Annular seal and method of manufacture

By designing a double-layer structure of the crosslinkable rubber composition in the annular seal, the problems of easy fracture and core overflow of the outer layer material is solved, and a more stable sealing effect is achieved.

CN118974454APending Publication Date: 2024-11-15NIPPON VALQUA IND LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380031821.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-17
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing manufacturing method of annular seals, the outer layer material is prone to break, the core overflows from the outer layer, and it is difficult to achieve complete coverage, resulting in poor sealing effect.

Method used

An annular seal design is adopted including a central core and an outer layer, wherein the outer layer has a thick film portion and a non-thick film portion in the cross-section in the circumference direction, and the average ratio of the thickness of the thick film portion to the non-thick film portion is from 1.05 to Between 1.20, a two-layer structure of the crosslinkable rubber composition is formed through a hot pressing process to ensure the strength of the outer layer and the stability of the core.

Benefits of technology

It effectively suppresses the cracking of the outer layer and the overflow of the central core, and improves the stability and sealing effect of the seal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974454A_ABST
    Figure CN118974454A_ABST
Patent Text Reader

Abstract

The present invention relates to an annular seal, in which the annular seal includes a core and an outer layer covering a periphery of the core, the outer layer having a thick film portion and a non-thick film portion in a cross-section in a circumferential direction. According to the present invention, there is provided an annular seal and a method of manufacturing the same, the annular seal comprising a core and an outer layer, cracking of the outer layer and overflow of the core from the outer layer being suppressed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an annular seal and also to a manufacturing method thereof. Background Art

[0002] As seals (gaskets, packings, etc.) used for various purposes, annular (O-ring) seals are known. Annular seals are often produced by, for example, placing a material in a mold and performing press molding while heating.

[0003] Japanese Patent No. 4148493 (Patent Document 1) describes a method for manufacturing a composite structure O-ring, which describes the following: a composite structure is produced by inserting an inner layer portion formed into a rope shape into the internal space of a tubular outer layer portion, cutting the composite structure and setting it in an O-ring mold, and then setting the material for the outer layer portion formed into a rope shape in the gap between the cut surfaces of the composite structure to perform pressurized and heated molding.

[0004] Japanese Patent Laid-Open No. 10-323847 (Patent Document 2) describes a method for manufacturing a composite structure O-ring, which uses a core having a shape roughly the same as that of a core material to pre-form two covering parts. After removing the core, a supercritical extraction-treated O-ring rubber core material is inserted into the cavity to form it as a whole with the covering part.

[0005] Japanese Patent Application Laid-Open No. 10-52885 (Patent Document 3) describes a method for producing a double-layered O-ring, which is characterized in that a rope-shaped body including an outer layer and an inner layer is extruded and hot-pressed to vulcanize the inner and outer layers simultaneously.

[0006] In Japanese Patent Publication No. 10-329271 (Patent Document 4), the following manufacturing methods are described as methods for manufacturing an O-ring with a double-layer structure: a manufacturing method in which an outer layer material comprising a perfluoroelastomer is formed into a strip and wound around a core material, and then heated and pressurized; and a manufacturing method in which the outer layer material is freeze-crushed to form particles, attached to the core material, and then heated and pressurized.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent No. 4148493

[0010] Patent Document 2: Japanese Patent Application Laid-Open No. 10-323847

[0011] Patent Document 3: Japanese Patent Application Laid-Open No. 10-52885

[0012] Patent Document 4: Japanese Patent Application Laid-Open No. 10-329271 Summary of the invention

[0013] Problems to be solved by the invention

[0014] In the manufacturing method described in Japanese Patent No. 4148493 (Patent Document 1), when the outer layer is expanded, the outer layer material may be broken. In addition, since a connecting member including the outer layer material is arranged at the connection, the layer structure of the connection does not have a double-layer structure. Furthermore, the process is complicated and the cost is high.

[0015] In the manufacturing method described in Japanese Patent Application Laid-Open No. 10-323847 (Patent Document 2), when integral molding is performed in a mold, the core material may overflow from the gap between the upper and lower outer layers.

[0016] In the production method described in Japanese Patent Application Laid-Open No. 10-52885 (Patent Document 3), the inner layer portion may overflow from the connection portion during molding using a mold.

[0017] In the manufacturing method described in Japanese Patent Laid-Open No. 10-329271 (Patent Document 4), when the material is simply made into a strip and wound, wrinkles are formed on the inner diameter curve of the O-ring when it is put into the mold, making it difficult to put the material in. In addition, the possibility of the core material overflowing from the gap of the strip is high, and it is difficult to deal with it. Furthermore, in the case where the outer layer material is freeze-crushed to particle it and attach it to the core material, it is difficult to completely cover the core because the material and the core material cannot be bonded by particle formation alone.

[0018] Thus, in most annular seals including a core and an outer layer, the outer layer is broken or the core overflows from the outer layer.

[0019] An object of the present invention is to provide an annular seal member including a core and an outer layer, wherein rupture of the outer layer and leakage of the core from the outer layer are suppressed, and a method for manufacturing the same.

[0020] Solutions for solving problems

[0021] The present invention provides the following annular seal and a method for manufacturing the same.

[0022] [1] An annular seal including a core and an outer layer covering the periphery of the core, wherein the outer layer has a thick film portion and a non-thick film portion in a cross section in a circumferential direction.

[0023] [2] The annular seal according to [1], wherein an average ratio of the thickness of the outer layer of the thick film portion to the thickness of the outer layer of the non-thick film portion is 1.05 or more and 1.20 or less.

[0024] [3] The annular seal according to [1] or [2], wherein a difference in diameter of a cross section of the annular seal near a boundary between the thick film portion and the non-thick film portion is 0.01 mm or less.

[0025] [4] The annular seal according to any one of [1] to [3], wherein a width of the thick film portion in the circumferential direction is 1 mm or more and 100 mm or less.

[0026] [5] An annular seal according to any one of [1] to [4], wherein the outer layer comprises at least one cross-linked product selected from the group consisting of perfluoroelastomer and fluororubber, and the core comprises at least one cross-linked product selected from the group consisting of perfluoroelastomer, fluororubber, silicone rubber and fluorosilicone rubber.

