Multilayer resin sheet and molded container

By adjusting the structural proportion and dynamic viscoelastic characteristics of the resin layer in the multi-layer resin sheet, the problem of cracking and threading of the cover material after heat sealing is solved, and the stable peeling and good cut-breaking properties of the food packaging container are achieved, ensuring that Safety and quality of containers.

CN112895644BActive Publication Date: 2024-11-08DENKA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911219109.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-03
Publication Date
2024-11-08
Estimated Expiration
2039-12-03

AI Technical Summary

Technical Problem

The existing multi-layer resin sheets are prone to cracking or wire drawing after heat sealing, and the cut is poorly cracked, resulting in safety and quality problems in food packaging containers when used and separated.

Method used

Using a multi-layer resin sheet composed of a polyolefin resin layer, an oxygen barrier layer, a base layer and an outermost layer, the structural proportion and dynamic viscoelastic characteristics of the resin layer are adjusted to ensure that the cover material does not break when peeled off, and Improve the incision cracking of the container.

Benefits of technology

The stable peeling of the cover material is achieved, wire drawing is suppressed, and the cut-breaking properties of the container are improved, so that multiple containers can be easily separated into a single container, ensuring the safety and quality of food packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112895644B_ABST
    Figure CN112895644B_ABST
Patent Text Reader

Abstract

The present invention provides a multilayer resin sheet, which is a multilayer resin sheet formed by laminating a skin layer, an oxygen barrier layer, an intermediate layer, a substrate layer, and an outermost layer through an adhesive layer, wherein the skin layer is formed by a polyolefin resin layer containing a mixture of polyethylene resin and polypropylene resin; the outermost layer is formed by a polystyrene resin layer, and the thickness of the outermost layer is greater than 1% and less than 8% relative to the overall thickness of the sheet. The multilayer resin sheet of the present invention and its thermoformed container have oxygen barrier properties and good heat sealing properties, so that when used as a food packaging container, it can fully contact with a cover material and can be stably peeled off, thereby suppressing the cracking or wire drawing of the cover material, and has good incision fracture properties, so that when multiple containers are made into a whole container group, individual containers can be easily separated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thermoplastic multilayer resin sheet and a molded container obtained by thermoforming the same. Background Art

[0002] In recent years, multilayer resin sheets and containers formed therefrom as described in Patent Documents 1 to 5 have become popular, wherein the multilayer resin sheets are thermoplastic resin sheets used to form food packaging containers that need to have oxygen barrier properties, and the food packaging containers include, for example, containers used to package foods containing a large amount of water or dairy products such as yogurt containing anaerobic ingredients. The thermoplastic resin sheet is a thermoplastic resin layer such as a polystyrene resin layer as a base layer, and an ethylene-vinyl alcohol copolymer resin layer is provided on its inner layer via an adhesive layer such as a modified polyolefin resin to obtain oxygen barrier properties. At the same time, a polyolefin resin is provided on the surface layer of the multilayer resin sheet that contacts the package contents such as food, so that the container formed by such a multilayer resin sheet can inhibit oxygen penetration from the inside of the container, and can prevent moisture penetration inside and outside the container due to moisture absorption or volatilization of the contents, thereby reducing the quality of the package contents.

[0003] Furthermore, the main feature of the multilayer resin sheets of Patent Documents 1 to 4 is that a thermoplastic resin layer, a polyolefin resin layer having excellent oxygen barrier properties, and an ethylene-vinyl alcohol copolymer resin layer having excellent oxygen barrier properties are laminated together and given thermoformability. Patent Document 5 focuses on making the multilayer resin sheet have the above-mentioned oxygen barrier properties and heat sealability.

[0004] Patent Document 1: Japanese Patent Application Laid-Open No. 11-58619

[0005] Patent Document 2: Japanese Patent Application Laid-Open No. 11-138705

[0006] Patent Document 3: Japanese Patent No. 3967899

[0007] Patent Document 4: Japanese Patent Application Laid-Open No. 2000-108287

[0008] Patent Document 5: Japanese Patent Application Laid-Open No. 2018-12263

[0009] However, in the technologies disclosed in the above-mentioned patent documents 1 to 5, when they are used as food packaging containers, when the heat-sealed cover material is peeled off, the cover material may break or the resin constituting the surface layer or the cover material sealing layer of the multi-layer resin sheet may be coagulated and broken, resulting in a phenomenon such as wire drawing (hereinafter referred to as "wire drawing phenomenon"). There is a risk that the residue of the broken cover material or the wire-drawn resin will be mixed into the contents of the packaging container. In addition, the molded containers formed of the multi-layer resin sheets disclosed in patent documents 1 to 5 also have the problem of poor cut-breakability when a single container body is separated from a container group composed of multiple containers. Summary of the invention

[0010] In view of the above problems in the prior art, the present invention aims to provide a multilayer resin sheet having oxygen barrier properties and good heat sealing properties, so that when used as a food packaging container, it can be fully bonded with a cover material and can be stably peeled off, thereby suppressing the above-mentioned cover material cracking and wire drawing phenomena, and having good cut fracture properties, so that when multiple containers are made into a container group, individual containers can be easily separated. The present invention also provides a molded container obtained by thermoforming the above-mentioned multilayer resin sheet.

[0011] A multilayer resin sheet according to one embodiment of the present invention is a multilayer resin sheet formed by laminating a skin layer, an oxygen barrier layer, an intermediate layer, a substrate layer, and an outermost layer through an adhesive layer, characterized in that: the skin layer is composed of a polyolefin resin layer, and the polyolefin resin layer contains a mixture of polyethylene resin and polypropylene resin; the outermost layer is composed of a polystyrene resin layer, and the thickness of the outermost layer is relative to the overall thickness of the sheet, and its layer structure ratio is greater than 1% and less than 8%.

[0012] In addition, in the above-mentioned multilayer resin sheet provided by the present invention, the dynamic viscoelasticity of the polyolefin resin layer is such that, in the temperature range of 110°C-130°C, the storage elastic modulus and the loss elastic modulus are both greater than 1E+04Pa and less than 1E+07Pa.

