Glass products
By introducing a lithium aluminosilicate structure and multi-stage ion exchange treatment into glass products, a specific stress distribution is formed, which solves the problem of existing glass products being easily damaged in electronic devices and achieves high strength and anti-cracking effects.
Patent Information
- Application Number
- CN202011469159.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-17
- Filing Date
- 2020-12-15
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-12-15
AI Technical Summary
Existing glass products in portable electronic devices are easily damaged by external impacts, and it is difficult to balance thin thickness and strength requirements.
By introducing a lithium aluminosilicate structure into glass products and using multi-stage ion exchange treatment, a specific stress distribution pattern is formed, including compression zones and tensile zones, to increase the strength and anti-cracking ability of the glass.
The high strength of glass products is achieved, which can effectively resist external impact, prevent cracks and breaks, and meet the needs of lightweight and high transmittance.
Smart Images

Figure CN112979158B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to and all benefits derived from Korean Patent Application No. 10-2019-0169013, filed on December 17, 2019, the entire contents of which are incorporated herein by reference. Technical Field
[0003] Exemplary embodiments of the present invention relate to glass articles and methods for making glass articles. Background Art
[0004] Glass products are widely used in electronic devices or building materials including display devices. Glass products are applied to substrates of flat panel display devices such as organic light emitting diode ("OLED") displays, micro LED displays, nano LED displays, quantum dot light emitting displays, liquid crystal displays, plasma displays, field emission displays, electrophoretic displays, and electrowetting displays, or applied to windows for protecting substrates.
[0005] As portable electronic devices such as smartphones and tablet personal computers ("PCs") become popular, glass products applied to portable electronic devices are often subjected to external impacts. Accordingly, it is desired to apply a glass product that is thin for the portability of such electronic devices and has good strength against external impacts. Summary of the invention
[0006] Exemplary embodiments of the present invention provide a method for manufacturing a glass product having good strength.
[0007] Exemplary embodiments of the present invention also provide glass articles having good strength.
[0008] However, the features of the present invention are not limited to those set forth herein. The above and other features of the present invention will become more apparent to those skilled in the art to which the present invention pertains by referring to the detailed description of the present invention given below.
[0009] An exemplary embodiment of a glass article containing lithium aluminosilicate includes a first surface, a second surface opposite to the first surface, a first compression zone extending from the first surface to a first compression depth, a second compression zone extending from the second surface to a second compression depth, and a tensile zone arranged between the first compression depth and the second compression depth, wherein the stress distribution of the first compression zone has a first local minimum point and a first local maximum point, the stress distribution is convex downward at the first local minimum point, and the stress distribution is convex upward at the first local maximum point, wherein the depth of the first local maximum point is greater than the depth of the first local minimum point, and wherein the stress of the first local maximum point is greater than the compressive stress of the first local minimum point.
[0010] Another exemplary embodiment of a glass article comprising lithium aluminosilicate includes a first surface, a second surface opposite to the first surface, a first compression zone extending from the first surface to a first compression depth, a second compression zone extending from the second surface to a second compression depth, and a tensile zone arranged between the first compression depth and the second compression depth, wherein the stress distribution of the first compression zone includes a crack prevention zone having a peak, and the crack prevention zone is arranged in a depth interval of 30 micrometers (μm) to 70 μm.
[0011] An exemplary embodiment of a method for manufacturing a glass product includes: providing LAS-type glass, immersing the LAS-type glass in a first mixed molten salt, immersing the LAS-type glass immersed in the first mixed molten salt in a second mixed molten salt, immersing the LAS-type glass immersed in the second mixed molten salt in a third mixed molten salt, and immersing the LAS-type glass immersed in the third mixed molten salt in a fourth mixed molten salt, wherein each of the first mixed molten salt to the fourth mixed molten salt includes sodium ions and potassium ions, wherein the order in which the proportion of sodium ions in the cations of the mixed molten salts is larger is the third mixed molten salt, the first mixed molten salt, the second mixed molten salt, the first mixed molten salt, and the fourth mixed molten salt, and wherein the order in which the proportion of potassium ions in the cations of the mixed molten salts is larger is the fourth mixed molten salt, the second mixed molten salt, the first mixed molten salt, and the third mixed molten salt.
[0012] The glass article in the exemplary embodiment may have high strength such that it is not easily broken by external impact.
[0013] In an exemplary embodiment of a method for manufacturing a glass product, it is possible to provide a glass product having high strength such that it is not easily broken by external impact.
[0014] The effects of the present invention are not limited to the above-mentioned effects, and various other effects are included in the specification. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The above and other exemplary embodiments and features of the present invention will become more apparent by describing in detail exemplary embodiments of the present invention with reference to the accompanying drawings, in which:
[0016] Figure 1 is a perspective view of an exemplary embodiment of a glass article;
[0017] Figure 2 is a cross-sectional view showing an exemplary embodiment in which a glass article is applied to a cover window of a display device;
[0018] Figure 3 is a cross-sectional view of an exemplary embodiment of a glass article having a flat plate shape;
[0019] Figure 4 is a graph illustrating an exemplary embodiment of stress distribution of a glass article;
[0020] Figure 5 yes Figure 4 An enlarged curve diagram of the vicinity of the first compression zone;
[0021] Figure 6 It is schematically shown Figure 5 A diagram showing a straight line diagram approximating the stress distribution of ;
[0022] Figure 7 yes Figure 5 An enlarged curve diagram of the vicinity of the first crack prevention zone in FIG.
[0023] Figure 8 is a flow chart of an exemplary embodiment of a method for making a glass article;
[0024] Fig. 9 is a schematic diagram showing an exemplary embodiment of an ion exchange treatment for a first strengthening operation in a method for manufacturing a glass article;
[0025] Fig.10 is a graph showing stress distribution of a glass product that has been subjected to a first strengthening operation;
[0026] Fig.11 is a schematic diagram showing an exemplary embodiment of an ion exchange treatment for a second strengthening operation in a method for manufacturing a glass article;
[0027] Fig.12 is a graph showing stress distribution of a glass product that has been subjected to a second strengthening operation;
[0028] Fig.13 is a schematic diagram showing an exemplary embodiment of an ion exchange treatment for a third strengthening operation in a method for manufacturing a glass article;
[0029] Fig.14 is a graph showing stress distribution of a glass product that has been subjected to a third strengthening operation; and
[0030] Fig.15 is a schematic diagram illustrating an exemplary embodiment of an ion exchange treatment of a fourth strengthening operation in a method for manufacturing a glass article. DETAILED DESCRIPTION
[0031] Now, hereinafter, with reference to the accompanying drawings showing preferred embodiments of the present invention, exemplary embodiments of the present invention will be described more fully. However, the present invention can be implemented in different forms and should not be construed as being limited to the exemplary embodiments set forth herein. On the contrary, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art.
[0032] It will also be understood that when a layer is referred to as being "on" another layer or substrate, it can be directly on the other layer or substrate, or intervening layers may also be present. In contrast, when an element is referred to as being "directly on" another element, there are no intervening elements present.
[0033] For ease of description, spatial relational terms such as "under", "below", "lower", "above", "upper", etc. may be used herein to describe the relationship of one element or feature to another (multiple) element or another (multiple features) as shown in the figure. It will be understood that the spatial relational terms are intended to cover different orientations of the device in use or operation other than the orientation depicted in the figure. For example, if the device in the figure is turned over, the elements described as "under" or "below" other elements or features will be oriented to be "above" other elements or features. Therefore, the exemplary term "under" can include both upper and lower orientations. The device can be oriented in other ways (rotated 90 degrees or located in other orientations), and the spatial relational descriptors used in this article are interpreted accordingly.
[0034] As used herein, "about" or "approximately" includes the referenced value and means within an acceptable range of deviation for the particular value as determined by one of ordinary skill in the art, taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" can mean within one or more standard deviations or within ±30%, ±20%, ±10%, ±5% of the referenced value.
[0035] Like reference numerals refer to like parts throughout the specification.
[0036] As used herein, the term "glass article" refers to an article made entirely or partially of glass.
[0037] Hereinafter, exemplary embodiments of the present invention will be described with reference to the accompanying drawings.
[0038] Figure 1 is a perspective view of an exemplary embodiment of a glass article.
[0039] Glass is used as a cover window for protecting a display, a substrate for a display panel, a substrate for a touch panel, an optical member such as a light guide plate, etc. in electronic devices including displays such as tablet personal computers ("PCs"), notebook PCs, smart phones, e-books, televisions, and PC monitors, and refrigerators and washing machines including display screens. Glass may also be employed as a cover glass for an instrument panel of a vehicle, a cover glass for a solar cell, an interior material for a building material, a window for a building and a house, etc.