[0027] [6] A method for manufacturing an annular seal, which is a method for manufacturing an annular seal as described in any one of [1] to [5], the manufacturing method comprising the following steps: a preforming step, preparing one or more rope-shaped preforms, the rope-shaped preforms comprising an uncrosslinked core formed of a crosslinkable rubber composition for the core, and an uncrosslinked outer layer formed of a crosslinkable rubber composition for an outer layer covering the uncrosslinked core; and a hot pressing step, bringing the two ends of the rope-shaped preform into contact and placing them in a mold for hot pressing molding.

[0028] [7] The method for producing an annular seal according to [6], wherein the pre-molding step includes a step of performing extrusion molding using the cross-linkable rubber composition for the core and the cross-linkable rubber composition for the outer layer.

[0029] [8] A method for manufacturing an annular seal according to [6] or [7], wherein, in the hot pressing process, before being placed in the mold, it also includes a process of winding an uncrosslinked film layer around the seam of the two ends of the rope-like preform formed by contact, and the material constituting the uncrosslinked film layer uses a cross-linkable rubber composition for the outer layer.

[0030] [9] The method for producing an annular seal according to any one of [6] to [8], further comprising, before the hot pressing step, a step of removing the uncrosslinked core from both ends of the rope-like preform.

[0031]

[10] The method for producing an annular seal according to any one of [6] to [9], further comprising a step of heating both end portions of the rope-shaped preform before the hot pressing step.

[0032]

[11] A method for manufacturing an annular seal according to any one of [6] to

[10] , wherein the hot pressing step further includes a step of configuring a connecting member between the two ends of the rope-like preform and arranging it in the mold, the connecting member including an uncrosslinked core formed by the crosslinkable rubber composition for the core, and an uncrosslinked outer layer formed by the crosslinkable rubber composition for the outer layer and covering the periphery of the uncrosslinked core, the thickness of the uncrosslinked outer layer of the connecting member being greater than the thickness of the uncrosslinked outer layer of the rope-like preform.

[0033]

[12] The method for producing an annular seal according to any one of [6] to

[11] , wherein two or more of the rope-like preforms are connected in the hot pressing step.

[0034] Effects of the Invention

[0035] According to the present invention, there can be provided an annular seal member including a core and an outer layer, in which rupture of the outer layer and leakage of the core from the outer layer are suppressed, and a method for manufacturing the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 A schematic cross-sectional view showing an annular seal.

[0037] Figure 2 A schematic cross-sectional view of an annular seal in the circumferential direction is shown.

[0038] Figure 3 A schematic cross-sectional view of an annular seal in the circumferential direction is shown.

[0039] Figure 4 A schematic cross-sectional view of the annular seal in the circumferential direction is shown for explaining one step of a method for manufacturing the annular seal.

[0040] Figure 5 A schematic cross-sectional view of the annular seal in the circumferential direction is shown for explaining another step of the method for manufacturing the annular seal.

[0041] Figure 6 A schematic cross-sectional view of the annular seal in the circumferential direction is shown for explaining still another step of the method for manufacturing the annular seal.

[0042] Figure 7 A schematic cross-sectional view of the annular seal in the circumferential direction is shown for explaining still another step of the method for manufacturing the annular seal.

[0043] Figure 8 The cross section of the annular seal produced in Example 1 in the circumferential direction is shown. DETAILED DESCRIPTION

[0044] The following describes the embodiments of the present invention with reference to the accompanying drawings, but the present invention is not limited to the following embodiments. In all the following drawings, the scales are appropriately adjusted to facilitate understanding of the various components, and the scales of the various components shown in the drawings may not be consistent with the scales of the actual components.

[0045] <Ring seal>

[0046] The annular seal of the present invention comprises a core and an outer layer covering the periphery of the core, wherein the cross section of the outer layer in the circumferential direction has a thick film portion and a non-thick film portion.

[0047] Figure 1 Represents the cross section of an annular seal. Figure 1 The annular seal 1 shown in (a) includes a core 2 and an outer layer 3 covering the periphery of the core 2. Figure 1 As shown in (a), the cross-sectional shape of the annular seal 1 is preferably circular, but may also have other cross-sectional shapes depending on the application. Figure 1 In the embodiment, the diameter of the cross section of the annular seal 1 is the maximum dimension D of the cross section of the annular seal 1, and the thickness of the outer layer 3 is the dimension T. Figure 1 (b)].

[0048] The average ratio of the thickness of the outer layer 3 of the annular seal 1 to the thickness of the entire cross section (hereinafter also referred to as the average ratio) is preferably 1 / 50 to 1 / 3, more preferably 1 / 35 to 1 / 4. The average ratio is the average of the ratios measured at two or more cross sections randomly selected from the annular seal excluding the connection. The ratio is, for example, Figure 2 The ratio T / D is the maximum thickness T of the outer layer 3 in the cross section of the annular seal 1 to the diameter D of the cross section of the annular seal 1 including the thickness T.

[0049] The thickness T of the outer layer 3 may be, for example, 0.1 to 10 mm, preferably 0.2 to 3 mm. The diameter D of the cross section of the sealing member 1 may be, for example, 3 to 50 mm, preferably 3 to 15 mm.

[0050] Reference Figure 2 The thick film portion and the non-thick film portion are described. Figure 2 1 is a cross-sectional view of the annular seal 1 in the circumferential direction. Figure 2 The annular seal 1 shown has a thick film portion A and a non-thick film portion B in the outer layer. The outer layer of the thick film portion A has a greater thickness than the outer layer of the non-thick film portion B. The annular seal 1 has a tendency to easily suppress the breakage of the outer layer and the overflow of the core from the outer layer by having the thick film portion A and the non-thick film portion B in the outer layer portion. The boundary between the thick film portion A and the non-thick film portion B can be smoothly connected without a height difference.