[0013] In the multilayer resin sheet provided by the present invention, the base layer is composed of a polystyrene resin layer, and the rubber content contained in the polystyrene resin of the base layer is 6% or less.

[0014] In the multilayer resin sheet provided by the present invention, the base material layer contains 1% or more of a polyolefin resin component that is incompatible with the polystyrene resin.

[0015] In the multilayer resin sheet provided by the present invention, the rubber content contained in the polystyrene-based resin of the base layer is 3% or more and 6% or less.

[0016] In the multilayer resin sheet provided by the present invention, the mixing ratio of the polypropylene-based resin in the polyolefin-based resin layer constituting the skin layer is 5% or more and 50% or less.

[0017] In addition, in the above-mentioned multilayer resin sheet provided by the present invention, the polyethylene-based resin is composed of low-density polyethylene; and the polypropylene-based resin is composed of a random copolymer or a block copolymer.

[0018] In addition, the present invention also provides a molded container, which is formed by thermoforming the multilayer resin sheet.

[0019] According to the multilayer resin sheet involved in the present invention, when it is used as a molded container, the skin layer that forms a heat-sealing surface with the cover material is a polyolefin resin layer using a mixed resin, and the mixed resin is a mixed resin dispersed and mixed by changing the mixing ratio of polyethylene resin and polypropylene resin. Therefore, the peeling strength when peeling the cover material can be adjusted, and the cover material can be suppressed from breaking, and the occurrence of wire drawing can be fully suppressed. In addition, since it has a thin outermost layer composed of polystyrene resin with a layer structure ratio of more than 1% and less than 8% relative to the overall thickness of the sheet, the crack propagation property can be improved when the individual container bodies are separated by the incision during container molding, thereby obtaining good incision fracture properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 is a longitudinal cross-sectional view showing an example of the layer structure of the multilayer resin sheet of the present invention;

[0021] Figure 2 is a perspective schematic diagram showing an example of a food packaging container as a molded container of the present invention;

[0022] Figure 3 Schematic diagram showing the method of evaluating bending resistance of the present invention. DETAILED DESCRIPTION

[0023] A multilayer resin sheet according to one embodiment of the present invention, such as Figure 1 As shown in FIG. 1 , the oxygen barrier layer 12 is laminated between the skin layer 10a and the intermediate layer 10b composed of a polyolefin resin layer via an adhesive layer 11a and an adhesive layer 11b, the intermediate layer 10b is laminated on the base layer 13 composed of a polystyrene resin layer via an adhesive layer 11c, and the base layer 13 is laminated on the outermost layer 14 composed of a polystyrene resin layer. That is, the structure of the multilayer resin sheet according to this embodiment is as follows: Figure 1 As shown, from top to bottom are skin layer 10a / adhesive layer 11a / oxygen barrier layer 12 / adhesive layer 11b / intermediate layer 10b / adhesive layer 11c / base material layer 13 / outermost layer 14.

[0024] The following describes each layer in the order of the skin layer 10a, the middle layer 10b, the adhesive layer 11a, 11b, 11c, the oxygen barrier layer 12, the substrate layer 13, and the outermost layer 14. On this basis, the multilayer resin sheet itself of the present invention and the food packaging container formed therefrom as a molded container are described.

[0025] 《Epidermis 10a, Intermediate Layer 10b》

[0026] The skin layer 10a and the middle layer 10b are layers required to impart water vapor barrier properties to the multilayer resin sheet, and the skin layer 10a is an important layer that becomes a heat-sealed surface with a lid material when the multilayer resin sheet is used as a food packaging container, and is formed of a resin mixture of a polyethylene resin and a polypropylene resin, which are polyolefin resins. In addition, in this embodiment, in order to facilitate the manufacture of the multilayer resin sheet, the middle layer 10b is composed of the same material as the skin layer 10a.

[0027] As the polyethylene resin constituting the main component of the resin mixture, generally, for example, low-density polyethylene, medium-density polyethylene, high-density polyethylene, straight-chain (linear) polyethylene, ethylene-α-olefin copolymers polymerized using metallocene catalysts, ethylene-vinyl acetate copolymers, ethylene-ionomer resins, ethylene-acrylic acid copolymers, ethylene-ethyl acrylate copolymers, ethylene-methacrylic acid copolymers, ethylene-methyl methacrylate copolymers, ethylene-propylene copolymers, etc. In addition, as the polypropylene resin constituting the resin mixture, generally, for example, homopolymers, random copolymers, and block copolymers can be used, that is, the resin mixture is a dispersed mixed resin in which any one of homopolymers, random copolymers, and block copolymers is mixed with polyethylene resins.

[0028] Among them, from the viewpoint of tearing property when the incision is formed, low-density polyethylene is preferably used as the polyethylene resin. In addition, from the viewpoint of film-forming property and thermoformability of the multilayer resin sheet, random copolymers and block copolymers are preferably used as the polypropylene resin.

[0029] The mixing method of the polyolefin resin mixture of the present embodiment is not particularly limited, and a common mixing method can be used. For example, a dry blending method in which individual small particles are simply mixed using a mixing agitator such as a drum, or a composite method in which resin pellets are heated and melt-mixed using an extruder, etc. can be used.

[0030] The mixing ratio of the above-mentioned resin mixture is preferably 5% or more and 50% or less of the polypropylene resin. When the mixing ratio of the polypropylene resin is 5% or more, the peeling strength when peeling the cover material can be appropriately suppressed, thereby suppressing the rupture of the cover material. When the mixing ratio is less than 50%, sufficient peeling strength can be obtained in practical applications. Furthermore, the mixing ratio of the resin mixture is preferably 10% or more and 40% or less of the polypropylene resin.

