A TC4 titanium alloy forging material and preparation method
By preparing TiAlN/Ti coating on the surface of TC4 titanium alloy forged materials, the problems of low hardness, high friction coefficient and poor erosion resistance of titanium alloy materials are solved, and higher hardness and erosion resistance are achieved, which is suitable for many applications. kind of application fields.
Patent Information
- Application Number
- CN202110480649.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-04-30
AI Technical Summary
Existing titanium alloy materials have limited application scope due to their low hardness, high friction coefficient, poor wear resistance and poor erosion resistance.
By preparing TiAlN/Ti-coated TC4 titanium alloy forgings, magnetic filter vacuum cathode arc and metal vapor vacuum arc methods are used to prepare multi-layer TiAlN/Ti coatings on the surface of titanium alloy forgings, controlling the coating thickness and preparation conditions, and improving Material hardness and erosion resistance.
It significantly improves the hardness and erosion resistance of titanium alloy forged materials, improves production efficiency and appearance quality, and is suitable for components in a variety of fields.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the application field of TC4 titanium alloy, and specifically relates to a TC4 titanium alloy forging material and a preparation method thereof. Background Art
[0002] Pure titanium has two isotopic isomers in the solid state, with 882.5℃ as the dividing line. The stable state at low temperature is α phase, and the stable state at high temperature is β phase. According to the different room temperature structures of titanium alloys, titanium alloys can be divided into three categories: α titanium alloy, β titanium alloy and α+β titanium alloy. TC4 stands for the fourth α+β dual-phase titanium alloy.
[0003] TC4 is a typical α+β titanium alloy, containing about 6%wt of Al and 4%wt of V. It was developed by a certain American college in the 1950s. It is the most common titanium alloy on the market, and its output exceeds half of the total industrial titanium alloy.
[0004] The existing titanium alloy materials have limited application scope due to their relatively low hardness, high friction coefficient and poor wear resistance, and the existing titanium alloy materials have poor erosion resistance. Summary of the invention
[0005] The object of the present invention is to provide a TC4 titanium alloy forging material and a preparation method thereof, so as to solve the problems of relatively low hardness, high friction coefficient, poor wear resistance and poor erosion resistance of existing titanium alloy materials.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing a TC4 titanium alloy forging comprises the following steps:
[0008] Unloading: Select titanium alloy ingots that meet the standards, unload them into the oven according to the process size, and remove the burrs on the end surface after unloading;
[0009] Forging heating: clean the furnace ash and slag, place the titanium alloy ingot fed into the furnace in the effective heating zone and start heating, heat the temperature to 960±10℃, the heating time shall not exceed 90min, put the heated titanium alloy ingot into the warm charging furnace, keep it warm for 30-40min and then start forging;
[0010] Billeting: preheat the billeting tool to 300±50℃, and forge the titanium alloy ingot to the size of the process sketch according to the requirements of roughening and drawing to obtain the billet;
[0011] Grinding: Grind the blank obtained by blanking, use a grinding wheel machine to grind away the surface defects of the blank and grind off the sharp edges;
[0012] Forging die heating: Place the polished blank in an oven and heat it to 960±10℃ for no more than 90 minutes. Then place the blank in a warm-loading furnace and keep it warm for 30-40 minutes before forging the die.
[0013] Forging die: preheat the die to 250-350℃, then evenly distribute graphite emulsion in the die, blow away the remaining oxide scale and graphite slag in the die, fill the die with the blank heated by the forging die, the starting temperature of the forging die shall not exceed 960℃, and the temperature before the end of the forging die shall not be less than 800℃;
[0014] Trimming: Install the trimming die to ensure uniform gaps and a trimming temperature of no less than 850°C. After trimming, place the die to room temperature and remove the die to obtain the titanium alloy forging material.
[0015] Coating: The forged titanium alloy forging is placed in a vacuum chamber to prepare a TiAlN / Ti coating on the surface of the forging.
[0016] Preferably, the coating is specifically prepared by placing the forged titanium alloy forging material into a vacuum chamber, using a magnetic filtration vacuum cathode arc and a metal vapor vacuum arc method to prepare several layers of TiAlN / Ti coating on the surface of the forging material, the nitrogen flow rate is 18-30sccm, and the vacuum chamber pressure is (3-5)×10 -5 Pa, the magnetic filtration deflection angle is 180°.
[0017] Preferably, the TiAlN / Ti coating comprises 4 TiAlN layers and 4 Ti layers, the TiAlN layers and the Ti layers are arranged alternately, and the first layer in contact with the surface of the forging material is the Ti layer.
[0018] Preferably, the thickness of each TiAlN layer is 2-5 μm, and the thickness of each Ti layer is 0.1-0.5 μm.
