Positive electrode active material for lithium secondary battery and preparation method thereof
By doping specific elements into the positive electrode active material of lithium secondary battery, the problem of insufficient particle strength and structural stability of lithium secondary battery under high nickel content is solved, and the formation of single-particle form at a lower calcination temperature is achieved, which improves the The battery life and resistance characteristics solve the problem of electrochemical performance deterioration caused by high-temperature calcination.
Patent Information
- Application Number
- CN201980076176.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-18
- Filing Date
- 2019-11-19
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2039-11-19
AI Technical Summary
The existing lithium secondary battery positive electrode active materials have insufficient particle strength and structural stability under high nickel content, resulting in deterioration of electrochemical performance and reduced capacity, and problems of life and resistance characteristics caused by high temperature calcination.
High nickel content lithium transition metal oxides of nickel, cobalt and manganese are prepared by doping specific elements such as B, Zr, Mg, Ti, Sr, W and Al to ensure single-particle form at lower calcination temperatures and improve rolls Pressure density and particle strength reduce lithium by-products and enhance structural stability.
It is realized that the high nickel content positive electrode active material is prepared at a lower calcination temperature, maintaining the form of a single particle, improving the life and resistance characteristics of the battery, enhancing the structural stability and capacity characteristics, and avoiding the electrochemical performance deterioration caused by high-temperature calcination.
Smart Images

Figure CN113169329B_ABST
Abstract
Description
Technical Field
[0002] CROSS-REFERENCE TO RELATED APPLICATIONS
[0003] This application claims the benefit of Korean Patent Application No. 10-2018-0143804, filed on November 20, 2018, and Korean Patent Application No. 10-2019-0147928, filed on November 18, 2019, in the Korean Intellectual Property Office, the disclosures of which are incorporated herein by reference in their entirety. Technical Field
[0004] The present invention relates to a positive electrode active material for a lithium secondary battery, a preparation method thereof, a positive electrode for a lithium secondary battery comprising the positive electrode active material, and a lithium secondary battery. Background Art
[0005] As the technology of mobile devices develops and the demand increases, the demand for secondary batteries as energy sources has increased significantly. Among these secondary batteries, lithium secondary batteries with high energy density, high voltage, long cycle life and low self-discharge rate have been commercialized and widely used.
[0006] Lithium transition metal composite oxides have been used as positive electrode active materials for lithium secondary batteries, and among these oxides, lithium cobalt composite metal oxides such as LiCoO2 having high operating voltage and excellent capacity characteristics are mainly used. However, LiCoO2 has very poor thermal properties due to an unstable crystal structure caused by delithiation, and because LiCoO2 is expensive, there are limitations in using a large amount of LiCoO2 as a power source for applications such as electric vehicles.
[0007] Lithium manganese composite metal oxides (LiMnO2 or LiMn2O4), lithium iron phosphate compounds (LiFePO4, etc.) or lithium nickel composite metal oxides (LiNiO2, etc.) have been developed as materials to replace LiCoO2. Among these materials, lithium nickel composite metal oxides, which can easily realize large-capacity batteries due to their high reversible capacity of about 200mAh / g, have been more actively studied and developed. However, the limitation of LiNiO2 is that LiNiO2 has poor thermal stability compared to LiCoO2, and when an internal short circuit occurs in a charged state due to external pressure, the positive electrode active material itself decomposes, causing the battery to rupture and catch fire. Therefore, as a method for improving the low thermal stability while maintaining the excellent reversible capacity of LiNiO2, lithium nickel cobalt manganese oxides in which a portion of the nickel is replaced by manganese (Mn) or cobalt (Co) have been developed.
[0008] However, lithium nickel cobalt manganese oxide has low particle strength, structural stability and capacity, especially when the amount of nickel is increased to more than 60 mol% to improve the capacity characteristics, there is a limitation in that the nickel in lithium nickel cobalt metal oxide tends to remain as Ni 2+ , so a large amount of lithium by-products such as LiOH and Li2CO3 are generated on the surface. Therefore, when the lithium nickel cobalt metal oxide having a large amount of lithium by-products on the surface is used, a swelling phenomenon may be caused in the lithium secondary battery due to a reaction with an electrolyte injected into the lithium secondary battery, and thus, the secondary battery including the lithium nickel cobalt metal oxide cannot fully exhibit battery performance.
[0009] Therefore, there is a need to develop a positive electrode active material that can be used to manufacture a secondary battery having high capacity and improved lifespan and resistance characteristics by enhancing particle strength and structural stability. Summary of the invention
[0010] Technical issues
[0011] One aspect of the present invention provides a positive electrode active material, wherein the positive electrode active material has a 3 Up to 3.3g / cm 3 After rolling at a rolling density of 4000 g, the average particle size (D 50 ), the positive electrode active material has a single particle form, and the positive electrode active material is doped with a specific doping element to obtain high capacity characteristics while having improved lifespan and resistance characteristics.
[0012] Another aspect of the present invention provides a method for preparing a positive electrode active material, wherein a specific doping element is doped when preparing the positive electrode active material, so that the positive electrode active material can still be 3.0 g / cm2 even when a conventional lithium transition metal oxide containing a large amount of nickel is calcined at a temperature relatively lower than the calcination temperature for preparing a lithium transition metal oxide in a single particle form. 3 Up to 3.3g / cm 3 After rolling at a rolling density of 4000 g, the average particle size (D 50 ) and is in single particle form without deteriorating the electrochemical performance.
[0013] Another aspect of the present invention provides a positive electrode for a lithium secondary battery, the positive electrode for a lithium secondary battery including the positive electrode active material.
[0014] Another aspect of the present invention provides a lithium secondary battery, the lithium secondary battery comprising the positive electrode for a lithium secondary battery.
[0015] Technical Solution
[0016] According to one aspect of the present invention, a positive electrode active material is provided, wherein the positive electrode active material is a lithium transition metal oxide containing nickel (Ni), cobalt (Co) and manganese (Mn), wherein the lithium transition metal oxide has 60 mol% or more of nickel (Ni) relative to the total molar number of transition metals other than lithium, and the lithium transition metal oxide is doped with at least any one doping element selected from the following: B, Zr, Mg, Ti, Sr, W and Al, and the positive electrode active material has a carbon content of 1.0 g / cm 3 Up to 3.3g / cm 3 After rolling at a rolling density of 4000 g, the average particle size (D 50 ), and the positive electrode active material has a single particle form.
[0017] According to another aspect of the present invention, a method for preparing a positive electrode active material is provided, the method comprising the following steps: preparing a transition metal hydroxide precursor, wherein the transition metal hydroxide precursor contains 60 mol% or more of nickel (Ni) relative to the total molar number of the transition metal hydroxide comprising nickel (Ni), cobalt (Co) and manganese (Mn); mixing and drying the transition metal hydroxide precursor with an aqueous solution containing a doping element raw material, the doping element being selected from: B, Zr, Mg, Ti, Sr, W and Al; and mixing a lithium raw material with the mixture and calcining at a temperature above 810°C to prepare a lithium transition metal oxide in the form of a single particle.
