Magnetic sensor with double TMR film and method for manufacturing the same
By using resistors composed of different TMR films in the TMR sensor and using the magnetization direction characteristics of the synthetic antiferromagnetic pinned layer, the problem of low efficiency of the existing TMR Wheatstone bridge is solved, and within the full magnetoresistance range is achieved maximum output voltage or sensitivity.
Patent Information
- Application Number
- CN202080006967.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-18
- Filing Date
- 2020-03-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-03-22
AI Technical Summary
Existing tunneling magnetoresistance (TMR)-based Wheatstone bridges are not efficient in magnetic field sensing, resulting in reduced output voltage or limited sensitivity because the ±45° sensor magnetic strip orientation limits the full range of magnetoresistance changes. use.
Design a TMR sensor device including four or more TMR resistors, wherein each resistor is composed of a different TMR film, the first and fourth resistors are made of the same TMR film, the second and third resistors are Made of different TMR films and differences in resistance response are achieved by synthesizing the magnetization direction of the antiferromagnetic pin layer orthogonal or antiparallel, thereby maximizing the output voltage or sensitivity over the full magnetoresistance range.
By using resistors of different TMR films, the output voltage or sensitivity is maximized within the full magnetoresistance range, and the efficiency and performance of the magnetic sensor are improved.
Smart Images

Figure CN113196076B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. Application No. 16 / 718,346, filed on December 18, 2019, which claims the benefit of U.S. Provisional Patent Application Serial No. 62 / 892,232, filed on August 27, 2019, both of which are incorporated herein by reference in their entirety. Background Art Technical Field
[0004] Embodiments of the present disclosure generally relate to tunneling magnetoresistive sensor devices, such as Wheatstone bridges, and methods of making the same.
[0005] Description of Related Art
[0006] A Wheatstone bridge is a circuit used to measure the resistance of an unknown component by balancing two legs of a bridge circuit, one of which contains the unknown component. The Wheatstone circuit provides extremely accurate measurements compared to a simple voltage divider.
[0007] Wheatstone bridges have recently been used in magnetic sensor applications. Wheatstone bridges include multiple resistors based on the magnetic Hall effect, anisotropic magnetoresistance (AMR) effect, giant magnetoresistance (GMR) effect, and tunneling magnetoresistance (TMR) effect. TMR-based magnetic sensors have very high sensitivity compared to other magnetic sensors.
[0008] A typical TMR-based Wheatstone bridge includes four resistors made of TMR film. In order to enable the Wheatstone bridge characteristics to be used for magnetic field sensing, the first and fourth resistors need to have opposite signs of resistance field dependence to the second and third resistors. One way to achieve this is to manufacture the first and fourth resistors with magnetic stripe orientations at +45° to the designed field sensing direction, and the second and third resistors with magnetic stripe orientations at -45° to the designed field sensing direction. All four resistors are made of the same TMR material or film, and in this way, the pinned layer of each of the four resistors has a similar magnetization direction, which is specified to be perpendicular to the field sensing direction.
[0009] When a magnetic field is applied to the Wheatstone bridge, the resistance of the first resistor and the fourth resistor increases or decreases with the applied magnetic field, while the resistance of the second resistor and the third resistor decreases or increases with the applied magnetic field, thereby achieving a bridge characteristic differential output. However, the efficiency of the Wheatstone bridge formed in this way is not optimal because the full range of magnetic resistance change cannot be utilized in this design due to the ±45° sensor magnetic strip orientation, resulting in a reduced output voltage or limited sensitivity.
[0010] Therefore, there is a need in the art for magnetic sensors and methods of making the same that operate within the full magnetoresistance range while achieving maximum output voltage or sensitivity. Summary of the invention
[0011] A TMR sensor device including four or more TMR resistors is disclosed. The TMR sensor device includes: a first TMR resistor including a first TMR film; a second TMR resistor including a second TMR film different from the first TMR film; a third TMR resistor including the second TMR film; and a fourth TMR resistor including the first TMR film. The first TMR resistor, the second TMR resistor, the third TMR resistor and the fourth TMR resistor are arranged in the same plane. The first TMR film includes a synthetic antiferromagnetic pinned layer, the magnetization direction of the reference layer of the synthetic antiferromagnetic pinned layer is orthogonal to the free layer. The second TMR film includes a dual synthetic antiferromagnetic pinned layer, the magnetization direction of the reference layer of the dual synthetic antiferromagnetic pinned layer is orthogonal to the magnetization of the free layer but opposite to the magnetization direction of the reference layer of the first TMR film.
[0012] In one embodiment, a TMR sensor device includes: a first TMR resistor, the first TMR resistor including a first TMR film, the first TMR film including a synthetic antiferromagnetic pinned layer, the magnetization direction of a first reference layer of the synthetic antiferromagnetic pinned layer being orthogonal to the first free layer; a second TMR resistor, the second TMR resistor including a second TMR film, the second TMR film including a dual synthetic antiferromagnetic pinned layer, the magnetization direction of the second reference layer of the dual synthetic antiferromagnetic pinned layer being orthogonal to the second free layer and opposite to the magnetization direction of the first reference layer of the first TMR film; a third TMR resistor, the third TMR resistor including the second TMR film; and a fourth TMR resistor, the fourth TMR resistor including the first TMR film, wherein the first TMR resistor, the second TMR resistor, the third TMR resistor and the fourth TMR resistor are arranged in the same plane.
[0013] In another embodiment, a method for manufacturing a TMR sensor device includes: forming one or more bottom leads; depositing a first TMR film over at least a first bottom lead and a second bottom lead; removing a first portion of the first TMR film disposed above the second bottom lead; depositing a second TMR film over the first TMR film and the second bottom lead, the second TMR film being different from the first TMR film; and removing a first portion of the second TMR film disposed over the first TMR film.
