Multilayer ceramic capacitor, method for manufacturing multilayer ceramic

By plating multi-layer electrode layers on the side electrodes of the laminated ceramic capacitors to increase the thickness difference, the problem of rupture of ceramic laminated bodies caused by substrate stress is solved, and higher stability and flexural resistance are achieved.

CN118922899APending Publication Date: 2024-11-08MURATA MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026469.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-01
Filing Date
2023-03-12
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When the substrate is deflected by stress on the mounting substrate, the ceramic laminated body of the laminated ceramic capacitor is prone to fracture and fragmentation, especially near the first end face electrode and the second end face electrode.

Method used

A laminated ceramic capacitor is designed, which has a plurality of ceramic layers and an internal electrode in the height direction, and forms a multi-layer electrode structure on the main and end surfaces, by plating a multi-layer electrode layer on the side electrodes to increase the thickness, Thus, a large thickness difference is formed at the solder joint to absorb stress and reduce transmission to the ceramic laminate.

Benefits of technology

The cracking and debris of the laminate when stress is applied to the substrate is effectively suppressed, and the stability and flexural resistance of the capacitor are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922899A_ABST
    Figure CN118922899A_ABST
Patent Text Reader

Abstract

The invention provides a laminated ceramic capacitor capable of suppressing the occurrence of cracks and fragments in a laminated body even if a substrate is bent by applying stress to the mounted substrate. The laminated ceramic capacitor includes: a laminated body having a plurality of ceramic layers laminated in a height direction, a plurality of first internal electrodes, and a plurality of second internal electrodes, the first main face and the second main face are located at the positions opposite to each other in the height direction, the first end face and the second end face are located at the positions opposite to each other in the length direction orthogonal to the height direction, and the first side face and the second side face are located at the positions opposite to each other in the width direction orthogonal to the height direction and the length direction. A first end surface electrode which is formed on the first end surface, extends from the first end surface, and covers a part of the first main surface, the second main surface, the first side surface, and the second side surface; a second end surface electrode which is formed on the second end surface, extends from the second end surface, and covers a part of the first main surface, the second main surface, the first side surface, and the second side surface; a first side surface electrode which is formed on the first side surface, extends from the first side surface, and covers a part of the first main surface and the second main surface; and a second side surface electrode which is formed on the second side surface, extends from the second side surface, and covers the first main surface and a part of the second main surface, the first internal electrode is connected to the first end surface electrode and the second end surface electrode, and the second internal electrode is connected to the first side surface electrode and the second side surface electrode. The first end surface electrode and the second end surface electrode each have a first base electrode layer, a first plated electrode layer formed on the first base electrode layer, and a second plated electrode layer formed on the first plated electrode layer. Each of the first side surface electrode and the second side surface electrode has a second base electrode layer, a third plated electrode layer formed on the second base electrode layer, a fourth plated electrode layer formed on the third plated electrode layer, a fifth plated electrode layer formed on the fourth plated electrode layer, and a sixth plated electrode layer formed on the fifth plated electrode layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a laminated ceramic capacitor, and more specifically, to a laminated ceramic capacitor having a first end surface electrode, a second end surface electrode, a first side surface electrode, and a second side surface electrode. In addition, the present invention relates to a method for manufacturing a laminated ceramic capacitor suitable for manufacturing the laminated ceramic capacitor of the present invention. In addition, the present invention relates to a mounting structure of a laminated ceramic capacitor that can be implemented using the laminated ceramic capacitor of the present invention. Background Art

[0002] A so-called three-terminal multilayer ceramic capacitor is widely used for noise countermeasures, etc. For example, Patent Document 1 (Japanese Patent Application No. 2020-167236) discloses a three-terminal multilayer ceramic capacitor.

[0003] The multilayer ceramic capacitor disclosed in Patent Document 1 includes a multilayer body (capacitor element) in which a plurality of ceramic layers, a plurality of first internal electrodes, and a plurality of second internal electrodes are stacked. The multilayer body has a first main surface, a second main surface, a first end surface, a second end surface, a first side surface, and a second side surface. The first main surface is a mounting surface for mounting on a substrate or the like of the multilayer ceramic capacitor.

[0004] The laminated ceramic capacitor disclosed in Patent Document 1 comprises: a first end surface electrode formed on a first end surface of a laminated body and formed so as to extend from the first end surface and cover a first main surface, a second main surface, a first side surface, and a part of a second side surface; a second end surface electrode formed on a second end surface and formed so as to extend from the second end surface and cover a part of the first main surface, the second main surface, the first side surface, and a part of the second side surface; a first side surface electrode formed on a first side surface and formed so as to extend from the first side surface and cover a part of the first main surface and the second main surface; and a second side surface electrode formed on a second side surface and formed so as to extend from the second side surface and cover a part of the first main surface and the second main surface. A first internal electrode is connected to the first end surface electrode and the second end surface electrode, and a second internal electrode is connected to the first side surface electrode and the second side surface electrode.

[0005] In the laminated ceramic capacitor disclosed in Patent Document 1, the first end surface electrode, the second end surface electrode, the first side surface electrode, and the second side surface electrode are all formed into a multilayer structure with the same structure, and the material and thickness size of each layer are also the same. Therefore, the thickness size of the first end surface electrode, the second end surface electrode, the first side surface electrode, and the second side surface electrode are the same as each other. Therefore, when the laminated ceramic capacitor disclosed in Patent Document 1 is joined to a substrate having the first connection pad electrode to the fourth connection pad electrode (the first connection pad electrode and the first end surface electrode, the second connection pad electrode and the second end surface electrode, the third connection pad electrode and the first side surface electrode, and the fourth connection pad electrode and the second side surface electrode are joined respectively by reflow solder), the thickness size of each solder existing between the first connection pad electrode and the first end surface electrode, between the second connection pad electrode and the second end surface electrode, between the third connection pad electrode and the first side surface electrode, and between the fourth connection pad electrode and the second side surface electrode becomes the same as each other.

[0006] The multilayer ceramic capacitor disclosed in Patent Document 1 can remove unnecessary noise flowing in the line by connecting the first end surface electrode and the second end surface electrode to the middle of the power line and the signal line and connecting the first side surface electrode and the second side surface electrode to the ground potential.

[0007] Prior Art Literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application No. 2020-167236 Summary of the invention

[0010] Problem that the invention aims to solve

[0011] When the multilayer ceramic capacitor disclosed in Patent Document 1 is mounted on a substrate, if stress is applied to the substrate to cause the substrate to bend (including the case where the substrate is twisted), the stress is transmitted to the multilayer ceramic capacitor via the solder, and cracks and fragments may occur in the portion of the ceramic multilayer body where the first end surface electrode and the second end surface electrode are formed, or in the vicinity of the portion. In addition, stress is less likely to be transmitted to the portion of the multilayer body where the first side surface electrode and the second side surface electrode are formed, or in the vicinity of the portion, and cracks and fragments are less likely to occur than in the portion where the first end surface electrode and the second end surface electrode are formed, or in the vicinity of the portion.

[0012] Therefore, an object of the present invention is to provide a multilayer ceramic capacitor in which cracks and fragments can be suppressed from occurring in a multilayer body even when stress is applied to a substrate to be mounted and the substrate is bent.

[0013] Technical solutions to solve problems

[0014] The present invention is made to solve the above-mentioned conventional problems. As a means thereof, a laminated ceramic capacitor according to one embodiment of the present invention comprises: a laminated body having a plurality of ceramic layers laminated in a height direction, a plurality of first internal electrodes and a plurality of second internal electrodes, and having a first main surface and a second main surface located at opposite positions in the height direction, a first end surface and a second end surface located at opposite positions in a length direction perpendicular to the height direction, and a first side surface and a second side surface located at opposite positions in a width direction perpendicular to the height direction and the length direction; a first end surface electrode formed on the first end surface and formed to extend from the first end surface and cover a portion of the first main surface, the second main surface, the first side surface, and the second side surface; a second end surface electrode formed on the second end surface and formed to extend from the second end surface and cover a portion of the first main surface, the second main surface, the first side surface, and the second side surface; a first side surface electrode formed On the first side surface, and formed to extend from the first side surface and cover a portion of the first main surface and the second main surface; and the second side electrode, formed on the second side surface, and formed to extend from the second side surface and cover a portion of the first main surface and the second main surface, the first internal electrode is connected to the first end surface electrode and the second end surface electrode, and the second internal electrode is connected to the first side electrode and the second side electrode, wherein the first end surface electrode and the second end surface electrode respectively have a first base electrode layer, a first plated electrode layer formed on the first base electrode layer, and a second plated electrode layer formed on the first plated electrode layer, and the first side electrode and the second side electrode respectively have a second base electrode layer, a third plated electrode layer formed on the second base electrode layer, a fourth plated electrode layer formed on the third plated electrode layer, a fifth plated electrode layer formed on the fourth plated electrode layer, and a sixth plated electrode layer formed on the fifth plated electrode layer.