[0031] The skin layer 10a composed of the polyolefin resin layer containing the resin mixture has a dynamic viscoelasticity of a storage elastic modulus and a loss elastic modulus of 1E + 04Pa or more and less than 1E + 07Pa in the temperature range of 110°C-130°C. When the storage elastic modulus and the loss elastic modulus are both above 1E + 04Pa, the thermal deformation of the skin layer 10a can be appropriately suppressed, thereby solving the problem of the skin layer 10a being entangled in the sealing layer of the cover material due to the large thermal deformation caused by the heat during heat sealing, and can also fully solve the problem of wire drawing when peeling off the cover material. When the storage elastic modulus and the loss elastic modulus are both less than 1E + 07Pa, since the thermal deformation of the skin layer 10a is moderate, it is possible to ensure that the bonding area with the cover material is moderate, and it is easy to obtain sufficient bonding strength required when peeling off the cover material in practical use. The dynamic viscoelasticity of the skin layer 10 a formed of the polyolefin-based resin layer containing the resin mixture can be adjusted by adjusting the mixing ratio of the polypropylene-based resin.

[0032] As described above, the resin constituting the skin layer 10a and the intermediate layer 10b generally only needs to contain polyethylene resin and polypropylene resin, but other resins such as methylpentene polymer and polybutylene polymer which do not contain polyethylene resin or polypropylene resin may be added within the scope that does not hinder the effect of the invention, and various additives other than the resin components may be added. Such additives include, for example, colorants such as pigments or dyes, granular lubricants such as talc, clay or silica, antistatic agents such as chlorine compounds such as sulfonic acid and alkali metals or polypropylene glycol, ultraviolet absorbers, antibacterial agents and the like.

[0033] In addition, the resin used as the sealing layer of the cover material for heat sealing may be, for example, low-density polyethylene, linear low-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-methacrylic acid copolymer, ethylene-methyl methacrylate copolymer, ethylene-type ionomer resin, ethylene-propylene copolymer, etc., but is not particularly limited.

[0034] The total thickness of the epidermis 10a and the middle layer 10b is preferably 1-30% relative to the overall thickness of the multilayer resin sheet. More preferably, the layer structure ratio is 2% or more and 10% or less. The layer structure ratio referred to herein refers to the value obtained by dividing the total thickness of the epidermis 10a and the middle layer 10b by the overall thickness of the sheet, converted into a percentage. When the layer structure ratio is 1% or more, especially even when the overall thickness of the multilayer resin sheet is thin, the polyolefin resin layer can be ensured to have sufficient thickness so that it can be fully utilized. When the layer structure ratio is less than 30%, the depth of insertion of the cutting blade can be made shallower when forming an incision in the container, thereby suppressing the appearance defect called whisker burr caused by the expansion of the resin.

[0035] When the multilayer resin sheet is thermoformed and used as a packaging container by using the skin layer 10a and the intermediate layer 10b formed by the above method, the peel strength with the cover material can be controlled to 4-30N. When the peel strength is 4N or more, sufficient sealing can be ensured to suppress leakage of the contents. When the peel strength is 30N or less, the cover material can be suppressed from cracking or pulling when peeling the cover material.

[0036] In addition, in the present embodiment, the intermediate layer 10 b is made of the same material as the skin layer 10 a , but the intermediate layer 10 b may be made of a material different from that of the skin layer 10 a .

[0037] <Adhesive layers 11a, 11b, 11c>

[0038] The adhesive layers 11a, 11b, and 11c of the present embodiment play an important role as adhesive materials for laminating different types of component resins, and modified polyolefin polymers are preferably used as their constituent materials. As modified polyolefin polymers constituting the adhesive layer, for example, homopolymers of olefins having 2 to 8 carbon atoms such as ethylene, propylene, and 1-butene can be used; copolymers of these olefins with other olefins having 2 to 20 carbon atoms such as ethylene, propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, and 1-decene; olefin resins; ethylene-propylene copolymers; ethylene-propylene copolymers; and copolymers of these olefins with other olefins having 2 to 20 carbon atoms such as ethylene, propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, and 1-decene; vinyl acetate, vinyl chloride, acrylic acid, methacrylic acid, acrylic acid esters, methacrylates, and vinyl compounds such as polystyrene. The copolymer rubbers such as ethylene-diene copolymers, ethylene-1-butene copolymers, propylene-1-butene copolymers are modified with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, isocrotonic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, tetrahydrophthalic acid, or their acyl halides, amides, imides, anhydrides, esters, etc., specifically maleyl chloride, maleimide, maleic anhydride, citraconic anhydride, monomethyl maleate, dimethyl maleate, glycidyl maleate, etc. under grafting reaction conditions.

[0039] Among the above materials for the modified polyolefin polymer, preferred are ethylene resins, propylene resins, or ethylene-propylene or 1-butene copolymer rubbers modified with unsaturated dicarboxylic acids or their anhydrides, particularly maleic acid or its anhydride.

[0040] The thickness of the adhesive layers 11a, 11b, and 11c is preferably 2 to 50 μm, and more preferably 10 to 30 μm. When the thickness is above 2 μm, sufficient adhesive strength can be obtained. When the thickness is below 50 μm, the appearance defect called whisker burrs produced by stamping after hot forming can be suppressed.

[0041] 《Oxygen barrier layer 12》

[0042] The oxygen barrier layer 12 of this embodiment is a layer required to impart oxygen barrier properties to the multilayer resin sheet. Representative materials of the oxygen barrier resin constituting the oxygen barrier layer 12 include ethylene-vinyl alcohol copolymer resin, polyamide resin, polyvinyl alcohol, polyvinyl chloride, etc., but are not limited to these. Among them, ethylene-vinyl alcohol copolymer resin is preferred from the perspective of processability and moldability.

[0043] Ethylene-vinyl alcohol copolymer resin is usually obtained by saponifying ethylene-vinyl acetate copolymer. In order to make it have both oxygen barrier properties and extrusion moldability, the ethylene content is preferably 10-65 mol% (more preferably 20-50 mol%), and the saponification degree is preferably above 90% (more preferably above 95%).

