Photosensitive bismaleimide composition

By using the photoinitiator and bismaleimide component in the photosensitive composition to form a photopolymer with low dielectric constant and low dissipation factor, the poor electrical properties of existing photolithographic materials at high frequencies are solved. problem, photosensitive dielectric films suitable for high-frequency microelectronics.

CN113126431BActive Publication Date: 2024-10-01杜邦电子材料国际有限责任公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011403098.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-30
Filing Date
2020-12-02
Publication Date
2024-10-01
Estimated Expiration
2040-12-02

AI Technical Summary

Technical Problem

It is difficult for existing photolithographic materials to maintain low dielectric constant and low dissipation factor at high frequencies, resulting in poor electrical properties and unable to meet the needs of high-frequency microelectronics.

Method used

A photosensitive composition containing a photoinitiator and a bismaleimide component is used to form a photopolymer with low dielectric constant and low dissipation factor through polymerization and cross-linking for preparing a photosensitive dielectric film.

Benefits of technology

It achieves low dielectric constant and low dissipation factor of the dielectric film at high frequencies, improves the electrical properties of the material, and is suitable for high-frequency microelectronics applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002813090260000031
    Figure BDA0002813090260000031
  • Figure BDA0002813090260000041
    Figure BDA0002813090260000041
  • Figure BDA0002813090260000042
    Figure BDA0002813090260000042
Patent Text Reader

Abstract

The present disclosure relates to a photosensitive composition comprising a photoinitiator and a bismaleimide component, a photopolymer comprising the photosensitive composition and its use, especially in electronic devices. The bismaleimide component comprises a bismaleimide compound or a bismaleimide oligomer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a photosensitive composition comprising a photoinitiator and a bismaleimide component, a photopolymer comprising the photosensitive composition and uses thereof, especially uses in electronic devices. Background Art

[0002] The rapid development of the microelectronics industry has created a huge demand for dielectric polymer materials for photolithography that have improved electrical properties for packaging each subsequent generation of microelectronic devices. Computers and other electronic devices are moving to higher frequencies as speeds increase. Many systems now operate at 1 to 10 GHz, while new applications will operate at frequencies up to 20 GHz, or 30 GHz, or up to 100 GHz.

[0003] Plastics are generally considered insulators, but they can transmit some electrical energy at higher frequencies. The effectiveness of a material as an insulator is often measured by quantities like the dielectric constant (Dk) and the dissipation factor (Df). Dk represents how well an insulator stores electrical energy, thereby isolating electrical components from each other and from ground. The dissipation factor (Df or tan delta) is an electrical property of plastics and other electrically insulating materials. It is defined as the reciprocal of the ratio of the capacitive reactance of an insulating material to its resistance (equivalent series resistance or ESR) at a specified frequency.

[0004] The more conductive a material is, the greater its Dk. Good dielectrics also tend to have a low dissipation factor (Df). That is, they do not allow the charge they carry to dissipate easily when the electric field is reversed rapidly at high frequencies, and they lose little energy as heat. A low dissipation factor indicates a high-quality, high-performance electrical or electronic system. This is important for plastic insulators in high-frequency applications. Therefore, it is desirable to provide a low dielectric constant photolithographic material with a low dissipation factor for high-frequency microelectronics. DETAILED DESCRIPTION

[0005] Many aspects and embodiments have been described above and are exemplary and non-limiting only. After reading this specification, skilled artisans will appreciate that other aspects and embodiments are possible without departing from the scope of the present disclosure.

[0006] As used throughout this specification, the following abbreviations shall have the following meanings, unless the context clearly indicates otherwise: °C = degrees Celsius; g = gram; nm = nanometer, μm = micrometer; mm = millimeter; sec. = second; and min. = minute. Unless otherwise indicated, all amounts are weight percent ("wt. %) and all ratios are molar ratios. All numerical ranges are inclusive and combinable in any order, except where it is apparent that the numerical ranges are limited to add up to 100%. Unless otherwise indicated, all molecular weights of polymers and oligomers are weight average molecular weights ("Mw"), in g / mol or Daltons, and are determined using gel permeation chromatography in comparison to polystyrene standards.

[0007] Unless the context clearly indicates otherwise, the articles "a", "an" and "the" refer to the singular and the plural. As used herein, the term "and / or" includes any and all combinations of one or more of the associated items. The term "curable" refers to a material that becomes harder under conditions of use and less soluble in solvents.

[0008] In this specification, the terms "film" and "layer" are used interchangeably. The term "monomer" refers to a molecule that can be polymerized or copolymerized to contribute structural units to the basic structure of a macromolecule (polymer). The term "oligomer" refers to a polymer with a limited and moderate number of repeating monomer structural units. The oligomers of the present disclosure typically have 2 to about 100 repeating monomer units, or 2 to about 30 repeating monomer units, or 2 to about 10 repeating monomer units. The term "polymer" refers to a molecule consisting of repeating monomer units. The term "polymer" used herein refers to a homopolymer consisting of one monomer unit, and / or a copolymer consisting of two or more different monomers as polymerized units. The polymers in the present disclosure may contain organic and / or inorganic additives.

[0009] The term "alkoxy" refers to the group RO-, where R is an alkyl group. The term "alkyl" refers to a group derived from an aliphatic hydrocarbon and includes a straight chain, branched chain, or cyclic group. A group "derived from" a compound represents a group formed by removing one or more hydrogen or deuterium. In some embodiments, the alkyl has 1 to 20 carbon atoms.

[0010] The term "aromatic compound" refers to an organic compound containing at least one unsaturated cyclic group with 4n+2 delocalized π electrons. The term "aryl" refers to a group with one or more attachment points derived from an aromatic compound. The term includes groups with a single ring and groups with multiple rings that can be connected or fused together by a single bond. Carbocyclic aryl groups have only carbon in the ring structure. Heteroaryl groups have at least one heteroatom in the ring structure. The term "alkaryl" refers to an aryl group with one or more alkyl substituents. The term "aryloxy" refers to the group RO-, where R is an aryl group.

[0011] The term "adjacent" as it relates to substituents refers to groups bonded to carbons that are linked together with single or multiple bonds. Exemplary adjacent R groups are shown below:

[0012]

[0013] The term "liquid composition" refers to a liquid medium in which a material is dissolved to form a solution, a liquid medium in which a material is dispersed to form a dispersion, or a liquid medium in which a material is suspended to form a suspension or emulsion. The term "solvent" refers to an organic compound that is liquid at room temperature (20° C.-25° C.). The term is intended to cover a single organic compound or a mixture of two or more organic compounds.

[0014] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which this disclosure belongs. Although methods and materials similar or equivalent to those described herein can be used in the practice or testing of embodiments of the present disclosure, suitable methods and materials are described below. In addition, the materials, methods, and examples are illustrative only and are not intended to be limiting.

[0015] In this specification, unless otherwise expressly indicated or indicated to the contrary by the context of use, where an embodiment of the inventive subject matter is stated or described as comprising, including, containing, having, consisting of, or composed of certain features or elements, one or more features or elements in addition to those explicitly stated or described may also be present in the embodiment. An alternative embodiment of the disclosed inventive subject matter is described as consisting essentially of certain features or elements, wherein features or elements of the embodiment that would substantially change the principle of operation or the distinguishing characteristics of the embodiment are absent therefrom. Another alternative embodiment of the described inventive subject matter is described as consisting of certain features or elements, in which embodiment or in insubstantial variations thereof, only the features or elements specifically stated or described are present.

