FRP tube steel bar composite ICCP-SS seawater sand concrete composite beam
Through the FRP pipe steel bar combination ICCP-SS system, carbon fiber-FRP composite rectangular pipes are used to provide impressed current cathodic protection and structural reinforcement, solving the problem of mechanical property degradation caused by steel bar corrosion in coastal environments, achieving the restoration of structural bearing capacity and concrete structures The durability is improved.
Patent Information
- Application Number
- CN202110539295.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-05-18
AI Technical Summary
Existing technologies cannot effectively solve the problem of mechanical property degradation caused by corrosion of reinforced concrete structures in coastal environments. ICCP technology can only inhibit corrosion but cannot restore the structural bearing capacity. SS technology cannot fundamentally solve the erosion of steel bars by harmful external and internal elements. .
The FRP pipe and steel bar combination ICCP-SS system is used to provide impressed current cathodic protection and structural reinforcement through carbon fiber-FRP composite rectangular pipes. The carbon fiber cloth is wrapped around the FRP rectangular pipe, and the steel cage is embedded in the seawater and sand concrete layer to utilize the impressed current. Protect steel bars to form dual functions of cathodic protection and structural reinforcement.
Prevent and delay corrosion of steel bars, improve and restore structural bearing capacity, enhance the mechanical properties and durability of concrete structures, effectively utilize seawater and sand resources, reduce material transportation costs, and improve resource utilization efficiency.
Smart Images

Figure CN113216511B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of prefabricated structure engineering, and in particular to an FRP tube steel bar combined ICCP-SS seawater and sea sand concrete composite beam. Background Art
[0002] The coastal areas are rich in seawater and sea sand resources. Using seawater and sea sand in concrete structures can effectively solve the problem of increasingly depleted river sand and freshwater resources and make full use of local resources. However, reinforced concrete structures using seawater and sea sand will have relatively serious corrosion problems, reducing the mechanical properties and durability of seawater and sea sand concrete structures.
[0003] Impressed Current Cathodic Protection (ICCP) is a technology that uses auxiliary anode materials to apply cathodic protection current to the steel bars inside the concrete structure, so that the potential shifts negatively to the corrosion-free area, thereby protecting the steel bars. It is recognized as an effective control method to prevent and delay steel corrosion; Structural Strengthening (SS) is a technology that uses structural reinforcement materials such as structural steel or fiber reinforced polymer (FRP) to jointly bear force and deformation with concrete structures, thereby improving or repairing the mechanical properties of the structure.
[0004] Among the existing technologies, although ICCP technology can inhibit the corrosion of steel bars in concrete structures in coastal environments, it cannot restore the deterioration of structural mechanical properties caused by steel bar corrosion; although SS technology can improve or restore the structural bearing capacity, it cannot fundamentally solve the continuous corrosion of steel bars by the external environment and internal harmful elements of concrete structures in coastal environments.
[0005] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0006] The technical problem to be solved by the present invention is that, in view of the above-mentioned defects of the prior art, a FRP tube steel bar combined ICCP-SS seawater and sea sand concrete composite beam is provided, aiming to solve the problem of loss of structural bearing capacity due to steel bar corrosion in the prior art.
[0007] The technical solution adopted by the present invention to solve the technical problem is as follows:
[0008] An FRP tube steel bar combined ICCP-SS seawater sea sand concrete composite beam, comprising: an impressed current cathodic protection and structural reinforcement system and a reinforced seawater sea sand concrete composite beam wrapped outside the impressed current cathodic protection and structural reinforcement system;
[0009] The impressed current cathodic protection and structural reinforcement system comprises:
[0010] FRP rectangular tube;
[0011] Carbon fiber cloth, wrapped outside the FRP rectangular tube;
[0012] The reinforced seawater and sea sand concrete composite beam comprises:
[0013] Seawater and sea sand concrete layer;
[0014] A steel cage is embedded in the seawater and sea sand concrete layer;
[0015] The impressed current cathodic protection and structural reinforcement system is located within the steel cage.