[0018] According to another aspect of the present invention, there is provided a positive electrode for a lithium secondary battery, the positive electrode for a lithium secondary battery comprising the positive electrode active material according to the present invention.
[0019] According to another aspect of the present invention, a lithium secondary battery is provided, wherein the lithium secondary battery comprises the positive electrode according to the present invention.
[0020] Beneficial Effects
[0021] According to the present invention, when preparing a cathode active material containing a large amount of nickel, by doping a specific doping element, even when calcining is performed at a relatively lower temperature than the temperature at which a conventional cathode active material in a single particle form is prepared, a cathode active material having a single particle form and a weight of 3.0 g / cm 3 Up to 3.3g / cm 3 After rolling at a rolling density of 4000 g, the average particle size (D 50 ) positive electrode active material. Therefore, without deteriorating the electrochemical characteristics of the positive electrode active material due to high-temperature calcination, a positive electrode active material with improved life and resistance characteristics can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is a SEM image of the positive electrode active material prepared in Example 1 of the present invention;
[0023] Figure 2 is a SEM image of the positive electrode active material prepared in Comparative Example 1 of the present invention;
[0024] Figure 3 is a SEM image of the positive electrode active material prepared in Comparative Example 3 of the present invention;
[0025] Figure 4 is a graph showing the capacity retention rate of lithium secondary batteries including the positive electrode active materials prepared in Examples 1 to 2 of the present invention and Comparative Examples 1 to 4 according to the presence or absence of B doping at each calcination temperature;
[0026] Figure 5 is a graph showing capacity retention rates according to cycles of lithium secondary batteries including the positive electrode active materials prepared in Examples 1 to 2 of the present invention and Comparative Examples 1 to 4;
[0027] Figure 6 is a graph showing resistance characteristics of lithium secondary batteries including the positive electrode active materials prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 2 according to the presence or absence of B doping at each calcination temperature; and
[0028] Figure 7 is a graph showing continuous charge characteristics of lithium secondary batteries including the positive electrode active materials prepared in Examples 1 and 2 and Comparative Example 3. DETAILED DESCRIPTION
[0029] Hereinafter, the present invention will be described in more detail.
[0030] It should be understood that the words or terms used in the specification and claims should not be interpreted as the meanings defined in commonly used dictionaries, and it should be further understood that, on the basis of the principle that the inventor can appropriately define the meanings of words or terms to best explain the present invention, the words or terms should be interpreted as having meanings consistent with their meanings in the relevant technical field background and technical concepts of the present invention.
[0031] In this specification, "particle" refers to a micron-sized crystal grain, and when it is magnified and observed, it can be classified as a "crystal grain" having a crystal form of tens of nanometers. When further magnified, it is seen that there are separate regions where atoms form a lattice structure in regular directions, which are called "crystals", and the size of the particle observed in XRD is defined by the size of the crystallite. The crystallite size can be measured using peak broadening of XRD data and quantitatively calculated using the Scherrer equation.
[0032] In this specification, the average particle size (D 50 The average particle size (D) is defined as the particle size corresponding to 50% of the volume cumulative amount in the particle size distribution curve of the particles. The average particle size (D) can be measured using, for example, a laser diffraction method. 50 ). In general, laser diffraction methods allow the measurement of particle sizes from submicrometers to several millimeters and can obtain results with high reproducibility and high resolution.
[0033] Positive electrode active material
[0034] Conventionally, in order to increase the capacity of lithium secondary batteries, positive electrode active materials with a high nickel content containing more than 60 mol% nickel relative to the total molar number of transition metals other than lithium are used. However, in this case, the excessive generation of lithium byproducts on the surface of the positive electrode active material causes an expansion phenomenon of the secondary battery, and there is also a limitation that the stability of the positive electrode active material is deteriorated due to low particle strength. In order to overcome the limitation, when a single-particle positive electrode active material is prepared by over-calcining a positive electrode active material with a high nickel content, the stability is improved, but there are limitations such as degradation of life and resistance characteristics due to high-temperature calcination.
[0035] In response, the inventors of the present invention have conducted thorough research to develop a high-nickel content positive electrode active material in the form of a single particle without deteriorating the life and resistance characteristics, and as a result, the inventors have discovered and completed the following method: by doping a high-nickel content transition metal oxide with a specific doping element, a positive electrode active material is prepared, which has a single particle form even after calcination at a relatively low temperature compared to the temperature at which a single-particle form of the positive electrode active material is prepared from a conventional high-nickel content positive electrode active material and also has improved life and resistance characteristics.
[0036] The positive electrode active material according to the present invention is a lithium transition metal oxide containing nickel (Ni), cobalt (Co) and manganese (Mn), wherein the lithium transition metal oxide has 60 mol% or more of nickel (Ni) relative to the total molar number of transition metals other than lithium, and the lithium transition metal oxide is doped with at least one doping element selected from the following: B, Zr, Mg, Ti, Sr, W and Al, and the positive electrode active material has a relative humidity of 3.0 g / cm 3 Up to 3.3g / cm 3 After rolling at a rolling density of 4000 g, the average particle size (D 50 ) and has a single particle form.
[0037] The lithium transition metal oxide according to an embodiment of the present invention contains nickel (Ni), cobalt (Co) and manganese (Mn), and can be an NCM-type lithium transition metal oxide with a high nickel content (high Ni) of 60 mol% or more, more preferably 80 mol% or more, and most preferably 85 mol% to 90 mol% of nickel (Ni) relative to the total amount of transition metals.
[0038] As described above, when a lithium transition metal oxide containing 60 mol % or more, preferably 80 mol % or more of nickel relative to the total moles of transition metal oxides other than lithium is used for a battery, high capacity characteristics can be obtained due to the high nickel content.
[0039] Furthermore, the lithium transition metal oxide having a high nickel content is doped with at least any one doping element selected from the group consisting of B, Zr, Mg, Ti, Sr, W and Al, most preferably B.
[0040] When the lithium transition metal oxide having a high nickel content is doped with at least one doping element selected from B, Zr, Mg, Ti, Sr, W and Al, the structural stability of the positive electrode active material is improved, thereby improving the life and resistance characteristics when applied to the battery. In particular, when B is included as a doping element, B promotes the growth of the positive electrode active material crystal, thereby after the positive electrode active material is prepared and pulverized, even when the positive electrode active material is pulverized at 3.0 g / cm 3 Up to 3.3g / cm 3 When rolling density is used for rolling, particle size (D 50 ) is a positive electrode active material having a diameter of 4 μm to 10 μm. In addition, due to the tetrahedral crystal structure of B, the covalent bond between B and O is stronger than the covalent bond between the transition metal and O. Therefore, during the insertion / deinsertion of lithium ions, the structural expansion is prevented and the SEI layer is formed more stably, thereby reducing the side reaction between the surface of the positive electrode active material and the electrolyte. Therefore, the specific surface area of the positive electrode active material is reduced, the particle strength is increased to prevent the breakage of the particles during rolling, and the amount of lithium byproducts is reduced to reduce the side reaction with the electrolyte, thereby when applied to a battery, a battery with improved life, stability and resistance characteristics can be provided.
