PTC planar heating element and method for manufacturing the same
By using flexible contact structures of aqueous polymer materials and conductive clip spacers, the thinness and environmental protection problems in the manufacturing process of PTC surface heating bodies are solved, the annealing time is shortened, and the production efficiency of PTC surface heating bodies is improved. Cost-effective.
Patent Information
- Application Number
- CN202110002242.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-05
- Filing Date
- 2021-01-04
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-01-04
AI Technical Summary
During the manufacturing process of the existing PTC surface heating body, it is difficult to make an extruded resistor as thin as a film, the coating resistor needs solvent adjustment, and the long annealing process time leads to low production efficiency and high cost. The problem.
The aqueous polymer material is used to replace the organic solvent, and the PTC resistor is configured in the insulating coating body and the flexible contact is achieved using conductive clip spacers to shorten the annealing time and improve the PTC characteristics.
It realizes thin flexibility and environmentally friendly PTC surface heating body, shortens the annealing time, improves production efficiency and cost-effectiveness.
Smart Images

Figure CN113225852B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a PTC planar heating element. Background Art
[0002] PTC (positive temperature coefficient) resistors, which have a rapid increase in resistance near the Curie temperature and thus have a self-control temperature function when powered on, have long been known in the fields of ceramic materials, polymer materials, etc. For example, it is known that a base polymer is composed of polyethylene or various elastomers, and materials such as carbon black, graphite, metal powder, wax, and adhesive are dispersed in an organic solvent to prepare a PTC coating, and the PTC coating is printed on a polymer film, etc., thereby forming a PTC resistor composed of a polymer material. Such a PTC resistor is used to make a PTC planar heating element. In addition, as another form, it is known that the above materials are mixed without using an organic solvent, and extruded into a linear or sheet shape together with an electrode wire to form a PTC heating element.
[0003] Figure 7 2 shows a general structure of a conventional PTC planar heating element 70d formed of a polymer material. Figure 7 The PTC planar heating element 70 shown is manufactured, for example, in the following manner. A pair of comb-shaped electrodes 61 and 62 are formed on the surface of a substrate 60 such as a polyester film by printing a solvent-based silver paste or the like. PTC coating 63 is printed on the comb teeth of the comb-shaped electrodes 61 and 62 to form a PTC resistor in a surface-exposed state. The surface of the PTC resistor exposed on the surface is covered with a polyester film 64 laminated with a hot-melt adhesive resin such as modified polyethylene. Through overall heat pressing, the hot-melt adhesive resin melts, and the upper and lower polyester films are firmly bonded to form a PTC planar heating element with a structure that ensures waterproofness and insulation. Power lines are connected to both ends of the common electrode portion of the comb-shaped electrodes 61 and 62, and the PTC planar heating element 70 functions as a heating element capable of self-controlling temperature by being energized.
[0004] PTC planar heating elements with other structures are also known. For example, the following structure has been proposed: a PTC coating is printed on the surface of a polyester woven or non-woven fabric, and a pair of electrode bodies are sandwiched from the inside and outside by a polyester film laminated with an adhesive, and these are sealed by heat pressing.
[0005] In addition, among the various PTC planar heating elements made of polymer materials, whether it is a planar heating element formed by a solvent-based PTC coating or a linear or planar heating element formed by non-solvent-based extrusion molding, a process of stabilizing the characteristics is required during the manufacturing process. That is, the following process is required: after the heating element is completed, the annealing process is repeated for several hours at a high temperature of more than 100°C.
[0006] The advantages of the various PTC planar heating elements formed using existing polymer materials listed above are as follows.
[0007] (1) It is possible to utilize existing conventional materials, equipment, and processes to easily construct a production line.
[0008] (2) Since PTC coating or kneaded material can be used, printing or extrusion molding can be used, the degree of freedom in productization is high.
[0009] (3) The PTC characteristics of the PTC resistor are relatively slow near the softening point of the base polymer, but near the melting point, the expansion and contraction between carbon particles is large, showing a sharp PTC characteristic.
[0010] The PTC planar heating element described above is recorded in, for example, Japanese Patent Publication No. 44-3826, Japanese Patent Publication No. 59-2693, Japanese Patent Application Publication No. 56-13689, Japanese Patent Application Publication No. 61-181859, Japanese Patent Application Publication No. 63-265961, Japanese Patent Application Publication No. 04-306582, Japanese Patent Application Publication No. 05-152056, Japanese Patent Application Publication No. 2001-076848, Japanese Patent Application Publication No. 2005-150663, Japanese Patent Application Publication No. 2009-193904, and Japanese Patent Application Publication No. 2010-244971. Summary of the invention
[0011] An object of the present invention is to provide an excellent PTC planar heating element.
[0012] According to one embodiment of the present invention, the PTC planar heating element includes: an insulating first covering material; an insulating frame fixed to the peripheral portion of the first covering material 1; an insulating second covering material fixed to the frame in a manner opposite to the first covering material 1 at a predetermined interval therebetween with the aid of the frame; a PTC resistor that can be telescopically arranged in an internal space formed by the first covering material, the frame and the second covering material; a pair of conductive spacers that are arranged in contact with the PTC resistor on a side of the internal space that is closer to the second covering material than the PTC resistor; and a pair of electrodes that are arranged in a manner such that at least a portion of each electrode is in contact with the corresponding conductive spacer between the conductive spacer and the second covering material, thereby making flexible contact with the PTC resistor with the aid of the conductive spacer.
[0013] According to the present invention, an excellent PTC planar heating element can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 1 is a diagram schematically showing a configuration example of a PTC planar heating element according to the present embodiment, and is a diagram showing a state in which the PTC planar heating element is viewed from above.
[0015] Figure 2A This is a diagram showing a disassembled PTC planar heating element, in which a frame is placed on an insulating first covering material, a PTC resistor is arranged in a recess formed by the frame, and a pair of conductive spacers are arranged at both ends.
[0016] Figure 2B It is a figure which shows the state which disassembled the PTC planar heating element, and it is a figure which shows the insulating frame for lifting.
[0017] Figure 2C The figure shows a state where the PTC planar heating element is disassembled, and shows a state where a pair of electrodes are arranged on a second insulating covering material.