[0015] In addition, an embodiment of the present invention relates to a mounting structure of a type of multilayer ceramic capacitor, in which a multilayer ceramic capacitor is mounted on a substrate, wherein the multilayer ceramic capacitor comprises: a stacked body having a plurality of ceramic layers stacked in a height direction, a plurality of first internal electrodes, and a plurality of second internal electrodes, and having a first main surface and a second main surface located at opposite positions in the height direction, a first end surface and a second end surface located at opposite positions in a length direction orthogonal to the height direction, and a first side surface and a second side surface located at opposite positions in a width direction orthogonal to the height direction and the length direction; a first end surface electrode, The first internal electrode is formed on the first end surface and is formed to extend from the first end surface and cover a portion of the first main surface, the second main surface, the first side surface, and the second side surface; the second end surface electrode is formed on the second end surface and is formed to extend from the second end surface and cover a portion of the first main surface, the second main surface, the first side surface, and the second side surface; the first side surface electrode is formed on the first side surface and is formed to extend from the first side surface and cover a portion of the first main surface and the second main surface; and the second side surface electrode is formed on the second side surface and is formed to extend from the second side surface and cover a portion of the first main surface and the second main surface, and the first internal electrode is connected to the first end surface electrode. The first internal electrode is connected to the first side electrode and the second side electrode, the first end surface electrode and the second end surface electrode respectively have a first base electrode layer and a first plated electrode layer formed on the first base electrode layer, the first side electrode and the second side electrode respectively have a second base electrode layer, a third plated electrode layer formed on the second base electrode layer, a fourth plated electrode layer formed on the third plated electrode layer, and a fifth plated electrode layer formed on the fourth plated electrode layer, and the substrate has a first connection pad electrode, a second connection pad electrode, a third connection pad electrode and a fifth connection pad electrode formed on the main surface. The 4th connecting disk electrode, the 1st end surface electrode and the 1st connecting disk electrode, the 2nd end surface electrode and the 2nd connecting disk electrode, the 1st side electrode and the 3rd connecting disk electrode, and the 2nd side electrode and the 4th connecting disk electrode are respectively joined by joining materials, and the thickness dimension of the joining material between the 1st end surface electrode and the 1st connecting disk electrode and the thickness dimension of the joining material between the 2nd end surface electrode and the 2nd connecting disk electrode are respectively larger than the thickness dimension of the joining material between the 1st side electrode and the 3rd connecting disk electrode and the thickness dimension of the joining material between the 2nd side electrode and the 4th connecting disk electrode.

[0016] Effects of the Invention

[0017] In the multilayer ceramic capacitor according to one embodiment of the present invention, even if stress is applied to a substrate to be mounted and the substrate is bent, cracks and chippings in the laminate can be suppressed.

[0018] Furthermore, in the mounting structure of the multilayer ceramic capacitor according to one embodiment of the present invention, even if stress is applied to the substrate and the substrate is bent, the generation of cracks or fragments in the laminated body of the multilayer ceramic capacitor can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 1 is a perspective view of the multilayer ceramic capacitor 100 .

[0020] Figure 2 is a cross-sectional view of a laminated ceramic capacitor 100, showing Figure 1 The XX portion is indicated by a single-dot chain arrow.

[0021] Figure 3 1 is an exploded perspective view of a main part of the multilayer ceramic capacitor 100 .

[0022] Figure 4 It is an explanatory diagram (cross-sectional view) of the mounting structure 200 .

[0023] Figure 5 (A)~ Figure 5 (C) are explanatory diagrams showing steps performed in the first method of manufacturing the multilayer ceramic capacitor 100.

[0024] Figure 6 (D)~ Figure 6 (F) is Figure 5 Continuation of (C) , each is an explanatory diagram showing the steps performed in the first method of manufacturing the multilayer ceramic capacitor 100 .

[0025] Figure 7 (A)~ Figure 7 (C) are explanatory diagrams showing steps performed in the second method of manufacturing the multilayer ceramic capacitor 100.

[0026] Figure 8 (D) Figure 8 (E) is Figure 7 Continuation of (C) , each is an explanatory diagram showing the steps performed in the second method of manufacturing the multilayer ceramic capacitor 100 .

[0027] Fig. 9 (F), Fig. 9 (G) is Figure 8 Continuation of (E) , each is an explanatory diagram showing the steps performed in the second method of manufacturing the multilayer ceramic capacitor 100 . DETAILED DESCRIPTION

[0028] The following, with the attached Figure 1The embodiments of the present invention are described together. In addition, each embodiment exemplifies the embodiment of the present invention, and the present invention is not limited to the contents of the embodiment. In addition, the contents described in different embodiments can be combined and implemented, and the implementation contents in this case are also included in the present invention. In addition, the drawings are used to help understand the description, and are sometimes drawn schematically. The ratio of the dimensions of the drawn components or components is sometimes inconsistent with the ratio of these dimensions recorded in the description. In addition, there are cases where the components recorded in the description are omitted in the drawings, and the number of components is omitted and drawn.

[0029] exist Figure 1 to Figure 3 FIG. 1 shows a multilayer ceramic capacitor 100 according to an embodiment. Figure 1 1 is a perspective view of the multilayer ceramic capacitor 100 . Figure 2 is a cross-sectional view of a laminated ceramic capacitor 100, showing Figure 1 The XX portion is indicated by a single-dot chain arrow. Figure 3 1 and 1 are exploded perspective views of the main parts of the multilayer ceramic capacitor 100. In addition, in these figures, the height direction T, the length direction L, and the width direction W of the multilayer ceramic capacitor 100 are shown, and these directions may be mentioned in the following description. In addition, in this embodiment, the stacking direction of the ceramic layer 1a described later is defined as the height direction T of the multilayer ceramic capacitor 100.

[0030] The multilayer ceramic capacitor 100 includes a multilayer body 1 having a rectangular parallelepiped shape. The multilayer body 1 has a first main surface 1A and a second main surface 1B facing each other in a height direction T, a first end surface 1C and a second end surface 1D facing each other in a length direction L that is perpendicular to the height direction T, and a first side surface 1E and a second side surface 1F facing each other in a width direction W that is perpendicular to both the height direction T and the length direction L.

[0031] The dimensions of the laminate 1 are arbitrary. For example, the dimension in the longitudinal direction L can be about 100 μm to 5700 μm, the dimension in the width direction W can be about 100 μm to 5000 μm, and the dimension in the height direction T can be about 100 μm to 2500 μm.

[0032] The laminated body 1 is composed of a laminated body in which a plurality of ceramic layers 1 a , a plurality of first internal electrodes 2 , and a plurality of second internal electrodes 3 are laminated.

[0033] The material of the laminate 1 (ceramic layer 1a) is arbitrary, and for example, a dielectric ceramic mainly composed of BaTiO3 can be used. However, a dielectric ceramic mainly composed of another material such as CaTiO3, SrTiO3, or CaZrO3 may be used instead of BaTiO3.

[0034] The thickness of the ceramic layer 1 a is arbitrary, and can be set to about 0.3 μm to 2.0 μm, for example, in an effective region forming a capacitor where the first internal electrode 2 and the second internal electrode 3 are formed.

[0035] The number of ceramic layers 1 a is arbitrary, and can be, for example, 1 to 6000 layers in an effective region forming a capacitor where the first internal electrodes 2 and the second internal electrodes 3 are formed.