[0040] Some glass products are expected to have high strength. For example, when glass is used as a window, it is expected to have a small thickness to meet the requirements of high transmittance and light weight, and it is also expected to have strength so that it is not easily broken by external impact. Strengthened glass can be manufactured by, for example, chemical strengthening or thermal strengthening. Examples of strengthened glass having various shapes are as follows: Figure 1 as shown in .
[0041] Reference Figure 1 In an exemplary embodiment, the glass article 100 (hereinafter, also referred to as a "cover window") may have a flat sheet shape or a flat plate shape. In another exemplary embodiment, the glass articles 101, 102, and 103 may have a three-dimensional shape including a curved portion. In an exemplary embodiment, for example, the edge of the flat portion may be curved (e.g., the glass article 101), or the flat portion may be integrally bent (e.g., the glass article 102) or folded (e.g., the glass article 103). The glass articles 101, 102, and 103 may include a first surface US, a second surface RS, and a side surface SS.
[0042] The planar shape of the glass articles 100 to 103 may be a rectangle, but is not limited thereto, and may have various shapes such as a rectangular shape with rounded corners, a square shape, a circular shape, and an elliptical shape. In the following embodiments, a flat plate having a rectangular planar shape is described as an example of the glass articles 100 to 103, but the present invention is not limited thereto.
[0043] Figure 2 is a cross-sectional view showing an exemplary embodiment in which a glass article is applied to a cover window of a display device.
[0044] Reference Figure 2 , the display device 500 may include a display panel 200, a cover window 100 disposed on the display panel 200, and an optically transparent bonding layer 300 disposed between the display panel 200 and the cover window 100 to bond the display panel 200 and the cover window 100 to each other.
[0045] Examples of display panel 200 may include not only self-luminous display panels such as organic light emitting diode (“OLED”) display panels, inorganic electroluminescent (“EL”) display panels, quantum dot (“QED”) display panels, micro LED display panels, nano LED display panels, plasma display panels (“PDP”), field emission display (“FED”) panels, and cathode ray tube (“CRT”) display panels, but may also include light receiving display panels such as liquid crystal display (LCD) panels and electrophoretic display (EPD) panels.
[0046] The display panel 200 includes a plurality of pixels PX, and an image can be displayed by light emitted from each pixel PX. The display device 500 may further include a touch member (not shown). In an exemplary embodiment, the touch member may be embedded in the display panel 200. In an exemplary embodiment, for example, since the touch member is directly arranged on the display member of the display panel 200, the display panel 200 itself may perform a touch function. In another exemplary embodiment, the touch member may be manufactured separately from the display panel 200, and then attached to the top surface of the display panel 200 through an optically transparent bonding layer.
[0047] The cover window 100 is arranged on the display panel 200. The cover window 100 is used to protect the display panel 200. The tempered glass article 100 may be applied to the main body of the cover window 100. Since the cover window 100 is larger in size than the display panel 200, the side surface of the cover window 100 may protrude outward from the side surface of the display panel 200, but is not limited thereto. The cover window 100 may further include a printed layer arranged on at least one surface of the glass article 100 at an edge portion of the glass article 100. The printed layer of the cover window 100 may prevent the frame area of the display device 500 from being visible from the outside, and may perform a decorative function in some cases.
[0048] The optically transparent bonding layer 300 is disposed between the display panel 200 and the cover window 100. The optically transparent bonding layer 300 is used to fix the cover window 100 to the display panel 200. For example, the optically transparent bonding layer 300 may include an optically clear adhesive ("OCA"), an optically clear resin ("OCR"), and the like.
[0049] Hereinafter, the strengthened glass article 100 will be described in more detail.
[0050] Figure 3 is a cross-sectional view of an exemplary embodiment of a glass article having a flat plate shape.
[0051] Reference Figure 3 The glass article 100 may include a first surface US, a second surface RS and a side surface SS (refer to Figure 1). In the glass article 100 having a flat plate shape, the first surface US and the second surface RS are main surfaces having a large area, and the side surfaces are outer surfaces connecting the first surface US and the second surface RS.
[0052] The first surface US and the second surface RS are opposite to each other in the thickness direction. When the glass article 100 is used to transmit light in the same manner as the cover window 100 of a display, light may be mainly incident on one of the first surface US and the second surface RS and pass through the other.
[0053] The thickness t of the glass article 100 is defined as the distance between the first surface US and the second surface RS. For example, the thickness t of the glass article 100 may be in the range of 0.1 to 2 millimeters (mm), but is not limited thereto. In an exemplary embodiment, for example, the thickness t of the glass article 100 may be about 1.5 mm or less. In another exemplary embodiment, for example, the thickness t of the glass article 100 may be about 1.2 mm or less. In another exemplary embodiment, for example, the thickness t of the glass article 100 may be about 1.0 mm or less. In another exemplary embodiment, for example, the thickness t of the glass article 100 may be about 0.8 mm or less. In another exemplary embodiment, for example, the thickness t of the glass article 100 may be about 0.75 mm or less. In another exemplary embodiment, for example, the thickness t of the glass article 100 may be about 0.6 mm or more. In another exemplary embodiment, for example, the thickness t of the glass article 100 may be about 0.65 mm or more. In some specific embodiments, for example, the thickness t of the glass article 100 may be in the range of 0.6 mm to 0.8 mm, or in the range of 0.65 mm to 0.75 mm. The glass article 100 may have a uniform thickness t, but is not limited thereto, and may have a different thickness t for each region.
[0054] The glass article 100 may be strengthened to have a predetermined stress distribution therein. Compared with the glass article 100 before strengthening, the strengthened glass article 100 more effectively prevents the generation of cracks, the propagation of cracks, breakage, etc. caused by external impact. The glass article 100 strengthened by the strengthening process may have different stresses for each zone. In an exemplary embodiment, for example, the compression zones CSR1 and CSR2 to which the compressive stress is applied may be arranged near the surface of the glass article 100, that is, close to the first surface US and the second surface RS, and the tensile zone CTR to which the tensile stress is applied may be arranged inside the glass article 100. The boundary between the compression zone CSR1 or CSR2 and the tensile zone CTR may have a zero stress value. The compressive stress in one compression zone CSR1 or CSR2 may have different stress values depending on the position (that is, the depth from the surface). In addition, the tensile zone CTR may have different stress values depending on the depth from the surface US or RS.
[0055] The position of the compression region CSR1 or CSR2 in the glass article 100, the stress distribution in the compression region CSR1 or CSR2, the compression energy of the compression region CSR1 or CSR2, the tensile energy of the tensile region CTR, etc. have a great influence on the mechanical properties (such as surface strength) of the glass article 100. A detailed description thereof will be given later.
[0056] Hereinafter, stress distribution of the strengthened glass article 100 will be described in detail.
[0057] Figure 4 is a graph showing an exemplary embodiment of stress distribution of a glass article. Figure 4 In the graph of , the X-axis represents the thickness direction of the glass article 100. Figure 4 In the formula (A), compressive stress has a positive value, while tensile stress has a negative value. In this article, the magnitude of compressive stress / tensile stress means the magnitude of the absolute value regardless of its sign.
[0058] Reference Figure 4 , the glass article 100 includes a first compression zone CSR1 extending (or expanding) from the first surface US to a first compression depth DOC1 and a second compression zone CSR2 extending (or expanding) from the second surface RS to a second compression depth DOC2. The tension zone CTR is arranged between the first compression depth DOC1 and the second compression depth DOC2. The overall stress distribution in the glass article 100 may be symmetrical between the two zones on the surfaces US and RS with respect to the center in the direction of the thickness t. Although in Figure 4 Not shown in FIG. 1 , compression and tension zones may be arranged between opposing side surfaces of the glass article 100 in a similar manner.
[0059] The first compression region CSR1 and the second compression region CSR2 resist external impact to prevent the occurrence of cracks or breakage of the glass article 100. When the maximum compressive stresses CS1 and CS2 of the first compression region CSR1 and the second compression region CSR2 are large, the strength of the glass article 100 generally increases. Since external impact is generally transmitted through the surface of the glass article 100, it is advantageous in terms of durability to have the maximum compressive stresses CS1 and CS2 at the surface of the glass article 100. From this perspective, the compressive stresses of the first compression region CSR1 and the second compression region CSR2 tend to be maximum at the surface and generally decrease toward the inside.