[0016] To the extent not described herein, many details regarding specific materials, processing activities, and circuits are conventional and may be found in textbooks and other sources in the field of photoresists, organic light emitting diode displays, photodetectors, photovoltaic cells, and semiconductor components.

[0017] A photosensitive composition is provided, comprising a photoinitiator and a bismaleimide (BMI) component, wherein the photoinitiator is an oxime ester compound, and the oxime ester compound is present in an amount of 0.5 to 25 weight percent based on the weight of the bismaleimide component.

[0018] In one aspect, the bismaleimide component is a bismaleimide compound. The bismaleimide compound can be represented by the general formula (I) shown below:

[0019]

[0020] Wherein R is a substituted or unsubstituted linking group selected from the group consisting of: alkylene, alkylene aryl, cycloalkylene, cycloalkylene aryl, cycloalkylene alkylene dialkyl siloxane, diaryl siloxane and combinations thereof; and R1 is selected from the group consisting of: hydrogen, deuterium, halogen, cyano, methyl, vinyl, allyl, isoprene, substituted or unsubstituted isoprene having 1-100 carbon atoms and combinations thereof. In one embodiment, R can be an alkylene group having 1 to 100 carbon atoms, or 2 to 50 carbon atoms, or 5 to 20 carbon atoms.

[0021] In another aspect, the bismaleimide compound can be a bismaleimide oligomer. The bismaleimide oligomer can be represented by the general formula (II) shown below:

[0022]

[0023] Where R2 is H or CH3; R3 is C1-C 40 Alkyl, alkyl polydimethylsiloxane or alkylaryl; R4 is selected from the group consisting of:

[0024]

[0025] and combinations thereof; and

[0026] n is an integer of 1-10.

[0027] Examples of bismaleimide components may include, but are not limited to, C36 alkylenediamine imides such as 1,1′-((4-hexyl-3-octylcyclohexane-1,2-diyl)bis(octane-8,1-diyl))bis(1H-pyrrole-2,5-dione) (BMI-689, commercially available from Designer Molecules, Inc.), 1,6′-bismaleimide-(2,2,4-trimethyl)hexane (TMH-BMI, commercially available from Daiwa Kasei Co., Ltd. Industry Co., Ltd., Japan)), 1,3-bis(3-maleimidophenoxy)benzene (APB-BMI, commercially available from Hampford Research), 1,1'-[2,2'-bis(trifluoromethyl)[1,1'-biphenyl]-4,4'-diyl]bis[1H-pyrrole-2,5-dione] (MA-TFMB), 2,2-bis[4-(4-maleimidophenoxy)phenyl]hexafluoropropane (BMP3 CF3) and 1,3-bis(4-maleimidophenoxy)benzene (1,3-bis-4-PhoBMI), 1-(3-(5-(2,5-dioxo-2,5-dihydro-1H-pyrrol-1-yl)benzo[d]oxazol-2-yl)phenyl)-1H-pyrrole-2,5-dione, 1,1'-(sulfonylbis(4,1-phenylene))bis(1H-pyrrole-2,5-dione), 1,1 '-(sulfonylbis(3,1-phenylene))bis(1H-pyrrole-2,5-dione), 1,1'-(1,1,3,3-tetramethyldisiloxane-1,3-diyl)bis(propane-3,1-diyl)bis(1H-pyrrole-2,5-dione), 1,1'-(methylenebis(2-ethyl-6-methyl-4,1-phenylene))bis(1H-pyrrole-2,5-dione)(BMI5 100, commercially available from Yamato Chemical Industry Co., Ltd., Japan), 1,1'-(1,3-phenylene)bis(1H-pyrrole-2,5-dione) (BMI3000H, commercially available from Yamato Chemical Industry Co., Ltd., Japan), 1,1'-(decane-1,10-diyl)bis(1H-pyrrole-2,5-dione), 1,1'-(1,3,5-triazine-2,4-diyl)bis(1H-pyrrole 1H-pyrrole-2,5-dione), 1,1'-((perfluoropropane-2,2-diyl)bis(4,1-phenylene))bis(1H-pyrrole-2,5-dione), 1,1'-((9H-fluorene-9,9-diyl)bis(4,1-phenylene))bis(1H-pyrrole-2,5-dione), and 1,1'-(methylenebis(4,1-phenylene))bis(1H-pyrrole-2,5-dione).More commercial bismaleimide components may include, but are not limited to, BMI 1400, BMI 1500, BMI 1700, BMI 4000, and BMI 5000, which are commercially available from Designer Molecules.

[0028] Based on the weight of the bismaleimide component, the oxime ester compound may be present in an amount of 0.5 to 25 weight percent, or 1 to 25 weight percent, or 2 to 10 weight percent, or 5 to 15 weight percent. Examples of oxime ester compounds may include, but are not limited to, the compounds shown below and combinations thereof:

[0029]

[0030]

[0031] wherein R1 is CO2Ph, CO2Me or CO2Et; R2 is a ketone, an aryl group, an aryl ether, a sulfide aryl ether or an alkyl group; R3 is H, OH, COOH or a methyl group; R4 and R5 are each independently an alkyl group, a cycloalkyl group or a phenyl group having 1 to 10 carbon atoms; R6 and R7 are each independently an alkyl group, a cycloalkyl group or a phenyl group having 1 to 10 carbon atoms; R8 is an alkyl group having 1 to 5 carbon atoms; R9 is H, a methyl group or an acetyl group; R 10 is NO2 or ArCO; R 11 is an alkyl group having 1 to 6 carbon atoms; and R 12 and R 13 Each is independently an alkyl group, a cycloalkyl group or a phenyl group having 1 to 10 carbon atoms. Ar is an aryl group, for example a phenyl group or a tolyl group.

[0032] Examples of commercially available products of oxime ester compounds may include, but are not limited to, IRGACURE OXE 01 (1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyl oxime)]) and IRGACURE OXE 02 (ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyl oxime)), commercially available from BASF; ADEKA ARKLS NCI-930 and ADEKA Optomer N-1919, commercially available from ADEKA CORPORATION; and DFI-091, commercially available from Daito Chemix, Corporation. More descriptions of oxime ester compounds can be found in U.S. Patent Application No. 2017 / 0003588A1, the entire contents of which are incorporated herein by reference.

[0033] In one embodiment, the oxime ester compound may be

[0034]

[0035]

[0036] In one aspect, the photosensitive composition may further comprise a thermosetting polymer. The thermosetting polymer may then be crosslinked under radiation. In one embodiment, the thermosetting polymer may be represented by the general formula (III) as shown below:

[0037]

[0038] wherein Ar1 is a heterocyclic ring containing N, S, O or P atoms; R2 is H, CH3, ethyl or tert-butyl; R3 is H, CH3, C1-C 12 Alkyl or C1-C 12 Olefin; R4 is cyclobutene, 1-cyclobutene, 1-oxy-cyclobutene or α-methylcyclobutene; l is an integer from 0 to 10; R6 is an alkyl group, a cycloalkyl group or an aryl group having 1 to 12 carbon atoms; n is an integer from 5 to 70; m is an integer from 5 to 50; and o is an integer from 5 to 50; and p is an integer from 5 to 50, wherein l+n+m+o+p=100.