[0041] For example, the doping element may be included in an amount of 100 ppm to 4000 ppm, preferably 500 ppm to 2000 ppm, relative to the total weight of the lithium transition metal oxide. When the doping element is included within the above range, lifespan and resistance characteristics may be further improved.
[0042] The positive electrode active material of the present invention is in the form of a single particle (i.e., a primary particle), rather than in the form of aggregated secondary particles. In the present invention, "primary particle" refers to a primary structure of a single particle, and "secondary particle" refers to an aggregate, i.e., a secondary structure formed by aggregating primary particles by physical or chemical bonding between primary particles without performing a deliberate aggregation or assembly process of the primary particles constituting the secondary particles.
[0043] In addition, at 3.0 g / cm 3 Up to 3.3g / cm 3 After rolling at a rolling density of 1000 μm, the positive electrode active material of the present invention may have an average particle size (D 50 For example, the positive electrode active material exists in the form of secondary particles in which primary particles are aggregated during the process of mixing and calcining the positive electrode active material precursor and the lithium raw material, and when the secondary particles are crushed and heated to 3.0 g / cm 3 Up to 3.3g / cm 3 When the positive electrode active material is rolled at a rolling density of 100,000, the aggregated positive electrode active material breaks around the grains. In particular, when the positive electrode active material is doped with a specific doping element, such as at least one doping element selected from B, Zr, Mg, Ti, Sr, W and Al, most preferably B, the crystal size of the positive electrode active material increases with the doping of the doping element B, so that the average particle size (D 50 ) satisfies the above range. That is, according to the present invention, the crystal size of the positive electrode active material is increased by doping the doping element, and in this case, even when calcined at a temperature lower than the calcination temperature (e.g., 900° C. or more) for conventional single particle formation, the positive electrode active material in the form of a single particle can be easily prepared, and the particle strength of the prepared positive electrode active material is increased to prevent the particles from breaking during rolling, increase the rolling density, reduce the specific surface area, and reduce lithium by-products, thereby reducing the amount of gas generated due to side reactions with the electrolyte.
[0044] The crystallite size of the lithium transition metal oxide can be 170 nm or more, preferably 180 nm to 200 nm. When the crystallite size of the lithium transition metal oxide satisfies the above range, the lithium transition metal oxide can have a single particle form. For example, when the crystallite size of the positive electrode active material exceeds 200 nm, the positive electrode active material has a single particle form, but an increase in the crystallite size may deteriorate the efficiency characteristics. In addition, when the crystallite size of the positive electrode active material is less than 170 nm, the lithium transition metal oxide may not have a single particle form but a secondary particle form formed by aggregation of primary particles. Since the positive electrode active material has a single particle form, the particle strength increases, whereby the occurrence of cracking of the positive electrode active material can be reduced during charging and discharging of the battery including the positive electrode active material, thereby improving the stability of the positive electrode active material.
[0045] More specifically, the lithium transition metal oxide according to an embodiment of the present invention can be represented by the following Formula 1.
[0046] [Formula 1]
[0047] Li 1+a Ni x Co y Mn z M 1 w O2
[0048] In Formula 1 above, 0 ≤ a ≤ 0.5, 0.6 ≤ x < 1, 0 < y ≤ 0.4, 0 < z ≤ 0.4 and 0 < w ≤ 0.04, and M 1 is at least any one selected from the following: B, Zr, Mg, Ti, Sr, W, and Al. More preferably, 0 ≤ a ≤ 0.5, 0.8 ≤ x < 1, 0 < y ≤ 0.2, 0 < z ≤ 0.2 and 0 < w ≤ 0.01, and M 1 is B.
[0049] Accordingly, a NCM-based positive electrode active material having a single particle form and 60 mol% or more of nickel (Ni) and doped with a specific doping element can achieve high capacity and excellent stability at the same time. Specifically, the specific surface area is reduced, the particle strength is increased to prevent particle cracking during rolling, and the amount of lithium by-products is reduced to reduce side reactions with the electrolyte. In addition, the NCM-based positive electrode active material with a high nickel content (high Ni) of the present invention ensures excellent structural stability and chemical stability, thereby reducing the amount of gas generated when driving the battery and obtaining thermal stability.
[0050] Method for preparing a positive electrode active material
[0051] Next, a method for preparing a positive electrode active material according to the present invention will be described.
[0052] Specifically, the method for preparing a positive electrode active material according to the present invention includes the following steps: preparing a transition metal hydroxide precursor, wherein the transition metal hydroxide precursor contains 60 mol% or more of nickel relative to the total molar number of the transition metal hydroxide having nickel (Ni), cobalt (Co) and manganese (Mn); mixing and drying the transition metal hydroxide precursor with an aqueous solution containing a doping element raw material, wherein the doping element is selected from: B, Zr, Mg, Ti, Sr, W and Al; and mixing a lithium raw material with the mixture and calcining at a temperature above 810°C to prepare a lithium transition metal oxide in the form of a single particle.
[0053] In more detail, first, a transition metal precursor is prepared, wherein the transition metal precursor contains 60 mol % or more of nickel relative to the total moles of a transition metal hydroxide having nickel (Ni), cobalt (Co), and manganese (Mn).
[0054] The transition metal precursor may be used by purchasing a commercially available precursor for a positive electrode active material, or may be prepared according to a method for preparing a precursor for a positive electrode active material well known in the art.
[0055] The precursor may be prepared by adding a complex forming agent containing ammonium cations and a basic compound to a transition metal solution containing a nickel-containing raw material, a cobalt-containing raw material, and a manganese-containing raw material and performing a coprecipitation reaction.
[0056] The nickel-containing raw material may be, for example, nickel-containing acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide or oxyhydroxide, specifically Ni(OH)2, NiO, NiOOH, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, fatty acid nickel salt, nickel halide or a combination of the above materials, but is not limited thereto.
[0057] The cobalt-containing raw material may be a cobalt-containing acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide or oxyhydroxyl, etc., specifically Co(OH)2, CoOOH, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, CoSO4, Co(SO4)2·7H2O or a combination of the above materials, but is not limited thereto.