[0060] The first compression region CSR1 and the second compression region CSR2 may include crack prevention regions CBR1 and CBR2 having higher stress than surroundings in a predetermined depth section from the first surface US. The stress in the crack prevention regions CBR1 and CBR2 may have a significant influence on the critical drop height of a model drop test using the glass article 100. Figure 5 The depth and stress of the crack prevention zones CBR1 and CBR2 are described.
[0061] The first compression depth DOC1 and the second compression depth DOC2 suppress the propagation of cracks or grooves defined in the first surface US and the second surface RS to the tensile zone CTR inside the glass article 100. When the first compression depth DOC1 and the second compression depth DOC2 are large, the propagation of cracks, etc. can be more effectively prevented. The points corresponding to the first compression depth DOC1 and the second compression depth DOC2 correspond to the boundaries between the compression zones CSR1 and CSR2 and the tensile zone CTR, and have a stress value of zero.
[0062] The tensile stress of the tensile region CTR may be balanced with the compressive stress of the compressive regions CSR1 and CSR2 throughout the glass article 100. That is, the total compressive stress (i.e., compressive energy) in the glass article 100 may be the same as the total tensile stress (i.e., tensile energy) in the glass article 100. The stress energy accumulated in one region having a constant width in the thickness direction of the glass article 100 may be calculated as an integral value of the stress distribution. When the stress distribution in the glass article 100 having a thickness t is represented as a function f(x), the following relational expression may be established.
[0063] [Mathematical expression 1]
[0064]
[0065] The greater the magnitude of the tensile stress in the glass article 100, the more likely the fragments will be violently released when the glass article 100 breaks, and the more likely the glass article 100 will break from the inside. The maximum tensile stress that satisfies the fragility requirements of the glass article 100 may satisfy, but is not limited to, the following relationship:
[0066] [Mathematical expression 2]
[0067] CT 1 ≤-38.7×ln(t)+48.2
[0068] In some exemplary embodiments, the maximum tensile stress CT 1 It may be 150 MPa or less, or 120 MPa or less. Maximum tensile stress CT of 50 MPa or more 1 It may be desirable to improve mechanical properties, such as strength. In an exemplary embodiment, the maximum tensile stress CT 1 It may be greater than or equal to 90 MPa and less than or equal to 110 MPa, but is not limited thereto.
[0069] Maximum tensile stress CT of glass product 100 1It can be generally disposed at the center portion in the thickness direction of the glass article 100. In an exemplary embodiment, for example, the maximum tensile stress CT of the glass article 100 is 1 It may be arranged at a depth in the range of 0.4t to 0.6t, or at a depth in the range of 0.45t to 0.55t, or at a depth of about 0.5t.
[0070] In order to increase the strength of the glass article 100, it is preferred that the compressive stress and the compression depths DOC1 and DOC2 have large values. However, as the compressive energy increases, the tensile energy also increases, and the maximum tensile stress CT 1 In order to satisfy the brittleness requirement while having high strength, it is desirable to adjust the stress distribution so that the maximum compressive stresses CS1 and CS2 and the compression depths DOC1 and DOC2 have large values while the compression energy becomes smaller.
[0071] The shape of the stress distribution (particularly, the shape of the stress distribution in the compression zone) can be precisely controlled by a multi-stage ion exchange treatment in which a mixed salt and a single salt having various salt ratios are applied alternately. In an exemplary embodiment, it can be controlled by a four-stage ion exchange treatment in which a mixed salt and a single salt are applied alternately four times. In another exemplary embodiment, it can be controlled by a four-stage ion exchange treatment in which a single salt and a mixed salt are applied alternately four times.
[0072] In the following, reference will be made to Figure 4 A detailed description of the stress distribution of the compression zone is given. The following description will focus on the stress distribution of the first compression zone CSR1, and since the first compression zone CSR1 and the second compression zone CSR2 have a symmetrical relationship in stress distribution, the repeated description of the stress distribution of the second compression zone CSR2 will be omitted or simplified.
[0073] Figure 5 yes Figure 4 An enlarged graph of the vicinity of the first compression zone. Figure 6 It is schematically shown Figure 5 Graph showing a straight line graph approximating the stress distribution.
[0074] Reference Figure 5 and Figure 6 , the stress distribution in the first compression zone CSR1 may decrease, increase, and decrease again as it reaches the first compression depth DOC1 from the first surface US. In the first compression zone CSR1, the stress distribution may include at least two first local minimum points LMN1 and first local maximum points LMX1 each having a tangent line whose slope is zero, and at least two first transition points TP1 and second transition points TP2 each having a rapidly changing slope.
[0075] The first local minimum point LMN1 and the first local maximum point LMX1 may be disposed between the first surface US and the first compression depth DOC1. The first local minimum point LMN1 may be disposed between the first surface US and the first local maximum point LMX1. The first local maximum point LMX1 may be disposed between the first local minimum point LMN1 and the first compression depth DOC1. The first transition point TP1 may be disposed between the first surface US and the first local minimum point LMN1. The second transition point TP2 may be disposed between the first local maximum point LMX1 and the first compression depth DOC1.
[0076] In the first compression zone CSR1, the stress distribution may decrease from the first surface US via a first transition point TP1 having a rapidly changing slope to a first local minimum point LMN1, increase from the first local minimum point LMN1 to a first local maximum point LMX1, and decrease from the first local maximum point LMX1 via a second transition point TP2 having a rapidly changing slope to a first compression depth DOC1.
[0077] The stress distribution in the first compression zone CSR1 may be divided into a first section SG1 to a fifth section SG5. Specifically, the stress distribution in the first compression zone CSR1 may include a first section SG1 extending from the first surface US to the first transition point TP1, a second section SG2 extending from the first transition point TP1 to the first local minimum point LMN1, a third section SG3 extending from the first local minimum point LMN1 to the first local maximum point LMX1, a fourth section SG4 extending from the first local maximum point LMX1 to the second transition point TP2, and a fifth section SG5 extending from the second transition point TP2 to the first compression depth DOC1.
[0078] The stress distribution may have a negative average slope in the first and second segments SG1 and SG2 , a positive average slope in the third segment SG3 , and a negative average slope in the fourth and fifth segments SG4 and SG5 as it extends from the first surface US toward the first compression depth DOC1 .
[0079] The maximum value of the stress in the stress distribution may occur at the first surface US. The maximum compressive stress CS1 may be 300 MPa or greater. In various exemplary embodiments, the maximum compressive stress CS1 may be 350 MPa or greater, 400 MPa or greater, 450 MPa or greater, or 500 MPa or greater. In addition, the maximum compressive stress CS1 may be 2000 MPa or less. In various exemplary embodiments, the maximum compressive stress CS1 may be 1800 MPa or less, 1500 MPa or less, or 1050 MPa or less. In some exemplary embodiments, the maximum compressive stress CS1 may be in the range of 800 MPa to 900 MPa.
[0080] The first transition point TP1 is disposed at a point where the first segment SG1 and the second segment SG2 intersect, and a tangent line at the first transition point TP1 may have a negative slope. The absolute value of the slope of the tangent line at the first transition point TP1 may be smaller than the absolute value of the average slope of the first segment SG1 and may be greater than the absolute value of the average slope of the second segment SG2. The stress CS_TP1 at the first transition point TP1 may be smaller than the stress CS_LMX1 at the first local maximum point LMX1 and may be greater than the stress CS_LMN1 at the first local minimum point LMN1. The depth DOL_TP1 of the first transition point TP1 is in a range of about 5 micrometers (μm) to about 10 μm, and the stress CS_TP1 at the first transition point TP1 may have a value in a range of about 180 MPa to about 220 MPa, but the present invention is not limited thereto.
[0081] The first local minimum point LMN1 may be disposed at a point where the second segment SG2 and the third segment SG3 intersect, and a tangent line TL_LMN1 at the first local minimum point LMN1 may have a slope of zero. The stress CS_LMN1 at the first local minimum point LMN1 may be less than the stress CS_TP1 at the first transition point TP1 and may be greater than the stress CS_TP2 at the second transition point TP2.
[0082] The depth DOL_LMN1 of the first local minimum point LMN1 may have a value in the range from about 0.24 times the first compression depth DOC1 to about 0.31 times the first compression depth DOC1. Specifically, the depth DOL_LMN1 of the first local minimum point LMN1 may be 20 μm or more, 25 μm or more, or 28 μm or more. In addition, the depth DOL_LMN1 of the first local minimum point LMN1 may be 40 μm or less, 35 μm or less, or 32 μm or less. In an exemplary embodiment, the depth DOL_LMN1 of the first local minimum point LMN1 may have a value in the range from about 28 μm to about 32 μm, but is not limited thereto. In reference to Figure 7 In the following description, a case where the depth DOL_LMN1 of the first local minimum point LMN1 is 30 μm will be described as an example.