[0051] The average ratio of the thickness of the outer layer of the thick film portion A to the thickness of the outer layer of the non-thick film portion B can be, for example, greater than 1.05 and less than 10, preferably greater than 1.5 and less than 8. By making the average ratio of the thickness of the outer layer of the thick film portion A to the thickness of the outer layer of the non-thick film portion B within the above range, there is a tendency to easily suppress the rupture of the outer layer and the overflow of the core from the outer layer. The average ratio of the thickness of the outer layer of the thick film portion A to the thickness of the outer layer of the non-thick film portion B is the average of the ratios of the thicknesses of the outer layers at two or more points randomly selected in the thick film portion A and the non-thick film portion B. In the annular seal 1, the thick film portion A and the non-thick film portion B may each have one, or may each have more than two. In the case where the annular seal 1 has multiple thick film portions A and non-thick film portions B, any average ratio is within the above range.

[0052] The difference in diameter of the cross section of the annular seal 1 near the boundary between the thick film portion A and the non-thick film portion B may be, for example, 0.05 mm or less, and preferably 0.

[0053] The width W of the thick film portion A in the peripheral direction may be, for example, 1 mm or more and 100 mm or less, and preferably 3 mm or more and 50 mm or less.

[0054] The outer layer 3 may have a multi-layer structure in the thick film portion A. Figure 3 The outer layer of the thick film portion A shown has a double-layer structure, which includes a first layer A1 and a second layer A2. The first layer A1 and the second layer A2 can be formed of the same material or different materials. The second layer A2 is preferably formed on the surface of the first layer A1 on the opposite side of the core 2 formed continuously with the outer layer 3 of the non-thick film portion B. The thickness of the first layer A1 can be the same as the thickness T of the outer layer 3, for example, it can be greater than 0.1 mm and less than 10 mm, preferably greater than 0.2 mm and less than 3 mm. The thickness of the second layer A2 can be, for example, greater than 0.05 mm and less than 5 mm, preferably greater than 0.1 mm and less than 3 mm.

[0055] The core 2 and the outer layer 3 may include a crosslinked product of a crosslinkable rubber composition. Hereinafter, the crosslinkable rubber composition forming the core 2 is referred to as a crosslinkable rubber composition for the core, and the crosslinkable rubber composition forming the outer layer 3 is referred to as a crosslinkable rubber composition for the outer layer. When both the crosslinkable rubber composition for the core and the crosslinkable rubber composition for the outer layer are referred to, they are also referred to as crosslinkable rubber compositions.

[0056] The crosslinkable rubber composition may include a crosslinkable rubber component. The crosslinkable rubber component can form an elastomer (crosslinked rubber) having a crosslinked structure through a crosslinking reaction. The crosslinkable rubber component may have a crosslinking site such as a carbon-carbon unsaturated group, a nitrile group, a hydroxyl group, an amino group, a carbonyl group, a halogen group, or the like.

[0057] Specific examples of cross-linkable rubber components include: perfluoroelastomer (FFKM), fluororubber (FKM), silicone rubber, fluorosilicone rubber, ethylene-propylene rubber (EPM), ethylene-propylene-diene rubber (EPDM), nitrile rubber (NBR, acrylonitrile butadiene rubber), hydrogenated nitrile rubber (HNBR, hydrogenated acrylonitrile butadiene rubber), butyl rubber (IIR), acrylic rubber. Among them, perfluoroelastomer, fluororubber, silicone rubber and fluorosilicone rubber are preferably used. In the cross-linkable rubber composition, the cross-linkable rubber component can be used alone or in combination of two or more.

[0058] Preferably, the outer layer 3 contains at least one cross-linked product selected from the group consisting of perfluoroelastomer and fluororubber, and the core 2 contains at least one cross-linked product selected from the group consisting of perfluoroelastomer, fluororubber, silicone rubber and fluorosilicone rubber. Therefore, the cross-linked rubber component in the cross-linked rubber composition for the outer layer is preferably at least one selected from the group consisting of perfluoroelastomer and fluororubber, more preferably perfluoroelastomer. The cross-linked rubber component in the cross-linked rubber composition for the core is preferably at least one selected from the group consisting of perfluoroelastomer, fluororubber, silicone rubber and fluorosilicone rubber. From the viewpoint of free radical resistance, it is advantageous that the outer layer 3 contains a cross-linked product of perfluoroelastomer. From the viewpoint of material cost, it is advantageous that the core 2 contains at least one cross-linked product selected from the group consisting of fluororubber, silicone rubber and fluorosilicone rubber.

[0059] There are no particular restrictions on perfluoroelastomers, and examples thereof include tetrafluoroethylene (TFE)-perfluoro(alkyl vinyl ether) copolymers, TFE-perfluoro(alkoxyalkyl vinyl ether) copolymers, and the like. These copolymers may further contain structural units derived from other perfluoromonomers. If a perfluoroelastomer composition containing a perfluoroelastomer is used, the ozone resistance can be further improved compared to a cross-linked rubber composition containing a fluoroelastomer containing a hydrogen atom. The cross-linked rubber composition may contain only one perfluoroelastomer, or may contain two or more perfluoroelastomers.

[0060] In the perfluoro(alkyl vinyl ether) constituting the tetrafluoroethylene (TFE)-perfluoro(alkyl vinyl ether) copolymer, the alkyl group may have 1 to 5 carbon atoms, and may be, for example, perfluoro(methyl vinyl ether), perfluoro(ethyl vinyl ether), perfluoro(propyl vinyl ether), etc. Perfluoro(methyl vinyl ether) is preferred.

[0061] In the perfluoro(alkoxyalkyl vinyl ether) forming the TFE-perfluoro(alkoxyalkyl vinyl ether) copolymer, the vinyl ether group (CF 2 =CFO-) can have 3 to 12 carbon atoms. For example, the perfluoro(alkoxyalkyl vinyl ether) can be: CF 2 =CFOCF2 CF(CF 3 )OC n F 2n+1 CF 2 =CFO(CF 2 ) 3 OC n F 2n+1 CF 2 =CFOCF 2 CF(CF 3 )O(CF 2 O) m C n F 2n+1 , or CF 2 =CFO(CF 2 ) 2 OC n F 2n+1 In the above formula, n is 1-5, for example, and m is 1-3, for example.

[0062] The perfluoroelastomer is preferably cross-linkable, and more specifically, is preferably a perfluoroelastomer obtained by further copolymerizing a cross-linking site monomer (a perfluoroelastomer further comprising a structural unit derived from a cross-linking site monomer). A cross-linking site refers to a site that can undergo a cross-linking reaction. Examples of the cross-linking site include a nitrile group, a halogen group (e.g., an I group, a Br group, etc.), and a perfluorophenyl group.