[0036] On the upper and lower sides of the laminate 1, the first internal electrode 2 and the second internal electrode 3 are not formed, and an outer layer (protective layer) consisting of only a ceramic layer 1a is provided. The thickness of the outer layer is arbitrary, and can be set to 15μm to 150μm, for example. In addition, the thickness of the ceramic layer 1a in the outer layer region can be greater than the thickness of the ceramic layer 1a in the effective region forming the capacitor formed with the first internal electrode 2 and the second internal electrode 3 (however, in Figure 1 to Figure 3 In the figure, the thickness of the ceramic layer 1a in the outer region and the effective region is shown as the same thickness.) In addition, the material of the ceramic layer 1a in the outer region may be different from the material of the ceramic layer 1a in the effective region.

[0037] Figure 3 The main part exploded perspective view is a diagram showing the laminate 1 exploded for each ceramic layer 1a. Figure 3 It can be seen that the first internal electrode 2 extends in the longitudinal direction L of the multilayer ceramic capacitor 100 and is led out to the first end face 1C and the second end face 1D of the multilayer body 1. The second internal electrode 3 extends in the longitudinal direction L of the multilayer ceramic capacitor 100 and is led out to the first side face 1E and the second side face 1F of the multilayer body 1. In principle, the first internal electrodes 2 and the second internal electrodes 3 are alternately stacked.

[0038] The material of the main component of the first internal electrode 2 and the second internal electrode 3 is arbitrary. In the present embodiment, Ni is used. However, other metals such as Cu, Ag, Pd, and Au may be used instead of Ni. In addition, Ni, Cu, Ag, Pd, and Au may be alloys with other metals.

[0039] The thickness of the first internal electrode 2 and the second internal electrode 3 is arbitrary, and can be set to about 0.3 μm to 1.5 μm, for example.

[0040] On the outer surface of the laminate 1 , a first end surface electrode 4 , a second end surface electrode 5 , a first side surface electrode 6 , and a second side surface electrode 7 are formed as external electrodes.

[0041] The first end surface electrode 4 is formed on the first end surface 1C, and is formed so as to extend from the first end surface 1C and cover a portion of the first main surface 1A, the second main surface 1B, the first side surface 1E, and the second side surface 1F.

[0042] The second end surface electrode 5 is formed on the second end surface 1D, and is formed so as to extend from the second end surface 1D and cover a part of the first main surface 1A, the second main surface 1B, the first side surface 1E, and the second side surface 1F.

[0043] The first side surface electrode 6 is formed on the first side surface 1E, and is formed so as to extend from the first side surface 1E and cover a part of the first main surface 1A and the second main surface 1B.

[0044] The second side surface electrode 7 is formed on the second side surface 1F, and is formed so as to extend from the second side surface 1F and cover a part of the first main surface 1A and the second main surface 1B.

[0045] The first internal electrode 2 led out to the first end surface 1C of the stacked body 1 is connected to the first end surface electrode 4. The first internal electrode 2 led out to the second end surface 1D of the stacked body 1 is connected to the second end surface electrode 5. The second internal electrode 3 led out to the first side surface 1E of the stacked body 1 is connected to the first side surface electrode 6. The second internal electrode 3 led out to the second side surface 1F of the stacked body 1 is connected to the second side surface electrode 7.

[0046] The multilayer ceramic capacitor 100 can be used as a three-terminal capacitor, for example, by dividing a power line or a signal line in the middle of a circuit, connecting the first end surface electrode 4 to one end of the division, connecting the second end surface electrode 5 to the other end of the division, and connecting the first side surface electrode 6 and the second side surface electrode 7 to a ground potential. In this case, the first internal electrode 2 becomes a through electrode, and the second internal electrode 3 becomes a ground electrode.

[0047] The first end surface electrode 4 and the second end surface electrode 5 have the same multilayer structure. Figure 2 As shown, the first end surface electrode 4 and the second end surface electrode 5 respectively include a first base electrode layer 11 formed on the outer surface of the stack 1, a first plated electrode layer 21 formed on the outer surface of the first base electrode layer 11, and a second plated electrode layer 22 formed on the outer surface of the first plated electrode layer 21.

[0048] The material of the main component of the first base electrode layer 11 is arbitrary. In this embodiment, Ni is used. However, other metals such as Cu, Ag, Pd, and Au may be used instead of Ni. In addition, Ni, Cu, Ag, Pd, and Au may be alloys with other metals.

[0049] The thickness of the first foundation electrode layer 11 is arbitrary, and for example, the thickness can be set to about 3.0 μm to 150.0 μm in the portion formed on the first principal surface 1A or the second principal surface 1B. In the present embodiment, the thickness of the first foundation electrode layer 11 on the first principal surface 1A or the second principal surface 1B is set to 9.0 μm.

[0050] In addition, the thickness dimension of the first main surface 1A or the second main surface 1B of the first base electrode layer 11 is obtained by the following method. First, a completed multilayer ceramic capacitor 100 is prepared. Next, the multilayer ceramic capacitor 100 is cut at 1 / 2 of the dimension in the width direction W, and a cross section parallel to the first side surface 1E and the second side surface 1F is observed. In this cross section, the first end surface electrode 4 and the second end surface electrode 5 are formed in the shape of a letter C (it can also be said to be the shape of a Japanese Katakana letter "コ") at both ends. That is, the first end surface electrode 4 is formed on the first main surface 1A, the first end surface 1C, and the second main surface 1B. The second end surface electrode 5 is formed on the first main surface 1A, the second end surface 1D, and the second main surface 1B. Next, among them, the maximum dimension of the first foundation electrode layer 11 formed on the first main surface 1A of the first end surface electrode 4, the maximum dimension of the first foundation electrode layer 11 formed on the second main surface 1B of the first end surface electrode 4, the maximum dimension of the first foundation electrode layer 11 formed on the first main surface 1A of the second end surface electrode 5, and the maximum dimension of the first foundation electrode layer 11 formed on the second main surface 1B of the second end surface electrode 5 are respectively obtained. Then, the average value of these four maximum dimensions is obtained, and the average value is used as the thickness dimension on the first main surface 1A or the second main surface 1B of the first foundation electrode layer 11. In addition, the thickness dimension on the first main surface 1A or the second main surface 1B of the first plated electrode layer 21 and the thickness dimension on the first main surface 1A or the second main surface 1B of the second plated electrode layer 22 are also obtained by the same method.

[0051] The material of the main component of the first plating electrode layer 21 is arbitrary, and Ni is used in the present embodiment. The first plating electrode layer 21 mainly realizes the function of improving solder heat resistance and improving bonding properties.

[0052] The thickness of the first plated electrode layer 21 is arbitrary, and for example, the thickness can be set to about 1.0 μm to 6.0 μm in the portion formed on the first main surface 1A or the second main surface 1B. In the present embodiment, the thickness of the first plated electrode layer 21 on the first main surface 1A or the second main surface 1B is set to 3.0 μm.

[0053] The material of the main component of the second plating electrode layer 22 is arbitrary, and in the present embodiment, Sn is used. The second plating electrode layer 22 mainly realizes the function of improving solderability.

[0054] The thickness of the second plated electrode layer 22 is arbitrary, and for example, the thickness can be set to about 1.5 μm to 6.0 μm in the portion formed on the first main surface 1A or the second main surface 1B. In the present embodiment, the thickness of the first plated electrode layer 21 on the first main surface 1A or the second main surface 1B is set to 3.0 μm.

[0055] According to the above results, the total thickness of the first plated electrode layer 21 and the second plated electrode layer 22 in the first main surface 1A or the second main surface 1B of the first end surface electrode 4 and the second end surface electrode 5 is about 2.5 μm to 12.0 μm. In the present embodiment, the total thickness of the first plated electrode layer 21 and the second plated electrode layer 22 in the first main surface 1A or the second main surface 1B of the first end surface electrode 4 and the second end surface electrode 5 is set to 6.0 μm.