[0058] The manganese-containing raw material can be, for example, manganese-containing acetates, nitrates, sulfates, halides, sulfides, hydroxides, oxides, oxyhydroxides or a combination of the above materials, specifically: manganese oxides, such as Mn2O3, MnO2 and Mn3O4; manganese salts, such as MnCO3, Mn(NO3)2, MnSO4, manganese acetate, dicarboxylic acid manganese salts, manganese citrate and fatty acid manganese salts; oxyhydroxide manganese; manganese chloride or a combination of the above materials, but not limited to these.
[0059] The transition metal solution can be prepared by adding a nickel-containing raw material, a cobalt-containing raw material and a manganese-containing raw material to a solvent (specifically water or a mixed solvent of an organic solvent that can be uniformly mixed with water (such as alcohol, etc.) and water), or the transition metal solution can be prepared by mixing an aqueous solution of a nickel-containing raw material, an aqueous solution of a cobalt-containing raw material and an aqueous solution of a manganese-containing raw material.
[0060] The complex forming agent containing ammonium cations can be, for example, NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, (NH4)2CO3 or a combination of the above materials, but is not limited thereto. On the other hand, the complex forming agent containing ammonium cations can be used in the form of an aqueous solution, and in this case, the solvent can be a mixture of water or an organic solvent (specifically alcohol, etc.) that can be uniformly mixed with water and water.
[0061] The alkaline compound may be: a hydroxide of an alkali metal or alkaline earth metal, such as NaOH, KOH or Ca(OH)2; a hydrate thereof; or a combination of the above materials. The alkaline compound may also be used in the form of an aqueous solution. In this case, the solvent may be water or a mixture of an organic solvent (specifically alcohol, etc.) that can be uniformly mixed with water and water.
[0062] The basic compound is added to adjust the pH of the reaction solution, and may be added in such an amount that the pH of the metal solution is 11 to 13.
[0063] On the other hand, the coprecipitation reaction can be carried out in an inert atmosphere such as nitrogen or argon at a temperature of 40°C to 70°C.
[0064] Through the above process, particles of nickel-cobalt-manganese hydroxide are generated and precipitated in the reaction solution. The concentrations of the nickel-containing raw material, the cobalt-containing raw material, and the manganese-containing raw material can be adjusted to prepare a precursor having 60 mol% or more of nickel (Ni) relative to the total amount of transition metals. The precipitated nickel-cobalt-manganese hydroxide particles are separated according to a conventional method and dried to obtain a nickel-cobalt-manganese precursor.
[0065] Subsequently, the aqueous solution containing the doping element raw material and the transition metal hydroxide precursor are mixed and dried.
[0066] As the doping element raw material, a sulfate, nitrate, acetate, halide, hydroxide or oxyhydroxide containing at least any one doping element selected from the following can be used: B, Zr, Mg, Ti, Sr, W and Al, and if it is soluble in a solvent such as water, it can be used without particular limitation. Preferably, the doping element raw material can be a sulfate, nitrate, acetate, halide, hydroxide or oxyhydroxide containing B, more preferably including at least any one selected from the following: boric acid, boron trioxide, boron carbide, boron trifluoride and boron monofluorine.
[0067] As described above, when the doping element is doped by a wet method in which a doping element raw material is dissolved in an aqueous solution and mixed with a transition metal hydroxide precursor, the doping element can be uniformly doped throughout the positive electrode active material. For example, when the doping element raw material is doped into a transition metal hydroxide precursor by using a dry method, the doping element may be partially aggregated and doped, so that when applied to a battery, the improvement of life and resistance characteristics may be deteriorated compared to the wet method.
[0068] For example, the doping element raw material may be dissolved in the aqueous solution at a concentration of 0.1 M to 0.5 M, preferably 0.2 M to 0.4 M. For example, when the above range is exceeded, the possibility of lithium reacting with the doping element increases, thereby reducing the reactivity of the precursor with lithium, in which case the structural integrity of the positive electrode active material is reduced, and the specific capacity, efficiency and life characteristics may be reduced.
[0069] For example, the positive electrode active material may be provided by mixing an aqueous solution of a raw material containing the doping element M so that the amount of the doping element becomes 100 ppm to 4000 ppm, preferably 500 ppm to 2000 ppm with respect to the total weight parts of the lithium transition metal oxide.
[0070] In particular, when the transition metal hydroxide precursor is doped with B as a doping element, even if the calcination temperature is lowered when preparing the positive electrode active material, B promotes the growth of the positive electrode active material crystallites, so that the positive electrode active material in the form of a single particle can be prepared. Generally, when a transition metal hydroxide precursor having a high Ni content of 60 mol% or more Ni relative to the total molar number of the transition metal is mixed with a lithium raw material (e.g., LiOH · H2O) and calcined, the reaction with the transition metal hydroxide precursor starts from the point where the lithium melts, and in this case, because the melting point of LiOH · H2O is about 400°C, the transition metal hydroxide precursor reacts with lithium at a temperature above 400°C. However, because B can react with Li at about 150°C, B and Li react at 150°C, and when Li and the transition metal hydroxide precursor react at a temperature above 450°C, B also acts as a catalyst. Therefore, the reaction temperature of Li and the transition metal hydroxide precursor is reduced, and when B is applied, a positive electrode active material in the form of a single particle can be prepared even when calcining is performed at a temperature lower than the calcination temperature of a mixture of a transition metal hydroxide precursor having a high nickel content and a lithium raw material. Therefore, the degradation of electrochemical characteristics conventionally caused by high-temperature calcination is prevented, thereby preparing a positive electrode active material with a high nickel content in the form of a single particle having improved life and resistance characteristics.
[0071] Drying is used to dry the aqueous solution in which the doping element raw material is dissolved, and can be used without particular limitation as long as the method can dry the solvent without causing chemical changes in the battery. For example, a method such as spray drying, drying using a rotary evaporator, vacuum drying or natural drying can be used.
[0072] Next, the lithium raw material is mixed with a mixture of an aqueous solution containing a doping element raw material and a transition metal hydroxide precursor, and calcined at a temperature of 810° C. or higher to prepare a positive electrode active material in the form of single particles.
[0073] The lithium raw material may be used without particular limitation as long as it is a compound containing a lithium source, but at least one selected from the group consisting of lithium carbonate (Li2CO3), lithium hydroxide (LiOH), LiNO3, CH3COOLi and Li2(COO)2 may be preferably used.
[0074] Calcination can be performed in an oxygen atmosphere at 810°C or above, preferably 810°C to 880°C, preferably 810°C to 850°C, and more preferably 810°C to 830°C for 12 to 24 hours. As described above, the positive electrode active material can be recrystallized and formed into single particles by calcining at a temperature of 810°C or above for 12 to 24 hours. For example, when the calcination process is performed at a temperature below 810°C, the positive electrode active material is not recrystallized, so that the positive electrode active material may be formed into secondary particles formed by aggregation of primary particles, and in this case, the particle strength of the positive electrode active material is poor, thereby the stability of the secondary battery using the positive electrode active material may be reduced. In addition, when the calcination process is performed at a temperature higher than 880°C, the positive electrode active material recrystallizes to form a single particle, and in the case of a transition metal hydroxide precursor with a high Ni content, mixing with lithium and performing high-temperature calcination results in the formation of Ni from the secondary particles. 3+ To You 2+ The phase transition of is replaced by Li sites, so that when applied to batteries, the capacity, life and resistance characteristics may be deteriorated.