[0018] Figure 3 It is shown along Figure 1 Schematic diagram showing a schematic cross section of a PTC planar heating element taken along line III-III shown.
[0019] Figure 4 1 is a graph showing the measurement results of the PTC characteristics according to Examples 1, 2, 3 and Comparative Example 1.
[0020] Figure 5 It is a graph showing the measurement results of the PTC characteristics according to Example 4 and Comparative Examples 2 and 3.
[0021] Figure 6 It is a graph showing the Ra change rate according to Example 1 and Comparative Example 4 with respect to the number of measurement days.
[0022] Figure 7 This is a diagram showing a general structure of a conventional PTC planar heating element formed of a polymer material. DETAILED DESCRIPTION
[0023] An embodiment of the present invention is described with reference to the accompanying drawings. The present embodiment relates to a PTC planar heating element. In a PTC planar heating element, a solvent-based PTC coating is generally used. In contrast, in the PTC planar heating element of the present embodiment, a water-based PTC coating is used. In addition, the PTC planar heating element of the present embodiment has a structure that can exhibit excellent characteristics even when a water-based PTC coating is used.
[0024] Various PTC planar heating elements known in the art have excellent PTC characteristics and are easy to construct production lines for. However, they have the following problems.
[0025] (1) It is difficult to make an extruded PTC resistor as thin as a film, and its applications are limited.
[0026] (2) Although paint-type PTC resistors can be made thinner, they require the use of solvents to adjust the viscosity, which poses environmental problems.
[0027] (3) For products made of existing polymer materials, a long waiting time is required in the final annealing process, which significantly reduces production efficiency and easily increases costs.
[0028] For the PTC surface heating element of this embodiment, organic solvents, which have been increasingly restricted in recent years for environmental reasons, are not used, but water-based polymer materials are used. Even so, the PTC surface heating element has sensitive PTC characteristics. In addition, for the PTC surface heating element of this embodiment, the annealing time in the final process, which is believed to be caused by the inherent properties of the constituent materials of the PTC resistor using existing polymer materials, is greatly shortened. As a result, the PTC surface heating element of this embodiment has good mass producibility and is inexpensive.
[0029] Figure 1 1 is a diagram schematically showing a configuration example of the PTC planar heating element 10 according to the present embodiment, and is a diagram showing a state in which the PTC planar heating element 10 is viewed from above. Figure 2A to Figure 2C The figure shows a state where the PTC planar heating element 10 is disassembled. Figure 3 It is shown along Figure 1 The schematic diagram of the cross section of the PTC planar heating element 10 taken along line III-III is shown.
[0030] [Overview of the structure of the PTC planar heating element]
[0031] The structure of the PTC planar heating element 10 is briefly described. The PTC planar heating element 10 includes a PTC resistor 4 as a heating element. The PTC resistor 4 includes: a coating substrate 3a, and a PTC coating film 3b formed by coating a water-based PTC coating on the coating substrate 3a. In the PTC planar heating element 10, the PTC resistor 4 is accommodated in the internal space of an insulating and flame-retardant coating. The coating has: a first coating material 1 and a second coating material 2 that are opposite to each other, and a frame 8 for adjusting the interval between the first coating material 1 and the second coating material 2. The PTC resistor 4 is arranged between the first coating material 1 and the second coating material 2 so as to be telescopically non-adhesive.
[0032] The PTC planar heating element 10 includes a pair of electrodes 5 for supplying power to the PTC resistor 4. The pair of electrodes 5 includes a first electrode 5a and a second electrode 5b. The first electrode 5a and the second electrode 5b are fixed to the second covering material 2. The first electrode 5a and the second electrode 5b are not directly connected to the PTC resistor 4. A first conductive spacer 6a is arranged between the first electrode 5a and the PTC resistor 4, and the first electrode 5a is connected to the PTC resistor 4 by means of the first conductive spacer 6a. A second conductive spacer 6b is arranged between the second electrode 5b and the PTC resistor 4, and the second electrode 5b is connected to the PTC resistor 4 by means of the second conductive spacer 6b. The first conductive spacer 6a and the second conductive spacer 6b are collectively referred to as conductive spacers 6.
[0033] [Details of each part]
[0034] Next, each part of the PTC planar heating element 10 will be described in detail.
[0035] 〈Structure of the coating〉
[0036] The first covering material 1, the second covering material 2 and the frame 8 constituting the covering body are formed of, for example, a flame-retardant polyester film. The first covering material 1 is a rectangular thin plate. The frame 8 is an insulating component fixed to the periphery of the first covering material 1. Figure 2B As shown, the frame 8 has an outer edge that is consistent with the outer edge of the first cladding material 1 and has a hollowed-out shape. Figure 2A As shown, the frame 8 is overlapped and bonded on the first covering material 1 in such a manner that the outer edges thereof are aligned. In this way, the peripheral edge of the first covering material 1 is raised by the frame 8. By stacking and fixing the second covering material 2 on the frame 8, a gap is provided between the first covering material 1 and the second covering material 2.
[0037] In order to raise the height, the adhesive for bonding the first covering material 1 and the second covering material 2 may be applied thickly to achieve the desired amount of raising. In this case, the adhesive functions as the frame 8. However, from the perspective of managing thickness, as shown in this embodiment, it is preferred to use the frame 8 made of the same material as the first covering material 1 and the second covering material 2. The first covering material 1 and the frame 8 may also be integrally molded.
[0038] On the inside of frame 8, as shown in Figure 2A and Figure 3 As described below, the PTC resistor 4 is stored in such a manner that the coated substrate 3a side is in contact with the first covering material 1 and the PTC coating film 3b is on the upper side. Figure 1 As shown, the second covering material 2 is a rectangular thin plate having longer long sides than the first covering material 1 and the frame 8. One end side of the second covering material 2 is arranged so as to protrude from the first covering material 1 and the frame 8.
