Battery

By using a combination of a thin layer 1 solid electrolyte layer and a thick layer 2 solid electrolyte layer with high organic compound content in an all-solid battery, the challenges of battery reliability and capacity improvement are solved, and efficient electrical short circuit suppression and membrane are achieved Reduced defects improve battery stability and capacity.

CN113196519BActive Publication Date: 2024-11-08PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980081950.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-02-15
Filing Date
2019-11-25
Publication Date
2024-11-08
Estimated Expiration
2039-11-25

AI Technical Summary

Technical Problem

Existing all-solid batteries have challenges in improving reliability and capacity, especially the difficulty in effectively suppressing electrical short circuits and membrane defects.

Method used

The thickness of the first solid electrolyte layer with a high organic compound content is used to combine the second solid electrolyte layer with a thin layer of the first solid electrolyte layer with a thicker organic compound content. The thickness of the first solid electrolyte layer is smaller than that of the second solid electrolyte layer, and is analyzed by energy dispersion type X-rays. The method ensures the characteristics of organic compound content and thickness to form a fully filled and less defective electrolyte layer to improve the reliability and capacity of the battery.

Benefits of technology

A high reliability and high capacity battery is realized, which effectively suppresses electrical short circuits and membrane defects, and improves the stability and capacity quality of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113196519B_ABST
    Figure CN113196519B_ABST
Patent Text Reader

Abstract

A battery (1) comprises: a first electrode (10); a first solid electrolyte layer (11) in contact with the first electrode (10); a second electrode (12); and a second solid electrolyte layer (13) located between the second electrode (12) and the first solid electrolyte layer (11). The content of an organic compound in the first solid electrolyte layer (11) is greater than the content of an organic compound in the second solid electrolyte layer (13), and the thickness of the first solid electrolyte layer (11) is smaller than the thickness of the second solid electrolyte layer (13).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to batteries. Background Art

[0002] Patent Document 1 discloses a method for manufacturing an all-solid-state battery, which includes a negative electrode film forming step, a first solid electrolyte layer film forming step, a positive electrode film forming step, a second solid electrolyte layer film forming step, a lamination step, and a bonding step. In this manufacturing method, the first solid electrolyte layer and the second solid electrolyte layer are formed using a slurry composition containing a binder.

[0003] Patent document 2 discloses a method for manufacturing an all-solid-state battery, which includes a step of joining a first stack and a second stack in a manner that a first solid electrolyte and a second solid electrolyte layer overlap each other. In this manufacturing method, the first stack is formed by joining a positive electrode layer and a first solid electrolyte layer. The second stack is formed by joining a negative electrode layer and a second solid electrolyte layer. Both the first solid electrolyte layer and the second solid electrolyte layer are formed using a slurry containing a solid electrolyte and a binder.

[0004] Prior Art Literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent No. 6175934

[0007] Patent Document 2: Japanese Patent Application Publication No. 2015-118870 Summary of the invention

[0008] In the prior art, improvements in reliability and capacity of batteries are desired.

[0009] The battery disclosed herein comprises:

[0010] 1st electrode;

[0011] a first solid electrolyte layer in contact with the first electrode;

[0012] a second electrode; and

[0013] a second solid electrolyte layer located between the second electrode and the first solid electrolyte layer,

[0014] The content of the organic compound in the first solid electrolyte layer is greater than the content of the organic compound in the second solid electrolyte layer, and

[0015] The thickness of the first solid electrolyte layer is smaller than the thickness of the second solid electrolyte layer.

[0016] According to the present disclosure, a battery having high reliability and high capacity can be realized. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic cross-sectional view showing an example of a battery according to an embodiment of the present disclosure.

[0018] Figure 2 It means there are multiple layers. Figure 1 The battery 1 shown is a schematic cross-sectional view of a first example of a stacked-type all-solid-state battery.

[0019] Figure 3 It means there are multiple layers. Figure 1 The battery 1 shown is a schematic cross-sectional view of a second example of a laminated all-solid-state battery.

[0020] Figure 4 It means there are multiple layers. Figure 1 The battery 1 shown is a schematic cross-sectional view of a third example of a stacked-type all-solid-state battery.

[0021] Figure 5 It means there are multiple layers. Figure 1 The battery 1 shown is a schematic cross-sectional view of a fourth example of a stacked-type all-solid-state battery. DETAILED DESCRIPTION

[0022] The following is a description of a battery representing one embodiment of the present disclosure using the accompanying drawings. In addition, the battery in the present disclosure is not limited to the following embodiment. The same or similar components are sometimes denoted by the same reference numerals and their description is omitted.