[0044] In addition, the following can be listed as polyamide resins: lactam polymers such as caprolactam and azacyclotridecan-2-one; aminocarboxylic acid polymers such as 6-aminocaproic acid, 11-aminohexadecanoic acid, and 12-aminododecanoic acid; fatty diamines such as 1,6-hexanediamine, 1,10-diaminodecane, dodecanediamine, 2,2,4- or 2,4,4-trimethylhexanediamine, alicyclic diamines such as 1,3- or 1,4-bis(aminomethyl)cyclohexane, 4,4'-diaminodicyclohexylmethane, condensation products formed by diamine units of aromatic diamines such as m-xylylenediamine or p-xylylenediamine and dicarboxylic acid units of aliphatic dicarboxylic acids such as adipic acid, suberic acid, and sebacic acid, alicyclic carboxylic acids such as cyclohexanedicarboxylic acid, terephthalic acid, and aromatic dicarboxylic acids such as isophthalic acid; and copolymers of the above substances.

[0045] Specific examples of polyamide resins include nylon 6, nylon 9, nylon 11, nylon 12, nylon 66, nylon 610, nylon 611, nylon 612, nylon 6T, nylon 6I, nylon MXD6, nylon 6 / 66, nylon 6 / 610, nylon 6 / 6T, nylon 6I / 6T, etc., among which nylon 6 and nylon MXD6 are the best.

[0046] In addition, the thickness of the oxygen barrier layer 12 is preferably 5-50 μm (more preferably 10-40 μm). When the thickness is 5 μm or more, the oxygen barrier layer will not break in the container after the multilayer resin sheet is thermoformed, and sufficient oxygen barrier properties can be obtained, thereby fully maintaining the quality of the contents sealed in the container. When the thickness is 50 μm or less, since the oxygen barrier layer can be sufficiently thermally stretched during container molding, sufficient thickness of the container can be ensured, thereby obtaining a molded container with a good appearance.

[0047] 《Base material layer 13》

[0048] The substrate layer 13 of the present embodiment is a polystyrene resin layer. The polystyrene resins constituting the polystyrene resin layer 13 include the following: homopolymers or copolymers of polystyrene monomers such as styrene, 2-phenyl-1-propylene, 4-methylstyrene, polydimethylstyrene, para-tert-butylstyrene, and polychlorostyrene; copolymers of these polystyrene monomers and other monomers such as styrene-acrylonitrile copolymer (AS resin), or graft polymers of the aforementioned polystyrene monomers and other polymers, such as graft polymers grafted in the presence of diene rubber polymers such as polybutadiene, polystyrene butadiene copolymers, polyisoprene, and polychloroprene, such as high impact polystyrene (HIPS resin), styrene-acrylonitrile graft polymer (ABS resin), etc.

[0049] As a polystyrene resin, from the perspective of rigidity and moldability, a mixture of polystyrene (GPPS resin) and high impact polystyrene (HIPS resin) is preferred, and it is preferred that the polystyrene resin contains a rubber content of less than 6%. It is further preferred that the rubber content in the polystyrene resin is more than 3% and less than 6%. When the rubber content in the polystyrene resin is more than 3%, sufficient impact resistance can be obtained, so that the container is not easily damaged when the molded container falls. When the rubber content is less than 6%, since cracks are easily propagated, when the individual containers are separated by the incisions formed when the containers are formed, the incisions can be easily broken.

[0050] In addition, it is preferred that the polystyrene resin layer contains 1% or more of a polyolefin resin as a component incompatible with the polystyrene resin. Since the multilayer resin sheet contains the polyolefin resin as an incompatible component, it becomes brittle and can be easily broken when the cut is bent. In addition, it is further preferred that the polyolefin resin as a component incompatible with the polystyrene resin contained in the polystyrene resin layer is 1% or more and 5% or less.

[0051] In the base material layer 13, as in other layers, other resins may be mixed in the range that does not hinder the effect of the invention of the present invention, and various additives other than the constituent resins may be added. As such additives, there may be compatible materials that make different components compatible, colorants such as pigments or dyes, release agents such as silicone oils or ethyl esters, fiber-shaped reinforcing agents such as glass fibers, granular lubricants such as talcum powder, clay or silica, chlorine compounds such as sulfonic acid and alkali metals, antistatic agents such as polypropylene glycol, ultraviolet absorbers, antibacterial agents, etc. In addition, waste resins generated in the manufacturing process of the multilayer resin sheet or food packaging container of the present invention may also be mixed and used.

[0052] The thickness of the substrate layer 13 is preferably 180-1300 μm (more preferably 250-1100 μm). When the thickness is 180 μm or more, the container obtained by thermoforming can have sufficient rigidity, and when the thickness is 1300 μm or less, the heat transfer in the thickness direction of the sheet during thermoforming can be more sufficient, so that the thermoforming property is good, and a molded container with good appearance can be obtained.

[0053] Outermost Layer 14

[0054] The outermost layer 14 is formed of a polystyrene resin, preferably a resin that is the same as or similar to the polystyrene resin mixed in the base layer 13. Therefore, as the polystyrene resin used, for example, homopolymers or copolymers of polystyrene monomers such as polystyrene, α-methyl polystyrene, p-methyl polystyrene, polydimethylstyrene, pt-polybutylstyrene, and polychlorostyrene can be used; copolymers of these polystyrene monomers and other monomers such as polystyrene-acrylonitrile copolymer (AS resin), or graft polymers of the aforementioned polystyrene monomers and other polymers, such as high-impact polystyrene (HIPS resin), polystyrene-acrylonitrile graft polymer (ABS resin), etc. From the perspective of rigidity and thermoformability, polystyrene (GPPS resin) and high-impact polystyrene (HIPS resin) are generally used.

[0055] The thickness of the outermost layer 14 is preferably 1% or more and 8% or less of the layer structure ratio relative to the thickness of the entire sheet. When the layer structure ratio is 8% or less, sufficient crack extension can be obtained when the individual container bodies are separated by the incisions formed when the container is molded, so that the incisions can be easily broken. More preferably, the thickness of the outermost layer 14 is 1% or more and 6% or less of the layer structure ratio relative to the thickness of the entire sheet. When the layer structure ratio is 1% or more, the appearance defects of the multilayer resin sheet caused by the waste resin returned to the base layer will not be revealed on the surface of the sheet, so that a multilayer resin sheet with good appearance can be obtained.