[0083] The stress CS_LMN1 of the first local minimum point LMN1 may have a value in the range from about 0.12 times the first maximum compressive stress CS1 at the first surface US to about 0.16 times the first maximum compressive stress CS1 at the first surface US. Specifically, the stress CS_LMN1 of the first local minimum point LMN1 may be 100 MPa or more, 110 MPa or more, or 115 MPa or more. In addition, the stress CS_LMN1 of the first local minimum point LMN1 may be 140 MPa or less, 130 MPa or less, or 125 MPa or less. In an exemplary embodiment, the stress CS_LMN1 of the first local minimum point LMN1 may have a value in the range from about 115 MPa to about 125 MPa, but is not limited thereto.
[0084] The first local maximum point LMX1 may be disposed at a point where the third segment SG3 and the fourth segment SG4 intersect, and a tangent line TL_LMX1 at the first local maximum point LMX1 may have a slope of zero. The stress CS_LMX1 at the first local maximum point LMX1 may be less than the first maximum compressive stress CS1 at the first surface US and may be greater than the stress CS_TP1 at the first transition point TP1.
[0085] The depth DOL_LMX1 of the first local maximum point LMX1 may have a value in the range from about 0.41 times the first compression depth DOC1 to about 0.50 times the first compression depth DOC1, but is not limited thereto. Specifically, the depth DOL_LMX1 of the first local maximum point LMX1 may be 40 μm or more, 45 μm or more, or 48 μm or more. In addition, the depth DOL_LMX1 of the first local maximum point LMX1 may be 60 μm or less, 55 μm or less, or 52 μm or less. In an exemplary embodiment, the depth DOL_LMX1 of the first local maximum point LMX1 may have a value in the range from about 48 μm to about 52 μm, but is not limited thereto. In reference to Figure 7 In the following description, a case where the depth DOL_LMX1 of the first local maximum point LMX1 is 50 μm will be described as an example.
[0086] The stress CS_LMX1 of the first local maximum point LMX1 may be 150 MPa or more, 200 MPa or more, or 250 MPa or more. In addition, the stress CS_LMX1 of the first local maximum point LMX1 may be 600 MPa or less, 550 MPa or less, or 500 MPa or less. In an exemplary embodiment, the stress CS_LMX1 of the first local maximum point LMX1 may have a value in a range of about 262.2 MPa to about 481.2 MPa, but is not limited thereto. Figure 7A more detailed description is given of the range of the stress CS_LMX1 of the first local maximum point LMX1.
[0087] The second transition point TP2 is set at the point where the fourth segment SG4 and the fifth segment SG5 intersect, and the tangent at the second transition point TP2 may have a negative slope. The absolute value of the slope of the tangent at the second transition point TP2 may be less than the absolute value of the average slope of the fourth segment SG4 and may be greater than the absolute value of the average slope of the fifth segment SG5. The stress CS_TP2 at the second transition point TP2 may be greater than zero and less than the stress CS_LMN1 at the first local minimum point LMN1.
[0088] The depth DOL_TP2 of the second transition point TP2 may be 60 μm or more, 65 μm or more, or 68 μm or more. In addition, the depth DOL_TP2 of the second transition point TP2 may be 80 μm or less, 75 μm or less, or 72 μm or less. In an exemplary embodiment, the depth DOL_TP2 of the second transition point TP2 may have a value in a range from about 68 μm to about 72 μm, but is not limited thereto. In reference to Figure 7 In the following description, a case where the depth DOL_TP2 of the second transition point TP2 is 70 μm will be described as an example.
[0089] The stress CS_TP2 of the second transition point TP2 may be 30 MPa or more, 35 MPa or more, or 40 MPa or more. In addition, the stress CS_TP2 of the second transition point TP2 may be 55 MPa or less, 50 MPa or less, or 45 MPa or less. In an exemplary embodiment, the stress CS_TP2 of the second transition point TP2 may have a value in a range from about 40 MPa to about 45 MPa, but is not limited thereto. In reference to Figure 7 In the following description, a case where the stress CS_TP2 at the second transition point TP2 is 43.1 MPa will be described as an example.
[0090] A point where the stress is zero in the stress distribution may occur at a point where the first compression depth DOC1 is reached away from the first surface US in the depth direction. The first compression depth DOC1 may have a value greater than the depth DOL_TP2 of the second transition point TP2. In the glass article 100, a section having a depth less than the first compression depth DOC1 may be a first compression zone CSR1, and a section having a depth greater than the first compression depth DOC1 may be a tension zone CTR. The first compression depth DOC1 may be 80 μm or greater. In various exemplary embodiments, the first compression depth DOC1 may be 90 μm or greater, 95 μm or greater, 100 μm or greater, or 105 μm or greater. In addition, the first compression depth DOC1 may be 130 μm or less, 125 μm or less, 120 μm or less, or 115 μm or less. In some exemplary embodiments, the first compression depth DOC1 may be in the range of 105 μm to 115 μm.
[0091] The stress distribution of the first compression zone CSR1 may further include a first crack prevention zone CBR1 having a peak. When the compressive stress in the first crack prevention zone CBR1 is large, the occurrence of cracks can be effectively prevented. However, when the stress in the first crack prevention zone CBR1 is too large, the tensile energy in the glass will increase according to Mathematical Expression 1, which may result in failure to meet the fragility requirements of the glass article 100. Therefore, it is preferred to adjust the stress of the first crack prevention zone CBR1 to an appropriate level.
[0092] In an exemplary embodiment, the stress distribution of the glass article may have a first crack prevention zone CBR1 including one peak. Four ion exchange treatments may be involved to form the first crack prevention zone CBR1 including one peak. In another exemplary embodiment, the stress distribution of the glass article may have a first crack prevention zone CBR1 including multiple peaks. In an exemplary embodiment, for example, six ion exchange treatments may be involved to form the first crack prevention zone CBR1 including two peaks. Eight ion exchange treatments may be involved to form the first crack prevention zone CBR1 including three peaks, but the number of peaks included in the first crack prevention zone CBR1 is not limited thereto. As a result, "2n+2" ion exchange treatments may be involved to form the first crack prevention zone CBR1 including n peaks. In this case, in order to form the first crack prevention zone CBR1, a molten salt containing sodium ions at a ratio of about 90 mol% or more may be used in the (2n+1)th ion exchange treatment. Hereinafter, the depth and stress of the first crack prevention zone CBR1 will be described in more detail.
[0093] The depth of the first crack prevention zone CBR1 will be described in conjunction with a model drop test using the glass article 100. In the model drop test, after a fixture model of a smartphone model to which the glass article 100 is applied is dropped, when no cracks occur, the drop is repeated by increasing the height by 5 centimeters (cm). Finally, when cracks occur, the height immediately before the cracks occur (i.e., the maximum height without the occurrence of cracks) is determined as the critical drop height h.
[0094] [Mathematical expression 3]
[0095]
[0096] Mathematical expression 3 represents the relationship between the critical drop height h based on the experimental results and various factors affecting the critical drop height h. As shown in mathematical expression 3, the factors affecting the critical drop height h include: the horizontal length L1 of the fixture model, the vertical length L2 of the fixture model and the height L3 of the fixture model, the Young's modulus E of the fixture model including the glass comp , the weight of the fixture model m, the compressive stress CS_50 at a depth of 50 μm from the surface of the glass sample, and the fracture toughness K of the glass sample IC , constant Y according to the crack shape, crack length c, attenuation coefficient α defined as the ratio of bending energy to total kinetic energy, Young's modulus E of the glass sample glass Etc. "g" refers to the acceleration due to gravity.
[0097] According to Mathematical Expression 3, the stress affecting the critical drop height h may be the compressive stress CS_50 at a depth point of 50 μm from the surface. As described above, since the depth of the crack generated in the glass product 100 has a median value of about 50 μm as an experimental result, the stress at the depth point of the crack, that is, the compressive stress CS_50 at a depth point of about 50 μm from the first surface US, may have a significant influence on the critical drop height h. Therefore, in the stress distribution, when there is a first crack prevention region CBR1 having a high stress near a depth point of about 50 μm from the first surface US, the occurrence of cracks can be effectively prevented.