[0023] Figure 1 It is a schematic cross-sectional view showing an example of a battery according to an embodiment of the present disclosure. Figure 1 The battery 1 shown is a unit cell as a basic unit structure of a stacked all-solid battery 2 described later. The battery 1 includes a first electrode 10, a first solid electrolyte layer 11, a second electrode 12, and a second solid electrolyte layer 13. The first solid electrolyte layer 11 is in contact with the first electrode 10. The second solid electrolyte layer 13 is located between the second electrode 12 and the first solid electrolyte layer 11. The content of the organic compound in the first solid electrolyte layer 11 is greater than the content of the organic compound in the second solid electrolyte layer. The thickness of the first solid electrolyte layer 11 is smaller than the thickness of the second solid electrolyte layer 13.

[0024] Furthermore, the content rate of the organic compound in the first solid electrolyte layer 11 is the content rate of the organic compound when only one kind of organic compound is contained in the first solid electrolyte layer 11, and is the total content rate of each organic compound when a plurality of organic compounds are contained in the layer. In addition, the content rate of the organic compound in the second solid electrolyte layer 13 is the content rate of the organic compound when only one kind of organic compound is contained in the second solid electrolyte layer 13, and is the total content rate of each organic compound when a plurality of organic compounds are contained in the layer.

[0025] Here, for example, it can be confirmed that the solid electrolyte layer contains the organic compound by performing energy dispersive X-ray analysis (EDX) on a cross section of the solid electrolyte layer.

[0026] In addition, the content of organic compounds in the solid electrolyte layer is obtained by, for example, thermogravimetric-differential thermal analysis (TG-DTA). By subjecting the solid electrolyte layer as a dry film to, for example, infrared drying, the organic compounds contained in the solid electrolyte layer are baked off. By measuring the mass change of the solid electrolyte layer at this time, the content of organic compounds in the solid electrolyte layer can be calculated. Furthermore, as an alternative method, for example, Fourier transform infrared spectroscopy (FT-IR) can be cited.

[0027] In addition, the thickness of the first solid electrolyte layer 11 and the thickness of the second solid electrolyte layer 13 can be the average value of the values ​​measured at any multiple points (at least 3 points, for example 3 points or 5 points). The thickness of each solid electrolyte layer can be measured using a microscope image of the cut surface or fracture surface. The microscope image is obtained using a scanning electron microscope, a laser microscope or an optical microscope. In addition, the thickness of each layer other than each solid electrolyte layer is also determined using the same method.

[0028] Hereinafter, the battery 1 will be described in more detail.

[0029] The first electrode 10 includes a first current collector 101 and a first active material layer 102. The first active material layer 102 is disposed on the first current collector 101 and in contact with the first current collector 101. The first solid electrolyte layer 11 may cover the surface of the first active material layer 102 disposed on the first current collector 101. In other words, the first solid electrolyte layer 11 may cover the surface of the first active material layer 102 except for the interface between the first current collector 101 and the first active material layer 102. The thickness of the first solid electrolyte layer 11 covering the surface of the first active material layer 102 may be, for example, 5 μm or less. According to the configuration in which the first solid electrolyte layer 11 covers the surface of the first active material layer 102, the occurrence of an electrical short circuit can be more effectively suppressed. The first solid electrolyte layer 11 may also cover the entire surface of the first active material layer 102 except for the interface between the first current collector 101 and the first active material layer 102. Furthermore, in Figure 1 , as an example, a configuration is shown in which the first solid electrolyte layer 11 covers all surfaces of the first active material layer 102 except the interface between the first current collector 101 and the first active material layer 102. However, the first solid electrolyte layer 11 only needs to be provided between the first electrode 10 and the second solid electrolyte layer 13. Therefore, the first solid electrolyte layer 11 may not cover the entire side surface of the first active material layer 102.

[0030] The second electrode 12 includes a second current collector 121 and a second active material layer 122. The second active material layer 122 is disposed on the second current collector 121 and in contact with the second current collector 121. For example, the second solid electrolyte layer 13 may cover the surface of the second active material layer 122. In other words, the second solid electrolyte layer 13 may cover the surface of the second active material layer 122 except for the interface between the second current collector 121 and the second active material layer 122. The second solid electrolyte layer 13 may also cover the entire surface of the second active material layer 122 except for the interface between the second current collector 121 and the second active material layer 122. Furthermore, in Figure 1 , as an example, a configuration is shown in which the second solid electrolyte layer 13 covers all surfaces of the second active material layer 122 except the interface between the second current collector 121 and the second active material layer 122. However, the second solid electrolyte layer 13 only needs to be provided between the second electrode 12 and the first solid electrolyte layer 11. Therefore, the second solid electrolyte layer 13 may not cover the entire side surface of the second active material layer 122.