[0056] The first side electrode 6 and the second side electrode 7 have the same multilayer structure. Figure 2 As shown, the first side electrode 6 and the second side electrode 7 respectively include a second base electrode layer 12 formed on the outer surface of the laminate 1, a third plated electrode layer 23 formed on the outer surface of the second base electrode layer 12, a fourth plated electrode layer 24 formed on the outer surface of the third plated electrode layer 23, a fifth plated electrode layer 25 formed on the outer surface of the fourth plated electrode layer 24, and a sixth plated electrode layer 26 formed on the outer surface of the fifth plated electrode layer 25. Figure 2 Although the second side electrode 7 is shown and the first side electrode 6 is not shown, the first side electrode 6 has the same structure as the second side electrode 7 .

[0057] The material of the main component of the second base electrode layer 12 is arbitrary. In this embodiment, Ni is used. However, other metals such as Cu, Ag, Pd, and Au may be used instead of Ni. In addition, Ni, Cu, Ag, Pd, and Au may be alloys with other metals.

[0058] The thickness of the second foundation electrode layer 12 is arbitrary, and for example, the thickness can be set to about 3.0 μm to 150.0 μm in the portion formed on the first principal surface 1A or the second principal surface 1B. In the present embodiment, the thickness of the first foundation electrode layer 11 on the first principal surface 1A or the second principal surface 1B is set to 9.0 μm.

[0059] In addition, the thickness dimension of the first main surface 1A or the second main surface 1B of the second base electrode layer 12 is obtained by the following method. First, a completed multilayer ceramic capacitor 100 is prepared. Next, the multilayer ceramic capacitor 100 is cut at a dimension of 1 / 2 in the length direction L, and a cross section parallel to the first end surface 1C and the second end surface 1D is observed. In this cross section, the first side electrode 6 and the second side electrode 7 are formed in the shape of a letter C (it can also be said to be the shape of a Japanese Katakana letter "コ") on both sides. That is, the first side electrode 6 is formed on the first main surface 1A, the first side surface 1E, and the second main surface 1B. The second side electrode 7 is formed on the first main surface 1A, the second side surface 1F, and the second main surface 1B. Next, among them, the maximum dimension of the second base electrode layer 12 formed on the first main surface 1A of the first side electrode 6, the maximum dimension of the second base electrode layer 12 formed on the second main surface 1B of the first side electrode 6, the maximum dimension of the second base electrode layer 12 formed on the first main surface 1A of the second side electrode 7, and the maximum dimension of the second base electrode layer 12 formed on the second main surface 1B of the second side electrode 7 are respectively calculated. Then, the average value of these four maximum dimensions is calculated, and the average value is used as the thickness dimension of the second base electrode layer 12 on the first main surface 1A or the second main surface 1B. In addition, the thickness dimension of the first principal surface 1A or the second principal surface 1B of the third plating electrode layer 23, the thickness dimension of the first principal surface 1A or the second principal surface 1B of the fourth plating electrode layer 24, the thickness dimension of the first principal surface 1A or the second principal surface 1B of the fifth plating electrode layer 25, and the thickness dimension of the first principal surface 1A or the second principal surface 1B of the sixth plating electrode layer 26 are also calculated by the same method.

[0060] The material of the main component of the third plating electrode layer 23 is arbitrary, and Ni is used in the present embodiment. The third plating electrode layer 23 mainly realizes the function of improving the bonding property.

[0061] The thickness of the third plated electrode layer 23 is arbitrary, and for example, the thickness can be set to about 1.0 μm to 6.0 μm in the portion formed on the first main surface 1A or the second main surface 1B. In the present embodiment, the thickness of the third plated electrode layer 23 on the first main surface 1A or the second main surface 1B is set to 3.0 μm.

[0062] The material of the main component of the fourth plated electrode layer 24 is arbitrary, and in the present embodiment, Sn is used. The fourth plated electrode layer 24 is provided mainly to increase the thickness of the first side electrode 6 and the second side electrode 7. In addition, when Sn is used as the material of the main component of the fourth plated electrode layer 24, since Sn is a soft material, when the multilayer ceramic capacitor 100 is mounted on a substrate, the stress transmitted from the substrate to the laminated body 1 of the multilayer ceramic capacitor 100 can be effectively absorbed by the fourth plated electrode layer 24. Therefore, it helps to suppress the occurrence of cracks and fragments in the laminated body 1.

[0063] The thickness of the fourth plated electrode layer 24 is arbitrary, and for example, the thickness can be set to about 30.0 μm to 50.0 μm in the portion formed on the first main surface 1A or the second main surface 1B. In the present embodiment, the thickness of the first plated electrode layer 21 on the first main surface 1A or the second main surface 1B is set to 40.0 μm.

[0064] The material of the main component of the fifth plating electrode layer 25 is arbitrary, and in the present embodiment, Ni is used. The fifth plating electrode layer 25 mainly realizes the function of improving solder heat resistance and improving bonding properties.

[0065] The thickness of the fifth plated electrode layer 25 is arbitrary, and for example, the thickness can be set to about 1.0 μm to 6.0 μm in the portion formed on the first main surface 1A or the second main surface 1B. In the present embodiment, the thickness of the first plated electrode layer 21 on the first main surface 1A or the second main surface 1B is set to 3.0 μm.

[0066] The material of the main component of the sixth plating electrode layer 26 is arbitrary, and in the present embodiment, Sn is used. The sixth plating electrode layer 26 mainly realizes the function of improving solderability.

[0067] The thickness of the sixth plated electrode layer 26 is arbitrary, and for example, the thickness can be set to about 1.5 μm to 6.0 μm in the portion formed on the first main surface 1A or the second main surface 1B. In the present embodiment, the thickness of the first plated electrode layer 21 on the first main surface 1A or the second main surface 1B is set to 3.0 μm.

[0068] According to the above results, the total thickness of the third plated electrode layer 23, the fourth plated electrode layer 24, the fifth plated electrode layer 25, and the sixth plated electrode layer 26 on the first main surface 1A or the second main surface 1B of the first side electrode 6 and the second side electrode 7 is about 33.5 μm to 68.0 μm. In the present embodiment, the total thickness of the third plated electrode layer 23, the fourth plated electrode layer 24, the fifth plated electrode layer 25, and the sixth plated electrode layer 26 on the first main surface 1A or the second main surface 1B of the first end surface electrode 4 and the second end surface electrode 5 is set to 49.0 μm.

[0069] As described above, the total thickness of the first plated electrode layer 21 and the second plated electrode layer 22 on the first main surface 1A or the second main surface 1B of the first end surface electrode 4 and the second end surface electrode 5 is about 2.5 μm to 12.0 μm. In contrast, the total thickness of the third plated electrode layer 23, the fourth plated electrode layer 24, the fifth plated electrode layer 25, and the sixth plated electrode layer 26 on the first main surface 1A or the second main surface 1B of the first side surface electrode 6 and the second side surface electrode 7 is about 33.5 μm to 68.0 μm. Therefore, when the total thickness dimension of the third plated electrode layer, the fourth plated electrode layer, the fifth plated electrode layer and the sixth plated electrode layer in the first main surface 1A or the second main surface 1B is set to 100%, the total thickness dimension of the first plated electrode layer 21 and the second plated electrode layer 22 in the first main surface A becomes greater than 3.68% and less than 35.8%, and becomes approximately greater than 3.6% and less than approximately 36.0%.

[0070] Table 1 shows the above relationship.

[0071] [Table 1]

[0072]

[0073] In addition, in the present embodiment, as described above, the total thickness dimension of the first plated electrode layer 21 and the second plated electrode layer 22 of the first end surface electrode 4 and the second end surface electrode 5 in the first main surface 1A or the second main surface 1B is 6.0 μm, and the total thickness dimension of the third plated electrode layer 23, the fourth plated electrode layer 24, the fifth plated electrode layer 25 and the sixth plated electrode layer 26 of the first side electrode 6 and the second side electrode 7 is 49.0 μm. Therefore, when the total thickness dimension of the third plated electrode layer 23, the fourth plated electrode layer 24, the fifth plated electrode layer 25 and the sixth plated electrode layer 26 in the first main surface 1A or the second main surface 1B is set to 100%, the total thickness dimension of the first plated electrode layer 21 and the second plated electrode layer 22 in the first main surface A is approximately 12.2%.

[0074] Assuming that the thickness dimension of the first base electrode layer 11 in the first main surface 1A or the second main surface 1B is the same as the thickness dimension of the second base electrode layer 12, the thickness dimension of the first side electrode 6 and the second side electrode 7 in the first main surface 1A or the second main surface 1B is 43.0 μm larger than the thickness dimension of the first end surface electrode 4 and the second end surface electrode 5.