[0063] An example of a crosslinking site monomer having a nitrile group as a crosslinking site is a nitrile group-containing perfluorovinyl ether. Examples of the nitrile group-containing perfluorovinyl ether include: CF 2 =CFO(CF 2 ) n OCF(CF 3 )CN (n is, for example, 2 to 4), CF 2 =CFO(CF 2 ) n CN (n is, for example, 2 to 12), CF 2 =CFO[CF 2 CF(CF 3 )O] m (CF 2 ) n CN (n is, for example, 2, m is, for example, 1 to 5), CF 2 =CFO[CF 2 CF(CF 3 )O] m (CF 2 ) n CN (n is, for example, 1 to 4, m is, for example, 1 to 2), CF 2 =CFO[CF 2CF(CF 3 )O] n CF 2 CF(CF 3 )CN (n is, for example, 0 to 4), etc.

[0064] An example of a crosslinking site monomer having a halogen group as a crosslinking site is a halogen group-containing perfluorovinyl ether. As the halogen group-containing perfluorovinyl ether, for example, a halogen group-containing perfluorovinyl ether obtained by replacing the nitrile group with a halogen group in the specific example of the nitrile group-containing perfluorovinyl ether mentioned above can be cited.

[0065] The cross-linkable perfluoroelastomer may have a cross-linked structure in which two main chains are cross-linked.

[0066] The ratio of structural units derived from TFE / structural units derived from perfluoro(alkyl vinyl ether) or perfluoro(alkoxyalkyl vinyl ether) / structural units derived from crosslinking site monomers in the perfluoroelastomer is generally 50% to 79.6% / 20% to 49.8% / 0.2% to 5%, preferably 60% to 74.8% / 25% to 39.5% / 0.5% to 2% in terms of molar ratio. The crosslinkable rubber composition may also contain two or more perfluoroelastomers having different ratios of the structural units.

[0067] Fluororubbers include binary vinylidene fluoride rubbers such as vinylidene fluoride / hexafluoropropylene copolymers, vinylidene fluoride / tetrafluoroethylene / hexafluoropropylene copolymers, vinylidene fluoride / tetrafluoroethylene / perfluoroalkyl vinyl ether copolymers, ternary vinylidene fluoride rubbers such as vinylidene fluoride / tetrafluoroethylene / propylene copolymers, tetrafluoroethylene / propylene copolymers, ethylene / tetrafluoroethylene / perfluoromethyl vinyl ether copolymers, thermoplastic fluororubbers, and liquid fluororubbers with perfluoropolyether skeletons (e.g., "SIFEL (registered trademark)" manufactured by Shin-Etsu Chemical Co., Ltd.). Fluororubbers may be used alone or in combination of two or more.

[0068] The fluororubber may also be a fluororubber containing a functional group. The functional group may be introduced, for example, by copolymerizing a crosslinking site monomer having the functional group. The crosslinking site monomer may be a monomer containing a halogen group.

[0069] The cross-linkable rubber composition may contain a co-cross-linking agent (cross-linking aid) and arbitrarily contain a cross-linking agent corresponding to the cross-linking system of the cross-linkable rubber component. Examples of the cross-linking system of the perfluoroelastomer include: a peroxide cross-linking system, a triazine cross-linking system, an oxazole cross-linking system, an imidazole cross-linking system, a thiazole cross-linking system, and a bisphenol cross-linking system. Examples of the cross-linking system of the vinylidene fluoride rubber and the tetrafluoroethylene-propylene rubber include: a peroxide cross-linking system, a polyamine cross-linking system, and a polyol cross-linking system. The cross-linkable rubber composition may be cross-linked using any cross-linking system, or may be cross-linked using two or more cross-linking systems.

[0070] Peroxide crosslinking agents may be, for example, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (commercially available products include "Perhexa25B" and "Perhexa25B-40" manufactured by NOF Corporation); diisopropylbenzene peroxide (commercially available products include "Percumyl D" manufactured by NOF Corporation); 2,4-dichlorobenzoyl peroxide; di-tert-butyl peroxide; t-butyl dicumyl peroxide; peroxide); benzoyl peroxide (commercially available example: "NyperB" manufactured by NOF Corporation); 2,5-dimethyl-2,5-(tert-butylperoxy)hexyne-3 (commercially available example: "Perhexyne 25B" manufactured by NOF Corporation); 2,5-dimethyl-2,5-di(benzoyl peroxide)hexane; α,α'-bis(tert-butylperoxy-m-isopropyl)benzene (commercially available example: "PERBUTYLP" manufactured by NOF Corporation); tert-butylperoxyisopropyl carbonate; p-chlorobenzoyl peroxide, etc. The peroxide crosslinking agent may be used alone or in combination of two or more.

[0071] As co-crosslinking agents used in the peroxide crosslinking system, there can be listed: triallyl isocyanurate (commercially available example: "TAIC" manufactured by Mitsubishi Chemical Corporation); triallyl cyanurate; triallyl methyl acetal; triallyl trimellitate; N, N'-phenylene bismaleimide; dipropargyl terephthalate; diallyl phthalate; tetraallyl terephthalamide and other compounds (unsaturated multifunctional compounds) that can be co-crosslinked by free radicals. The co-crosslinking agent can be used alone or in combination of two or more. Among the above, from the viewpoint of reactivity and heat resistance (compression set characteristics), the co-crosslinking agent preferably includes triallyl isocyanurate.

[0072] In the triazine crosslinking system, the following crosslinking catalysts can be used: organic tin compounds; onium salts such as quaternary phosphonium salts and quaternary ammonium salts; urea; silicon nitride, etc.

[0073] Examples of the crosslinking agent used in the oxazole crosslinking system include 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (BOAP), 4,4'-sulfonylbis(2-aminophenol), and 9,9-bis(3-amino-4-hydroxyphenyl)fluorene. BOAP is preferably used.