[0031] In other words, the battery 1 has a configuration in which the first electrode 10 and the second electrode 12 are arranged opposite to each other via the first solid electrolyte layer 11 and the second solid electrolyte layer 13. In addition, the solid electrolyte layer of the battery 1 is composed of both the first solid electrolyte layer 11 and the second solid electrolyte layer 13. The sum of the thickness of the first solid electrolyte layer 11 and the thickness of the second solid electrolyte layer 13 is required to have the following important characteristics: (i) to be small in order to increase the capacity of the battery; and (ii) to suppress short circuits caused by electrical contact between the first active material layer 102 and the second active material layer 122.

[0032] Furthermore, if the battery 1 is driven only, a single layer consisting of only one of the first solid electrolyte layer 11 and the second solid electrolyte layer 13 may be formed. However, for the battery 1, in view of the need to stably achieve the above-mentioned required characteristics (i) and (ii) and considering the possibility of defects in the solid electrolyte layer, it is not desirable to form a solid electrolyte layer consisting of only one of the first solid electrolyte layer 11 and the second solid electrolyte layer 13. For example, in the case where the solid electrolyte layer is composed of a single layer, a solid electrolyte material with a small particle size is used to form the solid electrolyte layer thinner. The specific surface area of ​​a solid electrolyte material with a small particle size is large. Therefore, in the case of using a solid electrolyte material with a small particle size to form a solid electrolyte layer, when the solid electrolyte material is slurried, the amount of solvent and the amount of organic compounds such as a binder increase. In the case where the solid electrolyte layer is a single layer, the solid electrolyte layer as a whole contains more organic compounds. As a result, the solid electrolyte layer becomes a layer with high resistance throughout the whole. Moreover, by thinning the layer, the possibility of defects such as pinholes occurring throughout the whole solid electrolyte layer also increases. Therefore, simply reducing the thickness of the single-layer solid electrolyte layer may cause a decrease in characteristics, that is, it may be difficult to suppress short circuits and may cause a decrease in capacity.

[0033] In the battery 1 of the present embodiment, the solid electrolyte layer includes two layers, namely, the first solid electrolyte layer 11 and the second solid electrolyte layer 13. The first solid electrolyte layer 11 is thinner than the second solid electrolyte layer 13, and the content of the organic compound in the first solid electrolyte layer 11 is greater than the content of the organic compound in the second solid electrolyte layer 13. Therefore, even if the first solid electrolyte layer 11 is formed using a solid electrolyte material having a small particle size, since a sufficient amount of organic compound is used, it can be a solid electrolyte layer fully filled with the solid electrolyte material. Therefore, although the first solid electrolyte layer 11 is thinned, it is difficult to generate defects such as pinholes, and as a result, the effect of suppressing short circuits is also obtained. Moreover, by thinning the first solid electrolyte layer 11, the thickness of the entire solid electrolyte layer becomes smaller, so that the battery 1 can also achieve a high capacity. Moreover, for the production of the second solid electrolyte layer 13 having a larger thickness, since it is not necessary to use a solid electrolyte material with a small particle size for thinning, the possibility of defects such as pinholes is low. Therefore, the second solid electrolyte layer 13 improves the short circuit suppression function of the solid electrolyte layer as a whole. In this way, the solid electrolyte layer of the battery 1 includes the first solid electrolyte layer 11 that is thinned without causing film defects, and the second solid electrolyte layer 13 that is less likely to contain defects such as pinholes and can fully suppress short circuits. Therefore, the battery 1 can stably achieve both the above-mentioned required characteristics (i) and (ii).

[0034] The thickness of the first solid electrolyte layer 11 may be 0.5 μm to 5 μm, or 1 μm to 3 μm. When the thickness of the first solid electrolyte layer 11 is within this range, the risk of film defects in the formation method described later can be suppressed, and the occurrence of electrical short circuits can be more reliably suppressed.