[0056] By means of the substrate layer 13 and the outermost layer 14 of the above-mentioned structure, the folding times as an index of the bending resistance of the multilayer resin sheet is less than 5 times, and the sheet can be easily broken when the bending angle of the sheet is less than 60 degrees, and can be easily separated into individual container bodies through the incision formed when the container is molded.

[0057] 《Multilayer resin sheet》

[0058] The layer structure of the multilayer resin sheet according to one embodiment of the present invention is as follows: Figure 1 As shown in FIG. 1 , the layer structure is basically composed of skin layer 10a / adhesive layer 11a / oxygen barrier layer 12 / adhesive layer 11b / intermediate layer 10b / adhesive layer 11c / base material layer 13 / outermost layer 14, but the layer structure is not limited thereto. For example, each layer may be composed of two or more layers. In addition, the waste generated during the manufacturing process of the multilayer resin sheet or molded container of the present invention will not be discarded, but can be crushed and reused, or can be re-granulated after heat melting as a recycled material and returned to the structure of the multilayer resin sheet to form a new layer.

[0059] The thickness of the multilayer resin sheet is preferably 200-1300 μm. When the thickness is 200 μm or more, the sides and bottom of the thermoformed container can be sufficiently thick, thereby obtaining sufficient container strength. When the thickness is 1300 μm or less, heat conduction in the thickness direction of the sheet during thermoforming is easily and sufficiently performed, so that the thermoformability is good, and a molded container with a good appearance can be obtained.

[0060] The method for producing the multilayer resin sheet is not particularly limited, and a general method can be used, for example, a method of using 4 or more single-shaft extruders or twin-shaft extruders to melt-extrude each raw material resin, and then pass through a distributor with a guide column and a T-die to obtain a multilayer resin sheet, or a method of obtaining a multilayer resin sheet through a multi-flow die, etc.

[0061] Food packaging containers

[0062] The molded container of the present invention is formed by thermoforming the multilayer resin sheet of the present invention. As the thermoforming method, conventional vacuum molding, pressure molding, or a plunger-assisted pressure method in which a plunger contacts one side of the sheet for molding, or a molding method called double-mold molding in which a pair of male and female molds contact both sides of the sheet for molding can be cited. However, the method is not limited to this. At the same time, as a method for heating and softening the sheet before molding, a well-known sheet heating method such as non-contact heating by radiation heating with an infrared heater can be used.

[0063] When the molded container of the present invention is used as a food packaging container, the surface and the outer surface are both formed with cuts. For example, the food packaging container is formed by connecting a plurality of detachable containers, and the connection positions of each container can be broken and separated by bending. The container is provided with a cut at the bending position for the convenience of bending. The cross-sectional shape of the cut is generally formed into a V-shape, which can be formed by inserting a V-shaped blade after heating by a hot plate method or the like. Figure 2 An example of a yogurt container having a cutout is shown.

[0064] 《Implementation Examples》

[0065] Hereinafter, the present invention will be specifically described by way of examples and comparative examples, but the present invention is not limited to the contents of the following examples and the like.

[0066] The resin raw materials used in the examples are as follows:

[0067] (1) Polyolefin resin layer

[0068] LDPE resin: Q400

[0069] (Produced by Sinopec Shanghai Petrochemical Co., Ltd., MI: 4.0g / 10min, (190℃, 2.16kgf))

[0070] HDPE resin: J2200

[0071] (Manufactured by Lotte Chemical, MI: 5.0g / 10min, (190°C, 2.16kgf))

[0072] PP resin: PPB-M09

[0073] (Produced by Zhenhai Refining and Chemical Company of Sinopec, MI: 9.0g / 10min, (190℃, 2.16kgf))

[0074] (2) Oxygen barrier layer

[0075] Ethylene vinyl alcohol copolymer (EVOH): EVAL J171B

[0076] (produced by Kuraray, MI: 1.7 g / 10 min, (190°C, 2.16 kgf), ethylene content 32 mol%)

[0077] (3) Adhesive layer

[0078] Modified olefin polymer (modified PO): MODIC F502C

[0079] (Mitsubishi Chemical Corporation, MI: 1.3 g / 10 min, (190°C, 2.16 kgf))

[0080] (4) Polystyrene resin layer

[0081] HIPS resin: 4241

[0082] (Produced by Total Petrochemicals, MI: 4.0 g / 10 min, (200°C, 5.0 kgf))

[0083] GPPS resin: 1050

[0084] (Total Petrochemicals, MI: 2.8 g / 10 min, (200°C, 5.0 kgf))

[0085] The various evaluations of the multilayer resin sheet were carried out by the following methods:

[0086] (A) Thickness of each layer

[0087] A test piece was cut out at five points at evenly spaced positions in the width direction perpendicular to the flow direction of the multilayer resin sheet, the test piece was sliced ​​into thin slices using a single-edged knife, and the thickness of each layer was measured using an electron microscope.

[0088] The thickness of each layer is calculated as the average value of the thickness of each layer at five points in the width direction of the multilayer resin sheet.

[0089] Measuring equipment: Electron microscope KH7700 (manufactured by Hirox)

[0090] (B) Peel strength with cover material

[0091] Under the following conditions, the surface of the skin layer 10a of the multilayer resin sheet and the cover material were heat-sealed, and after being placed at a temperature of 23±2°C and a relative humidity of 50±10% for 1 hour, the unsealed end was clamped and fixed, and then the peel strength was measured by a universal testing machine at a temperature of 23±2°C and a relative humidity of 50±10%.

[0092] (Heat sealing conditions)

[0093] Heat sealing temperature: 185℃

[0094] Heat sealing pressure: 0.1MPa

[0095] Heat sealing time: 1.6 seconds

[0096] (Peeling conditions)

[0097] Peeling machine: Precision universal testing machine AGS-X (manufactured by Shimadzu Corporation)

[0098] Measurement conditions: vertical peeling was performed at a tensile speed of 250 mm / min, and the average value of the peel strength stable region was calculated.