[0016] The FRP tube steel bar combined ICCP-SS seawater and sea sand concrete composite beam, wherein the steel cage comprises:
[0017] Longitudinal reinforcement;
[0018] A plurality of stirrups are arranged on the longitudinal steel bars and arranged along the length direction of the longitudinal steel bars.
[0019] The FRP tube steel bar combined ICCP-SS seawater and sea sand concrete composite beam, wherein the distance between the four sides of the FRP rectangular tube and the stirrups is not less than 30 mm.
[0020] The FRP tube steel bar combined ICCP-SS seawater and sea sand concrete composite beam, wherein side forms are provided at both ends of the FRP rectangular tube.
[0021] The FRP tube steel bar combined ICCP-SS seawater sea sand concrete composite beam, wherein a plurality of holes are arranged on the side of the impressed current cathodic protection and structural reinforcement system, the diameter of the holes is 1 / 3-2 / 3 of the height of the FRP rectangular tube, and the spacing between two adjacent holes is 1 / 2-3 / 2 of the height of the FRP rectangular tube.
[0022] The FRP tube steel bar combined ICCP-SS seawater sea sand concrete composite beam, wherein the FRP rectangular tube is selected from one of a glass fiber FRP rectangular tube, a carbon fiber FRP rectangular tube, an aramid fiber FRP rectangular tube, and a basalt FRP rectangular tube.
[0023] The FRP tube steel bar combined ICCP-SS seawater sand concrete composite beam, wherein both ends of the FRP rectangular tube extend outside the steel bar seawater sand concrete composite beam; and / or
[0024] The thickness of the FRP rectangular tube is 3-15 mm.
[0025] The FRP tube steel bar combined ICCP-SS seawater and sea sand concrete composite beam, wherein a conductive sheet is arranged outside the carbon fiber cloth, and the conductive sheet is connected to the FRP rectangular tube.
[0026] A method for preparing an FRP tube steel bar combined ICCP-SS seawater and sea sand concrete composite beam, comprising the steps of:
[0027] Provide composite beam molds, fillers, seawater and sea sand concrete, steel cages, carbon fiber cloth and FRP rectangular tubes;
[0028] Wrapping and pasting the carbon fiber cloth on the outside of the FRP rectangular tube to form an impressed current cathodic protection and structural reinforcement system;
[0029] Put the filler into the FRP rectangular tube, then place the impressed current cathodic protection and structural reinforcement system in the steel cage, and put them into the composite beam mold together;
[0030] pouring the seawater and sea sand concrete into the composite beam mold and solidifying it to form a reinforced seawater and sea sand concrete composite beam;
[0031] The composite beam mold is removed, and the carbon fiber cloth and the steel cage are connected by a power supply to protect the steel cage, thereby obtaining an FRP tube steel bar composite ICCP-SS seawater and sea sand concrete composite beam.
[0032] The method for preparing the FRP tube steel bar combined ICCP-SS seawater sand concrete composite beam, wherein the seawater sand concrete is poured into the composite beam mold and solidified to form a reinforced seawater sand concrete composite beam, comprises:
[0033] The seawater-sand concrete is poured into the composite beam mold by a layered pouring and vibrating method, and then smoothed. A rough steel brush is used to roughen the concrete and the concrete is cured to obtain a reinforced seawater-sand concrete composite beam.
[0034] Beneficial effect: The impressed current cathodic protection and structural reinforcement (ICCP-SS) system based on carbon fiber-FRP composite rectangular tubes is used. The carbon fiber-FRP composite rectangular tubes are used as anodes and the steel cage is used as cathodes. The steel bars in the seawater and sea sand concrete composite beams are protected by impressed current, which can prevent and delay the corrosion of the steel bars. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a cross-sectional view of the FRP tube steel bar combination ICCP-SS seawater sand concrete composite beam when the FRP tube is located in the composite beam in the present invention.
[0036] Figure 2 It is a cross-sectional view of the FRP tube steel bar composite ICCP-SS seawater sand concrete composite beam when the FRP tube is located outside the composite beam in the present invention.