[0075] (Mounting Structure 200 of Multilayer Ceramic Capacitor 100)

[0076] As an example of an installation configuration, Figure 4 A mounting structure 200 in which the multilayer ceramic capacitor 100 is mounted on the substrate 50 is shown. Figure 4 It is an explanatory diagram (cross-sectional view) of the mounting structure 200 .

[0077] A first land electrode 51, a second land electrode 52, a third land electrode 53, and a fourth land electrode 54 are formed on the main surface of the substrate 50. The first end surface electrode 4 of the multilayer ceramic capacitor 100 is bonded to the first land electrode 51 by solder 61, the second end surface electrode 5 is bonded to the second land electrode 52 by solder 62, the first side surface electrode 6 is bonded to the third land electrode 53 by solder 63, and the second side surface electrode 7 is bonded to the fourth land electrode 54 by solder 64. Figure 4 Although the portion where the first side electrode 6 is joined to the third land electrode 53 via the solder 63 is not visible, this portion has the same structure as the portion where the second side electrode 7 is joined to the fourth land electrode 54 via the solder 64 .

[0078] The solders 61, 62, 63, and 64 are solders that are supplied as paste solder to the first land electrode 51, the second land electrode 52, the third land electrode 53, and the fourth land electrode 54 before manufacturing the mounting structure 200, melted by reflow, and then cooled and resolidified. The solders 61, 62, 63, and 64 form solder molten hillocks at the joint portions.

[0079] The solders 61, 62, 63, and 64 are examples of bonding materials. However, the material of the bonding material is arbitrary and is not limited to solder, and other materials such as conductive resin may be used.

[0080] As described above, in the present embodiment, the thickness dimension of the first side electrode 6 and the second side electrode 7 in the first main surface 1A or the second main surface 1B is 43.0 μm larger than the thickness dimension of the first end surface electrode 4 and the second end surface electrode 5. Therefore, the thickness dimension of the solder 61 between the first land electrode 51 and the first end surface electrode 4 and the thickness dimension of the solder 62 between the second land electrode 52 and the second end surface electrode 5 are 43.0 μm larger than the thickness dimension of the solder 63 between the third land electrode 53 and the first side electrode 6 and the thickness dimension of the solder 64 between the fourth land electrode 54 and the second side surface electrode 7, respectively.

[0081] In the mounting structure 200 of the multilayer ceramic capacitor 100, the thickness of the solder 61 between the first land electrode 51 and the first end surface electrode 4 and the thickness of the solder 62 between the second land electrode 52 and the second end surface electrode 5 are large, respectively. Therefore, even if stress is applied to the substrate 50 and the substrate 50 is bent, the generation of cracks and fragments in the portion of the multilayer body 1 made of ceramic where the first end surface electrode 4 is formed and the vicinity of the portion and the portion where the second end surface electrode 5 is formed and the vicinity of the portion can be suppressed. That is, the solders 61 and 62 with large thickness absorb the stress transmitted from the substrate 50 and reduce the stress transmitted to the multilayer body 1. Therefore, the generation of cracks and fragments in the portion of the multilayer body 1 where the first end surface electrode 4 is formed and the vicinity of the portion and the portion where the second end surface electrode 5 is formed and the vicinity of the portion can be suppressed.

[0082] In the mounting structure 200 , it can also be considered that the multilayer ceramic capacitor 100 is supported on the substrate 50 mainly by the first side surface electrode 6 and the second side surface electrode 7 , and the first end surface electrode 4 and the second end surface electrode 5 are in a floating state.

[0083] (Experiment 1)

[0084] In order to confirm the effectiveness of the present invention, the following experiment was conducted. First, 10 multilayer ceramic capacitors according to Example 1, 10 multilayer ceramic capacitors according to Example 2, and 10 multilayer ceramic capacitors according to Comparative Example 1 were manufactured. Figure 2 The following description will be given with reference to a cross-sectional view of a multilayer ceramic capacitor 100 .

[0085] In the multilayer ceramic capacitors of Example 1, Example 2, and Comparative Example 1, the thickness dimension of the first plated electrode layer 21 of the first end surface electrode 4 and the second end surface electrode 5 on the first main surface 1A or the second main surface 1B is set to 3.0 μm, and the thickness dimension of the second plated electrode layer 22 is set to 3.0 μm.

[0086] In the multilayer ceramic capacitor of Example 1, the thickness dimension of the third plated electrode layer 23 of the first side electrode 6 and the second side electrode 7 in the first main surface 1A or the second main surface 1B is set to 3.0 μm, the thickness dimension of the fourth plated electrode layer 24 is set to 30.0 μm, the thickness dimension of the fifth plated electrode layer 25 is set to 3.0 μm, and the thickness dimension of the sixth plated electrode layer 26 is set to 3.0 μm.

[0087] In the multilayer ceramic capacitor of Example 2, the thickness dimension of the third plated electrode layer 23 of the first side electrode 6 and the second side electrode 7 in the first main surface 1A or the second main surface 1B is set to 3.0 μm, the thickness dimension of the fourth plated electrode layer 24 is set to 50.0 μm, the thickness dimension of the fifth plated electrode layer 25 is set to 3.0 μm, and the thickness dimension of the sixth plated electrode layer 26 is set to 3.0 μm.

[0088] In the multilayer ceramic capacitor of Comparative Example 1, the thickness dimension of the third plated electrode layer 23 of the first side electrode 6 and the second side electrode 7 on the first main surface 1A or the second main surface 1B is set to 0 μm, the thickness dimension of the fourth plated electrode layer 24 is set to 0 μm, the thickness dimension of the fifth plated electrode layer 25 is set to 3.0 μm, and the thickness dimension of the sixth plated electrode layer 26 is set to 3.0 μm. That is, the multilayer ceramic capacitor of Comparative Example 1 does not form the third plated electrode layer 23 and the fourth plated electrode layer 24.

[0089] Ten multilayer ceramic capacitors of Example 1, ten multilayer ceramic capacitors of Example 2, and ten multilayer ceramic capacitors of Comparative Example 1 were mounted on a substrate having a vertical dimension of 4 cm and a horizontal dimension of 10 cm.

[0090] The 30 substrates with stacked ceramic capacitors were subjected to a flexural resistance test one by one. Specifically, after fixing the two opposing sides (short sides) of the substrate, a pressure rod was placed against the central part of the back side of the substrate, and the pressure rod was pressed into the substrate in the order of 1.0 mm, 2.0 mm, 3.0 mm, 4.0 mm, 5.0 mm, 6.0 mm, and 7.0 mm to bend the substrate. Then, the cracks and fragments generated in the stacked body 1 of the stacked ceramic capacitor were observed. In addition, the amount of pressure of the pressure rod was set as the amount of deflection of the substrate.

[0091] The results of the experiment are shown in Table 2. The number of pieces in each column indicates the cumulative number of pieces in which cracks or fragments occurred among 10 pieces.

[0092] [Table 2]

[0093]

[0094] (Remarks) Thickness of each plated electrode layer of the first end surface electrode 4 and the second end surface electrode 5

[0095]

[0096] According to Table 2, for the laminated ceramic capacitor of Comparative Example 1, 4 of them had cracks and fragments at a deflection of 2.0 mm, and then as the deflection increased, the cumulative number increased, and at a deflection of 6.0 mm, all 10 had cracks and fragments. In contrast, for the laminated ceramic capacitor of Example 1 in which the thickness dimension of the fourth plated electrode layer 24 was set to 30.0 μm, although 1 of them had cracks and fragments at a deflection of 5.0 mm, only 2 of them had cracks and fragments at a deflection of 6.0 mm, and only 6 of them had cracks and fragments at a deflection of 7.0 mm. In addition, for the laminated ceramic capacitor of Example 2 in which the thickness dimension of the fourth plated electrode layer 24 was set to 50.0 μm, although 2 of them had cracks and fragments at a deflection of 7.0 mm, the remaining 8 did not have cracks and fragments. Through the above, the effectiveness of the present invention can be confirmed. In addition, it is considered that the effect of suppressing cracking and chipping becomes greater as the thickness of the fourth plating electrode layer 24 increases.