[0099] (C) Wire drawing phenomenon

[0100] The peeling strength test sample with the cover material was visually observed for peeling appearance and evaluated according to the following criteria:

[0101] 1: No wire drawing phenomenon

[0102] 2: There is wire drawing less than 10mm

[0103] 3: There is wire drawing phenomenon of more than 10mm

[0104] (D) Dynamic viscoelasticity experiment

[0105] Cut a test piece (5 mm wide) from any position of the multilayer resin sheet, cut it with a single-edged knife, and peel it off by hand at the cut point to separate the skin layer. Fix both ends of the peeled skin layer and use a dynamic viscoelasticity measuring device to evaluate under the following conditions.

[0106] Fixed distance: 10mm

[0107] Measuring temperature: 50-150℃

[0108] Heating rate: 5℃ / min

[0109] Frequency: 1Hz

[0110] Strain: 0.1%

[0111] Measurement mode: Tensile

[0112] (E) Rubber content of polystyrene resin in the resin component of the substrate layer

[0113] The measurement is carried out by thermal decomposition gas chromatography. A test piece is cut from an arbitrary position of the multilayer resin sheet, and the corresponding multilayer resin sheet layer component is scraped off from the test piece. The scraped test piece is thermally decomposed in an environment heated to a certain high temperature by a thermal decomposition gas chromatograph, and then the gas peak area of ​​the generated butadiene monomer and styrene monomer is measured. Based on the calibration curve of other resins for judging the rubber content, the rubber content contained in the test piece is calculated.

[0114] In addition, the corresponding multilayer resin sheet layer constituent part refers to the base material layer. Specifically, firstly, the layers other than the analysis object are cut off by a blade, and only the base material layer is sampled as the analysis object.

[0115] (F) Bending resistance / folding times

[0116] Cut out a test piece (15 mm x 100 mm) from any position of the multilayer resin sheet, clamp both ends of the test piece, and perform a folding strength test using a folding tester.

[0117] Folding test machine: FPC folding test machine

[0118] Measurement conditions: Under a load of 1100g, bend the test piece at a bending angle of 80° and a bending speed of 135rpm until the multilayer resin sheet breaks.

[0119] (G) Bending resistance / bending angle

[0120] Cut a test piece (15 mm x 100 mm) from an arbitrary position of the multilayer resin sheet, and measure the bending angle when the multilayer resin sheet breaks when the test piece is bent.

[0121] The cut fracture property of the molded container body is an important property that allows consumers to easily separate the individual container bodies. In the above (F) bending resistance / folding number, the fewer the number of bends until the multilayer resin sheet is broken when it is bent, the easier it is to break. The above (G) bending resistance / bending angle, as shown in FIG. Figure 3 As shown in FIG. 1 , the smaller the angle until the multilayer resin sheet is broken when bent, the easier it is to break. (F) Bending resistance / number of folding times and (G) Bending resistance / bending angle are indicators of the ease of breaking.

[0122] 《Example 1》

[0123] Using two φ45 mm single-screw extruders, one φ65 mm single-screw extruder, one φ75 mm single-screw extruder, and one φ120 mm single-screw extruder, a dispenser method was used to obtain a multilayer resin sheet having a layer structure of 40 μm skin layer 10a / 10 μm adhesive layer 11a / 30 μm oxygen barrier layer 12 / 10 μm adhesive layer 11b / 40 μm intermediate layer 10b / 10 μm adhesive layer 11b / 1035 μm base material layer 13 / 25 μm outermost layer 14 and a total thickness of 1200 μm.

[0124] Among them, as a resin mixture of polyethylene resin and polypropylene resin, the surface layer 10a and the middle layer 10b use a material obtained by mixing LDPE resin "Q400" and PP resin "M09" in the form of a mass ratio of 80 / 20, the adhesive layers 11a, 11b and 11c use a modified olefin polymer "MODIC F502C", the oxygen barrier layer 12 uses an ethylene-vinyl alcohol copolymer "EVAL J171B", the base material layer 13 uses a material obtained by mixing HIPS resin "4241", GPPS resin "1050" and LDPE "Q400" in the form of a mass ratio of 50 / 50 / 1, and the outermost layer uses HIPS resin "4241".

[0125] The obtained multilayer resin sheet and container were subjected to various evaluations using the above-mentioned various evaluation methods for multilayer resin sheets. The results are shown in Table 1.

[0126] As shown in Table 1, the peel strength of the container formed by the multilayer resin sheet of Example 1 with the lid material is 18N (within the range of 4-30N), and the index of the wire drawing phenomenon is 1. In addition, the number of folding resistance as a bending characteristic is 2 times, which meets the standard of less than 5 times, and the bending angle as a bending characteristic is 40 degrees, which meets the standard of less than 60 degrees. The dynamic viscoelasticity of the skin layer 10a in Example 1 has a storage elastic modulus of 1.3E+05Pa (within the range of 1E+04Pa or more and less than 1E+07Pa) and a loss elastic modulus of 5.2E+04Pa (within the range of 1E+04Pa or more and less than 1E+07Pa), so that the thermal deformation of the skin layer 10a during heat sealing is controlled within an appropriate range, and the involvement of the sealing layer of the lid material is reduced, so that the wire drawing phenomenon can be suppressed while obtaining sufficient peel strength required for practical use. Therefore, the container formed by the multilayer resin sheet of Example 1 has good heat sealing properties, can be fully bonded with the cover material, can be stably peeled off, can suppress the cracking and wire drawing of the cover material, and has good cut and rupture properties, which can easily separate multiple container bodies formed into an integrated container.

[0127] 《Examples 2-12, Comparative Examples 1-6》

[0128] The multilayer resin sheet was formed in the same manner as in Example 1 except that the mixing ratio of the skin layer 10 a , the intermediate layer 10 b , and the base layer 13 and the thickness of each layer were changed as shown in Tables 1 and 2.