[0074] As the crosslinking agent used in the imidazole crosslinking system and the thiazole crosslinking system, a conventionally known crosslinking agent can be used. Examples of the crosslinking agent used in the imidazole crosslinking system include 3,3',4,4'-tetraaminobenzophenone and 3,3'-diaminobenzidine.

[0075] The content of the crosslinking agent in the crosslinkable rubber composition (the total amount when two or more types are used) is, for example, 0.1 to 10 parts by mass, preferably 0.2 to 5 parts by mass, and more preferably 0.3 to 3 parts by mass, based on 100 parts by mass of the total amount of the crosslinkable rubber component.

[0076] The content of the co-crosslinking agent (the total amount when two or more kinds are used) in the crosslinkable rubber composition is, for example, 0.5 to 10 parts by mass, and preferably 1 to 8 parts by mass from the viewpoint of improving heat resistance, relative to 100 parts by mass of the total amount of the crosslinkable rubber component.

[0077] For the purpose of improving processability and adjusting physical properties, the crosslinkable rubber composition may contain additives such as anti-aging agents, antioxidants, vulcanization accelerators, processing aids (stearic acid, etc.), stabilizers, tackifiers, silane coupling agents, plasticizers, flame retardants, mold release agents, waxes, lubricants, etc. as needed. Other examples of additives are (anti) adhesion reducing agents such as fluorine oils (e.g., perfluoroethers, etc.). Only one type of additive may be used, or two or more types may be used in combination.

[0078] However, when an annular seal is used in a high temperature environment, etc., volatilization, dissolution or precipitation may occur, so the amount of additives is preferably as small as possible (for example, 10 parts by mass or less, preferably 5 parts by mass or less, more preferably 2 parts by mass or less, and further preferably 1 part by mass or less, relative to 100 parts by mass of the total amount of the cross-linkable rubber component), and ideally no additives are contained.

[0079] In addition, the cross-linkable rubber composition may contain a colorant (e.g., an inorganic pigment, an organic pigment, etc.), a filler (e.g., a fluororesin, silica, alumina, zinc oxide, titanium oxide, clay, talc, diatomaceous earth, barium sulfate, calcium carbonate, magnesium carbonate, calcium oxide, mica, graphite, aluminum hydroxide, aluminum silicate, hydrotalcite, metal powder, glass powder, ceramic powder, etc.) as needed. The filler may be used alone or in combination of two or more. The content of the filler in the cross-linkable rubber composition (the total amount when two or more are used) is, for example, 0.1 to 40 parts by mass or less relative to 100 parts by mass of the total amount of the cross-linkable rubber component, and is preferably 1 to 30 parts by mass or less from the viewpoint of improving mechanical strength, and more preferably more than 1 to 30 parts by mass or less. In this specification, in order to distinguish the filler from the organic pigment and the inorganic pigment as the above-mentioned colorant, a substance of a different type from the organic pigment and the inorganic pigment may be used.

[0080] When the cross-linkable rubber composition contains a fluororesin filler, the ozone resistance and mechanical strength of the cross-linked product can be further improved. The fluororesin can be contained in the cross-linkable rubber composition in the form of fluororesin particles, for example.

[0081] Fluororesin used as fillers are resins having fluorine atoms in the molecule, for example, polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-ethylene copolymer (ETFE), polychlorotrifluoroethylene (PCTFE), chlorotrifluoroethylene-ethylene copolymer (ECTFE), polyvinylidene fluoride (PVDF), polyvinyl fluoride (PVF), vinylidene fluoride-hexafluoropropylene copolymer (VDF-HFP copolymer), vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer (VDF-HFP-TFE copolymer), etc. Fluororesin may be used alone or in combination of two or more.

[0082] Among the above, from the viewpoint of preventing the resin from melting under high temperature environment and impairing the properties such as compression set, it is preferable to use a fluororesin having a relatively high melting point such as PFA and PTFE.

[0083] The fluororesin used as a filler may also contain a functional group. The functional group can be introduced, for example, by copolymerizing a monomer having the functional group. If the above-mentioned crosslinking site monomer is copolymerized as a monomer having a functional group, the crosslinking of the fluororesin and the perfluoroelastomer can also be carried out using the above-mentioned crosslinking agent, thereby further improving the mechanical strength of the crosslinked product of the perfluoroelastomer composition. Examples of fluororesins containing functional groups include nitrile-containing polytetrafluoroethylene described in Japanese Patent Gazette No. 2013-177631. In addition, the fluororesin may also be a modified fluororesin such as "TFM-modified PTFE" (manufactured by Dyneon).

[0084] In the case where the cross-linkable rubber composition contains a perfluoroelastomer and a fluororesin filler, for example, a perfluoroelastomer added with a fluororesin produced by the following methods can be used: 1) a method of kneading a perfluoroelastomer powder and a fluororesin powder using a mixing roll; 2) a method of melt-kneading a perfluoroelastomer powder or granules and a fluororesin powder or granules using a mixer, a twin-screw extruder or the like; and 3) a method of adding a fluororesin during the preparation stage of the perfluoroelastomer.

[0085] The method of 3) is a method of mixing an aqueous dispersion of a perfluoroelastomer and an aqueous dispersion of a fluororesin, both of which are obtained by emulsion polymerization, and then performing co-coagulation to obtain a mixture of the perfluoroelastomer and the fluororesin.

[0086] The cross-linkable rubber composition can be prepared by uniformly kneading the cross-linkable rubber component, the colorant, the cross-linking agent, the co-cross-linking agent added as needed, the filler and the additives. As a mixer, for example, a mixer, a pressure kneading machine, a closed mixer (Banbury mixer) and the like known mixers can be used. Each compounding component can be mixed and kneaded at once, or it can be mixed in multiple stages as follows: first, the components other than the components that contribute to the cross-linking reaction (cross-linking accelerator, cross-linking delay agent, cross-linking agent, etc.) in each compounding component are uniformly kneaded, and then the components that contribute to the cross-linking reaction are mixed, etc.

[0087] <Method for manufacturing annular seal>

[0088] The method for manufacturing the annular seal may include, for example, the following steps.

[0089] The preforming step prepares one or more rope-shaped preforms, wherein the rope-shaped preforms include an uncrosslinked core formed of a crosslinkable rubber composition for a core and an uncrosslinked outer layer formed of a crosslinkable rubber composition for an outer layer and covering the uncrosslinked core.