[0035] The first solid electrolyte layer 11 may include a solid electrolyte material having an average particle size of 0.5 μm or less as a main component. Thus, it becomes easy to make a first solid electrolyte layer 11 with a small thickness. Here, the so-called main component in the first solid electrolyte layer 11 refers to the component with the highest content (mass %) among the components constituting the first solid electrolyte layer 11. On the other hand, in the same manner as when forming the second solid electrolyte layer 13 described later, a solid electrolyte material powder having an average particle size of 0.5 μm or more and 20 μm or less is used, and the first solid electrolyte layer 11 is made to have a thickness of 0.5 μm or more and 5 μm or less, due to the presence of a powder having a large particle size, uniform filling of the solid electrolyte material becomes difficult. As a result, defects are easily generated in the membrane. Therefore, it is sometimes difficult to suppress a short circuit caused by the solid electrolyte layer.

[0036] Here, in this specification, the average particle size of the solid electrolyte material is D50 (that is, the median particle size of the volume distribution) evaluated based on the volume particle size distribution measured by a laser diffraction scattering particle size distribution measuring device.

[0037] Furthermore, as mentioned above, since the specific surface area of ​​the solid electrolyte material with a small particle size is large. Therefore, when slurrying is performed to form a solid electrolyte layer, the amount of solvent and the amount of organic compounds such as adhesives increase. However, the increase in organic compounds effectively plays a role in the bonding with the second solid electrolyte layer 13. Through the organic compound contained in the first solid electrolyte layer 11, the bonding between the first solid electrolyte layer 11 and the surface of the second solid electrolyte layer 13 becomes easy and strong, which can further suppress short circuits.

[0038] The content of the organic compound in the first solid electrolyte layer 11 may be 5% by mass or more and 10% by mass or less. When the organic compound contained in the first solid electrolyte layer 11 is 5% by mass or more, a thin layer of solid electrolyte material fully filled with solid electrolyte material can be formed even when a solid electrolyte material with a small particle size is used. Moreover, when the organic compound contained in the first solid electrolyte layer 11 is 5% by mass or more, flexibility can be imparted to the first solid electrolyte layer 11, so it becomes easy to form the first solid electrolyte layer 11 with few defects. Moreover, when the organic compound contained in the first solid electrolyte layer 11 is 5% by mass or more, the bonding adhesion between the first solid electrolyte layer 11 and the second solid electrolyte layer 13 can also be manifested. On the other hand, when the content of the organic compound in the first solid electrolyte layer 11 is 10% by mass or less, the increase of the resistance caused by the organic compound can be suppressed, so the function of suppressing electrical short circuit of the solid electrolyte layer as a whole is improved. Therefore, according to this configuration, the battery 1 can more stably achieve the above-mentioned required characteristics (i) and (ii).

[0039] The thickness of the second solid electrolyte layer 13 may be 3 μm or more and 50 μm or less, or 5 μm or more and 30 μm or less. When the second solid electrolyte layer 13 has a thickness of 3 μm or more, the occurrence of an electrical short circuit can be more reliably suppressed. When the second solid electrolyte layer 13 has a thickness of 50 μm or less, the capacity of the battery 1 can be increased.

[0040] Hereinafter, the case where the first electrode 10 is a negative electrode, the first solid electrolyte layer 11 is a solid electrolyte layer on the negative electrode side, the second electrode 12 is a positive electrode, and the second solid electrolyte layer 13 is a solid electrolyte layer on the positive electrode side will be described as an example.

[0041] As the first electrode 10 and the second electrode 12 , for example, a negative electrode and a positive electrode used in a known all-solid-state battery (for example, a lithium-ion battery) can be respectively applied.

[0042] The first current collector 101 may be a negative electrode current collector used in a known all-solid battery (eg, a lithium ion battery). For example, Cu foil, Al foil, SUS foil, etc. may be used. The thickness of the first current collector 101 may be, for example, not less than 5 μm and not more than 100 μm.

[0043] In the first active material layer 102, the negative electrode active material used in the known all-solid-state battery (such as a lithium-ion battery) can be applied. For example, known negative electrode active materials such as graphite and metal Li can be used. The active material used for the first active material layer 102 is not limited thereto, and various materials that can be separated from and inserted into ions such as Li or Mg can be used. In addition, as materials other than active material materials that can be included in the first active material layer 102, any solid electrolyte such as a sulfide solid electrolyte and an oxide solid electrolyte can be listed. As a sulfide solid electrolyte, for example, a Li2S:P2S5 mixture can be used. In addition, the first active material layer 102 may also contain a conductive aid such as acetylene black and a bonding adhesive such as polyvinylidene fluoride. The thickness of the first active material layer 102 can be, for example, more than 5 μm and less than 300 μm.