[0039] The first covering material 1, the second covering material 2 and the frame 8, which function as insulating covering materials, need to ensure strength, insulation and flame retardancy. The first covering material 1, the second covering material 2 and the frame 8 can be a polymer film made of a polymer such as polyethylene, polypropylene, polyester, polyurethane, acrylic, nylon, vinyl chloride resin, etc. From the viewpoint of ensuring the adhesion, heat resistance and rigidity of the first covering material 1, the second covering material 2 and the frame 8, a polyester film is preferred. Moreover, for the first covering material 1, the second covering material 2 and the frame 8, even when the PTC resistor 4 wrapped therein expands and contracts, it is necessary to ensure the mechanical strength, heat resistance and flame retardancy as the outer covering layer, and it is also necessary to ensure dimensional stability. Therefore, it is preferred that: a flame retardant grade polyester film is hardened by crystallization treatment to improve the mechanical strength and heat resistance, and used as the first covering material 1, the second covering material 2 and the frame 8. Here, the crystallization treatment is performed by heating to a generally known crystallization temperature of polyester resin, that is, about 130° C. or higher, preferably 140° C. or higher, and then slowly cooling.
[0040] 〈PTC resistor structure〉
[0041] (Coating substrate)
[0042] A conventional polymer film can be used as the coating substrate 3a of the PTC resistor 4. As conventional polymer films, films made of polyethylene, polypropylene, polyester, polyurethane, acrylic, nylon, vinyl chloride resin, etc. are widely known. Among these conventional polymer films, it is particularly preferable to use a heat-resistant and inexpensive polyester film as the coating substrate 3a.
[0043] As reasons for particularly selecting a conventional polyester film from among numerous polymer films, the following reasons can be cited. The PTC resistor 4 of the present embodiment is made using a water-based PTC coating. When the water-based PTC coating forms the PTC resistor 4 after drying, the expansion and contraction caused by heat must be large. Therefore, the PTC coating cannot contain a large amount of materials with strong adhesive curing properties. Therefore, the adhesion of the PTC coating to the substrate is weak. For polyester film, sufficient adhesion with such a PTC coating can be ensured by simple surface activation treatment such as corona discharge. Moreover, the polyester film has a certain degree of rigidity and heat resistance, and the expansion and contraction caused by heat is large. In addition, polyester film is a conventional and inexpensive material.
[0044] The polyester film has the property of strongly showing the thermal history as described below. For conventional polyester film substrates, during the heating and cooling in the manufacturing process of the PTC planar heating element 10, or during the energized heating and cooling when working as a product, for example, according to the history of tensile stress in the manufacturing stage of the coated substrate 3a monomer such as biaxial stretching, it has the property of arbitrarily repeating expansion and contraction in the vertical and horizontal directions. The moderate rigidity and expansion and contraction of the coated substrate 3a will increase the expansion and contraction of the PTC coating film 3b. As a result, even if the PTC resistor 4 uses a water-based PTC coating, the expansion and contraction between the carbon particles in the PTC coating film 3b is also increased, showing sensitive PTC characteristics.
[0045] (PTC coating film)
[0046] The PTC coating film 3b of the PTC resistor 4 of the present embodiment is produced using a water-based PTC paint containing, for example, a water-based carbon paste, a polyurethane emulsion binder, a wax emulsion, and boric acid.
[0047] Aqueous carbon paste is an aqueous dispersion made by dispersing carbon black with a dispersant. Such carbon pastes are widely sold as antistatic products and electromagnetic wave shielding products. Among carbon pastes, there are anionic carbon pastes, cationic carbon pastes, and non-ionic carbon pastes as ionic products. According to preliminary experiments, the order of excellent PTC characteristics is: anionic > non-ionic > cationic. Therefore, it is preferred to use anionic carbon paste, but it is not limited to this.
[0048] Known water-based adhesives include acrylic, urethane, phenol, epoxy, etc. From the viewpoint of flexibility and elasticity of the coating film after drying, polyurethane emulsion adhesives are preferred, but the present invention is not limited to these.
[0049] As wax emulsions, well-known ones include paraffin wax, polyethylene wax, polypropylene wax, amide wax, etc., and ionic products include anionic, cationic, and nonionic products. From preliminary experiments, it is known that a product obtained by properly mixing paraffin wax and polyethylene wax emulsions has excellent PTC characteristics. Therefore, paraffin wax and polyethylene wax emulsions are preferably used, but are not limited to this.
[0050] Generally speaking, for a mixed coating made by mixing water-based carbon paste, polyurethane emulsion adhesive and wax emulsion, when it is directly dried, the components soften and become fluid in each cycle of measuring heating and power-on heating. Therefore, when cooling, the carbon particles in the mixed coating are prone to agglomeration. As a result, the room temperature resistance value increases and the maximum resistance value decreases, etc., which reduces the PTC characteristics.
[0051] In order to suppress fluidity, a crosslinking agent is generally used. In the case of water-based paint, there are the following problems.
[0052] (1) Generally, a crosslinking agent is a hydrophobic polymer powder or liquid. When such a crosslinking agent is added to a water-based PTC coating, it is poorly dispersed and uniform crosslinking cannot be expected.
[0053] (2) Although there are water-based crosslinking agents, they are either expensive or require ultraviolet irradiation, and therefore have poor mass productivity.
[0054] (3) Generally speaking, the reaction temperature of the crosslinking agent is relatively high, 100° C. or higher. At high temperatures, this will cause thermal deformation of the base material of the PTC resistor and deterioration of the components of the PTC coating. Therefore, it is difficult to use such a crosslinking agent.
[0055] For this purpose, not only the cross-linking of carbon paste was investigated, but also various materials that can be expected to have a curing effect on the mixed coating, including the cross-linking of other constituent materials. Among them, preliminary experiments were conducted with a view to boric acid, which is known to have the effect of cross-linking substances through hydrogen bonds. As a result, it was found that: using boric acid, the above-mentioned PTC coating has a curing effect at room temperature and has a viscosity adjustment effect. For this reason, boric acid was selected as a substance that can inhibit the flow and agglomeration of carbon particles in the PTC coating. Since the material of the PTC coating is water-based, the water-soluble boric acid can be directly mixed in the form of a powder, or it can be dissolved in a small amount of hot water and then mixed. It should be noted that phosphoric acid has also been considered as a substance to replace boric acid, but it is not preferred because it will become a stronger acid.
