation mechanism 23 is continued at least until the processing of the wafer 7 is completed.

[0118] (Film forming process): S904

[0119] If the temperature in the processing chamber 6 is stabilized at the preset processing temperature in S903, step 1: S9041 to step 4: S9044 are repeatedly executed in the film forming process S904. In addition, the valve 26 may be opened before starting step 1: S9041 to increase the supply of the purge gas (N2).

[0120] [Step 1: Raw material gas supply process]: S9041

[0121] In step 1, HCDS gas is supplied to the wafer 7 in the processing chamber 6. The valve 11 is opened and the valve 14 is opened at the same time, so that the HCDS gas flows into the gas supply pipe 9 and the N2 gas flows into the gas supply pipe 12. The HCDS gas and the N2 gas are flow-regulated by the MFCs 10 and 13, respectively, and are supplied to the processing chamber 6 through the nozzle chamber 42 and exhausted from the exhaust pipe 15. By supplying the HCDS gas to the wafer 7, a silicon (Si)-containing film is formed as a first layer on the outermost surface of the wafer 7.

[0122] [Step 2: Raw gas exhaust process]: S9042

[0123] After the first layer is formed, the valve 11 is closed to stop the supply of HCDS gas. At this time, the APC valve 17 is kept open, and the processing chamber 6 is evacuated by the vacuum pump 18 to exhaust the unreacted HCDS gas remaining in the processing chamber 6 or the HCDS gas used to form the first layer from the processing chamber 6. In addition, the valves 14 and 26 are kept open, and the supplied N2 gas is purged into the gas supply pipe 9, the reaction tube 4, and the furnace port.

[0124] [Step 3: Reaction gas supply process]: S9043

[0125] In step 3, NH3 gas is supplied to the wafer 7 in the processing chamber 6. The opening and closing control of the valves 11 and 14 is performed in the same procedure as the opening and closing control of the valves 11 and 14 in step 1. The NH3 gas and the N2 gas are respectively adjusted in flow rate by the MFCs 10 and 13, supplied to the processing chamber 6 through the nozzle chamber 42, and exhausted from the exhaust pipe 15. The NH3 gas supplied to the wafer 7 reacts with at least a portion of the first layer, i.e., the Si-containing layer, formed on the wafer 7 in step 1. As a result, the first layer is nitrided and changed (modified) into the second layer containing Si and N, i.e., the silicon nitride layer (SiN layer).

[0126] [Step 4: Reaction gas exhaust process]: S9044

[0127] After forming the second layer, the valve 11 is closed to stop the supply of NH3 gas. Then, the unreacted NH3 gas or the NH3 gas used to form the second layer and the reaction byproducts remaining in the processing chamber 6 are exhausted from the processing chamber 6 by the same processing steps as step 1.

[0128] By performing a cycle of performing the above four steps S9041 to S9044 a predetermined number of times (n times) in a non-simultaneous or non-overlapping manner, a SiN film having a predetermined composition and a predetermined film thickness can be formed on the wafer 7 (S9045).

[0129] As the processing conditions of the sequence of steps S9041 to S9044 in the above-mentioned film forming step: S904, for example, the following can be exemplified:

[0130] Processing temperature (wafer temperature): 250~700℃,

[0131] Processing pressure (pressure in the processing chamber): 1~4000Pa,

[0132] HCDS gas supply flow rate: 1~2000sccm,

[0133] NH3 gas supply flow rate: 100~10000sccm,

[0134] N2 gas supply flow rate (nozzle): 100~10000sccm,

[0135] N2 gas supply flow rate (rotation axis): 100~500sccm.

[0136] By setting each processing condition to a value within the respective range, the film forming process can be appropriately performed.

[0137] Thermally decomposable gases such as HCDS may form byproduct films on the surface of metals more easily than on quartz. Surfaces exposed to HCDS (and ammonia) are prone to SiO, SiON, etc., especially at 260°C or below.

[0138] (Purge and atmospheric pressure recovery): S905

[0139] After the film forming process is completed, the valve 14 is opened, N2 gas is supplied from the gas supply pipe 12 into the process chamber 6, and the gas is exhausted from the exhaust pipe 15. Thus, the atmosphere in the process chamber 6 is replaced with an inert gas (inert gas replacement), and the remaining raw materials and by-products are removed (purged) from the process chamber 6. Thereafter, the APC valve 17 is closed, and N2 gas is filled until the pressure in the process chamber 6 becomes normal pressure (atmospheric pressure recovery).

[0140] (Wafer boat unloading and wafer removal): S906

[0141] The sealing cap 19 is lowered by the boat elevator 27 to open the lower end of the manifold 5. The processed wafers 7 are carried out from the lower end of the manifold 5 to the outside of the reaction tube 4 while being supported by the boat 21 (boat unloading). The processed wafers 7 are taken out of the boat 21.