[0044] The second current collector 121 may be a positive electrode current collector used in a known all-solid battery (eg, a lithium ion battery). For example, Cu foil, Al foil, SUS foil, etc. may be used. The thickness of the second current collector 121 may be, for example, not less than 5 μm and not more than 100 μm.

[0045] In the second active material layer 122, the positive electrode active material used in the known all-solid-state battery (such as a lithium-ion battery) can be applied. For example, known positive electrode active materials such as lithium cobalt oxide and LiNO can be used. The active material used for the second active material layer 122 is not limited to this, and various materials that can be separated and inserted into ions such as Li or Mg can be used. In addition, as a material other than the active material material that can be included in the second active material layer 122, any solid electrolyte such as a sulfide solid electrolyte and an oxide solid electrolyte can be listed. As a sulfide solid electrolyte, for example, a Li2S:P2S5 mixture can be used. A material formed by coating the surface of the active material with a solid electrolyte can also be used. In addition, the second active material layer 122 may also contain a conductive aid such as acetylene black and a bonding adhesive such as polyvinylidene fluoride. The thickness of the second active material layer 122 can be, for example, more than 5 μm and less than 300 μm.

[0046] In the first solid electrolyte layer 11, any solid electrolyte material such as a sulfide solid electrolyte, a halogen-based solid electrolyte, and an oxide solid electrolyte can be used. As a sulfide solid electrolyte, for example, a Li2S:P2S5 mixture can be used. As a slurry coating for forming the first solid electrolyte layer 11, a solution synthesized by synthesizing the above-mentioned solid electrolyte material in a solvent can be used. By using such a solution as a slurry coating for forming the first solid electrolyte layer 11, a thin first solid electrolyte layer 11 such as 0.5 μm or more and 5 μm or less can be produced.

[0047] Furthermore, the first solid electrolyte layer 11 can also be produced by a method other than the method of using a solution synthesized by the above-mentioned solid electrolyte material in a solvent. For example, the first solid electrolyte layer 11 can be produced even by a general method of using a slurry coating containing a solid electrolyte material, a binder and a solvent.

[0048] In the second solid electrolyte layer 13, any solid electrolyte material such as a sulfide solid electrolyte, a halogen-based solid electrolyte, and an oxide solid electrolyte can be used. As a sulfide solid electrolyte, for example, a Li2S:P2S5 mixture can be used. In order to form a second solid electrolyte layer 13 having a thickness of, for example, 3 μm or more and 50 μm or less, for example, a powder having an average particle size of 0.5 μm or more and 20 μm or less can be used as a solid electrolyte material.

[0049] The second solid electrolyte layer 13 can be formed by preparing a slurry coating obtained by kneading solid electrolyte material powder and a solvent using an organic compound such as polyvinylidene fluoride and an elastomer, and applying the coating on the second active material layer 122 to cover the second active material layer 122 .

[0050] In the above-mentioned paste-like coating used to form the second solid electrolyte layer 13, the above-mentioned organic compound can be contained in the range of 0.5 mass % or more and 5 mass % or less of the total solid content as needed. In the case of containing more than 0.5 mass % of the above-mentioned organic compound, the thickness of the second solid electrolyte layer 13 can be fully maintained, so the overall function of the solid electrolyte layer to suppress electrical short circuits is improved. In the case where the content of the above-mentioned organic compound is less than 5 mass %, the increase in resistance caused by the organic compound can be suppressed, so that the high capacity and high output of the battery can be achieved.

[0051] As described above, the first solid electrolyte layer 11 has a smaller thickness than the second solid electrolyte layer 13, and has a larger content of organic compounds than the second solid electrolyte layer 13. According to this configuration, the bonding adhesion between the first solid electrolyte layer 11 and the second solid electrolyte layer 13 is improved, and the risk of short circuit can be reduced, so that the capacity quality of the battery 1 can be stabilized.

[0052] Furthermore, although Figure 1 Although not shown in the figure, in the battery 1, a sealing member can be provided in the area outside the power generation element and sandwiched by the first collector 101 and the second collector 121. The so-called power generation element refers to the first active material layer 102, the first solid electrolyte layer 11, the second active material layer 122 and the second solid electrolyte layer 13. The sealing member may also have insulating properties. According to the sealing member, it is possible to suppress the intrusion of moisture into the interior of the battery 1, maintain the structure of the battery 1, and prevent a short circuit caused by the contact between the first collector 101 and the second collector 121. As a result, the mechanical strength of the battery 1 can be ensured.