[0019] Preferably, the material unloading specifically includes selecting a titanium alloy ingot that meets the GB / T2965-2007 standard, unloading it into the baking furnace according to the process size, and checking the weight of the titanium alloy ingot before unloading.
[0020] Preferably, the flow rate of nitrogen is 20 sccm and the pressure of the vacuum chamber is 4×10 -5 Pa.
[0021] Preferably, the thickness of each TiAlN layer is 3.5 μm, and the thickness of each Ti layer is 0.25 μm.
[0022] The TC4 titanium alloy forging material has a thickness of 60 to 120 mm and a width of 40 to 2000 mm.
[0023] The present invention provides a TC4 titanium alloy forging material and a preparation method thereof. By arranging TiAlN / Ti on the surface of the titanium alloy forging material, the problem that the existing titanium alloy material has limited application scope due to its relatively low hardness, high friction coefficient and poor wear resistance, and the existing titanium alloy material has poor erosion resistance is solved. By limiting the preparation conditions of the coating and controlling the thickness of the coating, the coating has a better erosion resistance effect. The TC4 titanium alloy forging material is forged and the titanium alloy forging material is prepared into a forging method of the titanium alloy forging material according to the preparation standard. By using the forging method of the present invention, the titanium alloy forging material is forged with high production efficiency, good appearance quality, stable physical properties, and is suitable for components in various fields. DETAILED DESCRIPTION
[0024] In order to highlight the implementation purpose, technical scheme and structural advantages of the present invention, the technical scheme in the examples of the present invention is described in detail below. The examples described are part of the examples of the present invention, but not all of the examples. Based on the examples in the present invention, all other examples obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0025] Example 1
[0026] Unloading: Select titanium alloy ingots that meet the standards, unload them into the oven according to the process size, and remove the burrs on the end surface after unloading;
[0027] Forging heating: clean the furnace ash and slag, place the titanium alloy ingot fed into the furnace in the effective heating zone and start heating, heat the temperature to 960℃, and the heating time shall not exceed 90min. Put the heated titanium alloy ingot into the warm charging furnace, keep it warm for 30min and then start forging;
[0028] Billeting: preheat the billeting tool to 300°C, and forge the titanium alloy ingot to the size of the process sketch according to the requirements of roughening and drawing to obtain the billet;
[0029] Grinding: Grind the blank obtained by blanking, use a grinding wheel machine to grind away the surface defects of the blank and grind off the sharp edges;
[0030] Forging die heating: Place the polished blank in a furnace and heat it to 960°C for no more than 90 minutes. Then place the blank in a warm-loading furnace and keep it warm for 30 minutes before forging the die.
[0031] Forging die: preheat the die to 250℃, then evenly distribute graphite emulsion in the die, blow away the remaining oxide scale and graphite slag in the die, fill the die with the blank heated by the forging die, the starting temperature of the forging die shall not exceed 960℃, and the temperature before the end of the forging die shall not be less than 800℃;
[0032] Trimming: Install the trimming die to ensure uniform gaps and a trimming temperature of no less than 850°C. After trimming, place the die to room temperature and remove the die to obtain the titanium alloy forging material.
[0033] Coating: The titanium alloy forgings after forging were placed in a vacuum chamber, and several layers of TiAlN / Ti coating were prepared on the surface of the forgings using the magnetic filtration vacuum cathode arc and metal vapor vacuum arc methods. The nitrogen flow rate was 18 sccm and the vacuum chamber pressure was 3×10 -5 Pa, the magnetic filtration deflection angle is 180°, the number of TiAlN layers is two, and the number of Ti layers is two.
[0034] Example 2
[0035] Unloading: Select titanium alloy ingots that meet the standards, unload them into the oven according to the process size, and remove the burrs on the end surface after unloading;
[0036] Forging heating: clean the furnace ash and slag, place the titanium alloy ingot fed into the furnace in the effective heating zone and start heating. Heat the temperature to 950℃ for no more than 90 minutes. Put the heated titanium alloy ingot into the warm charging furnace and start forging after keeping it warm for 40 minutes.
[0037] Billeting: preheat the billeting tool to 250°C, and forge the titanium alloy ingot to the size of the process sketch according to the requirements of roughening and drawing to obtain the billet;
[0038] Grinding: Grind the blank obtained by blanking, use a grinding wheel machine to grind away the surface defects of the blank and grind off the sharp edges;
[0039] Forging die heating: Place the polished blank in a furnace and heat it to 970°C for no more than 90 minutes. Then place the blank in a warm-loading furnace and keep it warm for 35 minutes before forging the die.