[0075] Next, in order to remove lithium by-products present on the surface of the lithium transition metal oxide, a step of washing the lithium transition metal oxide may be further performed.
[0076] Lithium transition metal oxides with high nickel content are structurally less stable than lithium transition metal oxides with low nickel content, thereby generating more lithium byproducts, such as unreacted lithium hydroxide or lithium carbonate, during the preparation process. When a large amount of lithium byproducts are present in the positive electrode active material, the lithium byproducts react with the electrolyte to generate gas and expand, thereby causing significant degradation of high temperature stability. Therefore, a washing process for removing lithium byproducts from lithium transition metal oxides with high nickel content may be further performed.
[0077] The washing process can be performed, for example, by adding the lithium transition metal oxide to ultrapure water and stirring. In this case, the washing temperature can be 20°C or less, preferably 10°C to 20°C, and the washing time can be about 10 minutes to 1 hour. When the washing temperature and the washing time meet the above ranges, the lithium byproduct can be effectively removed.
[0078] positive electrode
[0079] Next, a positive electrode for a lithium secondary battery is provided, which includes the positive electrode active material according to the present invention.
[0080] Specifically, the positive electrode for a secondary battery includes a positive electrode collector and a positive electrode active material layer formed on the positive electrode collector, wherein the positive electrode active material layer includes the positive electrode active material according to the present invention.
[0081] In this case, since the positive electrode active material is the same as described above, the detailed description will be omitted, and only the remaining configuration will be described in detail hereinafter.
[0082] The positive electrode current collector is not particularly limited as long as it has conductivity and does not cause chemical changes in the battery, and for example: stainless steel; aluminum; nickel; titanium; fired carbon; or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can generally have a thickness of 3 μm to 500 μm, and fine concavoconvexity can be formed on the surface of the current collector to improve the adhesion of the positive electrode active material. For example, the positive electrode current collector can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam body, and a non-woven fabric body.
[0083] The positive electrode active material layer may include a conductive material and, optionally, a binder.
[0084] In this case, the positive electrode active material may be contained in an amount of 80 wt % to 99 wt %, more specifically 85 wt % to 98.5 wt %, relative to the total weight of the positive electrode active material layer. When the positive electrode active material is contained in an amount within the above range, excellent capacity characteristics may be obtained.
[0085] The conductive material is used to provide conductivity to the electrode, wherein any conductive material can be used without particular limitation, as long as it has electronic conductivity and does not cause chemical changes in the battery. Specific examples of conductive materials may be the following substances: graphite, such as natural graphite or artificial graphite; carbon materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black or carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum or silver; conductive whiskers, such as zinc oxide or potassium titanate; conductive metal oxides, such as titanium oxide; or conductive polymers, such as polyphenylene derivatives, and any one of the above materials or a mixture of two or more thereof may be used. The conductive material may be included in an amount of 0.1 wt % to 15 wt % relative to the total weight of the positive electrode active material layer.
[0086] Binder is used to improve the adhesion between positive active material particles and the adhesion between positive active material and collector. Specific examples of binders can be polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber or various copolymers of the above materials, and any one of the above materials or a mixture of two or more thereof can be used. Relative to the gross weight of the positive active material layer, the binder can be included in an amount of 0.1 wt % to 15 wt %.
[0087] In addition to using the above-mentioned positive electrode active material, the positive electrode can be prepared according to a typical method for preparing a positive electrode. Specifically, a composition for forming a positive electrode active material layer is coated on a positive electrode current collector, and then the coated positive electrode current collector is dried and rolled to prepare the positive electrode, wherein the composition is prepared by dissolving or dispersing the positive electrode active material and a selective binder and a conductive material in a solvent.
[0088] The solvent may be a commonly used solvent in the art, and may include dimethyl sulfoxide (DMSO), isopropanol, N-methylpyrrolidone (NMP), acetone or water, and any one of the above materials or a mixture of two or more thereof may be used. If the coating thickness and manufacturing yield of the slurry are taken into consideration, the solvent may dissolve or disperse the positive electrode active material, the conductive material and the binder, and may allow a viscosity that can provide excellent thickness uniformity during subsequent coating for preparing the positive electrode, then the amount of the solvent may be sufficient.
[0089] Furthermore, as another method, the positive electrode may be prepared by casting a composition for forming a positive electrode active material layer on a separate support and then laminating a film separated from the support on a positive electrode current collector.
[0090] Lithium secondary battery
[0091] In addition, in the present invention, an electrochemical device including the positive electrode can be prepared. The electrochemical device can be specifically a battery or a capacitor, and more specifically a lithium secondary battery.
[0092] The lithium secondary battery specifically includes a positive electrode, a negative electrode disposed to face the positive electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte, wherein since the positive electrode is the same as described above, its detailed description will be omitted, and only the remaining configuration will be described in detail hereinafter.
[0093] In addition, the lithium secondary battery may further selectively include a battery container accommodating an electrode assembly of a positive electrode, a negative electrode, and a separator, and a sealing member sealing the battery container.
[0094] In a lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector.
[0095] The negative electrode current collector is not particularly limited as long as it has high conductivity and does not cause chemical changes in the battery, and for example: copper; stainless steel; aluminum; nickel; titanium; fired carbon; copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc.; and aluminum-cadmium alloys can be used. In addition, the negative electrode current collector can generally have a thickness of 3 μm to 500 μm, and similar to the positive electrode current collector, fine concavoconvexities can be formed on the surface of the current collector to improve the adhesion of the negative electrode active material. For example, the negative electrode current collector can be used in various forms such as films, sheets, foils, nets, porous bodies, foams, and non-woven fabrics.
[0096] In addition to containing the negative electrode active material, the negative electrode active material layer selectively contains a binder and a conductive material.