[0056] 〈Electrical connection structure〉
[0057] On the inner side of the frame 8 between the first cladding material 1 and the second cladding material 2, as shown in FIG. Figure 2A and Figure 3 As shown, a PTC resistor 4 is accommodated, and the PTC coating film 3b is on the upper side in a manner that the coated substrate 3a side is in contact with the first coating material 1. In order not to hinder the expansion and contraction of the PTC resistor 4 caused by heating and cooling, the PTC resistor 4 cannot be fixed to the first coating material 1 and the second coating material 2 covering it by an adhesive or the like. Moreover, with respect to the electrode that supplies power to the PTC resistor 4, if the coating film 3b is brought into direct contact with the metal electrode, the PTC resistor 4 formed of a polymer material is easily firmly bonded to the electrode due to the heating during the manufacturing process and the energizing action. Such a firm bond will hinder the expansion and contraction of the PTC resistor 4. In order to prevent the adhesion between the PTC resistor 4 and the electrode 5, in the PTC planar heating element 10 involved in the present embodiment, a flexible contact structure is formed between the PTC resistor 4 and the electrode 5 using a spacer having conductivity, elasticity, and lubricity.
[0058] That is, Figure 2A As shown, along the two sides opposite to the PTC resistor 4, the first conductive spacer 6a and the second conductive spacer 6b are respectively arranged at both ends of the PTC resistor 4. The first conductive spacer 6a and the second conductive spacer 6b are, for example, carbon nonwoven fabrics cut into elongated shapes.
[0059] As a means of achieving flexible contact between the PTC resistor 4 and the electrode 5, various structures can be considered. For example: a structure in which the coating layer of the coated wire is made conductive to achieve flexible contact; a structure in which a metal braid is used as an electrode body and it is used as both a component for achieving flexible contact and a component as an electrode; or a contact structure using a carbon long fiber bundle, etc. Among these, for the method of making the coating layer of the wire conductive, the wire-shaped electrode will become thicker and the thin advantage of the film heater will be lost, so this method is not preferred. For the method of using a metal braid, the metal braid will sink deeply into the PTC resistor 4 during heating, and there is a possibility that the PTC resistor 4 will be partially cut. In addition, since the metal braid is expensive, this method is not preferred. For the method of using a carbon long fiber bundle, the carbon long fiber bundle is extremely weak to bending. In addition, since the carbon long fiber bundle is expensive, this method is not preferred.
[0060] Therefore, the sheet-like formed product of conductive short fibers is focused on. That is, in the present embodiment, the sheet-like formed product of conductive short fibers is appropriately cut and used as a conductive spacer 6 with a flexible contact structure. As the sheet-like formed product of conductive short fibers, non-woven fabrics using copper fine wires or stainless steel fine wires can also be considered. However, for metal non-woven fabrics, there is a possibility that the metal non-woven fabrics may sink into the PTC resistor 4 when heated, thereby partially cutting the PTC resistor 4; even in the case of fibers, hard burrs are easily generated and the removal process is labor-intensive and expensive. For carbon non-woven fabrics formed from scraps of carbon long fibers, it is a cheap and preferred material when used as the conductive spacer 6 involved in the present embodiment.
[0061] On the surface of the second cladding material 2 opposite to the first cladding material 1, Figure 2A The first conductive spacer 6a and the second conductive spacer 6b are overlapped, as shown in FIG. Figure 2C As shown in FIG. 1 , a pair of first electrodes 5a and second electrodes 5b are attached. Figure 1 and Figure 2CAs shown, one end of the first electrode 5a and the second electrode 5b is longer than the first conductive spacer 6a and the second conductive spacer 6b, and is extended to the end of the second covering material 2 on the side extending from the first covering material 1 and the frame 8. In the portion of the first electrode 5a and the second electrode 5b extending from the first covering material 1 and the frame 8, the lead wire is connected to the first electrode 5a and the second electrode 5b.
[0062] For the first electrode 5a and the second electrode 5b, a copper foil tape with a non-solvent adhesive attached to one side is preferably used. Although silver paste is also considered, silver paste is solvent-based and expensive, so it is preferably not used. In contrast, a metal tape can be used as a suitable material. Among metal tapes, copper foil tape is widely used, cheap, and easy to obtain.
[0063] [Method for producing a PTC planar heating element]
[0064] The PTC planar heating element 10 of the present embodiment is manufactured as follows.
[0065] like Figure 2A As shown in FIG. 1 , a frame 8 is attached to the first covering material 1. For example, a modified silicone adhesive can be used to bond the first covering material 1 to the frame 8. The PTC resistor 4 is received in the recess formed by the first covering material 1 and the frame 8 with the PTC coating film 3b facing upward. Furthermore, conductive spacers 6 made of carbon nonwoven fabric cut into elongated shapes are disposed at both ends of the PTC resistor 4. Thus, the following is prepared: Figure 2A The first assembly 11 is shown.
[0066] like Figure 2C As shown, the electrode 5 is attached to the second coating material 2 to prepare the second assembly 12. The second assembly 12 is turned over and bonded to the first assembly 11. At this time, the bonding method of the second coating material 2 is as follows: the side of the electrode 5 that does not extend to the outer edge of the second coating material 2 is consistent with the outer edge of the frame 8. The peripheral portion of the second coating material 2 and the frame 8 are bonded and sealed by, for example, a modified silicone adhesive. At this time, the electrode 5 overlaps on the conductive spacer 6 and contacts the conductive spacer 6.
[0067] In this way, the end of the PTC resistor 4, the conductive spacer 6 of the carbon nonwoven fabric, and the electrode 5 of the copper foil tape are stacked. Due to the elasticity of the conductive spacer 6, mechanical and electrical flexible contact can be achieved. It should be noted that a thermally conductive sheet or a thermally conductive woven fabric of appropriate thickness can also be sandwiched in the gap between the PTC coating film 3b of the PTC resistor 4 and the second covering material 2.
[0068] [About PTC heating element]
[0069] According to the present embodiment, a PTC surface heating element 10 having sensitive PTC characteristics made of a water-based polymer material can be provided without using an organic solvent. Generally speaking, the density of the solute of a water-based paint is thinner than that of a solvent-based paint. For example, even if the water-based paint is directly applied to the outer shell to make a PTC surface heating element as with a solvent-based paint, the excellent PTC characteristics cannot be exerted. In contrast, in the present embodiment, by applying a water-based PTC paint to the coating substrate 3a, since the coating substrate 3a can expand the expansion and contraction of the PTC resistor 4 during heating and cooling, a PTC surface heating element 10 having sensitive PTC characteristics can be provided.