[0014] In another embodiment, a method for manufacturing a TMR sensor device includes: forming one or more bottom leads; depositing a first TMR film over the one or more bottom leads, the first TMR film including a synthetic antiferromagnetic pinning layer, the magnetization direction of a first reference layer of the synthetic antiferromagnetic pinning layer being orthogonal to the magnetization direction of the first free layer; depositing a first photoresist over a first portion of the first TMR film and at least the first bottom lead; etching a second portion of the first TMR film to expose at least the second bottom lead; removing the first photoresist; depositing a second TMR film over the first TMR film and the second bottom lead, the second TMR film including a dual synthetic antiferromagnetic pinning layer, the magnetization direction of a second reference layer of the dual synthetic antiferromagnetic pinning layer being orthogonal to the magnetization direction of the second free layer and opposite to the magnetization direction of the first reference layer of the first TMR film; depositing a second photoresist over the first portion of the second TMR film and the second bottom lead; etching a second portion of the second TMR film to expose the first TMR film; and removing the second photoresist. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Thus, a detailed understanding of the manner in which the above-described features of the present disclosure are understood, a more particular description of the present disclosure, the above brief overview, may be obtained by reference to the embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the drawings illustrate only typical embodiments of the present disclosure and are therefore not to be considered limiting of its scope, as the present disclosure may admit to other equally effective embodiments.
[0016] Figure 1 Schematic diagram designed for a TMR sensor device or Wheatstone bridge.
[0017] Figure 2 FIG. 5 is a schematic diagram showing a first TMR film and a second TMR film for forming a resistor of a TMR sensor device or a Wheatstone bridge according to one embodiment.
[0018] Figure 3A-3C A first TMR film or TMR film A is shown at various stages of formation according to one embodiment.
[0019] Figure 4A-4C A second TMR film or TMR film B is shown at various stages of formation according to another embodiment.
[0020] Figure 5 A method of forming a TMR sensor device or Wheatstone bridge according to one embodiment is shown.
[0021] Figure 6A-6HA corresponding schematic diagram of depositing a first TMR film to serve as a first resistor and a fourth resistor of a TMR sensor device or a Wheatstone bridge and depositing a second TMR film to serve as a second resistor and a third resistor according to another embodiment is shown.
[0022] Fig. 7A A TMR sensor device or Wheatstone bridge comprising four TMR resistors according to another embodiment is shown.
[0023] Figure 7B Four TMR resistor arrays are shown according to one embodiment.
[0024] To facilitate understanding, identical reference numerals have been used, where possible, to designate identical elements that are common to the figures. It is contemplated that elements disclosed in one embodiment may be beneficially utilized on other embodiments without specific recitation. DETAILED DESCRIPTION
[0025] Hereinafter, reference is made to the embodiments of the present disclosure. However, it should be understood that the present disclosure is not limited to the embodiments specifically described. On the contrary, any combination of the following features and elements (whether or not related to different embodiments) is considered to realize and practice the present disclosure. In addition, although the embodiments of the present disclosure can achieve advantages that are superior to other possible solutions and / or superior to the prior art, whether a specific advantage is achieved by a given embodiment is not a limitation to the present disclosure. Therefore, the following aspects, features, embodiments and advantages are merely illustrative, and are not considered to be elements or limitations of the appended claims, unless explicitly stated in the claims. Similarly, reference to "the present disclosure" should not be interpreted as a summary of any inventive subject matter disclosed herein, and should not be considered to be elements or limitations of the appended claims, unless explicitly stated in the claims.
[0026] A tunnel magnetoresistance (TMR) sensor device including four or more TMR resistors is disclosed. The TMR sensor device includes: a first TMR resistor, the first TMR resistor including a first TMR film; a second TMR resistor, the second TMR resistor including a second TMR film different from the first TMR film; a third TMR resistor, the third TMR resistor including the second TMR film; and a fourth TMR resistor, the fourth TMR resistor including the first TMR film. The first TMR resistor, the second TMR resistor, the third TMR resistor and the fourth TMR resistor are arranged in the same plane. The first TMR film includes a synthetic antiferromagnetic pinned layer, the magnetization direction of the reference layer of the synthetic antiferromagnetic pinned layer is orthogonal to the free layer. The second TMR film includes a dual synthetic antiferromagnetic pinned layer, the magnetization direction of the reference layer of the dual synthetic antiferromagnetic pinned layer is orthogonal to the magnetization direction of the free layer but opposite to the magnetization direction of the reference layer of the first TMR film.
[0027] Figure 1 A schematic diagram such as a Wheatstone bridge is designed for the TMR sensor device 100. The TMR sensor device 100 includes a bias source 102, a first resistor 104, a second resistor 106, a third resistor 108, a fourth resistor 110, a first output pad 112, a second output pad 114, and a ground connection 116. The resistors 104, 106, 108, 110 are formed by patterning a TMR film. The resistors 104, 106, 108, 110 are formed by magnetic sensors. A bias voltage is applied to the TMR sensor device 100 or bridge from the bias source 102 to the ground connection 116. The bridge output is the potential difference across the first output pad 112 and the second output pad 114. Due to the nature of the differential output, any changes in resistance due to temperature changes of the resistors 104, 106, 108, 110 are invalid.
[0028] As discussed herein, each of resistors 104, 106, 108, 110 is made of a TMR film. In one embodiment, each of the TMR resistors is unique and different, such that resistors 104, 106, 108, 110 have different resistances. In another embodiment, the TMR films are the same, but resistors 104, 106, 108, 110 are different. In another embodiment, resistors 104, 110 are the same as each other (the TMR films forming resistors 104, 110 are also the same), and resistors 106, 108 are the same as each other (the TMR films forming resistors 106, 108 are also the same), but are different from resistors 104, 110.
[0029] Figure 2FIG. 1 is a schematic diagram showing a first TMR film 220 or film A and a second TMR film 230 or film B for forming TMR resistors 202, 204, 206, 208 of a TMR sensor device 200 (such as a TMR-based magnetic sensor or a Wheatstone bridge) according to one embodiment. The TMR sensor device 200 may be Figure 1 The TMR sensor device 100.
[0030] like Figure 2 As shown, both the first resistor R1 202 and the fourth resistor R4 208 include the first TMR film 220, while both the second resistor R2 204 and the third resistor R3 206 include the second TMR film 230. The TMR resistance of the first resistor R1 202 and the fourth resistor R4 208 formed by the first TMR film 220 increases with the external magnetic field, while the TMR resistance of the second resistor R2 204 and the third resistor R3 206 formed by the second TMR film 230 decreases with the external magnetic field. Alternatively, the TMR resistance of the first resistor R1 202 and the fourth resistor R4 208 formed by the first TMR film 220 may decrease with the external magnetic field, while the TMR resistance of the second resistor R2 204 and the third resistor R3 206 formed by the second TMR film 230 may increase with the external magnetic field. In this way, the two different TMR films 220, 230 provide two different magnetoresistive responses.