[0142] If the above-mentioned film forming process is performed, a SiN film containing nitrogen can be deposited on the surfaces of the components in the heated reaction tube 4, such as the inner wall of the outer tube 4A, the surface of the nozzle 8, the surface of the inner tube 4B, the surface of the wafer boat 21, etc., to form a thin film. Therefore, when the amount of these deposits, that is, the cumulative film thickness, reaches a predetermined amount (thickness) before the deposits are peeled off and fall off, a cleaning process is performed. The cleaning process is performed by supplying a fluorine-based gas (such as F2 gas) into the reaction tube 4.

[0143] (Cooling process): S907

[0144] When the substrate holder 127 is completely unloaded into the transfer chamber 124, the temperature of the wafer 7 is lowered (cooled) in the transfer chamber 124 until the wafer 7 reaches a predetermined temperature. At this time, the gas is continuously supplied from the cleaning unit 162 at the first flow rate and the first flow rate, and the gas is supplied from the gas pipe 176 to the substrate holder 127 at a third flow rate greater than the first flow rate and a third flow rate less than the first flow rate and greater than the second flow rate. Here, the predetermined temperature is a temperature at which the wafer 7 can be unloaded, and is a temperature lower than the heat resistance temperature of the tweezers 156a or the wafer box 160.

[0145] The third flow rate is, for example, 20 to 40 cm / s, and the third flow rate is, for example, 15 to 70 L / min. When the third flow rate is less than 20 cm / s or the third flow rate is less than 15 L / min, a horizontal gas flow cannot be formed in the area between the wafer 7 at the bottom of the wafer boat 21 and the heat insulating portion 144. When the third flow rate is greater than 40 cm / s or the third flow rate is greater than 70 L / min, the wafer 7 vibrates.

[0146] When the above-mentioned film forming process is performed, a SiN film containing nitrogen can be deposited on the surfaces of the components in the heated reaction tube 4, such as the inner wall of the outer tube 4A, the surface of the nozzle 8, the surface of the inner tube 4B, the surface of the wafer boat 21, etc., to form a thin film. Therefore, when the amount of these deposits, that is, the cumulative film thickness reaches a predetermined amount (thickness) before the deposits are peeled off and fall off, a cleaning process is performed. The cleaning process is performed by supplying a fluorine-based gas (such as F2 gas) into the reaction tube 4.

[0147] When the wafer boat is unloaded, cooling gas is used to cool the wafer 7, the wafer boat 21, and the heat insulation assembly. At this time, if the dummy substrate is exposed to a strong airflow, there is a possibility of film peeling and particle generation due to sudden cooling, so the supply amount of cooling gas can be controlled to reduce the flow rate.

[0148] [For the management of continuous use of Si spray dummy]

[0149] The Si-sprayed dummy wafer 820 has its pores gradually clogged by SiN and other materials after film formation, and its surface area is reduced. In a wafer boat 21 capable of carrying N wafers, when each loading position is set to Slot N, Slot N-1, Slot N-2, etc. from the top, for example, a wafer that has been used less than n times is loaded in Slot N, a wafer that has been used more than n+1 times and less than 2n times is loaded in Slot N-1, a wafer that has been used more than 2n+1 times and less than 3n times is loaded in Slot N-2, and a wafer that has been used more than i×n+1 times and less than (i+1)×n times is loaded in Slot Ni. Here, n is the number of times that it can be repeatedly used while being loaded in one loading position, and i is an index starting from 0.

[0150] If the number of Si molten-spray dummy wafers 820 on the upper side of the wafer boat 21 is set to 4, when the wafer boat descends, when the Si molten-spray dummy wafer 820 that has been used 4n times is located in Slot N-3, the transfer machine takes out the Si molten-spray dummy wafer 820 from the wafer boat 21 and transfers it to a specified container, and transfers the Si molten-spray dummy wafers 820 located in Slot N to Slot N-2 to the next level Slot N-1 to Slot N-3 respectively. In addition, a new Si molten-spray dummy wafer 820 is loaded in Slot N.

[0151] The same is true for the Si spray dummy wafer 820 on the lower side of the wafer boat 21. In addition, the portion whose number of uses or surface area has decreased by more than a specified amount may be set as a secondary dummy wafer, and the Si spray dummy wafer 820 may be divided into dummy wafers and secondary dummy wafers for group management.

[0152] In addition, here, the Si spraying dummy wafer 820 that is used less frequently is arranged farther from the product wafer 810 , but conversely, the Si spraying dummy wafer 820 that is used less frequently may be arranged closer to the product wafer 810 .