[0053] As a sealing material constituting the sealing component, for example, a thermoplastic resin can be used. By using a thermoplastic resin, the range of material selection is expanded. In addition, a thermosetting resin and a photocurable resin can also be used as a sealing material. They can be used alone or in combination of two or more. When the glass transition temperature of the sealing material is sufficiently high, the sealing strength of the sealing component can be fully maintained. In order to enhance the function of the sealing component, the sealing material may also contain other materials such as functional powders and fibers. As other materials, inorganic fillers and silica gel can be listed. Inorganic fillers can enhance the structural retention. Silica gel can enhance water resistance. These functional powders or fibers can be used alone or in combination of two or more.

[0054] Next, an example of a method for manufacturing the battery 1 in Embodiment 1 will be described. However, the method for manufacturing the battery of the present disclosure is not limited to this.

[0055] The materials used for the first current collector 101 , the first active material layer 102 , the second current collector 121 , the second active material layer 122 , the first solid electrolyte layer 11 , and the second solid electrolyte layer 13 are as described above.

[0056] First, an example of a method for producing the first electrode 10 is described. A slurry coating is prepared by kneading the material contained in the first active material layer 102 with a solvent. The solvent can be a known solvent used when producing the negative electrode active material layer of a known all-solid-state battery (such as a lithium-ion battery). The first active material layer 102 is formed by applying the produced coating to the first current collector 101 and drying the coating. In order to increase the density of the first active material layer 102, the obtained dry film can be pressed. Thus, the first electrode 10 having the first active material layer 102 in contact with the first current collector 101 provided on the first current collector 101 can be obtained.

[0057] The first electrode 10 may have a larger area than the second electrode 12. According to this configuration, it is possible to prevent a problem caused by the precipitation of Li or Mg.

[0058] Next, the first solid electrolyte layer 11 is formed on the first active material layer 102 of the first electrode 10. For example, in the case of forming the first solid electrolyte layer 11 having a thickness of 0.5 μm or more and 5 μm or less, for example, a solution synthesized by synthesizing a solid electrolyte material in a solvent, or a slurry containing a solid electrolyte material, an organic compound such as a binder, and a solvent can be used as a coating for forming the first solid electrolyte layer 11. Furthermore, in the step of forming the first solid electrolyte layer 11, in order to give the first solid electrolyte layer 11 flexibility so that it can be easily covered with the first active material layer 102, and in order to improve the bonding adhesion between the first solid electrolyte layer 11 and the second solid electrolyte layer 13, the coating for forming the first solid electrolyte layer 11 may also contain an organic compound in a range of 5% by mass or more and 10% by mass or less of the total solid content.

[0059] For forming the first solid electrolyte layer 11 , a coating method such as a die coating method, a doctor blade method, a roll coating method, a screen printing method, and an ink jet method can be applied, but the method is not limited to these methods.

[0060] By the above method, a stacked body on the first electrode side in which the first solid electrolyte layer 11 is formed on the first electrode 10 can be obtained.

[0061] Next, an example of a method for producing the second electrode 12 is described. A slurry coating is prepared by kneading the material contained in the second active material layer 122 with a solvent. The solvent can be a known solvent used in the production of a positive electrode active material layer of a known all-solid-state battery (e.g., a lithium-ion battery). The second active material layer 122 is formed by applying the produced coating to the second current collector 121 and drying the coating. In order to increase the density of the second active material layer 122, the obtained dry film can be pressed. Thus, the second electrode 12 having a second active material layer 122 in contact with the second current collector 121 provided on the second current collector 121 can be obtained.

[0062] Next, a second solid electrolyte layer 13 is formed on the second active material layer 122 of the second electrode 12. For example, in the case of forming a second solid electrolyte layer 13 having a thickness of 3 μm or more and 50 μm or less, the solid electrolyte material used to form the second solid electrolyte layer 13 can use, for example, a powder having an average particle size of 0.5 μm or more and 20 μm or less. The powder of the solid electrolyte material of the second solid electrolyte layer 13, an organic compound such as polyvinylidene fluoride and an elastomer, and a solvent are mixed to prepare a slurry coating. The prepared coating is applied to the second active material layer 122 and the coating is dried to form the second solid electrolyte layer 13. The second solid electrolyte layer 13 is formed, for example, in a manner that covers the surface of the second active material layer 122.