[0031] Figure 3A-3C According to one embodiment, Figure 2 2. The first TMR film 220 or film A is in various stages of formation. Figure 3A shows the first TMR film 220 during magnetic annealing, Figure 3B shows the first TMR film 220 after magnetic annealing, and Figure 3C The first TMR film 220 is shown after the FL magnetization direction has been reset when the TMR sensor device or Wheatstone bridge is completed. The first TMR film 220 can be used as a magnetic sensor.
[0032] exist Figure 3A-3C In the embodiment, the first TMR film 220 includes a free layer 302, a barrier layer 304 disposed below the free layer 302, a reference layer (RL) 306 disposed below the barrier layer 304, a spacer layer 308 disposed below the RL 306, a pinned layer (PL) 310 disposed below the spacer layer 308, and an antiferromagnetic (AFM) layer 312 disposed below the PL 310.
[0033] FL 302 may include a CoFe / CoFeB / Ta / NiFe multilayer stack. Suitable materials for free layer 302 include CoFe / CoFeB / Ta / NiFe multilayer stacks. The CoFe layer may have a thickness between about 3 angstroms and about 10 angstroms. The CoFeB layer may have a thickness between about 10 angstroms and about 20 angstroms. The Ta layer may have a thickness between about 0.5 angstroms and about 2 angstroms. The NiFe layer may have a thickness between about 3 angstroms and about 300 angstroms, such as between about 3 angstroms and about 10 angstroms or between about 10 angstroms and about 300 angstroms. The free layer 302 may be formed by a well-known deposition method such as sputtering. In addition, it should be understood that although CoFe / CoFeB / Ta / NiFe has been exemplified as a free layer 302 material, other materials are also contemplated, and the embodiments discussed herein are not limited to CoFe / CoFeB / Ta / NiFe for free layer 302.
[0034] Barrier layer 304 may include MgO and may have a thickness between about 10 angstroms to about 20 angstroms. It should be understood that while MgO is illustrated as barrier layer 304, other insulating materials are also contemplated. Spacer layer 308 includes a non-magnetic material, such as Ru. Spacer layer 308 may have a thickness between about 4 angstroms to about 10 angstroms. Spacer layer 308 may be formed by well-known deposition methods such as sputtering. In addition, it should be understood that while ruthenium has been illustrated as a spacer layer 308 material, other materials are also contemplated, and the embodiments discussed herein are not limited to ruthenium for spacer layer 308.
[0035] Suitable materials for reference layer 306 and pinning layer 310 include CoFe or Co / CoFe / Co multilayer stacks having a thickness between about 20 angstroms and about 30 angstroms. Reference layer 306 and pinning layer 310 may be formed by well-known deposition methods such as sputtering. Reference layer 306 and pinning layer 310 may each include CoFe / Ta / CoFeB / CoFe multilayers. Additionally, it should be understood that while CoFe or Co / CoFe / Co has been exemplified as reference layer 306 and pinning layer 310 materials, other materials are contemplated and the embodiments discussed herein are not limited to CoFe or Co / CoFe / Co for reference layer 306 and pinning layer 310.
[0036] Suitable materials for the AFM layer 312 include IrMn, PtMn, PdMn, or NiMn having a thickness between about 40 angstroms and about 500 angstroms. The AFM layer 312 can be formed by a well-known deposition method such as sputtering. In addition, it should be understood that although IrMn, PtMn, PdMn, or NiMn has been exemplified as the AFM layer 312 material, other materials are also contemplated, and the embodiments discussed herein are not limited to IrMn, PtMn, PdMn, or NiMn for the AFM layer 312.
[0037] exist Figure 3A , during magnetic annealing under a magnetic field applied along the x-direction, FL 302 has a first magnetization direction 320 pointing along the x-direction, RL 306 has a first magnetization direction 322 pointing along the x-direction, and PL 310 has a first magnetization direction 324 pointing along the x-direction.
[0038] exist Figure 3B , the FL 302 has a first magnetization direction 320 pointing in the x-direction, the RL 306 has a second magnetization direction 332 pointing in the −x-direction due to the Ruderman-Kittel-Kasuya-Yosida (RKKY) interlayer exchange coupling effect, and the PL 310 disposed adjacent to the AFM layer 312 has a first magnetization direction 324 pointing in the x-direction. Therefore, after magnetic annealing, the FL 302 and the PL 310 have parallel magnetization directions 320, 324, and the RL 306 has an antiparallel magnetization direction 332.
[0039] exist Figure 3C , FL 302 has a second magnetization direction 330 pointing in the -z direction (i.e., into the page), RL 306 has a second magnetization direction 332 pointing in the -x direction, and PL 310 has a first magnetization direction 324 pointing in the x direction. Thus, after the FL magnetization direction has been reset when the TMR sensor device or Wheatstone bridge is fabricated, FL 302 has a magnetization direction 330 that is orthogonal to the magnetization directions of RL 306 and PL 310, while RL 306 has a magnetization direction 332 that is antiparallel to the magnetization direction 324 of PL 310. The magnetization direction 330 of FL 302 can be reset by applying an additional magnetic field, such as applying a hard bias around FL 302 by a permanent magnet or applying an exchange bias on top of FL 302 by an AFM.
[0040] Figure 3C Shown in Figure 2 The first TMR film 220 used in the TMR sensor device 200. Figure 3CAs further shown in , the RL 306 and the PL 310 form a synthetic antiferromagnetic (SAF) pinned layer 314 .
[0041] Figure 4A-4C According to one embodiment, Figure 2 The second TMR film 230 or film B is in various stages of formation. Figure 4A shows the second TMR film 230 during magnetic annealing, Figure 4B shows the second TMR film 230 after magnetic annealing, and Figure 4C The second TMR film 230 is shown after the FL magnetization direction has been reset when the TMR sensor device or Wheatstone bridge is completed. The second TMR film 230 can be used as a magnetic sensor.
[0042] exist Figure 4A-4C In the embodiment, the second TMR film 230 includes a free layer 402, a blocking layer 404 disposed below the free layer 402, a reference layer (RL) 406 disposed below the blocking layer 404, a first spacer layer 408 disposed below the RL 406, a first pinned layer (PL') 418 disposed below the first spacer layer 408, a second spacer layer 422 disposed below the first PL' 418, a second pinned layer (PL") 410 disposed below the second spacer layer 422, and an AFM layer 412 disposed below the second PL" 410.