[0097] (First Method of Manufacturing Multilayer Ceramic Capacitor 100)

[0098] The multilayer ceramic capacitor 100 can be, for example, Figure 5 (A)~ Figure 6 In addition, in an actual production line, a general method is as follows, that is, a large number of laminated ceramic capacitors 100 are manufactured in batches by making and using mother ceramic green sheets and cutting the unfired mother laminated body into individual unfired laminated bodies during the process. However, here, for the sake of convenience, the case of manufacturing one laminated ceramic capacitor 100 is described.

[0099] First, make Figure 5 In the laminate 1 shown in (A), a first internal electrode 2 and a second internal electrode 3 are formed inside the laminate 1, and a first foundation electrode layer 11 and a second foundation electrode layer 12 are formed at predetermined positions on the outer surface.

[0100] Specifically, first, dielectric ceramic powder, a binder resin, a solvent, etc. are prepared and wet-mixed to prepare ceramic slurry.

[0101] Next, the ceramic slurry is applied to a carrier film in a sheet shape using a die coater, a gravure coater, a micro gravure coater, or the like, and then dried to prepare a ceramic green sheet.

[0102] Next, in order to form the first internal electrode 2 and the second internal electrode 3 on the main surface of the given ceramic green sheet, the conductive paste prepared in advance is applied (for example, printed) in a desired pattern shape. In addition, the conductive paste is not applied to the ceramic green sheet that becomes the outer layer. In addition, as for the conductive paste, for example, a conductive paste mixed with a solvent, a binder resin, a metal powder (for example, Ni powder), etc. can be used.

[0103] Next, the ceramic green sheets are stacked in a predetermined order and integrated by heat-compression bonding to produce an unfired stacked body.

[0104] Next, in order to form the first base electrode layer 11 and the second base electrode layer 12 on the outer surface of the unfired laminate, a pre-prepared conductive paste is applied in a desired shape and thickness. In addition, as for the conductive paste, for example, a conductive paste mixed with a solvent, a binder resin, a metal powder, a ceramic powder, etc. can be used.

[0105] Next, the unfired laminate is fired at a given temperature curve to complete the laminate 1. At this time, the ceramic green sheet is fired to form the ceramic layer 1a, the conductive paste applied to the main surface of the ceramic green sheet is fired to form the first internal electrode 2 and the second internal electrode 3, and the conductive paste applied to the outer surface of the unfired laminate is fired to form the first base electrode layer 11 and the second base electrode layer 12.

[0106] In addition, although in the present manufacturing method, the production of the stack 1 and the formation of the first base electrode layer 11 and the second base electrode layer 12 are simultaneously performed by simultaneous firing, it is also possible to first produce the stack 1 by firing, and then apply a conductive paste to the outer surface of the stack 1 and sinter it to form the first base electrode layer 11 and the second base electrode layer 12.

[0107] Then, if Figure 5 As shown in FIG. 2 (B), the third plated electrode layer 23 is formed on the second foundation electrode layer 12 after the first foundation electrode layer 11 is covered with the mask 71 .

[0108] Then, if Figure 5 As shown in FIG. 5 (C), the fourth plated electrode layer 24 is formed on the third plated electrode layer 23 after the first base electrode layer 11 is covered with the mask 71 .

[0109] Then, if Figure 6 As shown in (D) , the mask 71 is removed from the first underlying electrode layer 11 .

[0110] Then, if Figure 6 As shown in (E), the first plated electrode layer 21 is formed on the first base electrode layer 11 and the fifth plated electrode layer 25 is formed on the fourth plated electrode layer 24 at the same time.

[0111] Then, if Figure 6 As shown in (F), the second plated electrode layer 22 is formed on the first plated electrode layer 21, and the sixth plated electrode layer 26 is formed on the fifth plated electrode layer 25. As a result, the first end surface electrode 4, the second end surface electrode 5, the first side surface electrode 6, and the second side surface electrode 7 are formed at given positions on the outer surface of the stacked body 1, thereby completing the stacked ceramic capacitor 100.

[0112] (Second Method of Manufacturing Multilayer Ceramic Capacitor 100)

[0113] In addition, the multilayer ceramic capacitor 100 can also be Figure 7 (A)~ Fig. 9 It is manufactured by the second manufacturing method shown in (G).

[0114] First, the same method as the first manufacturing method described above is used to prepare Figure 7 In the laminate 1 shown in (A), a first internal electrode 2 and a second internal electrode 3 are formed inside the laminate 1, and a first foundation electrode layer 11 and a second foundation electrode layer 12 are formed at predetermined positions on the outer surface.

[0115] Then, if Figure 7 As shown in (B), a portion 21 a of the first plating electrode layer 21 is formed on the first foundation electrode layer 11 , and the third plating electrode layer 23 is formed on the second foundation electrode layer 12 at the same time.

[0116] Then, if Figure 7 As shown in (C), the seventh plating electrode layer 27 is formed on a portion 21 a of the first plating electrode layer 21 , and the fourth plating electrode layer 24 is formed on the third plating electrode layer 23 at the same time.

[0117] Then, if Figure 8 As shown in (D), one end of the stack 1 is immersed in the solvent 81, the seventh plated electrode layer 27 at one end of the stack 1 is peeled off and removed, and a portion 21a of the first plated electrode layer 21 is exposed at one end of the stack 1.

[0118] Then, if Figure 8 As shown in (E), the other end of the stack 1 is immersed in the solvent 81, the 7th plated electrode layer 27 at the other end of the stack 1 is peeled off and removed, and a portion 21a of the 1st plated electrode layer 21 is exposed at the other end of the stack 1.

[0119] Then, if Fig. 9As shown in (F), a portion 21a of the first plated electrode layer 21 is plated and grown to complete the first plated electrode layer 21, and at the same time, the fifth plated electrode layer 25 is formed on the fourth plated electrode layer 24. In addition, according to the second manufacturing method, the thickness dimension of the first plated electrode layer 21 becomes larger than that of the first manufacturing method.

[0120] Then, if Fig. 9 As shown in (G), the second plated electrode layer 22 is formed on the first plated electrode layer 21, and the sixth plated electrode layer 26 is formed on the fifth plated electrode layer 25. As a result, the first end surface electrode 4, the second end surface electrode 5, the first side surface electrode 6, and the second side surface electrode 7 are formed at given positions on the outer surface of the stacked body 1, thereby completing the stacked ceramic capacitor 100.

[0121] The multilayer ceramic capacitor 100 and the mounting structure 200 according to the embodiment have been described above. However, the present invention is not limited to the above-described contents, and various modifications can be made within the spirit of the invention.

[0122] For example, the material of the above-mentioned stacked body 1, the material of the main component of the first internal electrode 2 and the second internal electrode 3, the material of the main component of the first base electrode layer 11 and the second base electrode layer 12, the material of the main component of the first plated electrode layer 21, the second plated electrode layer 22, the third plated electrode layer 23, the fourth plated electrode layer 24, the fifth plated electrode layer 25, and the sixth plated electrode layer 26 are all examples and can be changed to other materials.

[0123] Furthermore, in the above-described embodiment, the first side electrode 6 and the second side electrode 7 are separate entities, but the first side electrode 6 and the second side electrode 7 may be connected and integrated on at least one of the first main surface 1A and the second main surface 1B of the stacked body 1 .

[0124] A multilayer ceramic capacitor according to one embodiment of the present invention is as described in the column of “Solution to Problem”.

[0125] It is also preferred that in the multilayer ceramic capacitor, the first plated electrode layer and the fifth plated electrode layer are made of the same material, and the second plated electrode layer and the sixth plated electrode layer are made of the same material. In this case, the first plated electrode layer and the fifth plated electrode layer, and the second plated electrode layer and the sixth plated electrode layer can be formed simultaneously, thereby improving the productivity of the multilayer ceramic capacitor.

[0126] It is also preferred that the third plated electrode layer is made of the same material as the first plated electrode layer and the fifth plated electrode layer, and the fourth plated electrode layer is made of the same material as the second plated electrode layer and the sixth plated electrode layer. In this case, only two types of plated electrode tanks need to be prepared, thereby improving the productivity of the laminated ceramic capacitor.