[0153] [Regeneration method of Si spray-sprayed dummy wafer]

[0154] Remelting

[0155] As with a normal regenerated wafer, the Si sprayed dummy wafer 820 is temporarily polished using a method such as CMP to remove the Si sprayed film 822. Alternatively, a polycrystalline or single crystal Si thick film is formed on the current Si sprayed film 822 to substantially block the opening of the pores. Si spraying is then performed.

[0156] Dry cleaning

[0157] Regeneration can be performed by selectively etching the material formed on the Si spray coating 822 of the Si spray dummy wafer 820. For example, in the case of SiN / Si, isotropic plasma etching using fluorinated olefins (hydrofluorocarbons) can be used.

[0158] Wet cleaning

[0159] Regeneration can be performed by a method of selectively etching the material formed on the Si spray film 822 of the Si spray dummy wafer 820. For example, in the case of SiN / Si, phosphoric acid etching can be used.

[0160] According to this embodiment, the load effect during processing of large-consumption wafers can be alleviated, and the inter-surface uniformity of a film formed on a product wafer and between a plurality of product wafers can be improved.

[0161] Example 2

[0162] In Example 1, a bare wafer having the same size as a product wafer is used to perform Si spraying on the surface side of the bare wafer to prepare a Si spraying dummy wafer, and as a second example, Fig.11 , a method of using a bare wafer having a smaller diameter than a bare wafer having the same size as a product wafer, and mounting a plurality of Si sprayed dummy wafers 1102 formed on the bare wafer having a smaller diameter by Si spraying on a tray 1101 is shown.

[0163] The structure of the substrate processing device used in Example 1 Figures 1 to 9 The configuration described is the same, so the description is omitted.

[0164] Instead of the Si spray dummy wafer 820 described in Example 1, the tray 1101 (made of any material, such as quartz, SiC, etc.) is mounted on the wafer boat 21. In this case, the surface area of ​​the appearance on the tray 1101 can be adjusted by changing the number of Si spray dummy wafers 1102 mounted instead of the spray film thickness.

[0165] According to the present embodiment, the load effect during processing of large-consumption wafers can be alleviated, and the inter-surface uniformity of a film formed on a product wafer between a plurality of product wafers can be improved.

[0166] Industrial Applicability

[0167] The present disclosure relates to a substrate processing device and a substrate processing method, which can be applied to the field of manufacturing semiconductor components that perform heat treatment on a semiconductor substrate to form a thin film on the surface.

[0168] Description of Reference Numerals

[0169] 1 Substrate processing device

[0170] 2 Treatment furnace

[0171] 3 Heater

[0172] 4 reaction tubes

[0173] 8 Nozzle

[0174] 19 Sealing cover

[0175] 21, 126 Crystal Boat

[0176] 27.132 Jingzhou Elevator

[0177] 29 Controller

[0178] 124 Transfer Room

[0179] 134 Gas supply mechanism

[0180] 162 Cleaning Unit

[0181] 402 Particle Counter

[0182] 820 Si sprayed dummy wafer.

Claims

1. A substrate processing device, characterized in that: include: A substrate holder that holds a plurality of substrates arranged at predetermined intervals; A reaction tube for accommodating the substrate holder, which has a top plate that closes the upper end and an opening at the bottom that allows the substrate holder to enter and exit; a cover that directly or indirectly holds the substrate holder and blocks the opening; as well as a gas supply mechanism for supplying a gas flow parallel to the surface of each of the plurality of substrates held on the substrate holder in the reaction tube, The substrate holder holds one or more dummy substrates having a Si spray layer formed on the front surface at the end of the array, and holds product substrates or monitor substrates having an integrated circuit pattern formed thereon at other positions.

2. The substrate processing device according to claim 1, characterized in that: The Si spraying layer formed on the front surface of the dummy substrate has a surface area equal to that of the product substrate.

3. The substrate processing device according to claim 1, characterized in that: The diameter of the via hole or the width of the groove of the product substrate falls within the range of pore diameters corresponding to 25% to 75% of the total volume in the cumulative pore volume distribution of the Si sprayed layer.

4. The substrate processing device according to claim 1, characterized in that: The substrate holder has a diameter less than half that of the product substrate or the monitor substrate, and places and holds a plurality of dummy substrates having Si spray layers formed on the surfaces on a tray.

5. The substrate processing device according to claim 1 or 4, characterized in that: Also includes: A furnace body, which surrounds the top and sides of the reaction tube; as well as A controller for controlling the temperature of the furnace and the gas supply mechanism so that a film of a predetermined thickness is deposited on the product substrate or the monitoring substrate. The controller further stores, for each of the plurality of dummy substrates, a history record of each of the dummy substrates being held by the substrate holder and processed together with the product substrate or the monitor substrate as a cumulative value of the film thickness or the number of times used.