[0090] In the hot pressing step, both ends of the rope-shaped preform are brought into contact with each other and placed in a mold to perform hot pressing molding.

[0091] With regard to the annular seal, the cross-linkable rubber composition for the core, and the cross-linkable rubber composition for the outer layer, the description of the annular seal mentioned above applies.

[0092] (Preforming process)

[0093] The preforming process may include a process of extrusion molding using a cross-linkable rubber composition for the core and a cross-linkable rubber composition for the outer layer. The rope-shaped preform can be made, for example, in the following manner. First, the cross-linkable rubber composition for the core and the cross-linkable rubber composition for the outer layer are formed into a sheet using a roller to make a sheet-shaped molded object. The thickness of the sheet-shaped molded object can be, for example, more than 1 mm and less than 5 mm. Then, using a cutting machine, the sheet-shaped molded object is cut into a strip-shaped molded object with a width of, for example, more than 5 mm and less than 30 mm. Then, by putting the strip-shaped molded object of the cross-linkable rubber composition for the core and the cross-linkable rubber composition for the outer layer into a screw extruder with a crosshead and extruding it into a rope, a rope-shaped preform with a double-layer structure in which the outer layer is composed of the cross-linkable rubber composition for the outer layer and the core is composed of the cross-linkable rubber composition for the core can be obtained. The speed of extrusion into a rope can be, for example, more than 100 mm / minute and less than 1000 mm / minute.

[0094] The cross-sectional diameter of the rope-shaped preform may be, for example, 3 to 50 mm, preferably 3 to 15 mm. The outer layer thickness of the rope-shaped preform may be, for example, 0.1 to 10 mm, preferably 0.2 to 3 mm. The length of the rope-shaped preform may be, for example, 100 to 5000 mm.

[0095] The strip-shaped molded product may be produced by feeding the core cross-linkable rubber composition and the outer layer cross-linkable rubber composition into a ram extruder and extruding them into a strip shape instead of producing the sheet-shaped molded product.

[0096] The number of the prepared rope-shaped preforms may be one, or two or more, for example, 3 to 10, and can be adjusted according to the inner diameter and / or outer diameter of the annular seal.

[0097] (Hot pressing process)

[0098] In the hot pressing step, the uncrosslinked core and the uncrosslinked outer layer are heated and pressed to obtain an annular seal including the core and the outer layer, wherein the core and the outer layer contain a crosslinked product of the crosslinkable rubber composition. The heating temperature of the hot pressing molding can be, for example, about 110° C. or more and 220° C. or less.

[0099] In the hot pressing process, a mold with an annular cavity can be used to make the two ends of the rope-like preform contact and hot press, thereby making an annular seal; or feed press molding can be performed, that is, using a mold with a straight or arc-shaped cavity, first hot press molding the rope-like preform except the ends to obtain a straight or arc-shaped molded body, and then hot press molding the joint formed by making the two ends of the straight or arc-shaped molded body contact, thereby making an annular seal. In the scheme of making the two ends contact, the state of the two end faces of the rope-like preform in contact is included. The length of the joint in the circumferential direction can be, for example, more than 100 mm and less than 1200 mm. Feed press molding will be described below.

[0100] From the viewpoint of preventing the outer layer from being broken and the core from overflowing from the outer layer at the joint formed by connecting the ends of the rope-like preform, the hot pressing step may be performed before being set in the mold having an annular cavity, or before the second hot pressing step described below (before being set in the mold having a linear or arc-shaped cavity) in the case of feed press molding, and further includes the following steps: Figure 4 As shown, a step (hereinafter also referred to as step a) is performed to wind the uncrosslinked film layer 30 around the joint between the two end portions of the contacted rope-shaped preform 11.

[0101] The thickness of the uncrosslinked film layer 30 may be, for example, 0.05 mm to 5 mm, and is preferably 0.1 mm to 1 mm from the viewpoint of reducing the height difference of the outer periphery of the rope-like preform 11 .

[0102] The material constituting the uncrosslinked film layer 30 is the above-mentioned crosslinkable rubber composition for outer layer, and is preferably the same type of crosslinkable rubber composition for outer layer as that constituting the outer layer 12 of the rope-shaped preform 11 .

[0103] The uncrosslinked film layer 30 is obtained by forming the crosslinkable rubber composition for the outer layer into a sheet using a roller, cutting it into a strip-shaped molded product having a width of about 5 mm or more and 100 mm or less using a cutting machine, and further cutting the strip-shaped molded product according to the length of the seam wound around the rope-shaped preform 11. In addition, a material obtained by removing the core material from the rope-shaped preform can also be used as the uncrosslinked film layer 30.

[0104] In step a, the uncrosslinked film layer 30 may be wound around the joint of the rope-like preform 11 once or twice or more. From the viewpoint of reducing the height difference of the outer periphery of the rope-like preform 11, the uncrosslinked film layer 30 is preferably wound around the joint of the rope-like preform 11 once or twice.

[0105] The uncrosslinked film layer 30 may be integrated with the outer layer after the heat pressing process, or may be Figure 3 As shown, the thick film portion becomes the second layer A2 constituting the multi-layer structure.

[0106] From the viewpoint of preventing the core from overflowing in the joint, the method for manufacturing the annular seal of the present invention may further include the following steps before the hot pressing step or before the second hot pressing step described below: Figure 5 The process of removing the uncrosslinked core 14 from both ends of the rope-shaped preform 11 as shown in a) (hereinafter also referred to as process b). Figure 5 As shown in b), the two ends (outer layer 12) from which the uncrosslinked core has been removed are brought into contact and arranged in a mold for hot pressing, which can easily prevent the core from overflowing from the joint.

[0107] Step b may be performed before the hot pressing step, and in the case of feed press molding, may be performed before the first hot pressing step described below, or may be performed between the first hot pressing step and the second hot pressing step.

[0108] The uncrosslinked core 14 to be removed may be within a range of, for example, 0.1 mm to 20 mm from the end surface to the inside. The uncrosslinked core 14 may be removed using, for example, scissors, a scalpel, or nippers.