[0037] Figure 3 It is a structural schematic diagram of the impressed current cathodic protection and structural reinforcement system and the steel cage in the present invention.
[0038] Figure 4 It is a schematic structural diagram of the impressed current cathodic protection and structural reinforcement system and the conductive sheet in the present invention.
[0039] Description of reference numerals:
[0040] 1. Carbon fiber cloth; 2. FRP rectangular tube; 3. Stirrups; 4. Composite beam mold; 5. Seawater and sea sand concrete layer; 6. Longitudinal steel bars; 7. Filler; 8. Carbon fiber-FRP composite rectangular tube; 9. Side mold; 10. Holes; 11. Conductive sheet; 12. Bolts. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solution and advantages of the present invention clearer and more specific, the present invention is further described in detail below with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0042] Please also see Figure 1-Figure 4 The present invention provides some embodiments of an FRP tube steel bar combined ICCP-SS seawater and sea sand concrete composite beam.
[0043] Fiber reinforced polymer (FRP) is a composite material made of polymer epoxy resin as the body and high-strength fiber as the reinforcement through a composite process. It has the advantages of light weight, high strength, corrosion resistance, fatigue resistance, and designable performance. It is a widely used material in SS technology. At the same time, carbon fiber has excellent conductivity and stable chemical properties and can be used as an auxiliary anode in ICCP technology. Therefore, FRP and carbon fiber materials can be developed into a combined system with ICCP and SS functions.
[0044] Seawater and sea sand concrete structures can make full use of seawater and sea sand resources in coastal areas. It is feasible to develop FRP and carbon fiber materials into a composite system (ICCP-SS) that provides impressed current cathodic protection and structural reinforcement functions to prevent and delay steel corrosion, and improve and restore the structural bearing capacity lost due to steel corrosion. Providing a reinforced seawater and sea sand prefabricated composite beam with impressed current cathodic protection and structural reinforcement functions is a technical problem that needs to be solved in this field.
[0045] like Figure 1-Figure 2 As shown, the FRP tube steel bar combined ICCP-SS seawater sea sand concrete composite beam of the present invention comprises: an impressed current cathodic protection and structural reinforcement system and a reinforced seawater sea sand concrete composite beam wrapped outside the impressed current cathodic protection and structural reinforcement system;
[0046] The impressed current cathodic protection and structural reinforcement system comprises:
[0047] FRP rectangular tube 2;
[0048] Carbon fiber cloth 1, wrapped outside the FRP rectangular tube 2;
[0049] The reinforced seawater and sea sand concrete composite beam comprises:
[0050] Seawater and sea sand concrete layer 5;
[0051] A steel cage is embedded in the seawater sand concrete layer 5;
[0052] The impressed current cathodic protection and structural reinforcement system is located within the steel cage.
[0053] It is worth noting that in the prior art, when using seawater and sea sand, the seawater is usually first desalinated, the sea sand is purified, and then the desalinated seawater and purified sea sand are used to make concrete. In addition, rust inhibitors are added and the surface coating of the steel bars is applied to prevent chloride ion corrosion. In the present application, the seawater and sea sand concrete layer refers to a concrete structure formed using undesalinated seawater and / or unpurified sea sand as raw materials. It should be noted that the undesalinated seawater and unpurified sea sand in the present application can be used directly as raw materials. For example, cement is added to unpurified sea sand and then undesalinated seawater is added to form seawater and sea sand concrete. Since the seawater and sea sand concrete layer is made using undesalinated seawater and / or unpurified sea sand, there are harmful media such as chlorides and sulfates inside the seawater and sea sand concrete layer. It should be noted that when preparing FRP tube steel bar combination ICCP-SS seawater sea sand concrete composite beams, the present application needs to use a power supply to connect the carbon fiber cloth and the steel cage, and perform protective treatment on the steel cage to remove harmful media, thereby actively intervening in the corrosion of the steel cage in the seawater sea sand concrete layer rich in harmful media. The present application utilizes the dual functions of structural reinforcement and cathodic protection of the impressed current cathodic protection and structural reinforcement system, and applies it to reinforced seawater sea sand concrete composite beams. Even when the seawater sea sand concrete layer is rich in harmful media or the external environment is harsh, the steel bars can be adequately protected. The steel cage refers to a cage structure formed by tying steel bars.