[0039] In another aspect, the photosensitive composition may further comprise at least one polymerizable monomer. The polymerizable monomer may be an arylcyclobutene monomer. In one embodiment, the arylcyclobutene monomer has formula (IV), (V) or (VI), as shown below:

[0040]

[0041]

[0042] in:

[0043] K 1 is a divalent group selected from the group consisting of: alkyl, aryl, carbocyclic

[0044] Aryl, polycyclic aromatic, heteroaryl, aryloxy, arylalkyl, carbonyl, ester, carboxyl, ether, thioester, thioether and tertiary amine;

[0045] L 1 It is a covalent bond or a multivalent linking group;

[0046] M is a substituted or unsubstituted divalent aromatic or polyaromatic group, or a substituted or unsubstituted divalent heteroaromatic group;

[0047] R2-R5 are the same or different and are each independently selected from the group consisting of substituted or unsubstituted alkyl, substituted or unsubstituted alkoxy, substituted or unsubstituted aryl, substituted or unsubstituted aryloxy, alkylthiol, arylthiol, substituted alkylamino and substituted arylamino;

[0048] R6-R8 are the same or different and are each independently selected from the group consisting of hydrogen, deuterium, cyano, halogen, methyl, vinyl, allyl, isoprene, and substituted or unsubstituted isoprene having 1 to 100 carbon atoms;

[0049] K 2 is a polymerizable functional group; and

[0050] x and y are the same or different and are integers from 1 to 5. 1 When it is a covalent bond, y=1.

[0051] Examples of aromatic cyclobutene monomers may include, but are not limited to, 1-(4-vinylphenoxy)-benzocyclobutene, 1-(4-vinylmethoxy)-benzocyclobutene, 1-(4-vinylphenyl)-benzocyclobutene, 1-(4-vinylhydroxynaphthyl)-benzocyclobutene, 4-vinyl-1-methyl-benzocyclobutene, 4-vinyl-1-methoxy-benzocyclobutene, and 4-vinyl-1-phenoxy-benzocyclobutene.

[0052] The polymerizable monomer in the photosensitive composition as described above may further comprise at least one dienophile monomer represented by the general formula (VII):

[0053]

[0054] wherein B is hydrogen, substituted or unsubstituted alkyl, substituted or unsubstituted aromatic moiety, substituted or unsubstituted heteroaromatic moiety, hydroxyl or substituted or unsubstituted alkoxy; and R9-R 11 are the same or different and are each independently selected from the group consisting of hydrogen, methyl, vinyl, allyl, isoprene, substituted or unsubstituted isoprene having 1 to 100 carbon atoms, substituted or unsubstituted alkyl groups having 1 to 100 carbon atoms, halogen, cyano, substituted or unsubstituted aryl groups having 6 to 100 carbon atoms, substituted or unsubstituted heteroaryl groups having 6 to 100 carbon atoms, and combinations thereof.

[0055] In one embodiment, the dienophile monomer can be an aromatic vinyl monomer having formula (VIII):

[0056]

[0057] in:

[0058] R 12 -R 14 is the same or different at each occurrence and is selected from the group consisting of: hydrogen and C 1-5 Alkyl; and

[0059] R 15 is the same or different at each occurrence and is selected from the group consisting of: hydrogen and C 1-5 Alkyl, where the adjacent R 15 The groups may be linked to form a fused 6-membered aromatic ring.

[0060] Examples of the aromatic vinyl monomer may include, but are not limited to, styrene, α-methylstyrene, vinyltoluene, 1-vinylnaphthalene, and 2-vinylnaphthalene.

[0061] The polymerizable monomer in the photosensitive composition as described above may further comprise at least one diene monomer. The diene monomer may have a general formula (IX), as shown below:

[0062]

[0063] Where R 9 is the same or different at each occurrence and is selected from hydrogen and methyl; and R 10 is the same or different at each occurrence and is selected from hydrogen, C 1-5 Alkyl, C 1-5 Alkoxy, C 1-5 Thioalkyl and C 5-12 Alkenyl.

[0064] Examples of the diene monomer may include, but are not limited to, butadiene, isoprene, 1,3-pentadiene, 2,4-hexadiene, cyclopentadiene, β-myrcene, ocimene, cyclooctadiene, farnesene, and polymerizable terpenes.

[0065] The polymerizable monomer in the photosensitive composition as described above may further comprise at least one heterocyclic ring-containing monomer. The heterocyclic ring-containing monomer may be a vinyl-substituted C 3-12 Heterocyclic or vinyl substituted C 3-5 In one embodiment, the heterocyclic ring may be further replaced by one or more C 1-6 Alkyl, C 6-12 Carbocyclic aromatic or C 3-12 Heteroaryl substitution.

[0066] The heterocycle-containing monomer is selected from the group consisting of nitrogen heterocycles, sulfur heterocycles, nitrogen-sulfur heterocycles, and substituted derivatives thereof.

[0067] In one embodiment, the monomer containing heterocycles may be a monomer containing nitrogen heterocycles. The monomer containing nitrogen heterocycles may contain at least one ring nitrogen. Examples of nitrogen heterocycle comonomers may include, but are not limited to, pyrrole, pyridine, diazine, triazine, imidazole, benzimidazole and quinolone.

[0068] The nitrogen-containing heterocyclic monomer may have the general formula (X) as shown below:

[0069]

[0070] Where Z 1 and Z 2 are the same or different and are N or CR 15a ; R 12 -R 14 and R 15a is the same or different at each occurrence and is selected from the group consisting of: hydrogen and C 1-5 alkyl.

[0071] Examples of such nitrogen-containing heterocyclic monomers may include, but are not limited to, 4-vinylpyridine, 4-vinyl-1,3-diazine, 2-vinyl-1,3,5-triazine, and 4-methyl-5-vinyl-1,3-thiazole.

[0072] In another embodiment, the heterocyclic monomer may be a sulfur-containing heterocyclic monomer. The sulfur-containing heterocyclic monomer may include at least one ring sulfur. Examples of sulfur-containing heterocyclic monomers may include, but are not limited to, thiophene, benzothiophene, and dibenzothiophene.

[0073] In yet another embodiment, the monomer containing heterocycles may be a monomer containing nitrogen-sulfur heterocycles. The monomer containing nitrogen-sulfur heterocycles may contain at least one ring nitrogen and at least one ring sulfur. Examples of monomers containing nitrogen-sulfur heterocycles may include, but are not limited to, thiazole, thiadiazole, and thiadiazine.

[0074] At least one solvent may be present in the photosensitive composition as described above. Examples of solvents may include, but are not limited to, cyclopentanone, cyclohexanone, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, gamma-butyrolactone, 3-methoxypropionate, dipropylene glycol dimethyl ether, 3-methoxybutyl acetate, anisole, mesitylene, 2-heptanone, cyrene, 2-butanone, ethyl lactate, amyl acetate, n-butyl acetate, n-methyl-2-pyrrolidone, N-butyl-2-pyrrolidone and combinations thereof.

[0075] The polymer may be formed by polymerizing one or more of the above-mentioned polymerizable monomers in the photosensitive composition, and the formed polymer may then be cross-linked under radiation. The polymer may be formed in the presence of a free radical initiator or other photosensitive compound. In one embodiment, the polymerization process may be carried out at a temperature of 50° C. to 150° C. for a period of 5 to 50 hours.