[0098] In an exemplary embodiment of the stress distribution of the glass article, the first crack prevention zone CBR1 may be defined as a zone between the first local minimum point LMN1 and the second transition point TP2 in the stress distribution. The first crack prevention zone CBR1 may be a zone including the third segment SG3 and the fourth segment SG4. The segment of the first crack prevention zone CBR1 may vary according to the positions of the first local minimum point LMN1 and the second transition point TP2. In an exemplary embodiment, the first crack prevention zone CBR1 may be arranged in an interval of about 20 μm to about 80 μm, in another exemplary embodiment, in an interval of about 25 μm to about 75 μm, and in another exemplary embodiment, in an interval of about 30 μm to about 70 μm, but not limited thereto. In addition, the first crack prevention zone CBR1 may be arranged in a depth interval of about 0.27 times the first compression depth DOC1 to about 0.64 times the first compression depth DOC1 from the first surface US.
[0099] The first crack prevention region CBR1 may exhibit a stress distribution such that the stress increases from the first local minimum point LMN1 to the first local maximum point LMX1, and decreases from the first local maximum point LMX1 to the second transition point TP2. The maximum stress value in the first crack prevention region CBR1 may be the stress CS_LMX1 at the first local maximum point LMX1. As described above, since the depth DOL_LMX1 of the first local maximum point LMX1 has a value of about 50 μm, the compressive stress CS_50 at a depth of 50 μm from the surface that affects the critical drop height h as shown in Mathematical Expression 3 may refer to the stress CS_LMX1 at the first local maximum point LMX1, but is not limited thereto.
[0100] The stress of the first segment SG1 disposed relatively close to the first surface US in the first compression region CSR1 may be mainly determined by the density of potassium ions. A section of the first segment SG1 may also include sodium ions, but the stress of the corresponding section may mainly depend on the density of potassium ions having a larger ion size. In the depth section of the first segment SG1, the greater the density of potassium ions, the higher the stress, and the stress distribution may be substantially similar to the density distribution of potassium ions.
[0101] The stress of the second segment SG2 disposed inwardly relative to the first segment SG1 may be mainly determined by the density of sodium ions. That is, in the depth section of the second segment SG2, the greater the density of sodium ions, the higher the stress, and the stress distribution may be substantially similar to the density distribution of sodium ions.
[0102] The stress of the third segment SG3 and the fourth segment SG4 disposed inwardly relative to the second segment SG2 may be mainly determined by the density of potassium ions. That is, in the depth section of the third segment SG3 and the fourth segment SG4, the greater the density of potassium ions, the higher the stress, and the stress distribution may be substantially similar to the density distribution of potassium ions. The second transition point TP2 may correspond to the maximum penetration depth of potassium ions.
[0103] The stress of the fifth segment SG5 disposed inwardly relative to the fourth segment SG4 may be mainly determined by the density of sodium ions. That is, in the depth section of the fifth segment SG5, the greater the density of sodium ions, the higher the stress, and the stress distribution may be substantially similar to the density distribution of sodium ions. The first compression depth DOC1 may correspond to the maximum penetration depth of sodium ions.
[0104] The first segment SG1 may be substantially approximated by a first straight line l1 connecting the coordinates of the first transition point TP1 and the coordinates of the first surface US in the corresponding segment. The first straight line l1 may be represented as a first function in the following mathematical expression 4 in a coordinate plane with depth indicated by the X axis and stress indicated by the Y axis.
[0105] [Mathematical expression 4]
[0106] y=m 1 x+a
[0107] In the first function, m 1 is the average slope of the first segment SG1, which is the first slope of the first straight line l1, and a is the y-axis intercept, which represents the first maximum compressive stress CS1 at the first surface US.
[0108] The second segment SG2 can be substantially approximated by a second straight line l2 connecting the coordinates of the first transition point TP1 and the coordinates of the first local minimum point LMN1 in the corresponding segment. The second straight line l2 can be expressed as a second function in the following mathematical expression 5 in a coordinate plane with the X-axis indicating the depth and the Y-axis indicating the stress.
[0109] [Mathematical expression 5]
[0110] y=m 2 x+b
[0111] In the second function, m 2 is the average slope of the second segment SG2, which is the second slope of the second straight line l2, and b represents the y-axis intercept.
[0112] The third segment SG3 can be substantially approximated by a third straight line l3 connecting the coordinates of the first local minimum point LMN1 and the coordinates of the first local maximum point LMX1 in the corresponding segment. The third straight line l3 can be represented as a third function in the following mathematical expression 6 in a coordinate plane where the X-axis indicates the depth and the Y-axis indicates the stress.
[0113] [Mathematical expression 6]
[0114] y=m 3 x+c
[0115] In the third function, m 3 is the average slope of the third segment SG3, which is the third slope of the third straight line l3, and c represents the y-axis intercept.
[0116] The fourth segment SG4 can be substantially approximated by a fourth straight line l4 connecting the coordinates of the first local maximum point LMX1 and the coordinates of the second transition point TP2 in the corresponding section. The fourth straight line l4 can be represented as a fourth function in the following mathematical expression 7 in a coordinate plane with the X-axis indicating the depth and the Y-axis indicating the stress.
[0117] [Mathematical expression 7]
[0118] y=m 4 x+d
[0119] In the fourth function, m 4 is the average slope of the fourth segment SG4, which is the fourth slope of the fourth straight line l4, and d represents the y-axis intercept.
[0120] The fifth segment SG5 may be substantially approximated by a fifth straight line l5 connecting the coordinates of the second transition point TP2 and the coordinates of the first compression depth DOC1 in the corresponding section. The fifth straight line l5 may be represented as a fifth function in the following mathematical expression 8 in a coordinate plane with depth indicated by the X axis and stress indicated by the Y axis.
[0121] [Mathematical expression 8]
[0122] y=m 5 x+e
[0123] In the fifth function, m 5 is the average slope of the fifth segment SG5, which is the fifth slope of the fifth straight line l5, e represents the y-axis intercept, and -e / m5 as the x-axis intercept represents the first compression depth DOC1. Some sections of the tension region CTR adjacent to the first compression region CSR1 may have a stress distribution following the fifth straight line l5.
[0124] The first segment SG1 may substantially have a first slope m 1 , the second segment SG2 may substantially have a second slope m2 , the third segment SG3 may substantially have a third slope m 3 , the fourth segment SG4 may substantially have a fourth slope m 4 , and the fifth segment SG5 may substantially have a fifth slope m 5 .
[0125] In the above function, the first slope m 1 To the fifth slope m 5 Among them, except for the third slope m 3 The first slope m 1 , the second slope m 2 , the fourth slope m 4 and the fifth slope m 5 Each of may have a negative value. The third slope m 3 May have a positive slope.
[0126] The first slope m 1 The absolute value of 4 The absolute value of the third slope m 3 The absolute value of the second slope m 2 The absolute value and the fifth slope m 5 However, the present invention is not limited thereto. In addition, the absolute value of the average slope of the first segment SG1 may be greater than the absolute value of the average slope of the fourth segment SG4, and the absolute value of the average slope of the fourth segment SG4 may be greater than the absolute value of the average slope of the third segment SG3. The absolute value of the average slope of the third segment SG3 may be greater than the absolute value of the average slope of the second segment SG2, and the absolute value of the average slope of the second segment SG2 may be greater than the absolute value of the average slope of the fifth segment SG5.
[0127] The first segment SG1 to the fifth segment SG5 may be generated by a plurality of ion exchange processes. An ion exchange process is a process of exchanging ions in the glass with other ions. By performing an ion exchange process, ions at or near the surface of the glass may be replaced or exchanged with larger ions having the same valence or oxidation state. In an exemplary embodiment, when the glass includes a monovalent alkali metal such as Li+, Na+, K+, and Rb+, for example, the monovalent cations on the surface may be replaced by Na+, K+, Rb+, or Cs+ ions having a larger ionic radius.
[0128] As an exemplary embodiment, for example, in the case where sodium ions in the glass are exchanged with potassium ions, when the glass including sodium ions is exposed to potassium ions by, for example, immersing the glass in a molten salt bath including potassium nitrate, the sodium ions in the glass are released to the outside and the potassium ions can replace them. Because they have an ionic radius larger than that of sodium ions, the exchanged potassium ions produce compressive stress. The greater the amount of exchanged potassium ions, the greater the compressive stress. Since the ion exchange is carried out through the glass surface, the amount of potassium ions on the glass surface is the largest. Although some of the exchanged potassium ions can diffuse into the glass to increase the depth of the compression zone (i.e., the compression depth), the amount will generally decrease as it is farther from the surface. Therefore, the glass may have a stress distribution with a maximum compressive stress on the surface and a decrease toward the inside. However, exemplary embodiments are not limited to the above examples. The stress distribution may be modified according to the temperature, time, number of times, presence or absence of heat treatment, etc. of the ion exchange treatment.