[0054] An impressed current cathodic protection and structural reinforcement (ICCP-SS) system based on carbon fiber-FRP composite rectangular tube 8 is adopted, with carbon fiber-FRP composite rectangular tube 8 as anode and steel cage as cathode. The steel bars in the seawater and sea sand concrete composite beam are protected by impressed current, which can prevent and delay the corrosion of the steel bars.
[0055] The length of the carbon fiber cloth 1 is the same as that of the FRP rectangular tube 2, and the width of the carbon fiber cloth 1 needs to be greater than the perimeter of the cross section of the FRP rectangular tube 2, that is, the carbon fiber cloth 1 can completely cover the four sides of the FRP rectangular tube 2. The carbon fiber cloth 1 used in the carbon fiber-FRP composite rectangular tube 8 is preferably an orthogonal bidirectional cloth, and the carbon fiber content can be adjusted according to actual needs.
[0056] The carbon fiber cloth 1 can be pasted on the FRP rectangular tube 2. During the pasting process, attention should be paid to the amount of epoxy resin adhesive. After the carbon fiber cloth 1 is pasted, the outer surface should not be covered by the epoxy resin adhesive so that the carbon fiber fibers are fully exposed. In other words, the carbon fiber fibers in the carbon fiber cloth 1 can fully contact with the reinforced seawater and sea sand concrete composite beam.
[0057] In a preferred implementation of the embodiment of the present invention, Figure 1-Figure 3 As shown, the steel cage comprises:
[0058] Longitudinal reinforcement 6;
[0059] A plurality of stirrups 3 are provided on the longitudinal reinforcement 6 and arranged along the length direction of the longitudinal reinforcement 6 .
[0060] Specifically, the longitudinal reinforcement 6 is extended along the length direction of the reinforced seawater and sea sand concrete composite beam, and there may be one or more longitudinal reinforcements 6, such as Figure 3 As shown, three longitudinal steel bars 6 are used. A plurality of stirrups 3 are arranged along the length direction of the longitudinal steel bars 6 , and the longitudinal steel bars 6 are located inside the stirrups 3 and connected to the stirrups 3 .
[0061] In a preferred implementation of the embodiment of the present invention, Figure 1-Figure 2 As shown, the distance between the four sides of the FRP rectangular tube 2 and the stirrups 3 is not less than 30 mm.
[0062] Specifically, the cross-sectional height of the FRP rectangular tube 2 should be less than the height of the stirrup 3 of the composite beam, and the cross-sectional width of the FRP rectangular tube 2 should be less than the width of the stirrup 3 of the composite beam. Then the stirrup 3 can be set outside the FRP rectangular tube 2. In order to ensure that the thickness of the reinforced seawater sea sand concrete layer 5 is relatively uniform, the distance between the four sides of the FRP rectangular tube 2 and the stirrup 3 is not less than 30 mm.
[0063] In a preferred implementation of the embodiment of the present invention, Figure 3As shown, a plurality of holes 10 are provided on the side of the impressed current cathodic protection and structural reinforcement system, the diameter of the hole 10 is 1 / 3-2 / 3 of the height of the FRP rectangular tube 2, and the spacing between two adjacent holes 10 is 1 / 2-3 / 2 of the height of the FRP rectangular tube 2.
[0064] Specifically, in order to increase the connection between the impressed current cathodic protection and structural reinforcement system and the reinforced seawater and sea sand concrete composite beam, a hole 10 is set on the side of the impressed current cathodic protection and structural reinforcement system. When the reinforced seawater and sea sand concrete composite beam is formed, the seawater and sea sand concrete layer 5 can be filled into the hole 10, and relative sliding is difficult to occur between the impressed current cathodic protection and structural reinforcement system and the reinforced seawater and sea sand concrete composite beam.