[0097] A compound capable of reversibly intercalating and deintercalating lithium may be used as the negative electrode active material. Specific examples of the negative electrode active material may be the following substances: carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; (semi)metallic materials capable of forming alloys with lithium, such as silicon (Si), aluminum (Al), tin (Sn), lead (Pb), zinc (Zn), bismuth (Bi), indium (In), magnesium (Mg), gallium (Ga), cadmium (Cd), Si alloy, Sn alloy, or Al alloy; metal oxides that may or may not be doped with lithium, such as SiO β (0<β<2), SnO2, vanadium oxide and lithium vanadium oxide; or a composite material comprising the (semi)metal material and a carbonaceous material, such as a Si-C composite material or a Sn-C composite material, and any one of the above materials or a mixture of two or more thereof can be used. In addition, a metallic lithium film can be used as a negative electrode active material. In addition, low-crystalline carbon and high-crystalline carbon can be used as carbon materials. Typical examples of low-crystalline carbon may be soft carbon and hard carbon, and typical examples of high-crystalline carbon may be irregular, plate-like, flaky, spherical or fibrous natural graphite or artificial graphite, condensed graphite, pyrolytic carbon, mesophase pitch-type carbon fibers, mesophase carbon microbeads, mesophase pitch, and high-temperature sintered carbon such as coke derived from petroleum or coal tar pitch.
[0098] The negative electrode active material may be included in an amount of 80 to 99 parts by weight relative to the total weight of the negative electrode active material layer.
[0099] The binder is a component that helps to bind the conductive material, the active material and the current collector, wherein the binder is generally added in an amount of 0.1 to 10 parts by weight relative to the total weight of the negative electrode active material layer. Examples of binders may be polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene monomer rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile rubber, fluororubber, various copolymers of the above materials, etc.
[0100] The conductive material is a component for further improving the conductivity of the negative electrode active material, wherein the conductive material can be added in an amount of 10 parts by weight or less, such as 5 parts by weight or less, relative to the total weight of the negative electrode active material layer. The conductive material is not particularly limited as long as it has conductivity and does not cause chemical changes in the battery, and for example: graphite, such as natural graphite or artificial graphite; carbon black, such as acetylene black, Ketjen black, channel black, furnace black, lamp black or thermal black; conductive fibers, such as carbon fibers or metal fibers; carbon fluoride; metal powders, such as aluminum powder or nickel powder; conductive whiskers, such as zinc oxide or potassium titanate; conductive metal oxides, such as titanium oxide; or polyphenylene derivatives.
[0101] For example, the negative electrode active material layer can be prepared by coating a composition for forming a negative electrode prepared by dissolving or dispersing a negative electrode active material and a selective binder and a conductive material in a solvent on a negative electrode collector, and drying the coated negative electrode collector; or can be prepared by casting the composition for forming a negative electrode on a separate carrier and then laminating the film separated from the carrier on the negative electrode collector.
[0102] Meanwhile, in a lithium secondary battery, the separator separates the negative electrode from the positive electrode and provides a path for the movement of lithium ions, wherein any separator can be used as the separator without particular restriction, as long as it is commonly used in lithium secondary batteries, in particular, a separator having high moisture retention capacity for electrolytes and low resistance to the migration of electrolyte ions can be used. Specifically, a porous polymer film, such as a porous polymer film prepared by a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer; or a laminated structure having more than two layers in the above porous polymer film. In addition, a typical porous non-woven fabric can be used, such as a non-woven fabric formed by a high melting point glass fiber or a polyethylene terephthalate fiber. In addition, a coated separator containing a ceramic component or a polymer material can be used to ensure heat resistance or mechanical strength, and a separator having a single layer or a multilayer structure can be selectively used.
[0103] In addition, the electrolyte used in the present invention may include an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel polymer electrolyte, a solid inorganic electrolyte or a molten inorganic electrolyte that can be used in preparing a lithium secondary battery, but the present invention is not limited thereto.
[0104] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0105] Any organic solvent can be used as the organic solvent without particular limitation, as long as it can be used as a medium through which ions participating in the electrochemical reaction of the battery can move. Specifically, the following substances can be used as organic solvents: ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; or carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC) and propylene carbonate (PC); alcohol solvents such as ethanol and isopropanol; nitrile, such as R-CN (wherein R is a linear, branched or cyclic C2-C20 hydrocarbon group and may contain a double bond, an aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolanes; or cyclopentane sulfone. Among these solvents, carbonate solvents can be used, for example, a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ion conductivity and high dielectric constant that can improve the charge / discharge performance of the battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) can be used. In this case, when the cyclic carbonate and the chain carbonate are mixed in a volume ratio of about 1:1 to about 1:9, the performance of the electrolyte can be excellent.
[0106] Lithium salts can be used without particular limitation, as long as they are compounds that can provide lithium ions used in lithium secondary batteries. Specifically, the following substances can be used as lithium salts: LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI or LiB(C2O4)2. Lithium salts can be used in a concentration range of 0.1M to 2.0M. When the concentration of the lithium salt is within the above range, because the electrolyte can have appropriate conductivity and viscosity, the excellent performance of the electrolyte can be obtained, and the lithium ions can be efficiently moved.
[0107] In order to improve the life characteristics of the battery, inhibit the reduction of the battery capacity and increase the discharge capacity of the battery, in addition to the electrolyte components, at least one additive may be added to the electrolyte, such as halogenated alkylene carbonate compounds (such as difluoroethylene carbonate), pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, (condensed) glycol dimethyl ethers, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted Oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol or aluminum trichloride. In this case, the additive may be included in an amount of 0.1 to 5 parts by weight relative to the total weight of the electrolyte.
[0108] As described above, since the lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics and life characteristics, the lithium secondary battery is suitable for: portable devices such as mobile phones, notebook computers and digital cameras; and electric vehicles such as hybrid electric vehicles (HEV).
[0109] Thus, according to another embodiment of the present invention, there are provided a battery module including the lithium secondary battery as a unit battery and a battery pack including the battery module.
[0110] The battery module or the battery pack may be used as a power source for at least one of the following medium and large-sized devices: a power tool; an electric vehicle, including an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0111] The shape of the lithium secondary battery of the present invention is not particularly limited, but a cylindrical type using a can, a prismatic type, a pouch type, or a coin type may be used.
[0112] The lithium secondary battery according to the present invention can be used not only in a battery cell used as a power source for small devices but also as a unit battery in a medium- and large-sized battery module including a plurality of battery cells.
[0113] Preferred Implementation
[0114] Hereinafter, the present invention will be described in detail according to specific embodiments. However, the present invention can be implemented in many different forms and should not be construed as being limited to the embodiments set forth herein. Rather, these exemplary embodiments are provided to make the description thorough and complete and to fully convey the scope of the present invention to those skilled in the art.
[0115] Example
[0116] Example 1
[0117] Nickel sulfate, cobalt sulfate and manganese sulfate were dissolved in ion exchange water in an amount such that the molar ratio of nickel:cobalt:manganese was 90:4:6 to prepare a transition metal aqueous solution (2.4M). In addition, a 9% ammonia aqueous solution and a 25% sodium hydroxide aqueous solution were prepared. The transition metal aqueous solution, the ammonia aqueous solution and the sodium hydroxide aqueous solution were added to a coprecipitation reactor at a constant rate, and a coprecipitation reaction was performed in a nitrogen atmosphere to synthesize a transition metal hydroxide precursor.