[0076] The free radical initiator is typically an azo compound or an organic peroxide. In one embodiment, the free radical initiator is an oil-soluble azo compound. Such initiators may include, for example, dimethyl 2,2'-azobis(2-methylpropionate) and 2,2'-azobis(2,4-dimethylvaleronitrile). Based on the weight of the starting reaction mixture, the total initiator added may be 1-5wt.%.

[0077] One or more additional inhibitors may be present in the photosensitive composition as described above. In some embodiments, the inhibitor is a hindered phenol or piperidine-N-oxide. The inhibitor may be selected from the group consisting of: 2,6-di-tert-butyl-4-methylphenol, 2,5-di-tert-butyl-1,4-benzohydroquinone, 2-tert-butylhydroquinone, 2,3,5-trimethyl-1,4-hydroquinone, 4-methoxyphenol, 2,2,6,6-tetramethyl-1-piperidinyloxy, 4-hydroxy-2,2,6,6-tetramethyl-1-piperidinyloxy, dibenzo-1,4-thiazine, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphate, triethylene glycol bis[β-(5-tert-butyl-4-hydroxy-3-methylphenyl) propionate] and 2,6-di-tert-butyl-4-octadecylphenol and combinations thereof.

[0078] Examples of inhibitors may include, but are not limited to, the following chemical structures shown below:

[0079]

[0080] One or more nonionic surfactants may be added to the photosensitive composition as described above. Examples of nonionic surfactants may include, but are not limited to:

[0081]

[0082] wherein R is CH2CF3 or CH2CF2CF3, n is an integer from 3 to 20, x is an integer from 5 to 20, y is an integer from 10 to 30, and z is an integer from 5 to 20. Such surfactants may be present in an amount of 0 to 40 g / L or 0 to 25 g / L.

[0083] The photosensitive composition as described above may further comprise at least one adhesion promoter. The adhesion promoter may be an oxygen, sulfur or nitrogen functionalized silane coupling agent.

[0084] In one embodiment, the adhesion promoter can be selected from the group consisting of: methacryloxy-3-propyl trialkoxysilane, 3-mercapto trialkoxysilane, 4-vinylphenylethyl trialkoxysilane, phenyl trialkoxysilane, 4-vinylphenyl trialkoxysilane, vinyl trialkoxysilane, vinyl triacetoxysilane, N-2-[3-(trialkoxysilyl)propyl]-1,3,5-triazine-2,4,6-triamine, 3-ureidopropyl-trialkoxysilane, bis[3-(trialkoxysilyl)propyl]fumarate, N-[3-(trialkoxysilyl)propyl]maleamic acid, bis[3-(trialkoxysilyl)propyl]maleate, trialkoxysilylpropyl succinic anhydride. The alkoxy group can be methoxy, ethoxy or isopropoxy. The adhesion promoter may also be one or more aromatic heterocycles containing two or more nitrogen atoms, such as imidazole, benzotriazole, 5-methylbenzotriazole, 5-carboxybenzotriazole, 1,3,5-triazine-2,4,6-trithiol, 1,3,4-thiadiazole-2,5-dithiol, and combinations thereof.

[0085] Examples of adhesion promoters may include, but are not limited to, the following chemical structures shown below:

[0086] Additionally, various vapor treatments known in the art may be used to increase the adhesion of the disclosed polymers to substrate surfaces, such as plasma treatments. In certain applications, it may be preferred to treat the substrate surface with an adhesion promoter prior to coating the surface with the composition of the present invention.

[0087] Suitable additives that can be used in the photosensitive composition of the present disclosure include, but are not limited to, one or more inorganic fillers, organic fillers, plasticizers, metal passivation materials, and any combination of the foregoing. Any suitable inorganic filler can be optionally used in the composition of the present invention and is well known to those skilled in the art. Exemplary inorganic fillers include, but are not limited to, silicon dioxide, silicon carbide, silicon nitride, aluminum oxide, aluminum carbide, aluminum nitride, zirconium oxide, etc. and mixtures thereof. The inorganic filler can be in the form of a powder, a rod, a ball, or any other suitable shape. Such an inorganic filler can have any suitable size. Such an inorganic filler can contain a conventional amount of a coupling agent, such as a silane or a titanate.

[0088] The inorganic filler may be used as a solid in an amount of 0 to 80 wt. % or 40 to 80 wt. %, based on the total weight of the composition. In some embodiments, the inorganic filler is not present.

[0089] In one embodiment, the metal passivating material is a copper passivating agent. Suitable copper passivating agents are well known in the art and include imidazole, benzotriazole, ethylenediamine or a salt or acid ester thereof, and iminodiacetic acid or a salt thereof.

[0090] The present disclosure also relates to photosensitive dielectric films. The photosensitive dielectric film can be prepared from the above-mentioned photosensitive composition. The photosensitive composition can be applied or deposited on the surface of the substrate using any known techniques and equipment. The composition can be applied as a substantially continuous film or in a discontinuous pattern, and heated to remove the solvent. The thickness of the deposited composition can vary, depending on the desired thickness of the resulting cured product. The composition of the present disclosure can be used to form a layer or film suitable for use as a dielectric layer, a permanent bonding adhesive, a stress buffer layer, etc. The dielectric film formed on the substrate can be used directly, or can be stripped and used on a different substrate in an electronic device.

[0091] Any substrate known in the art may be used in the present disclosure. Examples of substrates may include, but are not limited to, silicon, copper, silver, indium tin oxide, silicon dioxide, glass, silicon nitride, aluminum, gold, polyimide, and epoxy molding compound.

[0092] The photosensitive composition of the present disclosure can be deposited or coated on the substrate by any suitable method. Suitable methods for arranging the composition of the present invention include but are not limited to spin coating, curtain coating, spray coating, roller coating, dip coating, vapor deposition and lamination such as vacuum lamination, and other methods. In the semiconductor manufacturing industry, spin coating is a preferred method utilizing existing equipment and technology. When spin coating, the solid content of the composition can be adjusted along with the rotation speed to reach the desired composition thickness on the surface to which it is applied. The substrate deposited or coated can be cured under suitable radiation to form the photosensitive dielectric film of the present disclosure. If necessary, additional heating steps can be performed thereafter to further cure the film.

[0093] The radiation may typically extend from 150 nm to 600 nm, or from 190 nm to 600 nm (UV to visible range). Suitable radiation is present in, for example, sunlight or light from an artificial light source. The light source is not particularly limited and may be appropriately selected according to the purpose. Point light sources and arrays ("lamp carpets") are suitable. Examples include: carbon arc lamps, xenon arc lamps, low, medium, high and ultra-high pressure mercury lamps (metal halide lamps) that may have metal halide dopants, microwave-stimulated metal vapor lamps, excimer lamps, super actinic fluorescent tubes, fluorescent lamps, argon incandescent lamps, electronic flashlights, photographic floodlights, light emitting diodes (LEDs), electron beams and X-rays. The distance between the lamp and the substrate material to be exposed comprising the photosensitive composition of the present disclosure may vary according to the intended application and the type and output of the lamp, and may, for example, be 20 μm to 150 cm. Laser light sources, such as excimer lasers, such as F excimer lasers at 157 nm exposure, KrF excimer lasers for exposure at 248 nm, and ArF excimer lasers for exposure at 193 nm are also suitable. Lasers in the visible region may also be used. Optionally, other features of resolution enhancement, such as lenses, may be used. Where lenses are used, numerical apertures of 0.05 to 0.6 or 0.1 to 0.3 may be used.