6. The substrate processing device according to claim 5, characterized in that: The controller performs a predetermined recording operation, a reporting operation, or an operation of removing the corresponding dummy substrate from the substrate holder when the integrated value exceeds a predetermined value.

7. The substrate processing device according to claim 5, characterized in that: Also includes: an elevator that drives the cover up and down to move the substrate holder in and out of the reaction tube; as well as a cooler disposed below the opening of the reaction tube and configured to spray cooling gas toward the substrate holder being carried out or having been carried out, The cooler is controlled so as to spray the cooling gas at a flow rate different from that when the sprayed cooling gas contacts the dummy substrate and when the sprayed cooling gas does not contact the dummy substrate.

8. The substrate processing device according to claim 7, characterized in that: A particle counter is also provided, the particle counter measures particles in the injected cooling gas, The controller performs a predetermined recording operation, a reporting operation, or an operation of removing a corresponding dummy wafer from the substrate holder when the number of particles measured by the particle counter exceeds a predetermined value.

9. The substrate processing device according to claim 8, characterized in that: The particle counter measures particles in the injected cooling gas at a position opposite to the cooler. The controller performs a predetermined recording operation, a reporting operation, or an operation of removing the corresponding dummy wafer from the substrate holder when the number of particles measured by the particle counter from the cooling gas that crosses the dummy wafer exceeds a predetermined value.

10. The substrate processing apparatus according to claim 5, wherein: The substrate holder holds the dummy substrate at a plurality of holding positions, respectively. The controller applies a different prescribed value to each of the plurality of holding positions.

11. The substrate processing apparatus according to claim 10, wherein: The controller controls so as to remove a dummy substrate whose number of uses does not satisfy the predetermined value from the substrate holder and to transfer a dummy substrate at another holding position to the holding position where the removed dummy substrate was originally located.

12. The substrate processing apparatus according to claim 1, wherein: The dummy substrate is a substrate regenerated by re-spraying, dry etching or wet etching.

13. A method for manufacturing a semiconductor device, characterized in that: The steps include: A step of carrying a substrate holder that holds a plurality of substrates arranged at predetermined intervals into a cylindrical reaction tube using a carrying mechanism; The step of adjusting the pressure inside the cylindrical reaction tube into which the substrate holder holding the substrate is loaded using a pressure adjusting unit, and heating the reaction tube to a predetermined temperature using a heater; The step of adjusting the pressure and supplying a processing gas from a gas supply unit to the inside of the cylindrical reaction tube heated to the predetermined temperature; After the supply of the processing gas is completed, the interior of the cylindrical reaction tube is restored to atmospheric pressure; and The step of carrying out the substrate holder holding the substrate from the inside of the cylindrical reaction tube whose inside has returned to atmospheric pressure using the carrying-in mechanism, and cooling the substrate to room temperature, The supplying step is performed while a product substrate or a monitoring substrate having an integrated circuit pattern formed thereon and a dummy substrate having a Si spraying layer formed on the surface are arranged and held on the substrate holder, wherein the dummy substrate is located on both sides of the product substrate or the monitoring substrate.

14. The method for manufacturing a semiconductor device according to claim 13, wherein: In the supplying step, the temperature of the heater and the gas supply unit are controlled by a controller so that a film of a predetermined thickness is deposited on the product substrate or the monitoring substrate. The manufacturing method of the semiconductor device also includes the following steps: using the controller, for each of the multiple dummy substrates, maintaining a historical record of the dummy substrates held by the substrate holder and processed together with the product substrate or the monitoring substrate as a cumulative value of the film thickness, and performing a prescribed recording action or a prescribed reporting action when the cumulative value exceeds a prescribed value.

15. A substrate processing method, characterized in that: The steps include: A step of carrying a substrate holder that holds a plurality of substrates arranged at predetermined intervals into a cylindrical reaction tube using a carrying mechanism; The step of adjusting the pressure inside the cylindrical reaction tube into which the substrate holder holding the substrate is loaded using a pressure adjusting unit, and heating the reaction tube to a predetermined temperature using a heater; The step of adjusting the pressure and supplying a processing gas from a gas supply unit to the inside of the cylindrical reaction tube heated to the predetermined temperature; After the supply of the processing gas is completed, the interior of the cylindrical reaction tube is restored to atmospheric pressure; and The step of carrying out the substrate holder holding the substrate from the inside of the cylindrical reaction tube whose inside has returned to atmospheric pressure using the carrying-in mechanism, and cooling the substrate to room temperature, The supplying step is performed while a product substrate or a monitoring substrate having an integrated circuit pattern formed thereon and a dummy substrate having a Si spraying layer formed on the surface are arranged and held on the substrate holder, wherein the dummy substrate is located on both sides of the product substrate or the monitoring substrate.