[0129] 《Example 2-3》

[0130] Specifically, as shown in Table 1, in Example 2 and Example 3, only the composition of the skin layer is changed compared with Example 1, and the obtained molded containers have reached the corresponding standards in terms of peel strength with the cover material, index of wire drawing phenomenon, number of folding endurance as bending characteristics, and bending angle. In the dynamic viscoelasticity of the skin layer 10a in Example 2 and Example 3, the storage elastic modulus and loss elastic modulus are both within the range of 1E+04Pa or more and less than 1E+07Pa, so the thermal deformation of the skin layer 10a during heat sealing is controlled within an appropriate range, reducing the involvement of the sealing layer of the cover material, thereby suppressing the wire drawing phenomenon while obtaining sufficient peel strength required in practical use. Therefore, the containers formed by the multilayer resin sheets of Example 2 and Example 3 have good heat sealing properties, can be fully bonded with the cover material, can be stably peeled, can suppress the rupture and wire drawing of the cover material, and have good incision fracture properties, which can easily separate multiple container bodies formed as an integrated container.

[0131] 《Example 4, Example 7》

[0132] In Example 4 and Example 7, only the composition of the HIPS resin and the GPPS resin in the substrate layer is changed compared to Example 1. The formed containers have reached the corresponding standards in terms of peel strength with the cover material, index of wire drawing phenomenon, number of folding endurance as bending characteristics, and bending angle. In the dynamic viscoelasticity of the epidermis 10a in Example 4 and Example 7, the storage elastic modulus and loss elastic modulus are both within the range of 1E+04Pa or more and less than 1E+07Pa. Therefore, the thermal deformation of the epidermis 10a during heat sealing is controlled within an appropriate range, reducing the involvement of the sealing layer of the cover material, thereby suppressing the wire drawing phenomenon while obtaining practical and sufficient peel strength. Therefore, the containers formed by the multilayer resin sheets of Example 4 and Example 7 have good heat sealing properties, can be fully bonded with the cover material, can be stably peeled, can suppress the rupture and wire drawing of the cover material, and have good incision fracture properties, which can easily separate multiple container bodies formed into an integrated container.

[0133] 《Example 5》

[0134] In Example 5, only the composition of the polyolefin resin in the substrate layer is changed compared to Example 1. The formed container has reached the corresponding standards in terms of peel strength with the cover material, index of wire drawing phenomenon, number of folding endurance as bending characteristics, and bending angle. In the dynamic viscoelasticity of the epidermis 10a in Example 5, the storage elastic modulus and loss elastic modulus are both within the range of 1E+04Pa and less than 1E+07Pa. Therefore, the thermal deformation of the epidermis 10a during heat sealing is controlled within an appropriate range, reducing the involvement of the sealing layer of the cover material, thereby suppressing the wire drawing phenomenon while obtaining sufficient peel strength required in practical use. Therefore, the container formed by the multilayer resin sheet of Example 5 has good heat sealing properties, can be fully bonded with the cover material, can be stably peeled, can suppress the rupture and wire drawing of the cover material, and has good incision fracture properties, which can easily separate multiple container bodies formed as an integrated container.

[0135] 《Example 6, Example 8》

[0136] In Example 6 and Example 8, the thickness of the substrate layer and the outermost layer, and the composition ratio of the outermost layer are changed compared with Example 1. The peel strength with the cover material, the index of the wire drawing phenomenon, the number of folding resistance as a bending characteristic, and the bending angle of the formed container all meet the corresponding standards. In the dynamic viscoelasticity of the epidermis 10a in Example 6 and Example 8, the storage elastic modulus and the loss elastic modulus are both within the range of 1E+04Pa or more and less than 1E+07Pa. Therefore, the thermal deformation of the epidermis 10a during heat sealing is controlled within an appropriate range, reducing the involvement of the sealing layer of the cover material, thereby suppressing the wire drawing phenomenon while obtaining sufficient peel strength required in practical use. Therefore, the container formed by the multilayer resin sheet of Example 6 and Example 8 has good heat sealing, can be fully bonded with the cover material, can be stably peeled, can suppress the rupture and wire drawing of the cover material, and has good incision fracture properties, which can easily separate multiple container bodies formed as an integrated container.

[0137] 《Example 9》

[0138] In Example 9, compared with Example 1, no polyolefin resin is added to the substrate layer, and only the resin composition of the substrate layer is changed. The peel strength between the substrate and the lid material, the index of the wire drawing phenomenon, the number of folding resistance as a bending characteristic, and the bending angle of the formed container all meet the corresponding standards. In the dynamic viscoelasticity of the epidermis 10a in Example 9, the storage elastic modulus and the loss elastic modulus are both within the range of 1E+04Pa and less than 1E+07Pa. Therefore, the thermal deformation of the epidermis 10a during heat sealing is controlled within an appropriate range, reducing the involvement of the sealing layer of the lid material, thereby suppressing the wire drawing phenomenon while obtaining sufficient peel strength required in practical use. Therefore, the container formed by the multilayer resin sheet of Example 9 has good heat sealing properties, can be fully bonded with the lid material, can be stably peeled, can suppress the rupture and wire drawing of the lid material, and has good incision fracture properties, which can easily separate multiple container bodies formed as an integrated container.

[0139] 《Example 10》

[0140] In Example 10, compared with Example 1, the rubber content of the polystyrene resin in the resin component of the substrate layer is changed, and no polyolefin resin is added to the substrate layer. The formed container meets the corresponding standards in terms of peel strength with the cover material, wire drawing ratio index, number of folding resistance as bending characteristics, and bending angle. In the dynamic viscoelasticity of the epidermis 10a in Example 10, the storage elastic modulus and the loss elastic modulus are both within the range of 1E+04Pa and less than 1E+07Pa. Therefore, the thermal deformation of the epidermis 10a during heat sealing is controlled within an appropriate range, reducing the involvement of the sealing layer of the cover material, thereby suppressing the wire drawing phenomenon while obtaining sufficient peel strength required in practical use. Therefore, the container formed by the multilayer resin sheet of Example 10 has good heat sealing properties, can be fully bonded with the cover material, can be stably peeled, can suppress the rupture and wire drawing of the cover material, and has good incision fracture properties, which can easily separate multiple container bodies formed as an integrated container.