[0065] Specifically, since the hole 10 is connected to the central channel of the FRP rectangular tube 2, when forming the reinforced seawater sea sand concrete composite beam, in order to prevent the seawater sea sand concrete layer 5 from flowing into the central channel of the FRP rectangular tube 2 from the hole 10, a filler 7 is placed in the central channel of the FRP rectangular tube 2, and the seawater sea sand concrete layer 5 only fills the hole 10 to form a shear key protrusion, which is used to strengthen the integrity of the FRP rectangular tube 2 and the seawater sea sand concrete layer. The filler 7 can be made of wood, foam or a small-section FRP rectangular tube, and the filler 7 is taken out after the casting of the reinforced seawater sea sand concrete composite beam is completed. The filler 7 needs to reserve the thickness of the shear key protrusion, which should be greater than or equal to 10 mm, and the thickness is also greater than or equal to the thickness of the composite rectangular tube.
[0066] To ensure that the hole 10 does not affect the strength of the impressed current cathodic protection and structural reinforcement system, the diameter of the hole 10 is 1 / 3-2 / 3 of the height of the FRP rectangular tube 2, and the spacing between two adjacent holes 10 is 1 / 2-3 / 2 of the height of the FRP rectangular tube 2.
[0067] The carbon fiber-FRP composite rectangular tube 8 in the present invention serves as a novel impressed current cathodic protection and structural reinforcement (ICCP-SS) system, playing the dual role of preventing and delaying steel corrosion and strengthening against bending and shearing.
[0068] In a preferred implementation of the embodiment of the present invention, the FRP rectangular tube 2 is selected from one of glass fiber FRP rectangular tube (GFRP), carbon fiber FRP rectangular tube (CFRP), aramid fiber FRP rectangular tube (AFRP), and basalt FRP rectangular tube (BFRP).
[0069] Specifically, the FRP rectangular tube 2 can be made of various existing FRP pultruded or wound rectangular tubes.
[0070] In a preferred implementation of the embodiment of the present invention, both ends of the FRP rectangular tube 2 extend outside the reinforced seawater and sea-sand concrete composite beam.
[0071] Specifically, both ends of the FRP rectangular tube 2 should extend beyond both ends of the composite beam by at least 10 mm.
[0072] In a preferred implementation of the embodiment of the present invention, the thickness of the FRP rectangular tube 2 is 3-15 mm. Specifically, the thickness of the FRP rectangular tube 2 can be set as required.
[0073] In a preferred implementation of the embodiment of the present invention, Figure 4 As shown, a conductive sheet 11 is disposed outside the carbon fiber cloth 1 , and the conductive sheet 11 is connected to the FRP rectangular tube 2 .
[0074] Specifically, the conductive sheet 11 is used to connect the anode of the power supply. The conductive sheet 11 needs to be in full contact with the carbon fiber cloth 1. The conductive sheet 11 can be a metal conductive sheet, specifically a non-corrosive metal conductive sheet. The conductive sheet 11 is connected to the FRP rectangular tube 2 by bolts 12. The width of the conductive sheet 11 is the same as the length of the FRP rectangular tube 2 extending outside the reinforced seawater sea sand concrete composite beam, that is, the two ends of the FRP rectangular tube 2 extending outside the reinforced seawater sea sand concrete composite beam are connected to the conductive sheet 11.
[0075] The present invention provides a carbon fiber veneer FRP pipe-steel combined seawater and sea sand concrete composite beam, which has the following beneficial effects compared with the prior art:
[0076] The present invention utilizes seawater sand to replace increasingly depleted resources such as freshwater river sand, and fully utilizes the abundant seawater sand resources in coastal areas for the casting of prefabricated composite beams of reinforced concrete structures, thereby reducing material transportation costs, greatly improving the utilization efficiency of seawater sand resources, playing a positive role in protecting the ecological environment, and having great social and economic benefits.