[0094] In the photosensitive dielectric film of the present embodiment, when the total film thickness of two layers is set to 1 to 80 μm, the minimum transmittance of the photosensitive resin layer in the wavelength band of 248 nm to 436 nm may be 80% or more, or 85% or more.

[0095] In one embodiment, the photosensitive composition described herein can be spin cast onto a desired substrate. The composition can be cast by a slot die coater or other suitable equipment to form a desired dry film for electronic applications. The cast film can be soft baked at a temperature of 70°C-150°C or 90°C-120°C for 30 seconds to 10 minutes to remove residual solvent.

[0096] The soft baked film can then be subjected to curing conditions under radiation as described above. If necessary, the film can be further cured at 150° C.-250° C. for 30 minutes to 4 hours. The resulting cured film has good tensile strength, tensile elongation, good adhesion to desired substrates (e.g., copper and silicon wafers), and low dielectric loss at high frequencies. The photosensitive composition disclosed herein can achieve these good properties without the aid of any kind of inorganic filler.

[0097] In another embodiment, the layer of the photosensitive composition of the present disclosure can also be formed as a dry film and arranged on the surface of the substrate by lamination. A variety of suitable lamination techniques can be used, including vacuum lamination techniques, and are well known to those skilled in the art. When forming a dry film, the composition of the present invention is first arranged (e.g., coated) on a suitable film support sheet (e.g., a polyester sheet, preferably a polyethylene terephthalate (PET) sheet, or a polyimide sheet such as KAPTON) using a slot die coating, gravure printing or other appropriate method. TM The composition is then soft-baked at a suitable temperature (e.g., 90° C. to 140° C.) for an appropriate time (e.g., 1 to 30 minutes) to remove any solvent. A polymer film cover sheet (e.g., polyethylene) is then roller-laminated onto the dried composition at room temperature (20° C.-25° C.) to protect the composition during storage and handling. In order to arrange the dried composition onto the substrate, the cover sheet is first removed. The dried composition on the support sheet is then laminated onto the substrate surface using roller lamination or vacuum lamination. The lamination temperature can be from 20° C. to 120° C. The support sheet is then removed (peeled off), leaving the dried composition on the surface.

[0098] The photosensitive composition described herein can be used to form a dielectric film having a Dk value of less than 2.5 or less than 2.4 and a Df value of less than 0.006 or less than 0.005 or less than 0.004 or less than 0.0035 at high frequencies (20 to 40 GHz). In one embodiment, the dielectric film has a Dk of ≤2.5 or ≤2.4 and a Df of ≤0.004 or ≤0.035 at a frequency of 20 GHz. In another embodiment, the dielectric film has a Dk of ≤2.35 and a Df of ≤0.004 at a frequency of 30 GHz. In yet another embodiment, the dielectric film has a Dk of ≤2.35 and a Df of ≤0.006 at a frequency of 40 GHz.

[0099] The present disclosure also relates to a variety of electronic devices, which include at least one layer of dielectric film of the present application on an electrical substrate. A variety of electronic device substrates can be used in the present disclosure. An electronic device substrate is any substrate used to manufacture any electronic device. Exemplary electronic device substrates include, but are not limited to, semiconductor wafers, glass, sapphire, silicate materials, silicon nitride materials, silicon carbide materials, display device substrates, epoxy molding compound wafers, circuit board substrates, and thermally stable polymers. As used herein, the term "semiconductor wafer" is intended to cover semiconductor substrates, semiconductor devices, and various packages for various interconnect levels, including single-chip wafers, multi-chip wafers, packages for various levels, substrates for light-emitting diodes (LEDs), or other components that require solder connections. Semiconductor wafers, such as silicon wafers, gallium arsenide wafers, and silicon germanium wafers, can be patterned or unpatterned. As used herein, the term "semiconductor substrate" includes any substrate having one or more semiconductor layers or structures, and the semiconductor layers or structures include active or operable parts of semiconductor devices. The term "semiconductor substrate" is defined as meaning any structure containing semiconductor materials, such as semiconductor devices. Semiconductor device refers to a semiconductor substrate on which at least one microelectronic device has been or is being fabricated. Thermally stable polymers include, but are not limited to, any polymer that is stable to the temperature used to cure the arylcyclobutene material, such as polyimide, such as KAPTON TM Polyimide (DuPont, Wilmington, DE), liquid crystal polymers such as VECSTAR TM LCP membrane (Kuraray, Tokyo, Japan) and bismaleimide-triazine (BT) resin (Mitsubishi Gas Chemical Co., Ltd. (MGC), Tokyo, Japan).

[0100] The present disclosure also relates to a presensitized lithographic printing plate comprising a hydrophilic support and an imaging layer, the imaging layer comprising a photosensitive composition, and a photolithographic method for making the presensitized lithographic printing plate. The photolithographic method comprises the steps of: (a) imagewise heating a presensitized lithographic printing plate comprising a hydrophilic support and an imaging layer, the imaging layer comprising the photosensitive composition; (b) exposing the plate to ultraviolet (UV) light; and (c) dissolving and removing the non-imaged areas with a solution. The photosensitive composition is the same as those previously described.

[0101] The hydrophilic carrier can be made of metal, plastic or paper. The carrier can be a surface-treated aluminum plate, a hydrophilic plastic film or waterproof paper. Specifically, the carrier can be an anodized aluminum plate, a polyethylene terephthalate film provided with a hydrophilic layer or paper laminated with a polyethylene film.

[0102] In one embodiment, an aluminum plate subjected to anodizing can be used. The aluminum plate can be a pure aluminum plate, or an alloy plate containing a main component of aluminum and a small amount of other metals. Examples of metals other than aluminum include Si, Fe, Mn, Co, Mg, Cr, Zn, Bi, Ni and Ti. The amount of other metals can be 10wt.% or less. The thickness of the aluminum plate is 0.05 to 0.6mm, or 0.1 to 0.4mm, or 0.15 to 0.3mm.

[0103] The surface of the aluminum plate can be roughened. Roughening can be performed mechanically, electrochemically or chemically. Examples of mechanical roughening include ball milling, brush grinding, blast grinding and buffing. Electrochemical roughening can be performed by the following method, wherein direct current or alternating current is applied to the plate in an electrolytic solution containing an acid (e.g., hydrochloric acid or nitric acid). Electrolytic roughening can be performed in a mixture of two or more acids. Chemical roughening can be performed by the following method, wherein the aluminum plate is immersed in a saturated aqueous solution of an aluminum salt with an inorganic acid. After roughening, the surface roughness Ra (average value along the center line) of the aluminum plate can be 0.2 to 1.0 μm.

[0104] After the roughening treatment, the aluminum plate may be subjected to an alkali etching treatment. The alkali etching solution may be an aqueous solution of potassium hydroxide or sodium hydroxide. A neutralization treatment may be performed after the alkali etching treatment.

[0105] The aluminum plate can then be anodized to improve the wear resistance of the carrier. Anodizing can use various electrolytes to form a porous oxide film. Examples of electrolytes include sulfuric acid, hydrochloric acid, oxalic acid, chromic acid, and mixtures thereof.

[0106] Anodizing treatment is usually carried out under the following conditions: the concentration of the electrolytic solution is 1 to 80 wt.%, the temperature of the solution is 5 to 70°C, and the current density is 5 to 60 A / dm 2 , the voltage is 1 to 100 V, and the electrolysis time is 10 seconds to 5 minutes. The thickness of the oxide film formed by anodization is 1.0 to 5.0 g / m 2 , or 1.5 to 4.0 g / m 2 .

