Method for producing resin for semiconductor production
By converting alkaline ion exchange resin into acid form and performing appropriate expansion and washing, combined with chloromethylation and amination steps, the problems of insufficient resin stability and boron removal ability in the existing technology are solved, and low TOC and The production of resin with high resistivity ensures the physical stability and high boron removal performance of the resin.
Patent Information
- Application Number
- CN201980085824.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-11-19
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-11-19
AI Technical Summary
It is difficult to produce physically stable selective ion exchange resins with low total organic carbon (TOC), high resistivity, and high boron removal capabilities in semiconductor production with existing technologies, especially aminopolyol functionalized resins, and commonly used methods May affect other properties of the resin.
Adopt a method by converting the basic ion exchange resin into the acid form, adding an appropriate amount of expansion volume, and washing the resin with water or an aqueous acid solution, combined with chloromethylation and amination steps, to control the cross-linker and functional groups. Amount and type, the resin is prepared with 15% to 30% expansion and undergoes multiple acid treatments and washes to achieve low TOC and high resistivity.
It achieves low TOC and high resistivity of the resin, maintains the boron removal ability, and does not affect other properties of the resin, ensuring the physical stability and high boron removal performance of the resin.
Smart Images

Figure BDA0003128815700000021 
Figure BDA0003128815700000031 
Figure BDA0003128815700000051
Abstract
Description
Background Art
[0001] The present invention generally relates to methods of producing ion exchange resins for purifying water used in semiconductor production.
[0002] Recently, the trend of ultrapure water (UPW) design is towards reverse osmosis (RO) plus electrode ionization (EDI). With regard to this design, the key is to reduce boron to very low levels. To this end, boron selective ion exchange resins, for example, amino polyol functionalized resins are attractive options. However, the resin needs to be exceptionally clean, i.e., have low total organic carbon (TOC) and produce water with high resistivity. The resin also needs to be physically stable and have a high ability to remove boron. For example, JP4518112 discloses a method for reducing TOC in amino polyol resins. However, the method taught in this document uses harsh conditions that may affect other resin properties. Summary of the invention
[0003] The present invention relates to a method for producing an ion exchange resin. The method comprises the following steps:
[0004] (a) providing a basic ion exchange resin in acid form, said resin comprising amino polyol groups and having a swelling volume % of 15% to 30% upon conversion from said base form to the acid form, and
[0005] (b) washing the resin with water or an aqueous acid solution.
[0006] The present invention further relates to an ion exchange resin comprising 2 to 4 wt% polymerized crosslinker units, a macro-network structure, 2.0 to 3.2 equivalents / kg of active sites, the active sites comprising amino polyol functional groups. DETAILED DESCRIPTION
[0007] Unless otherwise stated, all percentages are weight percent (wt%) and all temperatures are in ° C. Unless otherwise stated, averages are arithmetic means. All operations were performed at room temperature (18° C. to 25° C.) unless otherwise stated.
[0008] The polymerization, chloromethylation and amination steps are designed to give a final product with 15%-30% expansion when converted from the free base form to the acid form. This expansion is determined by the crosslinking and the number and type of functional groups. There are three types of crosslinking: (i) crosslinking from copolymerization of the crosslinking agent with the styrenic monomer, (ii) methylene bridging which occurs in chloromethylation, and (iii) reaction of the amino polyol with two chloromethyl groups (strong base groups) in amination. The extent of chloromethylation and amination affects the relative amounts of the different functional groups.
[0009] "Styrenic monomers" include monoethylenically unsaturated aromatic compounds, such as styrene, vinyl toluene, ethylvinylbenzene, chlorostyrene and vinyl naphthalene. "Styrenic crosslinkers" include polyethylenically unsaturated aromatic compounds, such as divinylbenzene and trivinylbenzene. Other monoethylenically unsaturated compounds may be added, preferably in an amount less than 10 wt% (preferably less than 5 wt%), for product improvements such as strength, preferably, for example, methacrylic acids and their esters, vinyl pyridine, acrylonitrile, vinyl ethers, esters and ketones. Polyethylenically unsaturated compounds may also be used as crosslinking agents, preferably, for example, trivinylcyclohexane, and di- and trimethacrylate compounds, such as trimethylolpropane trimethacrylate. The percentage of monomer units in the polymer is based on the total polymer weight (dry weight). The term "gel" resin is applied to a resin that consists of a very low porosity (0-0.1 cm 3 / g), small average pore size and small BET surface area (0-10m 2 The term "macroreticular" (or MR) resin is applied to a resin synthesized from a high-pore copolymer having a surface area greater than that of a gel resin. MR resins have a total porosity between 0.1 and 0.7 cm 3 / g, the average pore size is between 17 and and a BET surface area between 10 and 200 m 2 / g. MR resins are typically prepared by incorporating an organic solvent ("pore former") into a monomer mixture. The term adsorption resin is applied to a resin that may or may not be functionalized and that has a very high surface area and porosity. The surface area of these adsorption resins is between 200 and 1300 m 2 / g, and the average pore size is between 17 and and the total porosity is between 0.7 and 200 cm 3 / g.
[0010] The Harmonic Mean Diameter (HMD) is defined by the following equation:
[0011]
[0012] where i is the index of a single bead; d i is the diameter of each individual particle; and N is the total number of beads. The resin beads are substantially spherical.