[0063] In the coating used to form the second solid electrolyte layer 13, the organic compound can be contained in a range of, for example, 0.5% by mass or more and 5% by mass or less of the total solid content as required. By including an organic compound of 0.5% by mass or more of the total solid content in the coating, the thickness of the second solid electrolyte layer 13 can be fully maintained, so the overall function of the solid electrolyte layer to suppress electrical short circuits is improved. By including an organic compound of 5% by mass or less of the total solid content in the coating, the increase in the resistance of the second solid electrolyte layer 13 can be suppressed, so that the battery can be increased in capacity and output.

[0064] The second solid electrolyte layer 13 can be formed by a coating method such as a die coating method, a doctor blade method, a roll coating method, and a screen printing method, but the method is not limited to these methods.

[0065] By the above method, a laminated body on the second electrode side in which the second solid electrolyte layer 13 is formed on the second electrode 12 can be obtained.

[0066] The battery 1 can be obtained by joining the stacked body on the first electrode side and the stacked body on the second electrode side so that the first solid electrolyte layer 11 and the second solid electrolyte layer 13 face each other.

[0067] Furthermore, in the present embodiment, the configuration in which the first electrode 10 is a negative electrode and the second electrode is a positive electrode is described as an example, but the first electrode 10 may be a positive electrode and the second electrode 12 may be a negative electrode. In this case, the solid electrolyte layer on the positive electrode side becomes the first solid electrolyte layer 11, and the solid electrolyte layer on the negative electrode side becomes the second solid electrolyte layer 13. Therefore, the solid electrolyte layer on the positive electrode side has a smaller thickness than the solid electrolyte layer on the negative electrode side, and the solid electrolyte layer on the positive electrode side has a smaller content of organic compounds than the solid electrolyte layer on the negative electrode side. Even with such a configuration, short circuits can be suppressed, and effects such as high capacity and stable capacity quality can be obtained.

[0068] The battery of this embodiment may also constitute a stacked all-solid battery. This all-solid battery can be constituted by stacking a plurality of unit cells, which are basic constituent units, of the battery of this embodiment.

[0069] Figure 2 It means there are multiple layers. Figure 1 Schematic cross-sectional view of a first example of a stacked all-solid battery of the battery 1 shown. In the stacked all-solid battery 2 of the first example, two adjacent batteries 1 are stacked by joining the first collector 101 of one battery 1 and the second collector 121 of the other battery 1. That is, the stacked all-solid battery 2 of the first example is a stacked battery in which a plurality of batteries 1 are electrically connected in series. The first collector 101 and the second collector 121 can be joined directly or by using a conductive adhesive or welding method.

[0070] Figure 3 It means there are multiple layers. Figure 1 A schematic cross-sectional view of a second example of a stacked all-solid battery of the battery 1 shown. In the stacked all-solid battery 3 of the second example, two adjacent batteries 1 are stacked by joining the first collector 101 of one battery 1 to the first collector 101 of another battery 1, and joining the second collector 121 of one battery 1 to the second collector 121 of another battery 1. That is, the stacked all-solid battery 3 of the second example is a stacked battery in which a plurality of batteries 1 are electrically connected in parallel. The first collectors 101 and the second collectors 121 can be directly joined to each other, or can be joined using a conductive adhesive or welding method.

[0071] Figure 4 It means there are multiple layers. Figure 1 The third example of the stacked all-solid battery 4 has the following structure: Figure 3In the stacked all-solid battery 3 shown, two adjacent batteries 1 share a first current collector 101, and two adjacent batteries 1 share a second current collector 121. The stacked all-solid battery 4 of the third example is a stacked battery in which a plurality of batteries 1 are electrically connected in parallel, similarly to the stacked all-solid battery 3 of the second example.

[0072] The stacked all-solid battery 4 can be formed using, for example, the following method.

[0073] A first component having a first active material layer 102 and a first solid electrolyte layer 11 formed on each of the upper and lower surfaces of a first current collector 101 and a second component having a second active material layer 122 and a second solid electrolyte layer 13 formed on each of the upper and lower surfaces of a second current collector 121 are prepared. By joining these first components and second components in such a manner that the first solid electrolyte layer 11 and the second solid electrolyte layer 13 face each other, a plurality of batteries 1 can be formed. Figure 4 Furthermore, the first current collector 101 or the second current collector 121 disposed at the upper end or the lower end of the stacked all-solid battery 4 has an active material layer and a solid electrolyte layer formed only on one surface.