[0107] In addition, a water-soluble outer coating may be provided on the imaging layer to protect the surface of the imaging layer from contamination caused by lipophilic substances. The water-soluble outer coating is made of a substance that can be easily removed during printing (e.g., a water-soluble organic polymer). Examples of water-soluble organic polymers may include, but are not limited to, polyvinyl alcohol, polyvinyl acetate, polyacrylic acid, salts thereof with alkali metals and amines, polymethacrylic acid, salts thereof with alkali metals and amines, polyacrylamide, polyhydroxyethyl acrylate, polyvinyl pyrrolidone, polyvinyl methyl ether, poly-2-acrylamide-2-methyl-1-propanesulfonic acid, salts thereof with alkali metals and amines, gum arabic, cellulose ethers (e.g., carboxymethyl cellulose, carboxyethyl cellulose, methyl cellulose), dextrin and its derivatives (e.g., white dextrin, dextrin decomposed by enzymes, etherified dextrin, pullulan).

[0108] The water-soluble organic polymer may be a copolymer. Examples of copolymers may include, but are not limited to, vinyl alcohol-vinyl acetate copolymers (partially saponified polyvinyl acetate) and vinyl methyl ether-maleic anhydride copolymers. In the case of preparing vinyl alcohol-vinyl acetate copolymers by partially saponifying polyvinyl acetate, the saponification degree may be 65% or more. Two or more water-soluble organic polymers may be used in combination. The amount of the water-soluble outer coating may be 0.1 to 2.0 g / m 2 .

[0109] The presensitized photolithographic printing plate can be heated imagewise to form an image. In one embodiment, a thermal head can be used to heat the presensitized plate imagewise. Image formation using a thermal head does not require an agent capable of converting light into heat. Because a thermal head typically gives an image with a low resolution, an agent capable of converting light into heat can be used. Exposure in an imagewise manner generally provides an image with a higher resolution.

[0110] The presensitized plate can be exposed imagewise by the original image (analog data). The presensitized plate can also be scanned with light corresponding to the original image data (usually digital data). In analog exposure, the light source can be a xenon discharge lamp or an infrared lamp. In the case of using a high-power lamp (e.g., a xenon lamp) as the light source, flash exposure can be performed in a short time.

[0111] In the latter scanning exposure, a laser, in particular an infrared laser, can be generally used. The infrared laser can emit light in the wavelength range of 700 to 1,200 nm. The laser can be a high-power solid infrared laser (eg, semiconductor laser, YAG laser).

[0112] When an imaging layer containing an agent capable of converting light into heat is exposed to a scanning laser beam, the light energy of the beam is converted into heat energy. The photosensitive composition of the present invention in the heated area (imaging area) of the presensitized plate is polymerized and / or cross-linked to harden the heated area. If the compound or polymer is contained in particles, the particles in the heated area will melt and fuse to form a hydrophobic area on the hydrophilic carrier. On the other hand, the compound or polymer in the unheated area (non-imaging area) is unchanged in the plate. In the above-mentioned photolithography method, a heating step can also be added between steps (b) and (c).

[0113] In the case where particles are not used in the imaging layer (where the imaging layer is homogeneous), acidic groups can be introduced into the polymer in the imaging layer to remove the unheated areas (non-imaged areas) by washing the plate with an alkaline developer solution.

[0114] In the case where particles are included in the imaging layer, the particles in the unheated area (non-imaging area) can be removed with water or an aqueous solution. The step of removing particles (development step) can be replaced by pressure development (press development). In pressure development, the plate heated in an imaging manner is installed in a printing press and subjected to a conventional printing process. The plate can be developed by a printing process using dampening water and ink, and then the printing method is carried out by using the plate, dampening water and ink. When the printing press is working, the unheated area (non-imaging area) of the imaging layer is removed by the friction of the dampening water, ink or printing process.

[0115] In one embodiment, the photolithography method may include the following steps: (a) mounting a presensitized photolithography printing plate comprising a hydrophilic support and an imaging layer on a cylinder of a printing press, the imaging layer comprising a photosensitive composition of the present disclosure, (b) exposing the plate to laser light (emitted from a light source connected to the printing press), and pressure developing the plate with dampening water and ink. The steps of exposure to printing may be performed continuously using a printing press equipped with a laser exposure device.

[0116] After development, the printing plate may be heated to cause reaction of unreacted compounds or polymers that remain in the imaged areas, thereby further improving the durability (plate wear) of the printing plate.

[0117] Examples

[0118] The concepts described herein will be further illustrated in the following examples, which do not limit the scope of the present disclosure described in the claims.

[0119] Material:

[0120] β-Myrcene was purchased from Vigon International. Styrene was purchased from Sigma-Aldrich Corporation. Vinyltoluene was obtained from Deltech Corporation. Vazo 65 azo initiator (V-65) and V-601 were purchased from FUJIFILM Wako Chemicals U.S.A. Corporation. 4-Vinylpyridine was obtained from Vertellus and used as received. Polyfox PF656 was obtained from Omnova Solutions. 7-Octenyltrimethoxysilane (KBM-1083) and difunctional aminosiloxane (PAM-E) were obtained from Shin-Etsu Chemical Company. Bismaleimide BMI-689 and BMI-1400 were obtained from Designer Molecular Corporation. 4-HydroxyTEMPO, Irgacure OXE01 (OXE01) and Irgacure OXE02 (OXE02) were from BASF and used as received. Omnirad 819 was obtained from IGM Resins. Bismaleimide BMI-4000, BMI-TMH and BMI-5100 were obtained from Yamato Chemical Industry Co., Ltd. 3a,4,7,7a-Tetrahydro-4,7-epoxyisobenzofuran-1,3-dione was obtained from Oakwood Chemical. 1-(4-vinylphenoxy)benzocyclobutene (BCB) was prepared according to U.S. Patent Application No. 20190169327A1, the entire contents of which are incorporated herein by reference. All other solvents and chemicals were obtained from Dow Chemical Company and used as received without additional purification.

[0121] Compound synthesis

[0122] Example 1-S1

[0123] Under nitrogen protection, 10g of PAM-E was added to a 250ml round-bottom flask equipped with a stirring rod and a reflux condenser and dissolved in 114g of tetrahydrofuran. When the dissolution was complete, 3a, 4, 7, 7a-tetrahydro-4, 7-epoxyisobenzofuran-1, 3-dione (12.78g) in solid form was added, and the solution was refluxed for ten hours. The solution was then cooled to about 25°C, and tetrahydrofuran was removed by rotary evaporation. 114g of toluene was added. The solution was refluxed again for 6 hours, and then toluene was removed by distillation. 14.77g of a light yellow, slightly viscous liquid was obtained, which contained 94% of the desired product.

[0124] Example 2-S2

[0125] The following monomers and solvents were added to a 5 L jacketed reactor with overhead stirring and heated to 80° C. under nitrogen: 1044.59 g 1-(4-vinylphenoxy)benzocyclobutene, 778.34 g vinyltoluene, 80.18 g 4-vinylpyridine, 447.67 g β-myrcene, and 997.04 g cyclohexanone. An initiator feed of 71.67 g V-65 and 888.21 g cyclohexanone was added to the reactor at a constant rate for 20 hours, and the temperature was maintained at 80° C. for another 2 hours and then reduced to 25° C. The solution was used directly to prepare the following polymerizable formulation.