[0109] From the viewpoint of improving the bonding property of the ends, the method for manufacturing an annular seal of the present invention may further include a step of heating both ends of the rope-shaped preform before the hot pressing step or, in the case of feed press molding, before the second hot pressing step described below (hereinafter also referred to as step c). After step c, by bringing both ends of the rope-shaped preform into contact and placing them in a mold for hot press molding, the bonding property of the ends can be enhanced and the core can be prevented from overflowing.

[0110] In step c, Figure 6 As shown in a), the heater 20 is sandwiched between the two ends of the rope-shaped preform 11, the end surface is heated to melt, and then, as shown in Figure 6 As shown in b), the molten ends are brought into contact with each other.

[0111] From the viewpoint of preventing the core from overflowing in the joint, the method for manufacturing the annular seal of the present invention may further include the following steps in the hot pressing step or in the case of feed press molding: Figure 7As shown in the figure, a process (hereinafter also referred to as process d) is to arrange the connecting member 40 between the two ends of the rope-like preform 11 placed in the mold and place it in the mold. In the case where the thickness of the uncrosslinked outer layer 42 of the connecting member 40 is greater than the thickness of the uncrosslinked outer layer 12 of the rope-like preform 11, it is easy to prevent the core in the joint from overflowing during hot pressing.

[0112] The ratio of the thickness of the uncrosslinked outer layer 42 of the connecting member 40 to the thickness of the uncrosslinked outer layer 12 may be, for example, about 1.1 to 10. The length of the connecting member 40 in the circumferential direction may be, for example, about 5 mm to 100 mm.

[0113] From the viewpoint of reducing the height difference of the outer periphery of the annular seal, the cross-sectional diameter of the connecting member 40 is preferably the same as or substantially the same as the cross-sectional diameter of the rope-like preform 11 , or larger than the cross-sectional diameter of the rope-like preform 11 .

[0114] The connecting member 40 may include an uncrosslinked core 41 formed of a crosslinkable rubber composition for a core described below, and an uncrosslinked outer layer 42 formed of a crosslinkable rubber composition for an outer layer described below and covering the periphery of the uncrosslinked core 41. The material constituting the uncrosslinked core 41 is preferably a crosslinkable rubber composition for a core of the same type as the crosslinkable rubber composition for a core constituting the uncrosslinked core 13 of the rope-shaped preform 11. The material constituting the uncrosslinked outer layer 42 is preferably a crosslinkable rubber composition for an outer layer of the same type as the crosslinkable rubber composition for an outer layer constituting the uncrosslinked outer layer 12 of the rope-shaped preform 11.

[0115] The hot pressing step including at least one of step a and step d tends to easily provide an annular seal including a core and an outer layer covering the core, wherein the outer layer has a thick film portion and a non-thick film portion in a cross section in the circumferential direction.

[0116] The method for producing an annular seal may further include a secondary crosslinking step after the hot pressing step to promote crosslinking of uncrosslinked or insufficiently crosslinked portions. The heating temperature in the secondary crosslinking step may be, for example, about 150° C. to 310° C.

[0117] (Feed Press Forming)

[0118] In the case where feed press molding is performed in a hot pressing process, the feed press molding may include the following processes.

[0119] In the first hot pressing step, the rope-shaped preform is placed in a first mold and the rope-shaped preform is hot-pressed except for the end portions.

[0120] In the second hot pressing step, both ends of the rope-shaped preform are brought into contact with each other and placed in a second mold to perform hot pressing molding.

[0121] In the first hot pressing step, the rope-shaped preform can be made to be in a cross-linked state except for the end. The first mold in which the rope-shaped preform is set in the first hot pressing step can have a straight or arc-shaped cavity. After the rope-shaped preform is set in the first mold, it can be pressurized while being heated by a C-type press. The temperature of the hot pressing molding in the first hot pressing step can be, for example, about 110°C or more and 220°C or less.

[0122] As a method of hot press molding the portion other than the end of the rope-like preform, for example, there can be cited a method of cooling the portion of the first mold corresponding to the end of the rope-like preform using a cooling device, etc. The length of the cooled portion can be set to the length of the end of the rope-like preform in the circumferential direction in the uncrosslinked state or the insufficiently crosslinked state, and can be, for example, 1 mm or more and 600 mm or less.

[0123] In the second hot pressing step, the ends of the rope-like preform are brought into contact with each other and placed in the second mold for hot pressing, so that the ends of the rope-like preform can be joined in a cross-linked state. An annular seal can be obtained by repeatedly joining the ends of two or more rope-like preforms to each other, or by joining the ends of one rope-like preform to each other.

[0124] The second mold in which the two ends of the rope-like preform are arranged may have a straight or arc-shaped cavity. The width of each of the two ends of the rope-like preform arranged in the second mold in the circumferential direction may be, for example, 50 mm or more and 600 mm or less. The two ends may be the two ends of one rope-like preform or one end of each of two rope-like preforms.

[0125] The temperature of the hot press molding in the second hot press step can be, for example, about 110° C. to 220° C. From the viewpoint of preventing cracks in the joint and overflow of the core, the temperature of the hot press molding in the second hot press step is preferably lower than the temperature of the hot press molding in the first hot press step, and more preferably 5° C. to 20° C. lower than the temperature of the hot press molding in the first hot press step.

[0126] Example

[0127] Hereinafter, the present invention will be described in further detail by way of Examples. Unless otherwise specified, "%" and "parts" in Examples are by mass % and by mass parts.

[0128] <Example 1>

[0129] The perfluoroelastomer is combined with 1 part by mass of a crosslinking agent (Perhexa25B) and 2 parts by mass of a crosslinking aid (TAIC) relative to 100 parts by mass of the perfluoroelastomer, and kneaded using a kneader to prepare a crosslinkable rubber composition for the outer layer. Next, the fluororubber is combined with 1 part by mass of a crosslinking agent (Perhexa25B) and 3 parts by mass of a crosslinking aid (TAIC) relative to 100 parts by mass of the fluororubber, and kneaded using a kneader to prepare a crosslinkable rubber composition for the core. Next, the crosslinkable rubber composition for the outer layer and the crosslinkable rubber composition for the core are formed into sheets in a manner of about 3 mm in thickness using a roller, and are cut into strips of about 15 mm in width using a cutting machine. The crosslinkable rubber composition for the outer layer and the crosslinkable rubber composition for the core formed into a strip are put into a screw extruder with a crosshead to prepare five rope-shaped preforms with a double-layer structure in which the outer layer is formed by the crosslinkable rubber composition for the outer layer and the core is formed by the crosslinkable rubber composition for the core. The cross-sectional diameter of the rope-shaped preform was about 7 mm, the thickness of the outer layer was about 1 mm, and the length was 800 mm.