[0074] As another method, the following method can be used: prepare a first component in which the first active material layer 102, the first solid electrolyte layer 11, the second solid electrolyte layer 13, and the second active material layer 122 are sequentially stacked on the first current collector 101, and a second component in which the second active material layer 122, the second solid electrolyte layer 13, the first solid electrolyte layer 11, and the first active material layer 102 are sequentially stacked on the second current collector 121, and stack these first components and second components. Even if this method is used, a plurality of batteries 1 can be formed. Figure 4 A stacked battery stacked as shown.

[0075] Figure 5 It means there are multiple layers. Figure 1 The fourth example of the stacked all-solid battery 5 has the following structure: Figure 2 In the stacked all-solid battery 2 shown, the first collector 101 and the second collector 121 of two adjacent batteries 1 share a common collector. The stacked all-solid battery 5 of the fourth example is a stacked battery in which a plurality of batteries 1 are electrically connected in series, similarly to the stacked all-solid battery 2 of the first example.

[0076] The stacked all-solid-state battery 5 can be formed using, for example, the following method.

[0077] A current collector that serves as both the first current collector 101 and the second current collector 121 is prepared. The first active material layer 102 and the first solid electrolyte layer 11 are formed on the bottom surface of the current collector, and the second active material layer 122 and the second solid electrolyte layer 13 are formed on the top surface of the first current collector 101. A plurality of such components are prepared, and the plurality of components are joined in such a manner that the first solid electrolyte layer 11 and the second solid electrolyte layer 13 face each other. Thus, a plurality of batteries 1 can be formed. Figure 5 Furthermore, the first current collector 101 or the second current collector 121 is arranged at the upper end or the lower end of the stacked all-solid battery 5.

[0078] As another method, the following method can be used: prepare a plurality of components in which the first active material layer 102, the first solid electrolyte layer 11, the second solid electrolyte layer 13, and the second active material layer 122 are sequentially stacked on the first current collector 101, and stack these components. In the stacked state, the first current collector 101 can function as the second current collector 121. Even by using this method, a plurality of batteries 1 can be formed. Figure 5 A stacked battery stacked as shown.

[0079] Although the battery modes for implementing the present disclosure have been specifically described above, the battery of the present disclosure is not limited thereto. The present disclosure can be widely applied to batteries having excellent reliability and good capacity characteristics.

[0080] Industrial Applicability

[0081] The battery disclosed herein can be advantageously used in various electronic devices, electric appliances, electric vehicles, and the like.

[0082] Description of Reference Numerals

[0083] 1: Battery

[0084] 2, 3, 4, 5: Laminated all-solid-state batteries

[0085] 10: 1st electrode

[0086] 11: 1st solid electrolyte layer

[0087] 12: Second electrode

[0088] 13: Second solid electrolyte layer

[0089] 101: The first collector

[0090] 102: First active material layer

[0091] 121: Episode 2

[0092] 122: Second active material layer

Claims

1. A battery having: 1st electrode; a first solid electrolyte layer in contact with the first electrode; a second electrode; and a second solid electrolyte layer located between the second electrode and the first solid electrolyte layer, The content of the organic compound in the first solid electrolyte layer is greater than the content of the organic compound in the second solid electrolyte layer, and The thickness of the first solid electrolyte layer is smaller than the thickness of the second solid electrolyte layer, The thickness of the first solid electrolyte layer is 1 μm or more and 3 μm or less. The first electrode includes a first current collector and a first active material layer in contact with the first current collector. The first solid electrolyte layer covers the surface of the first active material layer except for the interface between the first current collector and the first active material layer.

2. The battery according to claim 1, The first solid electrolyte layer contains a solid electrolyte material having an average particle size of 0.5 μm or less as a main component.

3. The battery according to claim 1 or 2, The content of the organic compound in the first solid electrolyte layer is 5 mass % or more and 10 mass % or less.

4. The battery according to claim 1 or 2, The second solid electrolyte layer has a thickness of 3 μm or more and 50 μm or less.

5. The battery according to claim 4, The second solid electrolyte layer has a thickness of 5 μm or more and 30 μm or less.

6. The battery according to claim 1 or 2, The first solid electrolyte layer covers the surface of the first active material layer except for the interface between the first current collector and the first active material layer with a thickness of 1 μm to 3 μm.