[0126] Example 3-S3

[0127] Alternatively in 100ml EasyMax TM The same procedure as in Example 2 was used in the reactor, and the following amounts of materials were used: 11.77 g 1-(4-vinylphenoxy)benzocyclobutene, 8.83 g vinyltoluene, 0.6 g vinylpyridine 6.33 g β-myrcene, and 11.79 g anisole. A photoinitiator charge of 0.41 g V-601 was added to the reactor and reacted for 15 hours, and then a charge of 0.41 g V-65 in 10.71 g anisole was fed to the reactor at a constant rate for another 15 hours, and the temperature was maintained at 80° C. for another 2 hours, then reduced to 25° C. The solution was used directly to prepare the following polymerizable formulation.

[0128] Polymerizable formulations

[0129] Example 4

[0130] To a 20 ml glass vial was added S3 prepared from Example 3 to make up 75.1 wt% solids; BMI-689 was added to equal 20 wt% solids; OXE01 was added to make up 2.5 wt% solids; and a blend of 2 parts 7-octenyltrimethoxysilane (KBM-1083), 0.2 parts 4-hydroxyTEMPO, and 0.2 parts Polyfox PF-656 was added to make up 2.4 wt% solids. Cyclopentanone was then added to make the solids content of the entire solution 51% and the total mass 15 grams. The vial was sealed and rolled overnight to homogenize. The contents of the vial were then passed through a 5 micron Nylon TM The solution was degassed at ambient conditions for 3 hours prior to coating.

[0131] Example 5

[0132] The formulation was prepared in the same manner as Example 4, except that S2 prepared from Example 2 was used instead of S3.

[0133] Example 6

[0134] The formulation was prepared in the same manner as Example 4, except that S2 prepared from Example 2 was used instead of S3, which was used to make up 70.1% of the solids, and BMI-689 was used to make up 25% of the solids.

[0135] Example 7

[0136] The formulation was prepared in the same manner as Example 4, except that S2 prepared from Example 2 was used instead of S3, which was used to constitute 80.1% of the solids, and BMI-689 was used to constitute 15% of the solids.

[0137] Example 8

[0138] The formulation was prepared in the same manner as Example 4, except that S2 prepared from Example 2 was used instead of S3, and OXE02 was used instead of OXE01.

[0139] Example 9

[0140] The formulation was prepared in the same manner as Example 4, except that S2 prepared from Example 2 was used instead of S3, and BMI-1400 was used instead of BMI-689.

[0141] Example 10

[0142] The formulation was prepared in the same manner as Example 4, except that S2 prepared from Example 2 was used instead of S3, and BMI-TMH was used instead of BMI-698.

[0143] Example 11

[0144] The formulation was prepared in the same manner as Example 4, except that S2 prepared from Example 2 was used instead of S3, and S1 prepared from Example 1 was used instead of BMI-689.

[0145] Example 12

[0146] The formulation was prepared in the same manner as Example 4, except BMI-689 was used to constitute 92.6 wt % of the solids and S3 was omitted.

[0147] Comparative Example 1

[0148] The formulation was prepared in the same manner as Example 4, except that S2 prepared from Example 2 was used instead of S3, and Omnirad 819 was used instead of OXE01.

[0149] Comparative Example 2

[0150] The formulation was prepared in the same manner as Example 4, except that S3 was used to constitute 77.6 wt% of the solids and OXE01 was removed.

[0151] Comparative Example 3

[0152] The formulation was prepared in the same manner as Example 4, except that S2 prepared from Example 2 was used instead of S3, and BMI-5100 was used instead of BMI-689.

[0153] Comparative Example 4

[0154] The formulation was prepared in the same manner as Example 4, except that S2 prepared from Example 2 was used instead of S3, and BMI-4000 was used instead of BMI-689.

[0155] Preparation of polymer films

[0156] The polymer formulations were deposited by spin coating onto silicon substrates for photolithographic evaluation or onto copper wafer substrates to obtain free-standing films for analysis with a diameter of 200 mm and soft baked at 120° C. for 3 minutes.

[0157] To determine the irradiation distance from the film and the total energy delivered, a Karl Süss mask aligner was used. An exposure and alignment gap of 20 μm was used. The mask aligner used a broadband UV light source during which the power was measured to be 30 W. 600 mj / cm was delivered to the film using a 20 second period. 2 The film is exposed through a multi-transmission mask that allows variable light intensities to pass through to determine the exposure speed.

[0158] The films were post exposed and baked for 90 seconds at 65° C. The films were puddle developed in propylene glycol methyl ether acetate (PGMEA) for twenty to thirty seconds, then spin dried, rinsed with PGMEA, and a post development bake of 120° C. was used for 1 minute.

[0159] For the free-standing film samples, the polymer films were then cured in a Blue M oven at 200°C under nitrogen, less than 100 ppm oxygen for one hour. The resulting substrate was cut to the appropriate size, and the film was lifted in a 5% ammonium sulfate water bath, rinsed and dried to obtain a free-standing film for analysis. Film thickness was measured using an optical Filmetrics F50 and corresponding software tools.

[0160] Characterization of polymer films

[0161] Test Method

[0162] (1) Dielectric properties:

[0163] The dielectric properties of the free-standing films were determined using IPC test method TM-650 2.5.5.1 using copper split cylinder resonators machined so that they each had cavity frequencies of 20, 30, and 40 GHz and a Keysight N5224A PNA network analyzer.

[0164] The geometry of the membrane was such that the substrate extended beyond the diameter of the two cylindrical cavity sections. Although the thickness of the dielectric substrate can vary from 0.05 mm to 5.0 mm, a substrate thickness of 0.02 mm was used.

[0165] The free-standing membrane was placed in the cavity of a split cylindrical resonator and the TE was measured using a network analyzer. 011 The resonant frequency and quality factor of the resonant mode are obtained from TE 011 The resonant modes are used to calculate the relative dielectric constant (Dk) and loss tangent (Df) of the film.

[0166] (2) Lithography data

[0167] The film thickness loss after development was measured using a Filmetrics F50 tool as described above. The gel point energy (Egel) was determined from an energy perspective when the film thickness was greater than or equal to eight percent of the film thickness over the entire twenty seconds of exposure (358 mJ / cm2 in this case). Resolution was determined by optical inspection of circular-sized through-holes, which were found to be resolved by optical microscopy.

[0168] (3) Dynamic mechanical analysis

[0169] The free-standing films were cut into 10 mm by 25 mm geometries and placed in a TA Instruments dynamic mechanical analyzer Q800 instrument at a strain rate of 0.06%, a preload force of 1 Newton, and a frequency of 1 Hertz. The temperature was equilibrated at 50° C. and then raised to 200° C. at a rate of 5° C. / min. The glass transition temperature value was taken as the maximum value of the tan delta curve.

[0170] Test Results

[0171] In Comparative Examples 1-4, material property data such as Dk, Df and Tg could not be obtained because the materials were not UV curable and completely dissolved in the developer, leaving a clean substrate and no film formed from the liquid formulation.

[0172] Table 1 lists the test results of Examples 4-12.

[0173] It should be noted that not all of the activities described above in the general description or examples are required, that a portion of a specific activity may not be required, and that one or more other activities may be performed in addition to those described. Furthermore, the order in which the activities are listed is not necessarily the order in which they are performed.