[0070] In the PTC planar heating element 10 of this embodiment, the PTC resistor 4 is not fixed to the housing. Although the thickness of the PTC planar heating element 10 is slightly increased by using a structure having a conductive spacer 6 and a flexible contact between the PTC resistor 4 and the electrode 5, the PTC resistor 4 is not bonded and fixed to any object. Therefore, the PTC resistor 4 has a large degree of freedom for expansion and contraction caused by heating and cooling, and as a result, the PTC planar heating element 10 has a sensitive PTC characteristic.
[0071] Generally speaking, when a solvent-based PTC coating is used, the resistance value of the PTC resistor may change due to repeated heating and cooling after assembly. Therefore, in order to produce a PTC planar heating element with stable performance, an annealing process of repeated heating and cooling is required after assembly, which takes a long time. In contrast, by utilizing the composition of the water-based PTC coating used for the PTC coating film 3b of this embodiment, the annealing time in the final process can be greatly shortened, and a PTC planar heating element 10 with good mass production performance and low cost can be provided.
[0072] By using a crystallized flame-retardant polyester film for the first covering material 1, the second covering material 2 and the frame 8, a PTC planar heating element 10 with minimal change in appearance can be provided even if the PTC resistor 4 expands and contracts due to heating and cooling.
[0073] It should be noted that the so-called "PTC resistor 4 is not bonded" also includes the following state: that is, although a part of it is bonded, the PTC resistor 4 is in a state where a large part is not bonded in a manner that can fully expand and contract to exert the PTC characteristics. In addition, in the above embodiment, the case where a water-based paint is used as the PTC paint is shown, but the structure of the above-mentioned PTC planar heating element 10 is also applicable to a PTC planar heating element using a solvent-based PTC paint.
[0074] The above-mentioned embodiment is only an example, and various modifications can be made thereto. Several modified examples can be given.
[0075] [First Modification]
[0076] In the above-mentioned embodiment, the electrode 5 is fixed to the second covering material 2. During manufacturing, the second assembly 12 in which the electrode 5 is fixed to the second covering material 2 is attached to the first assembly 11 including the first covering material 1, the frame 8, the PTC resistor 4 and the conductive spacer 6. However, this is not limited to this. The PTC planar heating element 10 can also be manufactured by, for example, the following method.
[0077] Similar to the above-mentioned embodiment, a frame 8 is attached to the first covering material 1, and the PTC resistor 4 is accommodated in the recess formed by the first covering material 1 and the frame 8 with the PTC coating film 3b facing upward. The conductive spacer 6, such as a carbon non-woven fabric cut into elongated pieces, and the electrode 5, such as a copper foil, are temporarily fixed in advance using a PTC paint or a conductive paint, and the conductive spacer 6 and the electrode 5 are arranged at both ends of the PTC resistor 4. Afterwards, the second covering material 2 is bonded to the frame 8 in a manner covering the recess. In this case, the electrode 5 may be fixed to the second covering material 2 using an adhesive or the like, or may not be fixed to the second covering material 2. That is, in the completed PTC planar heating element 10, the electrode 5 may not be fixed to the second covering material 2.
[0078] Alternatively, the conductive spacer 6 and the electrode 5 may be temporarily fixed on the second covering material 2 with PTC paint or conductive paint in advance, and the second covering material 2 may be bonded to the frame 8 in such a manner that the conductive spacer 6 contacts the PTC resistor 4 and covers the recess. In addition, in all the above-mentioned embodiments and variations, the lower covering material with the recess may be formed by attaching the frame 8 to the first covering material 1, or may be integrally formed, or may be formed by a thickly applied adhesive, etc. In any case, the lower covering material has a structure in which a frame is fixed to the peripheral portion of the first covering material.
[0079] Thus, in the manufacture of the PTC planar heating element 10, an insulating lower covering material having a concave portion is prepared, and a PTC resistor 4 is arranged in the concave portion of the lower covering material. Thereafter, a pair of conductive spacers 6 in contact with the PTC resistor 4 and a pair of electrodes 5 in contact with the pair of conductive spacers 6 are arranged on the PTC resistor 4, and a second covering material 2 fixed on the lower covering material is arranged in a manner covering the concave portion. Thus, a PTC planar heating element 10 having the functions described in the above-mentioned embodiment can be manufactured.
[0080] [Second Modification]
[0081] As a finished PTC heater, flexibility is sometimes required. In order to adapt to these uses, polyester fabric can be used instead of film for the first covering material 1, the second covering material 2, the coating substrate 3a and the frame 8. Here, for the first covering material 1 and the second covering material 2, in order to enhance the insulation and waterproof properties, a polyester fabric with a resin-coated outer surface can be used. Such a PTC planar heating element can have good PTC characteristics, softness and flexibility. In such a PTC planar heating element, when bonding the first covering material 1, the second covering material 2 and the frame 8, an adhesive that is also soft after bonding can be used. It should be noted that there are known PTC planar heating elements using polyester fabrics and non-woven fabrics as substrates, but these PTC performance materials still use existing types of polymer materials. In this case, the aforementioned problems exist.
[0082] [Example]
[0083] Specific examples of the PTC planar heating element 10 are described below.
[0084] [PTC surface heating element using water-based PTC paint]
[0085] In the PTC planar heating element 10 involved in this embodiment, the flame-retardant polyester film LUMIRROR#500-H10 (manufactured by Toray Industries, Inc.) is used as the first covering material 1, the second covering material 2, and the frame 8. Here, the first covering material 1, the second covering material 2, and the frame 8 are pre-crystallized. In the crystallization process, the object is clamped with an aluminum plate or the like and heated at 145°C for 30 minutes in a constant temperature bath with a light load applied, and then the power of the constant temperature bath is turned off and slowly cooled to room temperature.