[0043] FL 402 may include a CoFe / CoFeB / Ta / NiFe multilayer stack. Suitable materials for free layer 402 include CoFe / CoFeB / Ta / NiFe multilayer stacks. The CoFe layer may have a thickness between about 3 angstroms and about 10 angstroms. The CoFeB layer may have a thickness between about 10 angstroms and about 20 angstroms. The Ta layer may have a thickness between about 0.5 angstroms and about 2 angstroms. The NiFe layer may have a thickness between about 3 angstroms and about 300 angstroms, such as between about 3 angstroms and about 10 angstroms or between about 10 angstroms and about 300 angstroms. The free layer 402 may be formed by a well-known deposition method such as sputtering. In addition, it should be understood that although CoFe / CoFeB / Ta / NiFe has been exemplified as a free layer 402 material, other materials are also contemplated, and the embodiments discussed herein are not limited to CoFe / CoFeB / Ta / NiFe for free layer 402.
[0044] The barrier layer 404 may include MgO and may have a thickness between about 10 angstroms to about 20 angstroms. It should be understood that although MgO is exemplified as the barrier layer 404, other insulating materials are also contemplated. The first spacer layer 408 and the second spacer layer 422 may each include a non-magnetic material, such as Ru. The first spacer layer 408 and the second spacer layer 422 may each have a thickness between about 4 angstroms to about 10 angstroms. The first spacer layer 408 and the second spacer layer 422 may be formed by a well-known deposition method (such as sputtering). In addition, it should be understood that although ruthenium has been exemplified as the first spacer layer 408 and the second spacer layer 422 material, other materials are also contemplated, and the embodiments discussed herein are not limited to ruthenium for the first spacer layer 408 and the second spacer layer 422.
[0045] Suitable materials for the reference layer 406 and the first pinned layer 410 and the second pinned layer 418 include CoFe or a Co / CoFe / Co multilayer stack having a thickness between about 20 angstroms and about 30 angstroms. The reference layer 406 and the first pinned layer 410 and the second pinned layer 418 can be formed by well-known deposition methods (such as sputtering). The reference layer 406 may include a CoFe / Ta / CoFeB / CoFe multilayer. In addition, it should be understood that although CoFe or Co / CoFe / Co has been exemplified as the reference layer 406 and the first pinned layer 410 and the second pinned layer 418 materials, other materials are also contemplated, and the embodiments discussed herein are not limited to CoFe or Co / CoFe / Co for the reference layer 406 and the first pinned layer 410 and the second pinned layer 418.
[0046] Suitable materials for the AFM layer 412 include IrMn, PtMn, PdMn, or NiMn having a thickness between about 40 angstroms and about 500 angstroms. The AFM layer 412 can be formed by a well-known deposition method such as sputtering. In addition, it should be understood that although IrMn, PtMn, PdMn, or NiMn has been exemplified as the AFM layer 412 material, other materials are also contemplated, and the embodiments discussed herein are not limited to IrMn, PtMn, PdMn, or NiMn for the AFM layer 412.
[0047] exist Figure 4A , during magnetic annealing under a magnetic field applied along the x-direction, the FL 402 has a first magnetization direction 420 pointing along the x-direction, the RL 406 has a first magnetization direction 416 pointing along the x-direction, the second PL″ 410 has a first magnetization direction 424 pointing along the x-direction, and the first PL′ 418 has a first magnetization direction 426 pointing along the x-direction. Therefore, the magnetization directions of the FL 402, the RL 406, the second PL″ 410, and the first PL′ 418 of the second TMR film 230 are parallel to each other.
[0048] exist Figure 4B , FL 402 has a first magnetization direction 420 pointing along the x-direction, RL 406 has a first magnetization direction 416 pointing along the x-direction, the second PL″ 410 has a first magnetization direction 424 pointing along the x-direction, and the first PL′ 418 has a second magnetization direction 436 pointing along the −x-direction due to the RKKY interlayer exchange coupling effect. The second PL″ 410 disposed adjacent to the AFM 412 has a magnetization direction 424 parallel to the annealing magnetic field due to the setting of the AFM exchange bias or unidirectional anisotropy direction. Therefore, after magnetic annealing, the FL 402, the RL 406, and the second PL″ 410 have parallel magnetization directions 420, 422, 424, and the first PL′ 418 has an antiparallel magnetization direction 436.
[0049] exist Figure 4C , FL 402 has a second magnetization direction 430 pointing in the −z direction (i.e., into the page), RL 406 has a first magnetization direction 416 pointing in the x direction, second PL″ 410 has a first magnetization direction 424 pointing in the x direction, and first PL′ 418 has a second magnetization 436 pointing in the −x direction. Thus, after the FL magnetization directions have been reset when the TMR sensor device or Wheatstone bridge is fabricated, FL 402 has a magnetization direction 430 that is orthogonal to the magnetization directions of RL 406 and second PL″ 410, while first PL′ 418 has a magnetization direction 436 that is antiparallel to the magnetization directions of RL 406 and second PL″ 410. The magnetization direction 430 of FL 402 can be reset by applying an additional magnetic field, such as applying a hard bias around FL 402 by a permanent magnet or applying an exchange bias on top of FL 402 by an AFM.
[0050] Figure 4C Shown in Figure 2 The second TMR film 230 used in the TMR sensor device 200. Figure 4C As further shown, the RL 406, the second PL″ 410, and the first PL′ 418 form a dual SAF pinned layer 414. Because the first TMR film 220 and the second TMR film 230 have different RL magnetization directions, the TMR resistance response of each film is the same in magnitude but opposite in direction (i.e., the resistance of one film increases with increasing magnetic field while the resistance of the other film decreases, or vice versa). In this way, the TMR sensor device or Wheatstone bridge characteristic differential output is achieved and satisfied with maximum efficiency because the full range of the magnetoresistance range is available, thereby achieving maximum output voltage or sensitivity.
[0051] Figure 5A method 500 of forming a TMR sensor device, such as a TMR magnetic sensor or a Wheatstone bridge, by depositing a first film to serve as a first resistor and a fourth resistor and depositing a second film to serve as a second resistor and a third resistor according to embodiments disclosed herein is shown. Figure 6A-6H A corresponding schematic diagram showing a first TMR film 610 deposited to serve as first and fourth resistors of a TMR sensor device 600 (such as a TMR magnetic sensor or a Wheatstone bridge) and a second TMR film 618 deposited to serve as second and third resistors. Figure 5 Reference Figure 6A-6H Give a description.