[0127] It is also preferred that the first and fifth plated electrode layers contain Ni as a main component, and the second and sixth plated electrode layers contain Sn as a main component. In this case, the first and fifth plated electrode layers can function mainly to improve solder heat resistance and improve bonding properties, and the second and sixth plated electrode layers can function mainly to improve solderability.

[0128] It is also preferred that the first plated electrode layer, the third plated electrode layer, and the fifth plated electrode layer contain Ni as a main component, and the second plated electrode layer, the fourth plated electrode layer, and the sixth plated electrode layer contain Sn as a main component. In this case, only two types of plated electrode tanks need to be prepared, thereby improving the productivity of the laminated ceramic capacitor.

[0129] It is also preferred that the total thickness of the third plated electrode layer, the fourth plated electrode layer, the fifth plated electrode layer, and the sixth plated electrode layer on the first main surface or the second main surface is greater than the total thickness of the first plated electrode layer and the second plated electrode layer on the first main surface or the second main surface. In this case, when the multilayer ceramic capacitor is mounted on a substrate or the like by solder, solder having a sufficiently large thickness is formed directly below the first end surface electrode and directly below the second end surface electrode, so that even if stress is applied to the substrate and the substrate is bent (including twisted), etc., the generation of cracks and fragments in the stack can be well suppressed.

[0130] It is also preferred that, when the total thickness of the third plated electrode layer, the fourth plated electrode layer, the fifth plated electrode layer, and the sixth plated electrode layer on the first main surface or the second main surface is 100%, the total thickness of the first plated electrode layer and the second plated electrode layer on the first main surface or the second main surface is 3.6% or more and 36.0% or less. If it is within this range, when the multilayer ceramic capacitor is mounted on a substrate, etc., even if stress is applied to the substrate and the substrate is bent, etc., the generation of cracks and fragments in the multilayer body can be well suppressed.

[0131] It is also preferred that the total thickness of the third plated electrode layer, the fourth plated electrode layer, the fifth plated electrode layer, and the sixth plated electrode layer on the first or second main surface is 33.5 μm or more and 68.0 μm or less, and the total thickness of the first plated electrode layer and the second plated electrode layer on the first or second main surface is 2.5 μm or more and 12.0 μm or less. If it is within this range, when the multilayer ceramic capacitor is mounted on a substrate, even if stress is applied to the substrate and the substrate is bent, etc., the generation of cracks and fragments in the stack can be well suppressed.

[0132] It is also preferred that, as specific thickness dimensions of each plating electrode layer, the thickness dimension of the third plating electrode layer on the first or second main surface is 1.0 μm or more and 6.0 μm or less, the thickness dimension of the fourth plating electrode layer on the first or second main surface is 30.0 μm or more and 50.0 μm or less, the thickness dimensions of the first and fifth plating electrode layers on the first or second main surface are 1.0 μm or more and 6.0 μm or less, respectively, and the thickness dimensions of the second and sixth plating electrode layers on the first or second main surface are 1.5 μm or more and 6.0 μm or less, respectively. If it is within this range, each plating electrode layer can fully realize its desired function.

[0133] Preferably, the thickness of the first foundation electrode layer and the second foundation electrode layer on the first main surface or the second main surface is 3.0 μm or more and 150.0 μm or less. Within this range, each foundation electrode layer can fully achieve its required function.

[0134] Preferably, the first side surface electrode and the second side surface electrode are connected to each other on at least one of the first main surface and the second main surface. Even in this case, the multilayer ceramic capacitor functions as a three-terminal capacitor.

[0135] The multilayer ceramic capacitor of the present invention can be manufactured, for example, by the following manufacturing method. The manufacturing method of the multilayer ceramic capacitor comprises: a process of making a multilayer body; a process of forming a first base electrode of a first end surface electrode, a first base electrode of a second end surface electrode, a second base electrode of a first side surface electrode, and a second base electrode of a second side surface electrode on the multilayer body; a process of forming a third plated electrode on the second base electrode; a process of forming a fourth plated electrode on the third plated electrode; a process of forming a first plated electrode on the first base electrode and a fifth plated electrode on the fourth plated electrode; and a process of forming a second plated electrode on the first plated electrode and a sixth plated electrode on the fifth plated electrode.

[0136] The multilayer ceramic capacitor of the present invention can also be manufactured, for example, by the following manufacturing method. The manufacturing method of the multilayer ceramic capacitor comprises: a process of making a stacked body; a process of forming a first base electrode of a first end surface electrode, a first base electrode of a second end surface electrode, a second base electrode of a first side surface electrode, and a second base electrode of a second side surface electrode on the stacked body; a process of forming a part of a first plated electrode on the first base electrode and a third plated electrode on the second base electrode; a process of forming a seventh plated electrode on a part of the first plated electrode and a fourth plated electrode on the third plated electrode; a process of peeling and removing the seventh plated electrode to expose a part of the first plated electrode; a process of plating and growing a part of the first plated electrode to increase the thickness dimension, thereby completing the first plated electrode layer, and a process of forming a fifth plated electrode on the fourth plated electrode; and a process of forming a second plated electrode on the first plated electrode and a sixth plated electrode on the fifth plated electrode.

[0137] It is also preferred that in the manufacturing method of these multilayer ceramic capacitors, the step of manufacturing the multilayer body and the step of forming the first base electrode of the first end surface electrode, the first base electrode of the second end surface electrode, the second base electrode of the first side surface electrode, and the second base electrode of the second side surface electrode are simultaneously performed. In this case, the productivity of the multilayer ceramic capacitor is improved.

[0138] The mounting structure of the multilayer ceramic capacitor according to one embodiment of the present invention is as described in the column of “Solution to Problem”.

[0139] In the mounting structure of the multilayer ceramic capacitor, solder, for example, can be used as the bonding material.

[0140] In the mounting structure of the multilayer ceramic capacitor, the third land electrode and the fourth land electrode are preferably integrated into one land electrode. The third land electrode and the fourth land electrode are both at ground potential and can therefore be integrated.

[0141] Description of Reference Numerals

[0142] 1: laminate;

[0143] 1a: ceramic layer;

[0144] 1A: 1st main surface;

[0145] 1B: 2nd main surface;

[0146] 1C: 1st end face;

[0147] 1D: 2nd end surface;

[0148] 1E: 1st side;

[0149] 1F: 2nd side;

[0150] 2: 1st internal electrode;

[0151] 3: Second internal electrode;

[0152] 4: 1st end surface electrode (external electrode);

[0153] 5: Second end surface electrode (external electrode);

[0154] 6: 1st side electrode (external electrode);

[0155] 7: Second side electrode (external electrode);

[0156] 11: first base electrode layer;

[0157] 12: second base electrode layer;

[0158] 21: first plated electrode layer;

[0159] 22: second plated electrode layer;

[0160] 23: third plated electrode layer;

[0161] 24: 4th plated electrode layer;

[0162] 25: 5th plated electrode layer;

[0163] 26: 6th plated electrode layer.

Claims

1. A multilayer ceramic capacitor comprising: A laminate having a plurality of ceramic layers, a plurality of first internal electrodes, and a plurality of second internal electrodes stacked in a height direction, and having a first main surface and a second main surface located at opposite positions in the height direction, a first end surface and a second end surface located at opposite positions in a length direction orthogonal to the height direction, and a first side surface and a second side surface located at opposite positions in a width direction orthogonal to the height direction and the length direction; a first end surface electrode formed on the first end surface and formed to extend from the first end surface and cover a portion of the first main surface, the second main surface, the first side surface, and the second side surface; a second end surface electrode formed on the second end surface and formed to extend from the second end surface and cover a portion of the first main surface, the second main surface, the first side surface, and the second side surface; a first side surface electrode formed on the first side surface and formed to extend from the first side surface and cover a portion of the first main surface and the second main surface; and a second side surface electrode formed on the second side surface and formed to extend from the second side surface and cover a portion of the first main surface and the second main surface; The first internal electrode is connected to the first end surface electrode and the second end surface electrode. The second internal electrode is connected to the first side electrode and the second side electrode. in, The first end surface electrode and the second end surface electrode each include a first base electrode layer, a first plated electrode layer formed on the first base electrode layer, and a second plated electrode layer formed on the first plated electrode layer. The first side electrode and the second side electrode respectively have a second base electrode layer, a third plated electrode layer formed on the second base electrode layer, a fourth plated electrode layer formed on the third plated electrode layer, a fifth plated electrode layer formed on the fourth plated electrode layer, and a sixth plated electrode layer formed on the fifth plated electrode layer.