[0174] Table 1 - Membrane Properties

[0175]

Claims

1. A photosensitive composition comprising a photoinitiator and a bismaleimide component, wherein the photoinitiator is an oxime ester compound, the oxime ester compound is present in an amount of 0.5 to 25 weight percent based on the weight of the bismaleimide component, and wherein, The bismaleimide component includes a bismaleimide compound or a bismaleimide oligomer, and the bismaleimide compound is represented by the general formula (I): wherein R is a substituted or unsubstituted linking group selected from the group consisting of: alkylene, cycloalkylene, cycloalkylene aryl, cycloalkyl alkylene, and combinations thereof; and R1 is selected from the group consisting of: hydrogen, deuterium, halogen, cyano, methyl, vinyl, allyl, substituted or unsubstituted isoprene having 1 to 100 carbon atoms, and combinations thereof, and the bismaleimide oligomer is represented by the general formula (II): Where R2 is H or CH3; R3 is C1-C 40 Alkyl, alkyl polydimethylsiloxane or alkylaryl; R4 is selected from the group consisting of: and combinations thereof; and n is an integer from 1 to 10.

2. The photosensitive composition according to claim 1, wherein The photoinitiator is selected from the group consisting of: and combinations thereof, wherein R1 is CO2Ph, CO2Me or CO2Et; R2 is a ketone, an aryl group, an aryl ether, a sulfide aryl ether or an alkyl group; R3 is H, OH, COOH, a methyl group; R4 and R5 are each independently an alkyl group, a cycloalkyl group or a phenyl group having 1 to 10 carbon atoms; R6 and R7 are each independently an alkyl group, a cycloalkyl group or a phenyl group having 1 to 10 carbon atoms; R8 is an alkyl group having 1 to 5 carbon atoms; R9 is H, a methyl group or an acetyl group; R 10 is NO2 or ArCO; R 11 is an alkyl group having 1 to 6 carbon atoms; and R 12 and R 13 Each is independently an alkyl group, a cycloalkyl group or a phenyl group having 1 to 10 carbon atoms.

3. The photosensitive composition according to claim 1, further comprising a thermosetting polymer.

4. The photosensitive composition according to claim 3, wherein The thermosetting polymer is represented by the general formula (III): wherein Ar1 is a heterocyclic ring containing N, S, O or P atoms; R2 is H, CH3, ethyl or tert-butyl; R3 is H, C1-C 12 Alkyl or C1-C 12 Olefin; R4 is cyclobutene, 1-oxy-cyclobutene, α-methylcyclobutene; l is an integer from 0 to 10; R6 is an alkyl group, a cycloalkyl group or an aryl group having 1 to 12 carbon atoms; n is an integer from 5 to 70; m is an integer from 5 to 50; and o is an integer from 5 to 50; and p is an integer from 5 to 50, wherein l+n+m+o+p=100.

5. The photosensitive composition of claim 1, further comprising an arylcyclobutene monomer.

6. The photosensitive composition according to claim 5, wherein The aromatic cyclobutene monomer is represented by the general formula (IV), (V), or (VI), in: K1 is a divalent group selected from the group consisting of an alkyl group, an aryl group, a carbocyclic aromatic group, a polycyclic aromatic group, a heteroaryl group, an aryloxy group, an arylalkyl group, a carbonyl group, an ester, a carboxyl group, an ether, a thioester, a thioether and a tertiary amine; L1 is a covalent bond or a multivalent linking group; M is a substituted or unsubstituted divalent aromatic or polyaromatic group, or a substituted or unsubstituted divalent heteroaromatic group; R2-R5 are the same or different and are each independently selected from the group consisting of unsubstituted or substituted alkyl, unsubstituted or substituted alkoxy, unsubstituted or substituted aryl, unsubstituted or substituted aryloxy, alkylthiol, arylthiol, substituted alkylamino and substituted arylamino; R6-R8 are the same or different and are each independently selected from the group consisting of hydrogen, deuterium, cyano, halogen, methyl, vinyl, allyl, and substituted or unsubstituted isoprene having 1 to 100 carbon atoms; K2 is a polymerizable functional group; and x and y are the same or different and are an integer from 1 to 5, wherein when L1 is a covalent bond, y=1.

7. The photosensitive composition according to claim 6, wherein The aromatic cyclobutene monomer is selected from the group consisting of 1-(4-vinylphenoxy)-benzocyclobutene, 1-(4-vinylmethoxy)-benzocyclobutene, 1-(4-vinylphenyl)-benzocyclobutene, 1-(4-vinylhydroxynaphthyl)-benzocyclobutene, 4-vinyl-1-methyl-benzocyclobutene, 4-vinyl-1-methoxy-benzocyclobutene and 4-vinyl-1-phenoxy-benzocyclobutene.

8. The photosensitive composition of claim 5, further comprising at least one dienophile monomer.

9. The photosensitive composition according to claim 8, wherein The dienophile monomer is represented by the general formula (VII), wherein B is hydrogen, substituted or unsubstituted alkyl, substituted or unsubstituted aromatic moiety or substituted or unsubstituted heteroaromatic moiety, hydroxyl or substituted or unsubstituted alkoxy; and R9-R 11 are the same or different and are each independently selected from the group consisting of hydrogen, vinyl, allyl, substituted or unsubstituted isoprene having 1 to 100 carbon atoms, substituted or unsubstituted alkyl groups having 1 to 100 carbon atoms, halogen, cyano, substituted or unsubstituted aryl groups having 6 to 100 carbon atoms, substituted or unsubstituted heteroaryl groups having 6 to 100 carbon atoms, and combinations thereof.

10. The photosensitive composition according to claim 8 or 9, further comprising at least one diene monomer.

11. The photosensitive composition according to claim 10, wherein The diene monomer is represented by the general formula (VIII), Where R 9 is the same or different at each occurrence and is selected from hydrogen and methyl; and R 10 is the same or different at each occurrence and is selected from hydrogen, C 1-5 Alkyl, C 1-5 Alkoxy, C 1-5 Thioalkyl and C 5-12 Alkenyl.

12. The photosensitive composition of claim 10, further comprising at least one nitrogen-containing heterocyclic monomer.

13. The photosensitive composition of claim 1, further comprising an inhibitor.

14. The photosensitive composition according to claim 13, wherein The inhibitor is selected from the group consisting of: 2,6-di-tert-butyl-4-methylphenol, 2,5-di-tert-butyl-1,4-benzohydroquinone, 2-tert-butylhydroquinone, 2,3,5-trimethyl-1,4-hydroquinone, 4-methoxyphenol, 2,2,6,6-tetramethyl-1-piperidinyloxy, 4-hydroxy-2,2,6,6-tetramethyl-1-piperidinyloxy, dibenzo-1,4-thiazine, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphate, triethylene glycol bis[β-(5-tert-butyl-4-hydroxy-3-methylphenyl) propionate] and 2,6-di-tert-butyl-4-octadecylphenol and combinations thereof.

15. A photolithography method comprising the following steps: (a) imagewise heating a presensitized photolithographic printing plate comprising a hydrophilic support and an imaging layer comprising a photosensitive composition as claimed in any one of claims 1 to 14; (b) exposing the plate to UV light; and (c) Dissolve and remove the non-imaged areas with a solution.

16. The photolithography method according to claim 15, further comprising a step (b1) of heating the plate between the steps (b) and (c).