[0052] In operation 502, one or more bottom leads 604 (a first bottom lead 604a and a second bottom lead 604b are shown) and a dielectric layer 606 are formed over a substrate 602, and a chemical-mechanical planarization (CMP) stop layer 608 is deposited on the dielectric layer 606. The one or more bottom leads 604 may undergo a CMP process to reduce the surface roughness of the bottom leads 604.
[0053] In one embodiment, four bottom leads 604 are formed. In such an embodiment, a third bottom lead (not shown) may be disposed behind the first bottom lead 604a in the z-direction, and a fourth bottom lead (not shown) may be disposed behind the second bottom lead 604b in the z-direction. Although only the first bottom lead 604a and the second bottom lead 604b are shown, one or more bottom leads 604 may be included.
[0054] In operation 504, a first TMR film 610 or TMR film A is deposited on both the first bottom lead 604a and the second bottom lead 604b, as in Fig. 6A The first TMR film 610 includes a plurality of layers. In some embodiments, the first TMR film 610 is Figure 2 and Figure 3C The first TMR film 220. The first TMR film 610 includes a synthetic antiferromagnetic pinning layer.
[0055] In operation 506, a first photoresist 616 is deposited on the first portion 612 of the first TMR film 610, such as Figure 6B As shown. The length and width of the first photoresist 616 along the x-direction and the z-direction are selected to define the length and width of the first resistor and the fourth resistor (described below) along the x-direction and the z-direction. The first portion 612 is disposed above the first bottom lead 604a. The second portion 614 of the first TMR film 610 is disposed above the second bottom lead 604b. The first photoresist 616 has a greater width than the first bottom lead 604a.
[0056] In operation 508, the first TMR film 610 disposed in the second portion 614 is milled away under accurate control so that no first TMR film 610 remains disposed over the second bottom lead 604b and the second bottom lead 604b is not removed, as shown in FIG. Figure 6C The first TMR film 610 disposed in the first portion 612 is protected by a first photoresist 616. In operation 510, the first photoresist 616 is stripped and removed. Fig.6D As shown. Therefore, the second bottom lead 604b is exposed in the second portion 614, and the first TMR film 610 is exposed in the first portion 612. The remaining first TMR film 610 has the same length and width in the x-direction and the z-direction as the first photoresist 616. The remaining first TMR film 610a forms the first resistor and the fourth resistor.
[0057] In operation 512, a second TMR film 618 or TMR film B is deposited on the first TMR film 610 and the second bottom lead 604b. Fig. 6E The second TMR film 618 is shown as a single layer in FIG. 610 without involving a photoresist or mask to protect the remaining first TMR film 610. The second TMR film 618 includes multiple layers. In some embodiments, the second TMR film 618 is Figure 2 and Figure 4C The second TMR film 230. The second TMR film 618 includes a double synthetic antiferromagnetic pinning layer.
[0058] In operation 514, a second photoresist 624 is deposited on the third portion 620 of the second TMR film 618, as shown in FIG. Fig. 6F As shown. The length and width of the second photoresist 624 along the x-direction and the z-direction are selected to define the length and width of the second resistor and the third resistor (described below) along the x-direction and the z-direction. The second photoresist 624 has the same length and width as the first photoresist 616 along the x-direction and the z-direction. The third portion 620 is disposed above the second bottom lead 604b. The fourth portion 622 of the second TMR film 618 is disposed above the first bottom lead 604a and the first TMR film 610. The second photoresist 624 has a larger width along the x-direction than the second bottom lead 604b.
[0059] The third portion 620 may overlap the second portion 614, and the third portion 620 may have a smaller length along the x-direction than the second portion 614, such as Fig. 6F The fourth portion 622 may overlap the first portion 612, and the fourth portion 622 may have a greater length along the x direction than the first portion 612, as shown in FIG. Fig. 6F shown.
[0060] In operation 516, the second TMR film 618 disposed in the fourth portion 622 is milled away under accurate control so that no second TMR film 618 remains disposed over the first bottom lead 604a and the first TMR film 610 is not removed, as shown in FIG. Figure 6G The second TMR film 618 disposed in the third portion 620 is protected by a second photoresist 624. In operation 518, the second photoresist 624 is stripped and removed. Figure 6H The remaining second TMR film 618 has the same length and width along the x-direction and the z-direction as the second photoresist 624. The remaining second TMR film 618 forms a second resistor and a third resistor.
[0061] Because the third portion 620 may have the same length and width as the first portion 612, or because the second photoresist 624 may have the same length and width as the first photoresist 616, the remaining first TMR film 610 may have the same length and width along the x-direction and the y-direction as the second TMR film 618. The first TMR film 610 and the second TMR film 618 may have the same length, width, and height along the x-direction, the y-direction, and the z-direction. Therefore, the sizes of the first TMR film 610 and the second TMR film 618 may be equal.
[0062] After removing the second photoresist 624, the first TMR film 610 is exposed in the first portion 612 above the first bottom lead 604a, and the second TMR film 618 is exposed in the third portion 620 above the second bottom lead 604b, as shown in FIG. Figure 6H As shown. The first TMR film 610 is aligned with or disposed in the same plane as the second TMR film 618. The first TMR film 610 is spaced apart from the second TMR film 618. In one embodiment, the second TMR film 618 is deposited in operation 504 to form the first resistor and the fourth resistor, and the first TMR film 610 is deposited in operation 512 to form the second resistor and the third resistor.
[0063] In operation 520, the first TMR film 610 and the second TMR film 618 are annealed under a magnetic field. In a magnetic oven, the first TMR film 610 and the second TMR film 618 are annealed at a temperature between about 250 degrees Celsius and about 300 degrees Celsius and a magnetic field between about 1 Tesla and about 5 Tesla.
[0064] In operation 522, the TMR sensor device 600 (i.e., a Wheatstone bridge or a TMR magnetic sensor) is manufactured. The manufacture of the TMR sensor device 600 may include patterning four resistors having a specified geometry or shape. Top leads (not shown) are then formed over the first and fourth resistors formed by the first TMR film 610 and the second and third resistors formed by the second TMR film 618, respectively. Each of the four resistors includes a separate bottom lead and a top lead.
[0065] In operation 524, the magnetization direction of the FL of the first TMR film 610 is reset to a direction perpendicular to the magnetization direction of the RL of the first TMR film 610, and the magnetization direction of the FL of the second TMR film 618 is reset to a direction perpendicular to the magnetization direction of the RL of the second TMR film 618, as described above. Figure 3C and Figure 4C As described in.