[0040] Forging die: preheat the die to 300℃, then evenly distribute graphite emulsion in the die, blow away the remaining oxide scale and graphite slag in the die, fill the die with the blank heated by the forging die, the starting temperature of the forging die shall not exceed 960℃, and the temperature before the end of the forging die shall not be less than 800℃;
[0041] Trimming: Install the trimming die to ensure uniform gaps and a trimming temperature of no less than 850°C. After trimming, place the die to room temperature and remove the die to obtain the titanium alloy forging material.
[0042] Coating: The titanium alloy forgings after forging were placed in a vacuum chamber, and several layers of TiAlN / Ti coatings were prepared on the surface of the forgings using the magnetic filtration vacuum cathode arc and metal vapor vacuum arc methods. The nitrogen flow rate was 30 sccm and the vacuum chamber pressure was 5×10 -5 Pa, the magnetic filtration deflection angle is 180°, the number of TiAlN layers is 3, and the number of Ti layers is 3.
[0043] Example 3
[0044] Unloading: Select titanium alloy ingots that meet the standards, unload them into the oven according to the process size, and remove the burrs on the end surface after unloading;
[0045] Forging heating: clean the furnace ash and slag, place the titanium alloy ingot fed into the furnace in the effective heating zone and start heating. Heat the temperature to 950℃ for no more than 90 minutes. Put the heated titanium alloy ingot into the warm charging furnace and start forging after keeping it warm for 40 minutes.
[0046] Billeting: preheat the billeting tool to 250°C, and forge the titanium alloy ingot to the size of the process sketch according to the requirements of roughening and drawing to obtain the billet;
[0047] Grinding: Grind the blank obtained by blanking, use a grinding wheel machine to grind away the surface defects of the blank and grind off the sharp edges;
[0048] Forging die heating: Place the polished blank in a furnace and heat it to 970°C for no more than 90 minutes. Then place the blank in a warm-loading furnace and keep it warm for 35 minutes before forging the die.
[0049] Forging die: preheat the die to 300℃, then evenly distribute graphite emulsion in the die, blow away the remaining oxide scale and graphite slag in the die, fill the die with the blank heated by the forging die, the starting temperature of the forging die shall not exceed 960℃, and the temperature before the end of the forging die shall not be less than 800℃;
[0050] Trimming: Install the trimming die to ensure uniform gaps and a trimming temperature of no less than 850°C. After trimming, place the die to room temperature and remove the die to obtain the titanium alloy forging material.
[0051] Coating: The titanium alloy forgings after forging were placed in a vacuum chamber, and several layers of TiAlN / Ti coatings were prepared on the surface of the forgings using the magnetic filtration vacuum cathode arc and metal vapor vacuum arc methods. The nitrogen flow rate was 30 sccm and the vacuum chamber pressure was 5×10 -5 Pa, the magnetic filtration deflection angle is 180°, the number of TiAlN layers is 4, and the number of Ti layers is 4.
[0052] Example 4
[0053] Unloading: Select titanium alloy ingots that meet the standards, unload them into the oven according to the process size, and remove the burrs on the end surface after unloading;
[0054] Forging heating: clean the furnace ash and slag, place the titanium alloy ingot fed into the furnace in the effective heating zone and start heating. Heat the temperature to 950℃ for no more than 90 minutes. Put the heated titanium alloy ingot into the warm charging furnace and start forging after keeping it warm for 40 minutes.
[0055] Billeting: preheat the billeting tool to 250°C, and forge the titanium alloy ingot to the size of the process sketch according to the requirements of roughening and drawing to obtain the billet;
[0056] Grinding: Grind the blank obtained by blanking, use a grinding wheel machine to grind away the surface defects of the blank and grind off the sharp edges;
[0057] Forging die heating: Place the polished blank in a furnace and heat it to 970°C for no more than 90 minutes. Then place the blank in a warm-loading furnace and keep it warm for 35 minutes before forging the die.
[0058] Forging die: preheat the die to 300℃, then evenly distribute graphite emulsion in the die, blow away the remaining oxide scale and graphite slag in the die, fill the die with the blank heated by the forging die, the starting temperature of the forging die shall not exceed 960℃, and the temperature before the end of the forging die shall not be less than 800℃;
[0059] Trimming: Install the trimming die to ensure uniform gaps and a trimming temperature of no less than 850°C. After trimming, place the die to room temperature and remove the die to obtain the titanium alloy forging material.