[0129] The ion exchange treatment may be performed four or more times. In an exemplary embodiment, for example, the ion exchange treatment may include first to fourth ion exchange treatments. The first to fourth ion exchange treatments may be performed in different baths. Each ion exchange treatment may be performed on a plurality of glasses simultaneously. That is, by immersing a plurality of glasses in one bath, the ion exchange treatment may be performed on a plurality of glasses simultaneously. Figures 8 to 15 A detailed description of the ion exchange treatment is given.
[0130] Figure 7 yes Figure 5 In order to determine the range of the stress CS_LMX1 of the first local maximum point LMX1, in addition to the first crack prevention area CBR1, Figure 7 Also shown are the first anti-crack zone approximate triangle CBR1_2 with the first local maximum point LMX1, the second transition point TP2 and the coordinate point (DOL_LMN1, CS_TP2) as vertices, and the first anti-crack zone approximate rectangle CBR1_3 with four coordinate points (DOL_LMN1, CS_TP2), (DOL_LMN1, CS_LMX1), (DOL_TP2, CS_TP2) and (DOL_TP2, CS_LMX1) as vertices.
[0131] Reference Figure 5 and Figure 7, the range of the stress CS_LMX1 of the first local maximum point LMX1 may be determined based on the assumption that the area of the first crack prevention region CBR1 is greater than the area of the first crack prevention region approximate triangle CBR1_2 and less than the area of the first crack prevention region approximate rectangle CBR1_3. The area of the first crack prevention region CBR1 may be in the range from 10000 MPa*μm to 11000 MPa*μm. In an exemplary embodiment, the area of the first crack prevention region CBR1 may be 10486.1 MPa*μm, but is not limited thereto.
[0132] The area of the region CBR1_1 obtained by subtracting the lower portion of the first crack prevention region CBR1 having a horizontal length of 40 μm and a vertical length of 43.1 MPa from the first crack prevention region CBR1 may be greater than the area of the first crack prevention region approximate triangle CBR1_2. In addition, the value obtained by subtracting the area of a rectangle having a horizontal length DOL_TP2-DOL_LMN1 (e.g., 40 μm) and a vertical length CS_TP2 (e.g., 43.1 MPa) from the area of the first crack prevention region CBR1 may be less than the area of the first crack prevention region approximate rectangle CBR1_3. When the calculation is performed assuming that the area of the first crack prevention region CBR1 is 10486.1 MPa*μm, the following inequality as shown in Mathematical Expression 9 is obtained.
[0133] [Mathematical expression 9]
[0134]
[0135] When the mathematical expression 9 is summarized with respect to the stress CS_LMX1 at the first local maximum point LMX1, the stress CS_LMX1 of the first local maximum point LMX1 may have a value in the range of 262.2 MPa to 481.2 MPa. That is, the maximum stress of the first crack prevention region CBR1 (or the stress CS_LMX1 at the first local maximum point) may have a value in the range of 262.2 MPa to 481.2 MPa. The stress CS_LMX1 at the first local maximum point may be about 0.32 times to about 0.54 times the first maximum compressive stress CS1 at the first surface US.
[0136] Therefore, due to the crack prevention regions CBR1 and CBR2 disposed in a predetermined depth section from the first surface US and having higher stress than surroundings, the exemplary embodiment of the glass article 100 may have high strength such that it is not easily broken by external impact.
[0137] Figure 8 is a flow chart of an exemplary embodiment of a method for making a glass article. Fig. 9 is a schematic diagram illustrating an ion exchange process of a first strengthening operation in a method for manufacturing a glass article. Fig.10is a graph illustrating an exemplary embodiment of a stress distribution of a glass article that has undergone a first strengthening operation. Fig.11 is a schematic diagram illustrating an exemplary embodiment of an ion exchange treatment for a second strengthening operation in a method of manufacturing a glass article. Fig.12 is a graph showing stress distribution of a glass product that has been subjected to a second strengthening operation. Fig.13 is a schematic diagram illustrating an exemplary embodiment of an ion exchange treatment for a third strengthening operation in a method of manufacturing a glass article. Fig.14 is a graph showing stress distribution of a glass product that has been subjected to the third strengthening operation. Fig.15 is a schematic diagram illustrating an exemplary embodiment of an ion exchange treatment for a fourth strengthening operation in a method for manufacturing a glass article.
[0138] Reference Figures 8 to 15 An exemplary embodiment of the method for manufacturing the glass article 100 may include: providing LAS-type glass (operation S11); immersing the LAS-type glass in a molten salt (NaNO 3 +KNO 3 / Na: 55 to 65 mol%, K: 35 to 45 mol%) for 20 to 40 minutes (operation S12); immersing the glass having undergone the first strengthening operation in a molten salt (NaNO 3 +KNO 3 / Na: 30 to 40 mol%, K: 60 to 70 mol%) for 50 to 70 minutes (operation S13); immersing the glass subjected to the second strengthening operation in a molten salt (NaNO 3 +KNO 3 / Na: 85 to 95 mol%, K: 5 to 15 mol%) for 230 to 250 minutes (operation S14); and immersing the glass subjected to the third strengthening operation in a molten salt (NaNO 3 +KNO 3 / Na: 2 to 8 mol%, K: 92 to 98 mol%), a fourth strengthening operation (operation S15) for 20 to 40 minutes.
[0139] Operation S11 of providing the LAS-type glass may include preparing a glass composition and molding the glass composition.
[0140] The glass composition may include various compositions known in the art. In an exemplary embodiment, the glass composition may include LAS glass ceramics including lithium aluminosilicate. In an exemplary embodiment, for example, the glass composition may include 50 to 80 mol % of SiO 2 , 1 to 30 mol% Al 2 O 3 , 0 to 5 mol% B 2 O 3 , 0 to 4 mol% P 2 O 5 , 3 to 20 mol% Li 2 O, 0 to 20 mol% Na 2 O, 0 to 10 mol% K 2 O, 3 to 20 mol% MgO, 0 to 20 mol% CaO, 0 to 20 mol% SrO, 0 to 15 mol% BaO, 0 to 10 mol% ZnO, 0 to 1 mol% TiO 2 and 0 to 8 mol% ZrO 2 .
[0141] As used herein, the term "content is 0 mol%" means that it does not substantially contain the corresponding component. As used herein, the term "(composition) does not substantially contain (a certain component)" means that a certain component is not intentionally included in the raw materials, etc., and includes, for example, the case where a trace amount (e.g., 0.1 mol% or less) of impurities is inevitably contained.
[0142] In addition to the above components, the glass composition may also contain Y 2 O 3 ,La 2 O 3 , Nb 2 O 5 、 2 O 5 and Gd 2 O 3 The composition of the glass article 100 may be changed by a molding process, an ion exchange process, etc., which will be described later.
[0143] Generally, the viscosity of a glass composition varies with temperature, and a temperature at which the glass composition has a viscosity of 1014.5 poise is defined as a strain point. As the strain point increases, the scratch resistance of the glass improves. However, when the strain point is excessively increased, elasticity decreases, which may adversely affect the consistency of the product. Therefore, it is preferred to use a glass composition having a strain point within an appropriate range. In an exemplary embodiment, the strain point of the glass composition may be in the range of about 505°C to about 574°C.
[0144] The glass composition may be molded into a flat glass shape by various methods known in the art, and may be molded by a float process, a fusion drawing process, a slot drawing process, or the like.
[0145] Reference Figure 8 , Fig. 9 and Fig.10 , LAS-type glass is immersed in molten salt (NaNO) at a temperature of 380°C to 400°C 3 +KNO 3 In the first strengthening operation S12 of up to 20 minutes to 40 minutes in a molten salt containing sodium ions and sodium ions (Na: 55 to 65 mol%, K: 35 to 45 mol%), a first ion exchange treatment may be performed. Specifically, the first ion exchange treatment is a treatment of imparting compression depths DOC1 and DOC2 to the glass, and can generally be performed by exposing the glass to a mixed molten salt containing potassium ions and sodium ions. In an exemplary embodiment, for example, for the first ion exchange treatment, the glass is immersed in a bath containing a mixed molten salt mixed with sodium nitrate and potassium nitrate. The ratio of sodium ions to potassium ions in the bath can be adjusted within the range of 55 to 65 mol% Na and 35 to 45 mol% K. In an exemplary embodiment, the ratio of sodium ions to potassium ions in the mixed molten salt of the first ion exchange treatment may be 60:40, but is not limited thereto.
[0146] The first ion exchange treatment may be performed at a temperature ranging from about 380° C. to about 400° C. for 20 to 40 minutes. In an exemplary embodiment, the first ion exchange treatment may be performed at a temperature of 390° C. for 30 minutes, but is not limited thereto.