[0077] The present invention adopts an ICCP-SS system based on a carbon fiber-FRP composite rectangular tube, with the carbon fiber-FRP composite rectangular tube 8 as an anode and a steel bar as a cathode, and protects the steel bars in the seawater and sea sand concrete composite beam by applying an external current, thereby preventing and delaying the corrosion of the steel bars.
[0078] The carbon fiber-FRP composite rectangular tube 8 used in the present invention can provide structural reinforcement to compensate for and improve the loss of mechanical properties of the composite beam caused by steel bar corrosion, and has better mechanical properties and durability than traditional seawater and sea sand concrete structures.
[0079] Based on the FRP tube steel bar combination ICCP-SS seawater sea sand concrete composite beam described in any of the above embodiments, the present invention also provides a preferred embodiment of a method for preparing a FRP tube steel bar combination ICCP-SS seawater sea sand concrete composite beam:
[0080] The method for preparing the FRP tube steel bar combined ICCP-SS seawater and sea sand concrete composite beam according to the embodiment of the present invention comprises the following steps:
[0081] Step S100, providing a composite beam mold, fillers, seawater and sea sand concrete, a steel cage, a carbon fiber cloth 1 and an FRP rectangular tube 2.
[0082] Specifically, the cross-sectional height of the FRP tube steel bar composite ICCP-SS seawater sea sand concrete composite beam is 300 mm, the cross-sectional width is 200 mm, and the length is 3 m. According to the cross-sectional size and length of the composite beam, the cross-sectional size of the FRP rectangular tube 2 is determined to be 100 mm*50 mm*10 mm and the length is 3.03 m. The FRP rectangular tube 2 adopts a GFRP pultruded profile. According to the cross-sectional size and length of the FRP rectangular tube 2, a whole piece of bidirectional woven carbon fiber cloth 1 is cut, the carbon fiber content of the woven bundle is 3K, and its width and length are 300 mm and 3.03 m respectively.
[0083] Step S200: Wrap the carbon fiber cloth and stick it on the outside of the FRP rectangular tube to form an impressed current cathodic protection and structural reinforcement system.
[0084] Specifically, the cross-sectional dimensions and length of the FRP rectangular tube 2 are determined according to the cross-sectional dimensions and the dimensions of the stirrups 3 of the FRP tube steel bar combination ICCP-SS seawater sea sand concrete composite beam; the whole piece of bidirectional woven carbon fiber cloth 1 is cut according to the cross-sectional dimensions and length of the FRP rectangular tube 2. The carbon fiber cloth 1 is pasted on the outer surface of the FRP rectangular tube 2 using ordinary epoxy resin adhesive; after pasting, the carbon fiber cloth 1 is cured according to the standard curing time of the epoxy resin adhesive used to form an impressed current cathodic protection and structural reinforcement system (i.e., carbon fiber-FRP composite rectangular tube 8). During the pasting process, attention should be paid to the amount of epoxy resin adhesive used, and the epoxy resin adhesive should be avoided on the outer surface of the carbon fiber cloth 1 after pasting, so that the carbon fiber fibers are fully exposed.
[0085] Step S300: placing the filler into the FRP rectangular tube, placing the impressed current cathodic protection and structural reinforcement system in the steel cage, and placing them together into the composite beam mold.
[0086] Specifically, holes 10 are provided on the side of the impressed current cathodic protection and structural reinforcement system, and the side wall of the cured carbon fiber-FRP composite rectangular tube 8 is opened to strengthen the integrity of the carbon fiber-FRP composite rectangular tube 8 and the subsequently poured seawater and sea sand concrete layer 5. The diameter of the hole 10 on the side of the carbon fiber-FRP composite rectangular tube 8 is 40mm, and the spacing between the holes 10 is 100mm. A whole piece of filler 7 is added to the inside of the opened carbon fiber-FRP composite rectangular tube 8 to prevent concrete from leaking from the air during the pouring process. The filler 7 is made of plastic foam with a cross-section of 30mm*80mm.