2. The multilayer ceramic capacitor according to claim 1, wherein The first plated electrode layer and the fifth plated electrode layer are made of the same material. The second plated electrode layer and the sixth plated electrode layer are made of the same material.

3. The multilayer ceramic capacitor according to claim 2, wherein: The third plated electrode layer is made of the same material as the first plated electrode layer and the fifth plated electrode layer. The fourth plating electrode layer is made of the same material as the second plating electrode layer and the sixth plating electrode layer.

4. The multilayer ceramic capacitor according to claim 2, wherein: The first plated electrode layer and the fifth plated electrode layer contain Ni as a main component. The second plated electrode layer and the sixth plated electrode layer contain Sn as a main component.

5. The multilayer ceramic capacitor according to claim 3, wherein: The first plated electrode layer, the third plated electrode layer, and the fifth plated electrode layer contain Ni as a main component. The second plated electrode layer, the fourth plated electrode layer, and the sixth plated electrode layer contain Sn as a main component.

6. The multilayer ceramic capacitor according to any one of claims 1 to 5, wherein: The total thickness of the third plated electrode layer, the fourth plated electrode layer, the fifth plated electrode layer and the sixth plated electrode layer in the first main surface or the second main surface is greater than the total thickness of the first plated electrode layer and the second plated electrode layer in the first main surface or the second main surface.

7. The multilayer ceramic capacitor according to claim 6, wherein: When the total thickness of the third plated electrode layer, the fourth plated electrode layer, the fifth plated electrode layer, and the sixth plated electrode layer on the first main surface or the second main surface is taken as 100%, A total thickness of the first plating electrode layer and the second plating electrode layer on the first main surface or the second main surface is 3.6% or more and 36.0% or less.

8. The multilayer ceramic capacitor according to claim 6, wherein: The total thickness of the third plated electrode layer, the fourth plated electrode layer, the fifth plated electrode layer, and the sixth plated electrode layer on the first main surface or the second main surface is 33.5 μm or more and 68.0 μm or less. A total thickness of the first plating electrode layer and the second plating electrode layer on the first main surface or the second main surface is 2.5 μm or more and 12.0 μm or less.

9. The multilayer ceramic capacitor according to claim 8, wherein: The thickness of the third plated electrode layer on the first main surface or the second main surface is 1.0 μm or more and 6.0 μm or less. The thickness of the fourth plating electrode layer on the first main surface or the second main surface is 30.0 μm or more and 50.0 μm or less, The first plating electrode layer and the fifth plating electrode layer on the first main surface or the second main surface each have a thickness of 1.0 μm or more and 6.0 μm or less. The thickness of the second plating electrode layer and the sixth plating electrode layer on the first main surface or the second main surface is respectively 1.5 μm or more and 6.0 μm or less.

10. The multilayer ceramic capacitor according to any one of claims 1 to 9, wherein The thickness of the first foundation electrode layer and the second foundation electrode layer on the first main surface or the second main surface is respectively 3.0 μm or more and 150.0 μm or less.

11. The multilayer ceramic capacitor according to any one of claims 1 to 10, wherein: The first side surface electrode and the second side surface electrode are connected to each other on at least one of the first main surface and the second main surface.

12. A method for manufacturing a multilayer ceramic capacitor, comprising: A process for manufacturing the laminate; A step of forming the first base electrode of the first end surface electrode, the first base electrode of the second end surface electrode, the second base electrode of the first side surface electrode, and the second base electrode of the second side surface electrode on the stack; forming the third plated electrode on the second base electrode; forming the fourth plating electrode on the third plating electrode; forming the first plating electrode on the first base electrode and forming the fifth plating electrode on the fourth plating electrode; and A step of forming the second plating electrode on the first plating electrode and forming the sixth plating electrode on the fifth plating electrode.

13. The method for manufacturing a laminated ceramic capacitor according to claim 12, wherein: Also: A process for manufacturing the laminate; and A step of forming the first underlying electrode of the first end surface electrode, the first underlying electrode of the second end surface electrode, the second underlying electrode of the first side surface electrode, and the second underlying electrode of the second side surface electrode.

14. A method for manufacturing a multilayer ceramic capacitor, comprising: A process for manufacturing the laminate; A step of forming the first base electrode of the first end surface electrode, the first base electrode of the second end surface electrode, the second base electrode of the first side surface electrode, and the second base electrode of the second side surface electrode on the stack; forming a portion of the first plating electrode on the first base electrode and forming the third plating electrode on the second base electrode; forming a seventh plating electrode on a portion of the first plating electrode, and forming the fourth plating electrode on the third plating electrode; The step of peeling and removing the seventh plating electrode to expose a portion of the first plating electrode; A step of performing plating growth on a portion of the first plating electrode to increase the thickness dimension to complete the first plating electrode layer, and forming the fifth plating electrode on the fourth plating electrode; and A step of forming the second plating electrode on the first plating electrode and forming the sixth plating electrode on the fifth plating electrode.

15. The method for manufacturing a laminated ceramic capacitor according to claim 14, wherein: Also: A process for manufacturing the laminate; and A step of forming the first underlying electrode of the first end surface electrode, the first underlying electrode of the second end surface electrode, the second underlying electrode of the first side surface electrode, and the second underlying electrode of the second side surface electrode.

16. A mounting structure of a multilayer ceramic capacitor, wherein a multilayer ceramic capacitor is mounted on a substrate, wherein: The multilayer ceramic capacitor comprises: A laminate having a plurality of ceramic layers, a plurality of first internal electrodes, and a plurality of second internal electrodes stacked in a height direction, and having a first main surface and a second main surface located at opposite positions in the height direction, a first end surface and a second end surface located at opposite positions in a length direction orthogonal to the height direction, and a first side surface and a second side surface located at opposite positions in a width direction orthogonal to the height direction and the length direction; a first end surface electrode formed on the first end surface and formed to extend from the first end surface and cover a portion of the first main surface, the second main surface, the first side surface, and the second side surface; a second end surface electrode formed on the second end surface and formed to extend from the second end surface and cover a portion of the first main surface, the second main surface, the first side surface, and the second side surface; a first side surface electrode formed on the first side surface and formed to extend from the first side surface and cover a portion of the first main surface and the second main surface; and a second side surface electrode formed on the second side surface and formed to extend from the second side surface and cover a portion of the first main surface and the second main surface; The first internal electrode is connected to the first end surface electrode and the second end surface electrode. The second internal electrode is connected to the first side electrode and the second side electrode. The first end surface electrode and the second end surface electrode each include a first base electrode layer and a first plated electrode layer formed on the first base electrode layer. The first side electrode and the second side electrode each include a second base electrode layer, a third plated electrode layer formed on the second base electrode layer, a fourth plated electrode layer formed on the third plated electrode layer, and a fifth plated electrode layer formed on the fourth plated electrode layer. The substrate has a first land electrode, a second land electrode, a third land electrode, and a fourth land electrode formed on a main surface. The first end surface electrode and the first connection land electrode, the second end surface electrode and the second connection land electrode, the first side surface electrode and the third connection land electrode, and the second side surface electrode and the fourth connection land electrode are respectively bonded by bonding materials. The thickness dimension of the bonding material between the first end surface electrode and the first connecting disk electrode and the thickness dimension of the bonding material between the second end surface electrode and the second connecting disk electrode are respectively larger than the thickness dimension of the bonding material between the first side surface electrode and the third connecting disk electrode and the thickness dimension of the bonding material between the second side surface electrode and the fourth connecting disk electrode.

17. The mounting structure of a multilayer ceramic capacitor according to claim 16, wherein: The bonding material is solder.

18. The mounting structure of a multilayer ceramic capacitor according to claim 16 or 17, wherein: The third land electrode and the fourth land electrode are integrated into one land electrode.