[0147] By the first ion exchange treatment, lithium ions / sodium ions as smaller ions inside the glass are exchanged with sodium ions / potassium ions as larger ions in the molten salt, thereby increasing the concentration of sodium ions and / or potassium ions in the glass. The main ions exchanged by the first ion exchange treatment may be lithium ions in the glass and sodium ions of the mixed molten salt. Since lithium ions from the glass are provided to the molten salt, the molten salt of the bath after the first ion exchange treatment may also contain lithium ions in addition to sodium ions and potassium ions.
[0148] After the first ion exchange treatment is completed, a stress distribution corresponding to the fifth straight line l5 may be generated. That is, the sodium ions and / or potassium ions of the mixed molten salt are exchanged to penetrate into the glass and then diffuse in the depth direction. The sodium ions generally diffuse to the first compression depth DOC1 to form a first compression region CSR1 having a compressive stress from the first surface US to the first compression depth DOC1. That is, the first compression depth DOC1 is determined by the first ion exchange treatment.
[0149] The density of the diffused ions may be substantially inversely proportional to the diffusion distance. Since the sodium ions and potassium ions enter the glass from the surface of the glass through ion exchange and diffuse in the depth direction, the concentration of the sodium ions and potassium ions tends to decrease substantially linearly as the distance from the first surface US of the glass is increased. As a result, the stress distribution has a maximum compressive stress CS1_1 at the first surface US of the glass and decreases in the depth direction.
[0150] In addition, the degree of diffusion of ions is inversely proportional to the size of the ions. In other words, as the size of the ions decreases, more ions can be diffused. Therefore, when both sodium ions and potassium ions penetrate into the glass through the first ion exchange treatment, the sodium ions with a relatively small size can diffuse more easily and penetrate to a deeper level. The sodium ions diffuse to the first compression depth DOC1, while the potassium ions can diffuse to a smaller depth. However, as described above, since the main ions that penetrate into the glass through the first ion exchange treatment are sodium ions, the stress distribution of the glass that has been subjected to the first ion exchange treatment can be approximated to the density distribution of the sodium ions.
[0151] As described above, the first compression depth DOC1 is closely related to the maximum diffusion depth of sodium ions, which are smaller ions to be ion-exchanged. The first compression depth DOC1 may be the same as the maximum diffusion depth of sodium ions, or may be set near the maximum diffusion depth of sodium ions even if there is a slight difference, and is generally proportional to the maximum diffusion depth of sodium ions. As described above, the first ion exchange treatment is a treatment to form a predetermined first compression depth DOC1 by sufficient diffusion, and is performed for a sufficiently long time so that the ions can be sufficiently diffused.
[0152] Reference Figure 8 , Fig.11 and Fig.12 The glass which has undergone the first strengthening operation is immersed in a molten salt (NaNO 3 +KNO 3In the second strengthening operation S13 of the glass article 100 (Na: 30 to 40 mol%, K: 60 to 70 mol%) for up to 50 minutes to 70 minutes, a second ion exchange treatment may be performed. Specifically, the second ion exchange treatment is a treatment for increasing the compressive stress CS1_1 at the first surface US of the glass article 100, and is generally performed by exposing it to a mixed molten salt containing potassium ions and sodium ions. In an exemplary embodiment, for example, for the second ion exchange treatment, the glass that has been subjected to the first ion exchange treatment is immersed in a bath containing a mixed molten salt mixed with potassium nitrate and sodium nitrate. Even when a mixed molten salt is used, the salt ratio is adjusted so that the main ions that penetrate into the glass are potassium ions. That is, the content of potassium nitrate in the bath is greater than the content of potassium nitrate during the first ion exchange treatment, and in addition, the concentration of potassium nitrate may be greater than the concentration of sodium nitrate. In an exemplary embodiment, for example, the salt ratio of potassium nitrate to sodium nitrate in the bath may be adjusted in the range of 60:40 to 70:30. In an exemplary embodiment, the salt ratio of potassium nitrate to sodium nitrate in the mixed molten salt of the second ion exchange treatment may be 65:35, but is not limited thereto.
[0153] The second ion exchange treatment may be performed at the same temperature as the first ion exchange treatment for a longer time. In an exemplary embodiment, for example, the second ion exchange treatment may be performed at a temperature range of about 380° C. to about 400° C. for 50 to 70 minutes. In an exemplary embodiment, the second ion exchange treatment may be performed at a temperature of 390° C. for 60 minutes, but is not limited thereto.
[0154] By the second ion exchange treatment, the compressive stress in the shallow depth section of the first surface US can be significantly increased. The main ions exchanged by the second ion exchange treatment can be sodium ions of the glass and potassium ions of the mixed molten salt. When potassium ions penetrate into the glass, the compressive stress in the corresponding part becomes larger due to the larger size of potassium ions. The potassium ions that penetrate into the glass diffuse in the depth direction. Compared with the first ion exchange treatment, potassium ions have a slower diffusion rate than sodium ions, and the duration of the second ion exchange treatment is shorter than the duration of the first ion exchange treatment. Accordingly, the diffusion depth of the potassium ions diffused by the second ion exchange treatment can be less than the first compression depth DOC1.
[0155] The compressive stress CS1_1 of the first surface US is increased to the compressive stress CS1_2 by the second ion exchange treatment, and the penetration depth of potassium ions (or the first transition point TP1) is less than the first compression depth DOC1. Therefore, the compressive stress distribution of the glass subjected to the second ion exchange treatment may have a steep slope near the surface of the glass article 100, such that the slope becomes gentle as it approaches the interior of the glass article 100.
[0156] Reference Figure 8 , Fig.13 and Fig.14 The glass which has been subjected to the second strengthening operation is immersed in a molten salt (NaNO 3 +KNO 3 In the third strengthening operation S14 of 230 minutes to 250 minutes in the second ion exchange treatment (Na: 85 to 95 mol%, K: 5 to 15 mol%), a third ion exchange treatment may be performed. Specifically, the third ion exchange treatment is a treatment for diffusing potassium ions that have penetrated into the glass by the second ion exchange treatment in the depth direction of the glass article 100, and is generally performed by exposing the glass to a mixed molten salt containing potassium ions and sodium ions. In an exemplary embodiment, for example, for the third ion exchange treatment, the glass is immersed in a bath containing a mixed molten salt mixed with sodium nitrate and potassium nitrate. The ratio of sodium ions to potassium ions in the bath may be adjusted within the range of 85 to 95 mol% of Na and 5 to 15 mol% of K. In an exemplary embodiment, the ratio of sodium ions to potassium ions in the mixed molten salt of the third ion exchange treatment may be 90:10, but is not limited thereto.
[0157] The third ion exchange treatment may be performed at a temperature ranging from about 400° C. to about 420° C. for 230 to 250 minutes. In an exemplary embodiment, the third ion exchange treatment may be performed at a temperature of 410° C. for 240 minutes, but is not limited thereto.
[0158] Since the third ion exchange process is performed for a longer time at a higher temperature than the temperatures of other operations, ion exchange with the outside of the glass and ion diffusion into the glass may be actively performed in the glass article 100 during the third ion exchange process.
[0159] The potassium ions that penetrate into the glass through the second ion exchange treatment can diffuse in the depth direction of the glass product 100 through the third ion exchange treatment. As the potassium ions diffuse in the depth direction of the glass product 100, the lithium ions / sodium ions relatively distributed inside the glass can move toward the first surface US. In addition, the lithium ions that move toward the first surface US can be exchanged with the sodium ions of the mixed molten salt. That is, through the third ion exchange treatment, the potassium ions can move in the depth direction of the glass, and the lithium ions inside the glass can move toward the first surface US to exchange with the sodium ions of the mixed molten salt.
[0160] Through the third ion exchange treatment, the sodium ions in the mixed molten salt can be relatively exchanged with the lithium ions inside the glass, thereby increasing the concentration of sodium ions in the glass. Since lithium ions from the glass product 100 are provided to the molten salt, the molten salt of the bath after the third ion exchange treatment can also contain lithium ions in addition to sodium ions and potassium ions.
[0161] Potassium ions diffuse from the glass surface in the depth direction, while sodium ions penetrate from the mixed molten salt into the first surface US. Therefore, the concentration of potassium ions may tend to decrease, increase, and decrease again substantially linearly as it moves away from the first surface US. Accordingly, when the third ion exchange treatment is completed, a stress distribution similar to that of FIG. Figure 4 The crack prevention areas CBR1 and CBR2 correspond to the areas.