[0087] According to the relative position of the carbon fiber-FRP composite rectangular tube 8 in the composite beam, rectangular grooves are opened on the side molds 9 at both ends of the composite beam mold 4, corresponding to the size of the carbon fiber-FRP composite rectangular tube 8; the carbon fiber-FRP composite rectangular tube 8 is placed inside the steel cage formed by binding the stirrups 3 and the longitudinal steel bars 6 of the composite beam; after the side molds 9 at both ends of the composite beam mold 4 are put on the two ends of the carbon fiber-FRP composite rectangular tube 8, the steel cage and the carbon fiber-FRP composite rectangular tube 8 are placed in the composite beam mold 4 with the release agent brushed on the inner surface; according to the design, pads are placed on the bottom and side of the steel cage to fix the position of the steel cage, and the position of the composite rectangular tube is determined by the position of the rectangular groove on the side mold 9 and the position of the pad. Circular grooves can also be opened on the side mold 9, corresponding to the size of the longitudinal steel bars 6, and the circular grooves can be passed through by the longitudinal steel bars 6.
[0088] Step S400: pouring the seawater and sea-sand concrete into the composite beam mold and solidifying it to form a reinforced seawater and sea-sand concrete composite beam.
[0089] The seawater and sea-sand concrete is poured into the composite beam mold 4, and after the seawater and sea-sand concrete is solidified, a reinforced seawater and sea-sand concrete composite beam is formed.
[0090] Step S400 specifically includes:
[0091] Step S410: using a layered pouring and vibrating method, pouring the seawater and sea sand concrete into the composite beam mold and smoothing it, roughening it with a rough steel brush and performing a curing treatment to obtain a reinforced seawater and sea sand concrete composite beam.
[0092] Specifically, the mixed seawater and sea sand concrete is poured onto the top surface of the composite beam mold 4, and the pouring adopts the method of layered pouring and layered vibration; after pouring, the top surface of the composite beam is smoothed, and roughened with a coarse steel brush before initial setting, and the mold is removed after curing; at the same time, the filler 7 is removed; and then the composite beam is regularly watered and cured to a specified age of 28 days, thereby completing the production of the carbon fiber-FRP composite rectangular pipe-reinforced seawater and sea sand concrete composite beam.
[0093] Step S500, dismantling the composite beam mold, connecting the carbon fiber cloth and the steel cage with a power supply to protect the steel cage, and obtaining an FRP tube steel bar combined ICCP-SS seawater sand concrete composite beam.
[0094] Specifically, after demoulding, the conductive sheet 11 is installed at the end of the carbon fiber-FRP composite rectangular tube 8. The specific operation method is: open a hole around the exposed part of the carbon fiber-FRP composite rectangular tube 8. Bolt holes; drill holes at corresponding positions of two L-shaped stainless steel conductive sheets with a cross-section of 100mm*50mm*3mm and a width of 15mm, and weld power-carrying wires on the two conductive sheets 11; tighten the bolts 12 to press the conductive sheets 11 against the outer surface of the carbon fiber-FRP composite rectangular tube 8, so that the conductive sheets 11 are in full contact with the carbon fiber cloth 1; weld the power-carrying wires at the ends of the longitudinal steel bars 6 of the composite beam; connect the steel bar wires and the wires welded on the conductive sheets 11 to the cathode and anode of a DC power supply, respectively, and apply a strength of 10mA / m 2 The DC current can realize impressed current cathodic protection and prevent and delay steel corrosion.