[0118] Thereafter, boric acid (2.1 g) was dissolved in water (150 mL), and then a transition metal hydroxide precursor (350 g) was added to the boric acid aqueous solution (150 mL) and stirred. The mixed solution was vacuum dried using a rotary evaporator, and the slurry mixture was dried at 100° C. for more than 5 hours to prepare a transition metal hydroxide precursor.
[0119] The transition metal hydroxide precursor prepared above and LiOH were mixed in a Me:Li molar ratio of 1:1.02 and calcined at 810 °C for 11 hours to prepare a single-particle positive electrode active material (LiNi 0.90 Co 0.04 Mn 0.06 B 0.009 O2).
[0120] Example 2
[0121] A positive electrode active material was prepared in the same manner as in Example 1, except that the calcination temperature was 830° C. when the transition metal hydroxide precursor prepared in Example 1 was mixed with LiOH and calcined.
[0122] Example 3
[0123] In addition to dry-mixing boric acid (1000 ppm) with respect to the total weight of the positive active material precursor prepared in Example 1, and then calcining at 830° C. to prepare a positive active material (LiNi 0.89 Co 0.04 Mn 0.06 B 0.009 A positive electrode active material was prepared in the same manner as in Example 1 except for O2).
[0124] Comparative Example 1
[0125] A positive electrode active material was prepared in the same manner as in Example 1, except that boron was not doped in the preparation of the transition metal hydroxide precursor.
[0126] Comparative Example 2
[0127] A positive electrode active material was prepared in the same manner as in Example 2, except that boron was not doped in the preparation of the transition metal hydroxide precursor.
[0128] Comparative Example 3
[0129] In addition to mixing the transition metal hydroxide precursor prepared in Comparative Example 1 with LiOH at a molar ratio of 1:1.02 and calcining at 730°C for 11 hours to prepare and use the positive electrode active material (LiNi 0.90 Co 0.04 Mn 0.06 A positive electrode active material was prepared in the same manner as in Example 2 except for O2).
[0130] Comparative Example 4
[0131] A positive electrode active material was prepared in the same manner as in Example 1, except that the calcination temperature was 730° C. when the transition metal hydroxide precursor prepared in Example 1 was mixed with LiOH and calcined.
[0132] Experimental Example 1: Confirmation of the characteristics of the positive electrode active material
[0133] 1) SEM images
[0134] In order to confirm the surface characteristics of the positive electrode active materials prepared in Example 1, Comparative Examples 1 and 3, respectively, SEM images were examined using a scanning electron microscope. Figures 1 to 3 As shown in , it is confirmed that in Example 1 ( Figure 1 ) and Comparative Example 1 ( Figure 2 ) has a single particle form. On the other hand, it is confirmed that in Comparative Example 3 ( Figure 3 ) has the form of secondary particles formed by aggregation of primary particles.
[0135] 2) Measurement of average particle size of positive electrode active material
[0136] After the B-doped positive electrode active materials prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were pulverized for 4 minutes using a simple mixer (HMF600, Hanil Mixer), ultrasonic waves of about 28 kHz were irradiated at an output power of 60 W using a laser diffraction particle size measuring instrument (e.g., Microtrac MT 3000), and then the average particle size (D ) at 50% in the cumulative particle size distribution was calculated based on the particle size in the measuring instrument. 50 ) and are shown in the following Table 1. In addition, the B-doped positive electrode active materials prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were pulverized and subjected to 3 tons (3.1 to 3.2 g / cm 3) pressure, and then the average particle size (D 50 ) are also shown in Table 1 below.
[0137] 3) Pellet density of positive electrode active material
[0138] For the particle density of the positive electrode active materials prepared in Examples 1 to 3 and Comparative Examples 1 to 4, respectively, the internal volume was measured using a roll densitometer (4350, Carver) at a pressure of 3.0 tons. For the internal volume, a vernier caliper (Miltutoyo) was used to measure the volume inside the Sus, and the results are also shown in Table 1 below.
[0139] [Table 1]
[0140]
[0141] As shown in Table 1 above, in terms of the positive electrode active materials prepared in Examples 1 to 3, it was confirmed that the average particle size (D 50 ) is maintained at 4 μm to 6 μm. However, in the positive electrode active materials prepared in Comparative Examples 1 and 2, the crystal growth of the positive electrode active material particles doped with B is inferior to that of the embodiment, thereby confirming that the particle size after rolling is smaller than the range of the present invention. In addition, in the positive electrode active materials prepared in Comparative Examples 3 to 4, the calcination temperature is lower than the range of the present application. In this case, it is confirmed that regardless of whether B is doped, when the temperature is 3.1 g / cm 3 Up to 3.2g / cm 3 The positive electrode active material particles are broken during roll pressing at a roll pressing density of .
[0142] In addition, in the positive electrode active materials prepared in Examples 1 to 3, even when doped with B, the particle density was the same level as that of Comparative Examples 1 and 2 which were not doped with B. In addition, it was confirmed that the positive electrode active materials of Examples 1 to 3 had a more excellent particle density than Comparative Examples 3 to 4 which were in the form of secondary particles formed by aggregation of primary particles.
[0143] 4) Crystallite size of positive electrode active material
[0144] In the positive electrode active materials prepared in Examples 1 to 3 and Comparative Example 3, the crystallite sizes were measured using an X-ray diffractometer (Bruker AXS D4-Endeavor XRD), and the results are shown in Table 2 below.
[0145] [Table 2]
[0146] Crystallite size (nm) Example 1 178 Example 2 189 Example 3 208 Comparative Example 3 100
[0147] As shown in Table 2, it was confirmed that the positive electrode active materials prepared in Examples 1 to 3 were in the form of single particles having a crystallite size of 170 nm or more. On the other hand, in Comparative Example 3, since the positive electrode active material was prepared in the form of secondary particles formed by aggregation of primary particles, the crystallite size was significantly smaller than that of the present invention.
[0148] Experimental Example 2: Evaluation of Capacity Characteristics
[0149] Secondary batteries were prepared using the positive electrode active materials prepared in Examples 1 and 2 and Comparative Examples 1 to 4, and lithium secondary batteries including the positive electrode active materials of Examples 1 to 2 and Comparative Examples 1 to 4 were evaluated, respectively.
[0150] Specifically, the positive electrode active material prepared in Examples 1 and 2 and Comparative Examples 1 to 4, the carbon black conductive material and the polyvinylidene fluoride (PVdF) binder were mixed in an N-methylpyrrolidone (NMP) solvent at a weight ratio of 96.5:1.5:2 to prepare a positive electrode slurry. The positive electrode slurry was applied to one surface of an aluminum current collector, dried at 100°C, and then roll-pressed to prepare a positive electrode.
[0151] Meanwhile, lithium metal is used as the negative electrode.