[0086] The size of the first covering material 1 is set to 130×90 mm and the thickness is 0.5 mm. The size of the frame 8 is made to have an outer dimension of 130×90 mm, an inner dimension of 110×70 mm, and a thickness of 0.5 mm. As an adhesive, a modified silicone adhesive that can withstand a temperature of about 100°C is used, and the first covering material 1 and the frame 8 are bonded and then cured. The interval between the first covering material 1 and the second covering material 2, which is formed by the thickness of the frame 8 and the adhesive, is about 0.7 mm.
[0087] The second covering material 2 has a size of 140×90 mm and a thickness of 0.5 mm. The first electrode 5a and the second electrode 5b each have a size of 130×10 mm and a thickness of 0.07 mm. An acrylic emulsion adhesive is applied to each of the first electrode 5a and the second electrode 5b, thereby attaching the first electrode 5a and the second electrode 5b to the second covering material 2.
[0088] In the water-based PTC coating constituting the PTC resistor 4, as the water-based carbon paste, anionic LION PASTE W-310A (manufactured by LION SPECIALTY CHEMICALS) in which carbon black is processed into an aqueous dispersion is used. As the polyurethane emulsion adhesive, MC MAX BINDER 942C-U ECO (manufactured by Murayama Chemical Research Institute) is used. As the wax emulsion, non-ionic EMUSTAR-0136 (manufactured by Nippon Seiwa Co., Ltd.) which is an emulsified paraffin wax, and anionic oxidized high-density polyethylene wax emulsion AQUACER 507 (manufactured by BYK) are used. As the boric acid, a general chemical powder product (manufactured by Kenei Pharmaceutical Co., Ltd.) is used.
[0089] Furthermore, graphite and EVA (ethylene-vinyl acetate copolymer resin) are added. Graphite and EVA are also substances commonly used in PTC planar heating elements that use existing polymer materials such as polyethylene and various elastomers as a base. As graphite, powdered CB-100 (manufactured by Nippon Graphite Co., Ltd.) is used. As EVA, emulsion-type SUMIKAFLEX401HQ (manufactured by Sumitomo Chemical Co., Ltd.) is used.
[0090] These materials were blended as shown in Example 1 of Table 1, and stirred and mixed sufficiently to form a paste. In Table 1, the ratio of each component to the total of the components described herein is shown.
[0091] Table 1. Formulation of waterborne PTC coating (wt%)
[0092]
[0093] A conventional polyester film was used as the coating substrate 3a of the PTC resistor 4. The size of the coating substrate 3a was 109.5×69.5 mm and the thickness was 0.3 mm. The coating substrate 3a was subjected to a corona discharge treatment.
[0094] A thicker PTC coating film 3b is formed by casting on a coated substrate 3a treated with corona discharge using a paste-like aqueous PTC coating, air-dried for 1 hour, and then dried at 70°C for 1 hour to form a PTC resistor 4. The thickness of the PTC coating film 3b is about 0.2 mm. Therefore, the thickness of the PTC resistor 4 is about 0.5 mm.
[0095] The PTC resistor 4 thus manufactured is arranged inside the frame 8 on the first covering material 1. Furthermore, the first conductive spacer 6a and the second conductive spacer 6b made of carbon nonwoven fabric are arranged on the PTC resistor 4. The first conductive spacer 6a and the second conductive spacer 6b have a width of 10 mm, which is the same as the first electrode 5a and the second electrode 5b of the copper foil tape, a length of 110 mm that can be in contact with the PTC resistor 4, and a thickness of about 0.5 mm.
[0096] On a first assembly 11 including a first conductive spacer 6a and a second conductive spacer 6b, a second assembly 12 having a first electrode 5a and a second electrode 5b attached to a second coating material 2 is arranged in a manner such that the first electrode 5a and the second electrode 5b are respectively stacked on the first conductive spacer 6a and the second conductive spacer 6b, and the frame 8 is bonded to the second coating material 2.
[0097] As described above, the interval between the first covering material 1 and the second covering material 2 formed by the thickness of the frame 8 and the adhesive is about 0.7 mm. On the other hand, the thickness of the PTC resistor 4 is about 0.5 mm, and the total thickness of the compressed first conductive spacer 6a and the second conductive spacer 6b and the first electrode 5a and the second electrode 5b is estimated to be a maximum of 0.7 mm.
[0098] Assembled in the above manner, the PTC planar heating element 10 is manufactured.
[0099] The formula of the PTC coating of Example 1 shown in Table 1 is a formula that exhibits very good PTC properties in the preliminary compounding experiment. Based on this formula, PTC coatings of the formulas of Examples 2 and 3 shown in Table 1 were also produced. In Example 2, in the preparation of the PTC coating, the carbon paste was changed from the anionic LION PASTE W-310A to the non-ionic W-376R (manufactured by LION SPECIALTY CHEMICALS). In Example 3, in the preparation of the PTC coating, the paraffin emulsion was changed from the non-ionic EMUSTAR-0136 to the anionic EMUSTAR-0135 (manufactured by Nippon Seira Co., Ltd.).
[0100] Moreover, as Example 4, a PTC surface heating element having a different structure from that of Example 1 was produced. The PTC surface heating element involved in Example 4 is an example of a soft and flexible structure. As the material of the coating substrate 3a and the frame 8 of the PTC resistor 4, a polyester woven cloth with a thickness of 0.7 mm is used. In addition, as the material of the first covering material 1 and the second covering material 2, a polyester woven cloth with a thickness of 0.6 mm coated with vinyl chloride resin on one side is used. The other structures are basically the same as those in Example 1. That is, the structure of the electrode 5 and the conductive spacer 6 is the same as that in Example 1. The shape and size of each material and the adhesive used are the same as those in Example 1. In addition, the preparation of the PTC coating and the manufacturing method of the PTC resistor 4 are also the same as those in Example 1.
[0101] As a comparative example, a PTC coating material having the formulation of Comparative Example 1 shown in Table 1 was also prepared. Comparative Example 1 is a formulation obtained by removing boric acid from the formulation of Example 1.