[0066] The first TMR resistor may be Figure 1 The first resistor 104 or Figure 2 The first resistor 202 of . The second TMR resistor may be Figure 1 The second resistor 106 or Figure 2 The third TMR resistor may be Figure 1 The third resistor 108 or Figure 2 The fourth TMR resistor may be Figure 1 The fourth resistor 110 or Figure 2 The fourth resistor 208 is provided.
[0067] Fig. 7A A TMR sensor device 700 including four TMR resistors 702 , 704 , 706 , 708 , such as a Wheatstone bridge, is shown according to another embodiment. Figure 7B A TMR sensor device 750 including four TMR resistor arrays 752 , 754 , 756 , 758 , such as a Wheatstone bridge, is shown according to one embodiment. The TMR sensor devices 700 , 750 may be formed using the method 500 .
[0068] In the TMR sensor device 700, the first resistor 702 and the fourth resistor 708 include the first TMR film 220, and the second resistor 704 and the third resistor 706 include the second TMR film 230. The first TMR resistor 702 may be Figure 1 The first resistor 104 or Figure 2 The second TMR resistor 704 may be Figure 1 The second resistor 106 or Figure 2The third TMR resistor 706 may be Figure 1 The third resistor 108 or Figure 2 The fourth TMR resistor 708 may be Figure 1 The fourth resistor 110 or Figure 2 The fourth resistor 208 is provided.
[0069] The TMR sensor device 750 includes a first resistor array 752, a second resistor array 754, a third resistor array 756, and a fourth resistor array 758. Each of the resistor arrays 752, 754, 756, 758 includes a plurality of resistors coupled in series. To form the TMR sensor device 750, the method further includes: patterning four resistor arrays 752, 754, 756, 758 having resistors of a specified geometry, shape, and number connected in series; forming a top lead on two resistor arrays having resistors made of a first TMR film connected in series to form the first resistor array 752 and the fourth resistor array 758; and forming a top lead on two resistor arrays having resistors made of a second TMR film connected in series to form the second resistor array 754 and the third resistor array 756. Therefore, each of the resistors of the first resistor array 752 and the fourth resistor array 758 is composed of the first TMR film, and each of the resistors of the second resistor array 754 and the third resistor array 756 is composed of the second TMR film.
[0070] The number of resistors in each of the four resistor arrays 752, 754, 756, 758 can be selected to have an odd number of columns and an even number of rows so that the top leads are in direct contact with the end resistors of the arrays 752, 754, 756, 758 to avoid forming vias for the top lead contacts. The first resistor array 752, the second resistor array 754, the third resistor array 756, and the fourth resistor array 758 are arranged in the same plane. The first resistor array 752 is adjacent to the second resistor array 754 and the third resistor array 756, the second resistor array 754 is adjacent to the first resistor array 752 and the fourth resistor array 758, the third resistor array 756 is adjacent to the first resistor array 752 and the fourth resistor array 758, and the fourth resistor array 758 is adjacent to the second resistor array 754 and the third resistor array 756.
[0071] Therefore, utilizing the above-described TMR sensor device or Wheatstone bridge design with four resistors composed of two different TMR films results in the magnetic sensor operating at maximum efficiency and over the full range of magnetoresistance, thereby achieving maximum output voltage. By using the first TMR film for the first resistor and the fourth resistor and using the second TMR film for the second resistor and the third resistor, the TMR sensor device or Wheatstone bridge characteristic differential output is achieved and satisfied with maximum sensitivity.
[0072] In one embodiment, the TMR sensor is used in a camera that operates as a single-axis sensor. Examples of such sensors are found in U.S. Patent Application Publication: 2019 / 0020822 A1, which is incorporated herein by reference. However, it is expected that the TMR sensor can be used as a two-dimensional or even three-dimensional sensor. In addition, it is expected that the TMR sensor can be integrated and used in inertial measurement unit technologies other than cameras, such as wearable devices, compasses, and MEMS devices. In addition, the TMR sensor can be operated as a position sensor, a bridge angle sensor, a magnetic switch, a current sensor, or a combination thereof. The TMR sensor can be used to focus a camera, such as a smartphone camera, by using the TMR sensor as a position and angle sensor. In addition, the TMR sensor can also be used as a switch, current and angle sensor in the automotive industry to replace the current Hall, anisotropic magnetoresistance (AMR) and giant magnetoresistance (GMR) sensors. TMR sensors can also be used as position and angle sensors in drones and robotics industries. Medical devices can also use TMR sensors to control the flow of infusion systems, and endoscope camera sensors can also be used. Thus, the TMR sensors discussed herein have applications far beyond smartphone cameras, and therefore should not be limited to use as sensors for smartphone cameras. Furthermore, the TMR sensors need not be arranged in a Wheatstone bridge arrangement, but can be arranged in any number of ways.
[0073] In one embodiment, a TMR sensor device includes: a first TMR resistor, the first TMR resistor including a first TMR film, the first TMR film including a synthetic antiferromagnetic pinned layer, the magnetization direction of a first reference layer of the synthetic antiferromagnetic pinned layer being orthogonal to the first free layer; a second TMR resistor, the second TMR resistor including a second TMR film, the second TMR film including a dual synthetic antiferromagnetic pinned layer, the magnetization direction of the second reference layer of the dual synthetic antiferromagnetic pinned layer being orthogonal to the second free layer and opposite to the magnetization direction of the first reference layer of the first TMR resistor; a third TMR resistor, the third TMR resistor including the second TMR film; and a fourth TMR resistor, the fourth TMR resistor including the first TMR film, wherein the first TMR resistor, the second TMR resistor, the third TMR resistor and the fourth TMR resistor are arranged in the same plane.
[0074] The first TMR resistor is adjacent to the second TMR resistor and the third TMR resistor, the second TMR resistor is adjacent to the first TMR resistor and the fourth TMR resistor, the third TMR resistor is adjacent to the first TMR resistor and the fourth TMR resistor, and the fourth TMR resistor is adjacent to the second TMR resistor and the third TMR resistor. The magnetization direction of the first reference layer of the first TMR film is antiparallel to the magnetization direction of the first pinned layer of the first TMR film. The first TMR film also includes a first barrier layer, a first spacer layer and a first antiferromagnetic layer, and wherein the first barrier layer is disposed between the first reference layer and the first free layer, the first spacer layer is disposed between the first reference layer and the first pinned layer, and the first antiferromagnetic layer is disposed adjacent to the first pinned layer.