[0060] Plating: The titanium alloy forgings after forging were placed in a vacuum chamber, and several layers of TiAlN / Ti coating were prepared on the surface of the forgings using the magnetic filtration vacuum cathode arc and metal vapor vacuum arc methods. The nitrogen flow rate was 20 sccm and the vacuum chamber pressure was 4×10 -5 Pa, the magnetic filtration deflection angle is 180°, the number of TiAlN layers is 4, the number of Ti layers is 4, the thickness of each TiAlN layer is 3.5 μm, and the thickness of each Ti layer is 0.25 μm.
[0061] The titanium alloy forgings obtained in Examples 1-4 were tested, and the results are shown in Table 1 below.
[0062]
[0063] It can be seen from Table 1 that the titanium alloy forging material obtained by the forging method of the present invention has good mechanical strength; the transverse and longitudinal elongation is ≥12%, reaching the A-level flaw detection requirements, and is suitable for various fields.
[0064] The forged titanium alloy forgings obtained in Examples 1-4 and the TC4 titanium alloy forgings without the TiAlN / Ti layer were tested for their dust erosion resistance. The total mass loss and erosion rate of the forgings obtained in Examples 1-4 within 8 minutes were recorded. The test results are shown in Table 2 below.
[0065]
[0066] It can be seen from Table 2 that the titanium alloy forging obtained by the present invention has good anti-erosion function.
[0067] Finally, it is stated that the above detailed description is only for the implementation scheme of the present invention, and is not a limitation on the scope of the patent of the present invention. It should be pointed out that a person of ordinary skill in the art may make several deformations and modifications within the scope of the concept of the present invention, or make relevant replacements to some of the technical features therein, which all belong to the protection scope of the present invention. The above patent protection scope shall be subject to the attached claims. Finally, it should be explained that the above embodiments are only used to illustrate the technical scheme of the present invention, not to limit it; although the present invention is described in detail with reference to the aforementioned embodiments, a person of ordinary skill in the art should understand that it is still possible to modify the technical schemes recorded in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein; and these modifications or replacements do not make the essence of the corresponding technical scheme deviate from the spirit and scope of the technical schemes of the embodiments of the present invention.
Claims
1. A method for preparing TC4 titanium alloy forgings, characterized in that: The method comprises the following steps: Unloading: Select titanium alloy ingots that meet the standards, unload them into the oven according to the process size, and remove the burrs on the end surface after unloading; Forging heating: clean the furnace ash and slag, place the titanium alloy ingot fed into the furnace in the effective heating zone and start heating, heat the temperature to 960±10℃, the heating time shall not exceed 90min, put the heated titanium alloy ingot into the warm charging furnace and keep it warm for 30-40min; Billeting: preheat the billeting tool to 300±50℃, and forge the titanium alloy ingot to the size of the process sketch by upsetting and stretching as required to obtain the billet; Grinding: Grind the blank obtained by blanking, use a grinding wheel machine to grind away the surface defects of the blank and grind off the sharp edges; Heating: Place the polished blank in an oven and heat it to 960±10℃ for no more than 90 minutes. Then place the blank in a warm-loading furnace and keep it warm for 30-40 minutes. Die forging: preheat the die to 250-350℃, then evenly distribute graphite emulsion in the die, blow off the remaining oxide scale and graphite slag in the die, fill the die with the heated blank, the starting temperature of die forging is not more than 960℃, and the temperature before the end of die forging is not less than 800℃; Trimming: Install the trimming die to ensure uniform gaps and a trimming temperature of no less than 850°C. After trimming, place the die to room temperature and remove the die to obtain the titanium alloy forging material. Coating: placing the forged titanium alloy forging material into a vacuum chamber, and preparing a TiAlN / Ti coating on the surface of the forged titanium alloy forging material; Specifically, the coating comprises placing the forged titanium alloy forging material into a vacuum chamber, using a magnetic filtration vacuum cathode arc and a metal vapor vacuum arc method to prepare a TiAlN / Ti coating on the surface of the forged titanium alloy forging material, the nitrogen flow rate is 18-30 sccm, and the vacuum chamber pressure is (3-5)×10 -5 Pa, the magnetic filtration deflection angle is 180°; The TiAlN / Ti coating comprises four TiAlN layers and four Ti layers, the TiAlN layers and the Ti layers are arranged alternately, and the first layer in contact with the surface of the titanium alloy forging material after forging is the Ti layer; The thickness of each TiAlN layer is 3.5 μm, and the thickness of each Ti layer is 0.25 μm.
2. The preparation method according to claim 1, characterized in that: The material unloading is specifically to select titanium alloy ingots that meet the GB / T2965-2007 standard, unload them into the baking furnace according to the process size, and check the weight of the titanium alloy ingot before unloading.
3. The preparation method according to claim 1, characterized in that: The nitrogen flow rate is 20 sccm, and the vacuum chamber pressure is 4×10 -5 Pa.