[0095] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A FRP tube steel bar combined ICCP-SS seawater sand concrete composite beam, It is characterized in that include: An impressed current cathodic protection and structural reinforcement system and a reinforced seawater and sea-sand concrete composite beam wrapped outside the impressed current cathodic protection and structural reinforcement system; The side of the impressed current cathodic protection and structural reinforcement system is provided with a plurality of holes; The impressed current cathodic protection and structural reinforcement system comprises: FRP rectangular tube; Carbon fiber cloth, wrapped outside the FRP rectangular tube; The reinforced seawater and sea sand concrete composite beam comprises: Seawater and sea sand concrete layer; A steel cage is embedded in the seawater and sea sand concrete layer; The impressed current cathodic protection and structural reinforcement system is located within the steel cage; The steel cage comprises: Longitudinal reinforcement; A plurality of stirrups are provided on the longitudinal steel bars and arranged along the length direction of the longitudinal steel bars; The distance between the four sides of the FRP rectangular tube and the stirrups is not less than 30 mm; the hole is connected to the central channel of the FRP rectangular tube, and the seawater sand concrete layer fills the hole to form a shear key protrusion; Both ends of the FRP rectangular tube extend to the outside of the reinforced seawater and sea-sand concrete composite beam, a conductive sheet is arranged outside the carbon fiber cloth, the conductive sheet is connected to the FRP rectangular tube, and both ends of the FRP rectangular tube extend to the outside of the reinforced seawater and sea-sand concrete composite beam and are connected to the conductive sheet.
2. The FRP tube steel bar combined ICCP-SS seawater and sea sand concrete composite beam according to claim 1, It is characterized in that Side molds are arranged at both ends of the FRP rectangular tube.
3. The FRP tube steel bar combined ICCP-SS seawater and sea sand concrete composite beam according to claim 1, It is characterized in that The diameter of the hole is 1 / 3-2 / 3 of the height of the FRP rectangular tube, and the distance between two adjacent holes is 1 / 2-3 / 2 of the height of the FRP rectangular tube.
4. The FRP tube steel bar combined ICCP-SS seawater and sea sand concrete composite beam according to claim 1, It is characterized in that The FRP rectangular tube is selected from one of a glass fiber FRP rectangular tube, a carbon fiber FRP rectangular tube, an aramid fiber FRP rectangular tube, and a basalt FRP rectangular tube.
5. The FRP tube steel bar combined ICCP-SS seawater and sea sand concrete composite beam according to claim 1, It is characterized in that The thickness of the FRP rectangular tube is 3-15 mm.
6. A method for preparing the FRP tube steel bar composite ICCP-SS seawater and sea sand concrete composite beam according to any one of claims 1 to 5, It is characterized in that Includes steps: Provide composite beam molds, fillers, seawater and sea sand concrete, steel cages, carbon fiber cloth and FRP rectangular tubes; Wrapping and pasting the carbon fiber cloth on the outside of the FRP rectangular tube to form an impressed current cathodic protection and structural reinforcement system; Put the filler into the FRP rectangular tube, then place the impressed current cathodic protection and structural reinforcement system in the steel cage, and put them into the composite beam mold together; pouring the seawater and sea sand concrete into the composite beam mold and solidifying it to form a reinforced seawater and sea sand concrete composite beam; The composite beam mold is removed, and the carbon fiber cloth and the steel cage are connected by a power supply to protect the steel cage, thereby obtaining an FRP tube steel bar composite ICCP-SS seawater and sea sand concrete composite beam.
7. The method for preparing the FRP tube steel bar combined ICCP-SS seawater and sea sand concrete composite beam according to claim 6, It is characterized in that The method of pouring the seawater-sand concrete into the composite beam mold and solidifying it to form a reinforced seawater-sand concrete composite beam comprises: The seawater-sand concrete is poured into the composite beam mold by a layered pouring and vibrating method, and then smoothed. A rough steel brush is used to roughen the concrete and the concrete is cured to obtain a reinforced seawater-sand concrete composite beam.
Citation Information
Patent Citations
FRP-RC (fiber reinforced polymer-reinforced concrete) combined beam partially constrained by fiber sleeve and construction method of combined beam
CN103195211A
Sea sand concrete bending member
CN104018620A
Reinforced concrete cathode protection method and device of CFRP anode
CN106283071A
CFRP-embedded-anode reinforcing-steel-bar-concrete cathode protection method and device
CN106283072A
Hybrid FRP (Fiber Reinforced Plastics)-steel composite bar sea sand concrete beam
CN107217786A