[0075] The second TMR film includes a second reference layer, a second pinned layer, and a third pinned layer disposed between the second reference layer and the second pinned layer, the magnetization direction of the second reference layer being parallel to the magnetization direction of the second pinned layer and antiparallel to the magnetization direction of the third pinned layer. The second TMR film also includes a second barrier layer, a second spacer layer, a third spacer layer, and a second antiferromagnetic layer, and wherein the second barrier layer is disposed between the second reference layer and the second free layer, the second spacer layer is disposed between the second reference layer and the third pinned layer, the third spacer layer is disposed between the third pinned layer and the second pinned layer, and the second antiferromagnetic layer is disposed adjacent to the second pinned layer. The first reference layer of the first TMR film includes a Co / CoFe / Co multilayer stack having a thickness between about 20 angstroms and about 30 angstroms, and wherein the second reference layer of the second TMR film includes a Co / CoFe / Co multilayer stack having a thickness between about 20 angstroms and about 30 angstroms.
[0076] In another embodiment, a method for manufacturing a TMR sensor device includes: forming one or more bottom leads; depositing a first TMR film over at least a first bottom lead and a second bottom lead; removing a first portion of the first TMR film disposed above the second bottom lead; depositing a second TMR film over the first TMR film and the second bottom lead, the second TMR film being different from the first TMR film; removing a first portion of the second TMR film disposed over the first TMR film; and annealing the first TMR film and the second TMR film under a magnetic field.
[0077] The method also includes: patterning a first resistor, a second resistor, a third resistor, and a fourth resistor having a specified geometric structure or shape; and forming a first top lead on the first resistor and the fourth resistor including the first TMR film, and forming a second top lead on the second resistor and the fourth resistor including the second TMR film. The first resistor is adjacent to the second resistor and the third resistor, the second resistor is adjacent to the first resistor and the fourth resistor, the third resistor is adjacent to the first resistor and the fourth resistor, and the fourth resistor is adjacent to the second resistor and the third resistor. The first TMR film includes a synthetic antiferromagnetic pinning layer, the magnetization direction of the first reference layer of the synthetic antiferromagnetic pinning layer is orthogonal to the magnetization direction of the first free layer. The second TMR film includes a dual synthetic antiferromagnetic pinning layer, the magnetization direction of the dual synthetic antiferromagnetic pinning layer is orthogonal to the magnetization direction of the second free layer and opposite to the magnetization direction of the first reference layer of the first TMR film.
[0078] The magnetization direction of the first reference layer of the first TMR film is antiparallel to the magnetization direction of the first pinned layer of the first TMR film, and the second TMR film includes a second reference layer, a second pinned layer and a third pinned layer arranged between the second reference layer and the second pinned layer, and the magnetization direction of the second reference layer is parallel to the magnetization direction of the second pinned layer and antiparallel to the magnetization direction of the third pinned layer.
[0079] In another embodiment, a method for manufacturing a TMR sensor device includes: forming one or more bottom leads; depositing a first TMR film over the one or more bottom leads, the first TMR film including a synthetic antiferromagnetic pinning layer, the magnetization direction of a first reference layer of the synthetic antiferromagnetic pinning layer being orthogonal to the magnetization direction of a first free layer; depositing a first photoresist over a first portion of the first TMR film and at least the first bottom lead; etching a second portion of the first TMR film to expose at least a second bottom lead; removing the first photoresist; depositing a second TMR film over the first TMR film and the second bottom lead, the second TMR film including a dual synthetic antiferromagnetic pinning layer, the magnetization direction of a second reference layer of the dual synthetic antiferromagnetic pinning layer being orthogonal to the magnetization direction of the second free layer; depositing a second photoresist over the first portion of the second TMR film and the second bottom lead; etching a second portion of the second TMR film to expose the first TMR film; and removing the second photoresist.
[0080] The method also includes: patterning a first resistor, a second resistor, a third resistor, and a fourth resistor having a specified geometric structure or shape; and forming a first top lead on the first resistor and the fourth resistor including the first TMR film, and forming a second top lead on the second resistor and the fourth resistor including the second TMR film. The first resistor and the fourth resistor are composed of the first TMR film, and the second resistor and the third resistor are composed of the second TMR film. Each of the first resistor, the second resistor, the third resistor, and the fourth resistor is a TMR resistor or a TMR resistor array. The first resistor, the second resistor, the third resistor, and the fourth resistor are arranged in the same plane. The first resistor is adjacent to the second resistor and the third resistor, the second resistor is adjacent to the first resistor and the fourth resistor, the third resistor is adjacent to the first resistor and the fourth resistor, and the fourth resistor is adjacent to the second resistor and the third resistor. The first portion of the first TMR film and the first portion of the second TMR film are equal in size.
[0081] While the foregoing is directed to embodiments of the present disclosure, other and further embodiments of the present disclosure may be envisaged without departing from the basic scope of the present disclosure, and the scope of the present disclosure is determined by the appended claims.
Claims
1. A tunneling magnetoresistive (TMR) sensor device, the TMR sensor device comprising: a first tunneling magnetoresistive (TMR) resistor, the first TMR resistor comprising a first TMR film, the first TMR film comprising a synthetic antiferromagnetic pinned layer, a first reference layer, and a first free layer, wherein a magnetization direction of the first reference layer is orthogonal to a magnetization direction of the first free layer, wherein the first TMR film of the first TMR resistor is disposed on a first bottom lead; a second TMR resistor, the second TMR resistor comprising a second TMR film, the second TMR film comprising a dual synthetic antiferromagnetic pinned layer, a second reference layer, and a second free layer, wherein a magnetization direction of the second reference layer is orthogonal to a magnetization direction of the second free layer and antiparallel to the magnetization direction of the first reference layer of the first TMR film, wherein the second TMR film of the second TMR resistor is disposed on a second bottom lead, the second bottom lead being spaced apart from the first bottom lead by a dielectric layer; a third TMR resistor, the third TMR resistor comprising the second TMR film; and A fourth TMR resistor includes the first TMR film, wherein the first TMR resistor, the second TMR resistor, the third TMR resistor, and the fourth TMR resistor are disposed in the same plane.