[0152] The electrode assembly is prepared by inserting a porous polyethylene separator between the prepared positive electrode and the negative electrode, and then the electrode assembly is placed in a battery shell and an electrolyte is injected into the shell to prepare a lithium secondary battery. In this case, as an electrolyte, lithium hexafluorophosphate (LiPF6, 1.0M) is dissolved in an organic solvent of ethylene carbonate: ethyl methyl carbonate: diethyl carbonate (EC:EMC:DEC) mixed in a volume ratio of 3:4:3, and the electrolyte is injected to prepare lithium secondary batteries according to Examples 1 and 2 and Comparative Examples 1 to 4.
[0153] Each of the lithium secondary batteries prepared above according to Examples 1 to 2 and Comparative Examples 1 to 4 was charged to 4.25V at a constant current of 0.2C at room temperature and charged at 0.05C. Then, it was discharged at a constant current of 0.2C until it became 2.5V. The charging and discharging behavior was set to 1 cycle, and from the second cycle, charging to 4.25V at a constant current of 0.5C and charging at 0.05C and discharging to 2.5V at a constant current of 0.5C was set to 1 cycle. After repeating such cycles 30 times, the capacity retention rate according to the cycle of the secondary batteries according to Examples 1 to 2 and Comparative Examples 1 to 4 was measured, and the results are shown in Tables 3, 4 and 5 below.
[0154] [Table 3]
[0155] Initial discharge capacity (mAh / g) Capacity retention rate at 30 cycles (%) Example 1 201.7 91.3 Example 2 197.3 92.8 Comparative Example 1 199.8 91.1 Comparative Example 2 196.7 91.0 Comparative Example 3 206.2 88.5 Comparative Example 4 207.7 89.1
[0156] As shown in Table 3, Figure 4 and Figure 5 As shown, in the lithium secondary batteries containing positive electrode active materials of Example 1 and Comparative Example 1, Example 2 and Comparative Example 2 prepared under the same conditions but different in the presence or absence of B doping, it was confirmed that the initial discharge capacity of the secondary batteries prepared in Examples 1 and 2 with B doping was higher than the initial discharge capacity of the secondary batteries prepared in Comparative Examples 1 and 2 without B doping.
[0157] In addition, in the secondary batteries prepared in Comparative Examples 3 to 4, the initial discharge capacity was excellent, but the structural stability was lower than that of the secondary batteries prepared in Examples 1 to 2, so that the capacity retention rate was poor at 30 cycles or more.
[0158] Experimental Example 3: Evaluation of resistance characteristics
[0159] The resistance characteristics of each of the lithium secondary batteries according to Examples 1 to 3 and Comparative Examples 1 and 2 prepared in Experimental Example 2 were evaluated.
[0160] Specifically, each lithium secondary battery of Examples 1 to 3 and Comparative Examples 1 and 2 was charged to 4.25V at a constant current of 0.5C at room temperature and the charge was cut off at 0.05C. Then, it was discharged at a constant current of 0.5C until it became 2.5V. In this case, the voltage corresponding to 60 seconds was recorded, and the resistance was calculated by dividing the difference from the initial voltage by the applied current. The initial resistance of the secondary batteries according to Examples 1 to 3 and Comparative Examples 1 to 2 was measured, and the results are shown in Tables 4 and Figure 6 middle.
[0161] [Table 4]
[0162] Initial DCIR (%) Example 1 25.2 Example 2 33.7 Example 3 39.0 Comparative Example 1 41.6 Comparative Example 2 61.8
[0163] As shown in Table 4 and Figure 6 As shown, it was confirmed that the secondary batteries to which the positive electrode active materials prepared in Examples 1 to 3 were applied were superior to the secondary batteries to which the positive electrode active materials prepared in Comparative Examples 1 to 2 were applied in terms of initial resistance characteristics according to the present invention.
[0164] Experimental Example 4: Continuous Charging Test
[0165] Each of the lithium secondary batteries according to Examples 1 and 2 and Comparative Example 3 prepared in Experimental Example 2 was charged for 120 hours to maintain 4.5 V at 60° C., and the amount of current generated under the conditions was measured and the results are shown in FIG. Figure 7 middle.
[0166] like Figure 7As shown, in Comparative Example 3, it was confirmed that more current was generated during continuous charging than in Examples 1 and 2. In Comparative Example 3, because the stability of the positive electrode active material was worse than in Examples 1 and 2, the amount of current generated due to the side reaction between the surface of the positive electrode active material and the electrolyte was large.
Claims
1. A positive electrode active material, which comprises a lithium transition metal oxide containing nickel (Ni), cobalt (Co) and manganese (Mn). Wherein, relative to the total molar amount of transition metals other than lithium, the lithium transition metal oxide has nickel (Ni) of 60 mol% or more. The lithium transition metal oxide is doped with at least one doping element selected from the following: B, Zr, Mg, Ti, Sr, W and Al. The positive electrode active material has an average particle size D of 4 μm to 10 μm after rolling at a rolling density of 3.0 g / cm 3 to 3.3 g / cm 3 , and the positive electrode active material has a single particle form. 50 , and the microcrystalline size of the lithium transition metal oxide is 170 nm to 200 nm, and wherein the doping element contains B.
2. The positive electrode active material according to claim 1, wherein the lithium transition metal oxide is represented by the following formula 1: [Formula 1] Li 1+a Ni x Co y Mn z M 1 w O2 Wherein in the above formula 1, 0≤a≤0.5, 0.6≤x<1, 0<y≤0.4, 0<z≤0.4 and 0<w≤0.04, M 1 is at least one selected from the following: B, Zr, Mg, Ti, Sr, W and Al.
3. The positive electrode active material according to claim 1, wherein the content of the doping element is 100 ppm to 4000 ppm relative to the total weight of the lithium transition metal oxide.
4. A method for preparing the positive electrode active material according to any one of claims 1 to 3, the method comprising the following steps: Prepare a transition metal hydroxide precursor, wherein relative to the total molar amount of the transition metal hydroxide containing nickel (Ni), cobalt (Co) and manganese (Mn), the transition metal hydroxide precursor contains nickel of 60 mol% or more; Mix the transition metal hydroxide precursor with an aqueous solution of a raw material containing a doping element, the doping element being selected from: B, Zr, Mg, Ti, Sr, W and Al; and The lithium raw material is mixed with the mixture and calcined at a temperature above 810° C. to prepare a lithium transition metal oxide in the form of single particles, The doping element comprises B. 5 . The method according to claim 4 , wherein the doping element raw material comprises at least any one selected from the group consisting of boric acid, boron trioxide, boron carbide, boron trifluoride and boron monofluoride.
6. The method according to claim 4, wherein the calcination is performed at 810°C to 880°C. 7 . A positive electrode for a lithium secondary battery, comprising the positive electrode active material according to claim 1 . 8 . A lithium secondary battery comprising the positive electrode according to claim 7 .