[0141] Example 11

[0142] In Example 11, the rubber content of the polystyrene resin in the resin component of the substrate layer is changed compared to Example 1. The formed container meets the corresponding standards in terms of peel strength with the cover material, wire drawing ratio index, number of folding resistance as bending characteristics, and bending angle. In the dynamic viscoelasticity of the epidermis 10a in Example 11, the storage elastic modulus and the loss elastic modulus are both within the range of 1E+04Pa and less than 1E+07Pa. Therefore, the thermal deformation of the epidermis 10a during heat sealing is controlled within an appropriate range, reducing the involvement of the sealing layer of the cover material, thereby suppressing the wire drawing phenomenon while obtaining sufficient peel strength required in practical use. Therefore, the container formed by the multilayer resin sheet of Example 11 has good heat sealing properties, can be fully bonded with the cover material, can be stably peeled off, can suppress the rupture and wire drawing of the cover material, and has good incision fracture properties, which can easily separate multiple container bodies formed as an integrated container.

[0143] 《Example 12》

[0144] In Example 12, relative to Example 1, the rubber content of the polystyrene resin in the resin component of the substrate layer is changed to 7%. By changing the rubber content to 7%, the impact resistance of the multilayer resin sheet is improved. Although the number of folding times is increased and the bending angle is increased relative to other embodiments, the number of folding times of the formed molded container is still less than 5 times and the bending angle is also less than 60 degrees, so the multiple container bodies formed into an integrated container can be easily separated. In addition, in the dynamic viscoelasticity of the epidermis layer 10a in Example 12, the storage elastic modulus and the loss elastic modulus are both within the range of 1E+04Pa and less than 1E+07Pa, so the thermal deformation of the epidermis layer 10a during heat sealing is controlled within an appropriate range, reducing the involvement of the sealing layer of the cover material, thereby suppressing the wire drawing phenomenon while obtaining sufficient peeling strength required in practical use.

[0145] Comparative Example 1

[0146] On the other hand, as shown in Table 2, in Comparative Example 1, the skin layer is formed only of LDPE resin compared to Example 1. The peel strength of the molded container formed therefrom with the cover material exceeds 30N, and the index of the wire drawing phenomenon is 3. In the dynamic viscoelasticity of the skin layer, the storage elastic modulus and the loss elastic modulus are both larger than those of Example 1. Since the fluidity of the skin layer resin as the heat-sealing surface layer is large, the bonding area with the cover material becomes larger, making it difficult to peel the cover material from the container, and the wire drawing phenomenon also occurs.

[0147] Comparative Example 2

[0148] In Comparative Example 2, the skin layer is formed only of PP resin compared to Example 1. The peel strength of the molded container formed in this way with the cover material is zero, and the storage elastic modulus and loss elastic modulus of the dynamic viscoelasticity of the skin layer are smaller than those of Example 1. Since the fluidity of the skin layer resin as the heat-sealing surface layer is small, the bonding area with the cover material becomes small, and the cover material cannot be fully bonded to the container. At the same time, the folding endurance is 186 times, and multiple container bodies formed into an integrated container cannot be easily separated.

[0149] 《Comparative Example 3》

[0150] In Comparative Example 3, the skin layer was formed only of HDPE resin, as compared to Example 1. The molded container thus formed had a folding endurance of 127 times, and the plurality of container bodies formed into an integrated container could not be easily separated.

[0151] 《Comparative Example 4, Comparative Example 5, Comparative Example 6》

[0152] In Comparative Examples 4, 5 and 6, the thickness of the base layer and the outermost layer, and the composition ratio of the outermost layer were changed compared to Example 1. The molded container thus formed had a folding endurance of 5 or more times and a bending angle of 60 degrees or more, so that the multiple container bodies formed into an integrated container could not be easily separated.

[0153] Table 1

[0154] .

[0155] Table 2

[0156]

Claims

1. A multilayer resin sheet, which is a multilayer resin sheet formed by laminating a skin layer, an oxygen barrier layer, an intermediate layer, a base layer, and an outermost layer in this order via an adhesive layer, Features: The thickness of the multilayer resin sheet is 200-1300 μm; The skin layer is composed of a polyolefin resin layer, and the polyolefin resin layer contains a mixture of polyethylene resin and polypropylene resin; The polyethylene resin is low-density polyethylene, medium-density polyethylene, linear polyethylene, ethylene-αα olefin copolymer polymerized using a metallocene catalyst, ethylene-vinyl acetate copolymer, and ethylene-propylene copolymer; The middle layer is made of the same material as the epidermis layer; The substrate layer is composed of a polystyrene resin layer; The adhesive layer is composed of modified polyolefin polymer; The outermost layer is composed of a polystyrene resin layer, and the thickness of the outermost layer relative to the overall thickness of the sheet has a layer structure ratio of 1% or more and 8% or less; The mixing ratio of the polypropylene-based resin in the polyolefin-based resin layer as the skin layer is 10% to 40%.

2. The multilayer resin sheet according to claim 1, It is characterized in that The dynamic viscoelasticity of the polyolefin resin layer is such that, in a temperature range of 110° C. to 130° C., both the storage elastic modulus and the loss elastic modulus are greater than 1E+04 Pa and less than 1E+07 Pa.

3. The multilayer resin sheet according to claim 1 or 2, It is characterized in that The rubber content in the polystyrene-based resin of the base layer is 6% or less.

4. The multilayer resin sheet according to claim 3, It is characterized in that The base material layer contains 1% or more of a polyolefin resin component that is incompatible with the polystyrene resin.

5. The multilayer resin sheet according to claim 3, It is characterized in that The rubber content contained in the polystyrene-based resin of the base material layer is 3% or more and 6% or less.

6. The multilayer resin sheet according to claim 1 or 2, It is characterized in that The polyethylene resin is composed of low-density polyethylene; the polypropylene resin is composed of a random copolymer or a block copolymer.

7. A molded container formed by thermoforming the multilayer resin sheet according to any one of claims 1 to 6.