[0130] The cross-linkable rubber composition for an outer layer was formed into a sheet using a roll so as to have a thickness of about 0.5 mm, and cut into a sheet-like molded product of 15 mm in width and 26 mm in length to prepare a sheet-like molded product for an uncross-linked film layer.

[0131] Next, five rope-shaped preforms were respectively placed in a linear first mold (length 800 mm, cavity size 7 mm), and the two ends (width of a single end 100 mm) were cooled in a manner such that they were in an uncross-linked state, while the parts other than the two ends were hot-pressed at a temperature of 165°C using a C-type press.

[0132] After the ends of one side of each of the two rope-shaped preforms after hot press molding are brought into contact, the sheet-shaped molding for the uncrosslinked film layer is wound around the joint of the two ends for 1.5 turns, and then set in the second mold for the joint, and the joint is hot press molded at a temperature of 160°C. The same operation is performed on the ends of the remaining rope-shaped preforms to join five rope-shaped preforms, thereby obtaining an annular seal. The obtained annular seal is subjected to secondary crosslinking at a temperature of 200°C. It was confirmed that in the obtained annular seal, the core in the joint will not overflow from the outer layer. In the obtained annular seal, the thickness of the outer layer of the thick film part (the part wound with the uncrosslinked film layer) is 1.6 mm, the diameter of the cross section is 7.1 mm and the width is 10 mm, and the thickness of the outer layer of the non-thick film part is 1 mm, and the diameter of the cross section is 7.1 mm. The average ratio of the thickness of the outer layer of the thick film portion to the thickness of the outer layer of the non-thick film portion was 1.6, and the difference in diameter of the cross section of the annular seal near the boundary between the thick film portion and the non-thick film portion was 0.05 mm or less. The cross section of the manufactured annular seal in the circumferential direction is shown in FIG. Figure 8 middle.

[0133] Description of Reference Numerals

[0134] 1, 50: annular seal; 2: core; 3, 53: outer layer; 11: rope-shaped preform; 12: uncross-linked outer layer; 13: uncross-linked core; 14: removed uncross-linked core; 20: heater; 30: uncross-linked film layer; 40: connecting member; 41: uncross-linked core; 42: uncross-linked outer layer; 51: first part; 52: second part; A: thick film part; A1: first layer; A2: second layer; B: non-thick film part; T: thickness of outer layer; D: diameter of cross section; W: width of thick film part.

Claims

1. An annular seal, wherein: The annular seal comprises a core and an outer layer covering the periphery of the core. The cross section of the outer layer in the circumferential direction has a thick film portion and a non-thick film portion.

2. The annular seal according to claim 1, wherein: An average ratio of the thickness of the outer layer of the thick film portion to the thickness of the outer layer of the non-thick film portion is 1.05 or more and 10 or less.

3. The annular seal according to claim 1 or 2, wherein: The difference in diameter of the cross section of the annular seal near the boundary between the thick film portion and the non-thick film portion is 0.05 mm or less.

4. The annular seal according to any one of claims 1 to 3, wherein: The width of the thick film portion in the circumferential direction is 1 mm or more and 100 mm or less.

5. The annular seal according to any one of claims 1 to 4, wherein: The outer layer comprises at least one cross-linked product selected from the group consisting of perfluoroelastomer and fluororubber, and the core comprises at least one cross-linked product selected from the group consisting of perfluoroelastomer, fluororubber, silicone rubber and fluorosilicone rubber.

6. A method for manufacturing an annular seal, which is the method for manufacturing an annular seal according to any one of claims 1 to 5, the manufacturing method comprising the following steps: a preforming step of preparing one or more rope-shaped preforms, wherein the rope-shaped preforms include an uncrosslinked core formed of a crosslinkable rubber composition for a core, and an uncrosslinked outer layer formed of a crosslinkable rubber composition for an outer layer and covering the uncrosslinked core; and In the hot pressing step, both ends of the rope-shaped preform are brought into contact with each other and placed in a mold to perform hot pressing molding.

7. The method for manufacturing an annular seal according to claim 6, wherein: The pre-molding step includes a step of performing extrusion molding using the cross-linkable rubber composition for the core and the cross-linkable rubber composition for the outer layer.

8. The method for manufacturing an annular seal according to claim 6 or 7, wherein: In the hot pressing process, before being placed in the mold, it also includes a step of winding an uncrosslinked film layer around the joint between the two ends of the contacted rope-like preform, and the material constituting the uncrosslinked film layer uses a crosslinkable rubber composition for the outer layer.

9. The method for manufacturing an annular seal according to any one of claims 6 to 8, wherein: Before the hot pressing step, the method further includes removing the uncrosslinked core from both ends of the rope-shaped preform.

10. The method for manufacturing an annular seal according to any one of claims 6 to 9, wherein: Before the hot pressing step, the method further includes heating both end portions of the rope-shaped preform.

11. The method for manufacturing an annular seal according to any one of claims 6 to 10, wherein: The hot pressing step further includes a step of disposing a connecting member between the two ends of the rope-shaped preform and placing the connecting member in the mold. The connecting member includes an uncrosslinked core formed by the crosslinkable rubber composition for the core, and an uncrosslinked outer layer formed by the crosslinkable rubber composition for the outer layer and covering the uncrosslinked core. The thickness of the uncrosslinked outer layer of the connecting member is greater than the thickness of the uncrosslinked outer layer of the rope-shaped preform.

12. The method for manufacturing an annular seal according to any one of claims 6 to 11, wherein: In the hot pressing step, two or more of the rope-shaped preforms are connected together.

Citation Information

Patent Citations

  • Rubber molding of two-layer structure and its manufacture

    JP1998052885A