[0102] Moreover, as comparative examples 2, 3, and 4, PTC planar heating elements with different structures from those of Example 1 were prepared. Although the PTC planar heating element involved in Comparative Example 2 has basically the same formula and the same structure as those of Example 1, it has the following differences: namely, the structure in which the electrodes of the second covering material 2 of Example 1 and the coated surface of the PTC resistor 4 are fully bonded using a modified silicone adhesive. Although the PTC planar heating element involved in Comparative Example 3 has basically the same formula and the same structure as those of Example 1, a conductive spacer 6 is not configured. In this PTC planar heating element, as an alternative, a thermally conductive silicone rubber sheet with a thickness of about 0.3 mm is inserted between the non-coated surface of the PTC resistor 4 and the first covering material 1, so that the coated surface of the PTC resistor 4 is in direct contact with the electrode 5. Although the PTC planar heating element involved in Comparative Example 4 has basically the same formula and the same structure as those of Example 1, the first covering material 1, the second covering material 2, and the frame 8 are not subjected to crystallization treatment.
[0103] [Measurement of PTC characteristics]
[0104] The PTC characteristics of the samples of Examples 1, 2, 3, 4 and Comparative Examples 1, 2, and 3 were measured. The measurement method is as follows. The sample was placed in a thermostatic chamber and the temperature was raised from 25°C in a gradient of approximately 10°C. Sufficient stabilization time was set, and the resistance value of the sample was measured using a resistance meter.
[0105] In addition, for the samples involved in Example 1 and Comparative Example 4, the PTC characteristics from 25°C to 100°C were measured once a day under the same conditions as the above-mentioned measurement method. This was repeated for 7 days and the resistance value Ra at 25°C was measured every day.
[0106] Figure 4 The following are the measurement results of the PTC characteristics of Examples 1, 2, 3 and Comparative Example 1. Examples 1, 2, 3 and Comparative Example 1 are examples in which the formulations of the PTC coating materials are different from each other. Figure 5 The following are the measurement results of the PTC characteristics of Example 4 and Comparative Examples 2 and 3. Example 4 and Comparative Examples 2 and 3 are different from Example 1 in structure. Figure 4 and Figure 5 In FIG. 1 , the horizontal axis represents temperature, and the vertical axis represents resistance ratio RR. Here, “resistance ratio RR” is a value obtained by dividing the resistance value at each temperature by the resistance value Ra at 25° C.
[0107] in addition, Figure 6 The Ra change rates of Example 1 and Comparative Example 4 with respect to the measurement day are shown. Here, the Ra change rate is the change rate of Ra on each measurement day relative to Ra on the first day, and is shown as a percentage. Example 1 and Comparative Example 4 are different in structure from each other.
[0108] [Evaluation of the recipe]
[0109] The Curie temperature is considered to be near the temperature when Ra reaches about 2 times. If the rising characteristics of the PTC heater are sharp, the operating temperature of the PTC heater is considered to be near the Curie temperature. In addition, the Curie temperature is considered to vary depending on the properties of each material. The Ra of Example 1 is 4.36 kΩ. The Ra of Example 2 is 4.35 kΩ. The Ra of Example 3 is 4.19 kΩ. The Ra of Comparative Example 1 is 13.98 kΩ.
[0110] Figure 4 The PTC characteristics shown are as follows: from 25°C through the Curie temperature to the temperature range of 60°C where the resistance ratio RR rises, it is uniform and relatively steep. From this result, it can be seen that the basic properties of the selected materials are not easily affected by ionicity and formulation ratio, forming very stable internal properties.
[0111] On the other hand, Figure 4 As shown in the figure, in the region where the resistance ratio RR of the PTC characteristic shows the maximum value RRmax, the relationship with the ionicity is not clear when comparing Examples 1, 2, and 3. As the cause of the difference in RRmax, it can be expected that it is not only due to the ionicity of the material, but also the influence of the dispersant used in the carbon dispersion and each emulsion. Therefore, it is considered that it is necessary to judge whether the material selection is appropriate for each formulation.
[0112] In addition, in Comparative Example 1 in which boric acid is not used, there is no significant difference in the tendency of the PTC characteristics (the overall shape of the curve) compared to Example 1. However, since it is difficult to increase the viscosity of the PTC coating, it is difficult to thicken the coating film and it is difficult to reduce the Ra value. If the Ra value is not reduced, it is difficult to increase the power consumption as a heater, and the basic performance as a heater will deteriorate. Therefore, it is clear that the inclusion of boric acid has a greater effect on improving the performance as a heater.
[0113] [Evaluation of the structure]
[0114] like Figure 5 As shown, the rising characteristics near the Curie temperature of Comparative Examples 2 and 3 are not significantly different from those of Examples 1, 2, and 3. That is, the following fact is made clear: even if the structure of the PTC planar heating element changes significantly, the properties of the formulated material near the Curie temperature are not easily affected. The Ra of Example 4 is 2.70 kΩ. The Ra of Comparative Example 2 is 13.85 kΩ. The Ra of Comparative Example 3 is 4.27 kΩ.
[0115] On the other hand, the maximum value RRmax of the resistance ratio of the PTC characteristic is greatly reduced in both Comparative Examples 2 and 3. The following reasons can be considered as the reasons for this reduction. In Comparative Example 2, the expansion and contraction of the PTC resistor 4 during heating and cooling is greatly hindered by the bonding of the PTC resistor 4 and the second coating material 2, resulting in a reduction in RRmax. In addition, in Comparative Example 3, the PTC resistor and the electrode are in direct contact without the conductive spacer 6 sandwiched therebetween, so the two are bonded due to heating, which greatly hinders the expansion and contraction of the PTC resistor 4 during heating and cooling, resulting in a reduction in RRmax.
[0116] Thus, the PTC characteristics according to the present invention are based on the expansion and contraction of the PTC coating film 3b during heating and cooling, similarly to the existing PTC planar heating elements, but compared with the existing PTC planar heating elements, the present invention has the following superior characteristics. That is, the coating substrate 3a of the PTC resistor 4 does not hinder the expansion and contraction during heating and cooling, thereby increasing the expansion and contraction of the PTC coating film 3b. It can be seen that this has a great effect on exhibiting a large PTC characteristic.