2. The TMR sensor device according to claim 1, wherein: The first TMR resistor is adjacent to the second TMR resistor and the third TMR resistor, the second TMR resistor is adjacent to the first TMR resistor and the fourth TMR resistor, the third TMR resistor is adjacent to the first TMR resistor and the fourth TMR resistor, and the fourth TMR resistor is adjacent to the second TMR resistor and the third TMR resistor.
3. The TMR sensor device according to claim 1, wherein: A magnetization direction of the first reference layer of the first TMR film is antiparallel to a magnetization direction of the first pinned layer of the first TMR film.
4. The TMR sensor device according to claim 3, wherein: The first TMR film also includes a first barrier layer, a first spacer layer and a first antiferromagnetic layer, and wherein the first barrier layer is arranged between the first reference layer and the first free layer, the first spacer layer is arranged between the first reference layer and the first pinned layer, and the first antiferromagnetic layer is arranged to be adjacent to the first pinned layer.
5. The TMR sensor device according to claim 1, wherein: The second TMR film includes the second reference layer, a second pinned layer, and a third pinned layer disposed between the second reference layer and the second pinned layer, wherein a magnetization direction of the second reference layer is parallel to a magnetization direction of the second pinned layer and antiparallel to a magnetization direction of the third pinned layer.
6. The TMR sensor device according to claim 5, wherein: The second TMR film also includes a second barrier layer, a second spacer layer, a third spacer layer and a second antiferromagnetic layer, and wherein the second barrier layer is arranged between the second reference layer and the second free layer, the second spacer layer is arranged between the second reference layer and the third pinned layer, the third spacer layer is arranged between the second pinned layer and the third pinned layer, and the second antiferromagnetic layer is arranged to be adjacent to the second pinned layer.
7. The TMR sensor device according to claim 1, wherein: The first reference layer of the first TMR film includes a Co / CoFe / Co multilayer stack having a thickness between 20 and 30 angstroms, and wherein the second reference layer of the second TMR film includes a Co / CoFe / Co multilayer stack having a thickness between 20 and 30 angstroms.
8. A method of manufacturing a TMR sensor device, the method comprising: forming a plurality of bottom leads, wherein each of the plurality of bottom leads is spaced apart from an adjacent bottom lead by a dielectric layer; depositing a first TMR film over at least the first bottom lead, the second bottom lead, and the dielectric layer; removing a first portion of the first TMR film disposed over the second bottom lead so that the first TMR film is disposed on the first bottom lead; depositing a second TMR film over the first TMR film, the second bottom lead, and at least a portion of the dielectric layer, the second TMR film being different from the first TMR film; as well as A first portion of the second TMR film disposed over the first TMR film is removed so that the second TMR film is disposed on the second bottom lead.
9. The method according to claim 8, further comprising: The first resistor, the second resistor, the third resistor, and the fourth resistor are patterned to have a specified geometry.
10. The method according to claim 9, further comprising: forming a first top lead over the first resistor including the first TMR film and the fourth resistor, and forming a second top lead over the second resistor including the second TMR film and the third resistor, The first resistor is adjacent to the second resistor and the third resistor, the second resistor is adjacent to the first resistor and the fourth resistor, the third resistor is adjacent to the first resistor and the fourth resistor, and the fourth resistor is adjacent to the second resistor and the third resistor.
11. The method according to claim 10, wherein: The first TMR film includes a synthetic antiferromagnetic pinned layer, a first reference layer, and a first free layer. The magnetization direction of the first reference layer is orthogonal to the magnetization direction of the first free layer.
12. The method according to claim 10, wherein: The second TMR film includes a dual synthetic antiferromagnetic pinned layer, a second reference layer, and a second free layer. The magnetization direction of the second reference layer is orthogonal to the magnetization direction of the second free layer.
13. The method according to claim 8, wherein: The magnetization direction of the reference layer of the first TMR film is antiparallel to the magnetization direction of the first pinned layer of the first TMR film, and wherein the second TMR film includes a second reference layer, a second pinned layer and a third pinned layer arranged between the second reference layer and the second pinned layer, and the magnetization direction of the second reference layer is parallel to the magnetization direction of the second pinned layer and antiparallel to the magnetization direction of the third pinned layer.
14. A method of manufacturing a TMR sensor device, the method comprising: forming a plurality of bottom leads, wherein each of the plurality of bottom leads is spaced apart from an adjacent bottom lead by a dielectric layer; Depositing a first TMR film on the plurality of bottom leads and the dielectric layer, the first TMR film comprising a synthetic antiferromagnetic pinned layer, a first reference layer and a first free layer, wherein a magnetization direction of the first reference layer is orthogonal to a magnetization direction of the first free layer; depositing a first photoresist over a first portion of the first TMR film and at least a first bottom lead; etching a second portion of the first TMR film to expose at least a second bottom lead so that the first TMR film is disposed on the first bottom lead; removing the first photoresist; depositing a second TMR film on the first TMR film, the second bottom lead and the dielectric layer, the second TMR film comprising a dual synthetic antiferromagnetic pinned layer, a second reference layer and a second free layer, the magnetization direction of the second reference layer being orthogonal to the magnetization direction of the second free layer and opposite to the magnetization direction of the first reference layer of the first TMR film; depositing a second photoresist over the first portion of the second TMR film and the second bottom lead; etching a second portion of the second TMR film to expose the first TMR film so that the second TMR film is disposed on the second bottom lead; as well as The second photoresist is removed.
15. The method according to claim 14, further comprising: The first resistor, the second resistor, the third resistor, and the fourth resistor are patterned to have a specified geometry.
16. The method according to claim 15, further comprising: A first top lead is formed over the first resistor including the first TMR film and the fourth resistor, and a second top lead is formed over the second resistor including the second TMR film and the third resistor.
17. The method according to claim 15, wherein: Each of the first resistor, the second resistor, the third resistor, and the fourth resistor is a TMR resistor or a TMR resistor array.
18. The method according to claim 15, wherein: The first resistor, the second resistor, the third resistor, and the fourth resistor are disposed in the same plane.
19. The method according to claim 15, wherein: The first resistor is adjacent to the second resistor and the third resistor, the second resistor is adjacent to the first resistor and the fourth resistor, the third resistor is adjacent to the first resistor and the fourth resistor, and the fourth resistor is adjacent to the second resistor and the third resistor.
20. The method according to claim 14, wherein: The first portion of the first TMR film and the first portion of the second TMR film are equal in size.