[0162] That is, the first crack prevention region CBR1 may be generated so that the stress distribution has the highest stress at the first local maximum point LMX1 and decreases in the depth direction and / or in the direction toward the surface. The stress distribution in the first crack prevention region CBR1 may include a stress distribution in which the stress decreases from the first local maximum point LMX1 toward the first surface US and a stress distribution in which the stress decreases in the depth direction of the glass. In this way, the third ion exchange treatment is performed for a sufficient time to allow the ions to diffuse sufficiently.
[0163] As more ion diffusion is performed, the first maximum compressive stress CS1 can become smaller. The first maximum compressive stress CS1 increases with the increase of ion density. Therefore, when the same amount of ions enter the glass, the more diffusion, the lower the density and the lower the compressive stress. As described above, since the third strengthening operation has limitations in increasing the maximum compressive stress CS1_3 of the first surface US, the fourth ion exchange treatment is further performed after the third strengthening operation to form a larger surface compressive stress CS1_3.
[0164] Reference Figure 5 , Figure 8 and Fig.15 The glass which has been subjected to the third strengthening operation is immersed in a molten salt (NaNO 3 +KNO 3 / Na: 2 to 8mol%, K: 92 to 98mol%) for up to 20 minutes to 40 minutes in the fourth strengthening operation S15, a fourth ion exchange treatment may be performed. Specifically, the fourth ion exchange treatment is a treatment for increasing the first maximum compressive stress CS1, and is generally performed by exposing the glass to a single molten salt containing potassium ions or a mixed molten salt containing potassium ions and sodium ions. In an exemplary embodiment, for example, for the fourth ion exchange treatment, the glass that has been subjected to the third ion exchange treatment is immersed in a bath including a single molten salt containing potassium nitrate or a mixed molten salt mixed with potassium nitrate and sodium nitrate. Even when a mixed molten salt is used, the salt ratio is adjusted so that the main ions that penetrate into the glass are potassium ions. The concentration of potassium nitrate in the bath may be greater than the concentration of sodium nitrate in the bath. In an exemplary embodiment, for example, the salt ratio of potassium nitrate to sodium nitrate in the bath may be adjusted in the range of 92:8 to 98:2. In an exemplary embodiment, the salt ratio of potassium nitrate to sodium nitrate in the mixed molten salt of the fourth ion exchange treatment may be 95:5, but is not limited thereto.
[0165] The fourth ion exchange treatment may be performed at a lower temperature and for a shorter time than the third ion exchange treatment. In an exemplary embodiment, for example, the fourth ion exchange treatment may be performed at a temperature range of 370° C. to 390° C. for about 20 minutes to about 40 minutes.
[0166] By the fourth ion exchange treatment, the compressive stress in the shallow depth section of the first surface US can be significantly increased. Specifically, when potassium ions penetrate into the glass, the compressive stress in the corresponding portion becomes larger due to the larger size of the potassium ions. The potassium ions that penetrate into the glass diffuse in the depth direction. Since potassium ions have a slower diffusion speed than sodium ions, and the duration of the fourth ion exchange treatment is shorter than the duration of the third ion exchange treatment, the diffusion depth of the potassium ions diffused by the fourth ion exchange treatment can be less than the first local minimum point LMN1. The maximum diffusion depth of the potassium ions additionally penetrated by the fourth ion exchange treatment can be lower than the first transition point TP1.
[0167] The stress distribution provided by the potassium ions additionally infiltrated by the fourth ion exchange treatment has substantially the same shape as the first segment SG1. The first maximum compressive stress CS1 of the first surface US is increased by the fourth ion exchange treatment, and the penetration depth of the potassium ions by the fourth ion exchange treatment (or the first transition point TP1) is less than the first local minimum point LMN1. Therefore, the first slope m of the first straight line l1 is 1 The absolute value of the second straight line l2 is greater than the second slope m 2 That is, the compressive stress distribution may have a steep slope near the surface of the glass article 100.
[0168] In an exemplary embodiment of a method for manufacturing a glass product 100, it is possible to provide a glass product 100 having high strength by including crack prevention regions CBR1 and CBR2 arranged in a depth segment of about 30 m to about 70 m from a first surface US and having a stress higher than that of the surroundings, so that it is not easily damaged by external impact.
[0169] At the end of the detailed description, those skilled in the art will recognize that many changes and modifications can be made to the preferred embodiment without departing from the principles of the present invention in essence. Therefore, the preferred embodiments of the present invention disclosed are used only in a general sense and description sense, and not for the purpose of limitation.
Claims
1. A glass product comprising lithium aluminosilicate, wherein the glass product include: a first surface; a second surface, opposite to the first surface; a first compression zone extending from the first surface to a first compression depth; a second compression zone extending from the second surface to a second compression depth; as well as a stretching zone, arranged between the first compression depth and the second compression depth, wherein the stress distribution in the first compression zone has a first local minimum point, a first local maximum point, a first transition point, and a second transition point, wherein the stress distribution is convex downward at the first local minimum point, and the stress distribution is convex upward at the first local maximum point, wherein the depth of the first local maximum point is greater than the depth of the first local minimum point, wherein the stress at the first local maximum point is greater than the compressive stress at the first local minimum point, wherein the depth of the first transition point is less than the depth of the first local minimum point, wherein the depth of the second transition point is greater than the depth of the first local maximum point and less than the first compression depth, wherein the stress distribution in the first compression zone includes a first segment extending from the first surface to the first transition point, a second segment extending from the first transition point to the first local minimum point, a third segment extending from the first local minimum point to the first local maximum point, a fourth segment extending from the first local maximum point to the second transition point, and a fifth segment extending from the second transition point to the first compression depth, and Among them, the absolute value of the first slope of the first segment is greater than the absolute value of the fourth slope of the fourth segment, the absolute value of the fourth slope of the fourth segment is greater than the absolute value of the third slope of the third segment, the absolute value of the third slope of the third segment is greater than the absolute value of the second slope of the second segment, and the absolute value of the second slope of the second segment is greater than the absolute value of the fifth slope of the fifth segment.
2. The glass product according to claim 1, in, The stress at the first local maximum point is 0.32 to 0.54 times the compressive stress at the first surface.
3. The glass product according to claim 2, in, The compressive stress at the first local maximum point is within a range from 262.2 MPa to 481.2 MPa.
4. The glass product according to claim 1, in, The depth of the first local maximum point is 0.41 to 0.50 times the first compression depth.
5. The glass product according to claim 1, in, The stress at the first local minimum point is 0.12 to 0.16 times the compressive stress at the first surface.
6. The glass product according to claim 1, in, The depth of the first local minimum point is 0.24 to 0.31 times the first compression depth.
7. The glass product according to claim 1, in, The stress distribution of the second compression zone has a symmetrical relationship with the stress distribution of the first compression zone.
8. A glass product comprising lithium aluminosilicate, wherein the glass product include: a first surface; a second surface, opposite to the first surface; a first compression zone extending from the first surface to a first compression depth; a second compression zone extending from the second surface to a second compression depth; as well as a stretching zone, arranged between the first compression depth and the second compression depth, The stress distribution of the first compression zone includes a crack prevention zone with a peak, and the crack prevention zone is arranged in a depth range of 30 microns to 70 microns. The stress distribution in the first compression zone has a first local minimum point, a first local maximum point, a first transition point, and a second transition point. The stress distribution is convex downward at the first local minimum point, and is convex upward at the first local maximum point. wherein the depth of the first local maximum point is greater than the depth of the first local minimum point, wherein the stress at the first local maximum point is greater than the compressive stress at the first local minimum point, wherein the depth of the first transition point is less than the depth of the first local minimum point, wherein the depth of the second transition point is greater than the depth of the first local maximum point and less than the first compression depth, wherein the stress distribution in the first compression zone includes a first segment extending from the first surface to the first transition point, a second segment extending from the first transition point to the first local minimum point, a third segment extending from the first local minimum point to the first local maximum point, a fourth segment extending from the first local maximum point to the second transition point, and a fifth segment extending from the second transition point to the first compression depth, and Among them, the absolute value of the first slope of the first segment is greater than the absolute value of the fourth slope of the fourth segment, the absolute value of the fourth slope of the fourth segment is greater than the absolute value of the third slope of the third segment, the absolute value of the third slope of the third segment is greater than the absolute value of the second slope of the second segment, and the absolute value of the second slope of the second segment is greater than the absolute value of the fifth slope of the fifth segment.
9. The glass product according to claim 8, in, The maximum stress in the crack prevention zone is within the range from 262.2 MPa to 481.2 MPa.
10. The glass product according to claim 8, in, The crack prevention zone includes a plurality of peaks.