[0117] exist Figure 5In Example 4 showing the measurement results, the coated substrate 3a, the first covering material 1, the second covering material 2 and the frame 8 of the PTC resistor 4 serving as the skeleton are all made of soft polyester woven fabric. The woven fabric is composed of a plurality of fiber bundles, and there are gaps and slips between adjacent fibers, making it difficult to conduct the expansion and contraction stress of the fibers in the planar direction during heating and cooling. Therefore, the coated substrate 3a of the woven PTC resistor 4 will not expand and contract as much as the polyester film during heating and cooling. As a result, the expansion and contraction of the PTC coating film 3b itself is mainly what exhibits the PTC characteristics, and the PTC characteristics are the same as those of Examples 1, 2, and 3 until the Curie temperature is reached, but the RRmax is greatly reduced.
[0118] The shape of the curve graph shown in the measurement results of the PTC characteristics of Example 4 is similar to the shape of the curve graph shown in the measurement results of the PTC characteristics of Comparative Examples 2 and 3 in which the expansion and contraction of the substrate of the PTC resistor is intentionally hindered. Based on the comprehensive judgment of the measurement results of this embodiment, the following conclusion is drawn: without the expansion and contraction of the coating substrate 3a of the PTC resistor 4, the expansion and contraction of the PTC coating film 3b cannot be expanded.
[0119] [Evaluation on stability]
[0120] like Figure 6 As shown, in Example 1, each time the measurement is repeated, the Ra value is stable. This result indicates that there is an annealing effect. When this change is replaced by the annealing conditions in the final process, it can be estimated that the temperature required for this treatment is about 100°C, the time is about 30 minutes, and the number of times is about 2 times. These values are extremely small compared to the case of the PTC surface heating element using existing polymer materials. This clarifies the fact that, compared to the case of the PTC surface heating element using existing polymer materials, in the case of the PTC surface heating element 10 involved in this embodiment, the annealing time can be greatly shortened.
[0121] exist Figure 6 From the results of Comparative Example 4, it can be seen that even if the measurement is repeated, Ra is not stable, and on the contrary, it shows a tendency to increase the rate of change. When observing the sample, it was found that the heating and cooling during the repeated measurement caused the PTC planar heating element as a whole to have deformations that can be clearly visually confirmed, such as bending and twisting. By comparison with Example 1, it can be seen that this is a difference caused by not implementing a crystallization treatment on the first covering material 1, the second covering material 2, and the frame 8.
[0122] In this way, the following fact was clarified: that is, as made clear in the "Evaluation on the formulation" and the "Evaluation on the structure", "hindering the expansion and contraction of the PTC resistor" not only leads to a reduction in the PTC characteristics, but in the "Evaluation on the stability", the difference between the expansion and contraction direction of the PTC resistor and the expansion and contraction direction of the casing will also lead to hindering the expansion and contraction of the PTC resistor, thereby leading to a reduction in the PTC characteristics.
[0123] As described above, in the PTC planar heating element 10 involved in the present embodiment, the PTC resistor 4 formed with the PTC coating film 3b by coating the coating substrate 3a with a water-based PTC coating is accommodated in a gap formed by the first and second coating materials 1 and 2 as the insulating coating materials inside and outside and the frame 8 made of the same material, and is in flexible contact with the electrode 5 via the conductive spacer 6. As a result, the expansion and contraction of the PTC resistor 4 during heating and cooling is not hindered, and while exhibiting sensitive PTC characteristics, the annealing time in the final process is greatly shortened, and a PTC planar heating element with good mass production and low cost can be provided.
[0124] As mentioned above, although the preferred embodiment of the present invention was shown and described, it is obvious that the present invention is not limited to the above-mentioned embodiment, and can be implemented with various modifications within the scope of the present invention.
[0125] The PTC planar heating element 10 according to the present embodiment can be used for, for example, planar heating devices such as floor heating, heat preservation of vehicle batteries and power storage batteries, and the like.
Claims
1. A PTC planar heating element, It is characterized in that include: An insulating first covering material; an insulating frame fixed to the periphery of the first covering material; an insulating second covering material fixed to the frame so as to face the first covering material with a predetermined distance therebetween via the frame; A PTC resistor body that can be telescopically arranged in an internal space formed by the first covering material, the frame, and the second covering material; a pair of conductive spacers arranged on a side of the internal space closer to the second covering material than the PTC resistor so as to be in contact with the PTC resistor; and A pair of electrodes are arranged between the conductive spacer and the second covering material so that at least a portion of each electrode is in contact with the corresponding conductive spacer, thereby making flexible contact with the PTC resistor through the conductive spacer.
2. The PTC planar heating element according to claim 1, It is characterized in that The PTC resistor comprises a coating substrate and a PTC coating film formed by using a water-based PTC coating. The PTC resistor is arranged in the internal space in such a manner that the coating substrate side serves as the first covering material side and the PTC coating film side serves as the second covering material side. The conductive spacer is disposed on one side of the PTC coating film so as to be in contact with the PTC coating film.
3. The PTC planar heating element according to claim 2, It is characterized in that The water-based PTC coating at least comprises: water-based carbon paste, polyurethane emulsion adhesive, wax emulsion and boric acid.
4. The PTC planar heating element according to claim 2 or 3, It is characterized in that The coating substrate is formed using a polyester film.
5. The PTC planar heating element according to any one of claims 1 to 3, It is characterized in that The first covering material, the second covering material, and the frame are formed using a flame-retardant polyester film that has been subjected to a crystallization treatment.
6. The PTC planar heating element according to any one of claims 1 to 3, It is characterized in that The conductive spacer is formed using conductive short fibers.
7. The PTC planar heating element according to claim 2 or 3, It is characterized in that The coating substrate and the frame are formed using polyester woven fabric. The first covering material and the second covering material are formed of a resin-coated polyester woven fabric and have surfaces on the side opposite to the side of the internal space.
8. A method for manufacturing a PTC planar heating element, It is characterized in that include: A step of preparing an insulating lower covering material having a recessed portion formed by fixing a frame to the periphery of the first covering material, a step of disposing a PTC resistor in the recessed portion of the lower covering material, and The step of providing a pair of conductive spacers in contact with the PTC resistor and a pair of electrodes in contact with the pair of conductive spacers, respectively, on the PTC resistor, and providing an insulating second covering material fixed to the lower covering material so as to cover the recess.