[0013] Preferably, the alkaline ion exchange resin used in the method of the present invention comprises from 2 to 4 wt% polymerized crosslinker units; a macro-network structure; and 2.0-3.2 equivalents / kg of active sites, the active sites comprising amino polyol functional groups. The active sites are amino groups and quaternary ammonium groups.
[0014] Preferably, the crosslinking agent has two polymerizable carbon-carbon double bonds per molecule. Preferably, the molecular weight of the crosslinking agent is 100 to 400, preferably 100 to 250, preferably 120 to 200. Preferably, the resin comprises 2.5 to 3.5 wt% polymerized crosslinking agent units. Preferably, the resin comprises 96 to 98 wt% styrenic monomers, preferably 96.5 to 97.5 wt%. Preferably, the crosslinking agent is divinylbenzene. Preferably, the resin comprises 96 to 98 wt% polymerized styrene units and 2- to 4 wt% polymerized divinylbenzene units; preferably, 96.5 to 97.5 wt% polymerized styrene units and 2.5 to 3.5 wt% polymerized divinylbenzene units.
[0015] Preferably, the copolymer is chloromethylated, preferably under conditions giving 90%-100% substitution of the styrenic monomer. Chloromethylation is carried out under conditions that minimize methylene bridging, which can reduce swelling. The crosslinked chloromethylated styrenic polymer is then aminated with an amino polyol, preferably N-methylglucamine. Preferably, after amination, the resin contains 2.0-3.2 equivalents / kg active sites, preferably at least 2.3 equivalents / kg active sites, preferably at least 2.5 equivalents / kg active sites; preferably no more than 3.1 equivalents / kg active sites, preferably no more than 3.0 equivalents / kg active sites; preferably 2.5-3.0 equivalents / kg amino polyol groups.
[0016] Preferably, the aminopolyol group contains 3 to 9 carbon atoms, preferably at least 4, preferably at least 5, preferably at least 6; preferably no more than 8, preferably no more than 7. Preferably, the aminopolyol group contains 2 to 8 hydroxyl groups, preferably at least 3, preferably at least 4, preferably at least 5; preferably no more than 7, preferably no more than 6. Preferably, the aminopolyol group has both 7 carbon atoms and 5 hydroxyl groups. N-methylglucamine is particularly preferred. The aminopolyol groups in the resin are produced by reacting a chloromethylated crosslinked polymer comprising polymerized styrenic monomer units with an aminopolyol. The aminopolyol is bonded to one or two benzene rings via a nitrogen-carbon bond between the amino nitrogen and the methylene group attached to the benzene ring, as shown below for N-methylglucamine and crosslinked polystyrene.
[0017]
[0018] When the amino polyol N-methylglucamine is bonded to two benzene rings, the nitrogen is part of a quaternary amine group (strong base). This crosslinks the polymer and reduces swelling. Preferably, the resin after the amination process has 0-30% strong base, preferably 5%-20% strong base, preferably 5%-10% strong base, based on total basic sites.
[0019] The basic ion exchange resin in acid form is produced by adding an aqueous solution of an acid to the resin in the base form and allowing the resin to soak. Preferably, the acid soaking is repeated at least once. The conditions for the acid treatment of the ion exchange resin are well known. The water or aqueous solution washing of the acid after the acid treatment is carried out according to known methods. Preferably, the resin is washed with at least 20 BV of DI water, preferably at least 40 BV of DI water, preferably at least 60 BV of DI water. Preferably, the temperature of the DI water is 50° C. to 100° C., preferably 50° C. to 85° C. (greater than 85° C. may lose strong base), preferably 75° C. to 85° C. Preferably, water is used as a washing agent. If an aqueous solution of an acid is used, the acid concentration is preferably less than 10 wt %, preferably less than 5 wt %, preferably less than 1 wt %. Preferably, the resin is converted back to the base form by contacting the resin with an aqueous solution of an alkali under well-known conditions.
[0020] Preferably, the ion exchange resin particles have a harmonic mean diameter of 100-1500 μm, preferably at least 300 μm, preferably at least 400 μm; preferably no more than 1000 μm, preferably no more than 700 μm, preferably no more than 600 μm.
[0021] Examples
[0022] Abbreviations used: DI = deionized; BV = bed volume; TOC = total organic carbon; MHC = water holding capacity; WC = weight holding capacity (equivalent active sites / kg), VC is volume capacity on a liter basis; SB = strong base (equivalent of strong base / total equivalents (strong base and weak base)).
[0023] Examples:
[0024] Best Practice - Example 1 (Washing at 80°C after Acid Treatment)
[0025] 1. Add 7 liters of DowexTM BSR-1 chelating resin to a 5 gallon container. The resin was measured to have a 22% expansion (OH to Cl)
[0026] 2. Add 7 liters of 4 wt% HCl.
[0027] 3. Allow to soak for 30 minutes and remove the liquid using a siphon
[0028] 4. Repeat steps 2 and 3 twice (total 21 L HCl)
[0029] 5. Add 7 liters of DI water
[0030] 6. Allow to soak for 20 minutes and remove the liquid using a siphon
[0031] 7. Repeat steps 2 and 3 twice (total 21 liters of DI water)
[0032] 8. Repeat steps 1-7 to prepare a total of 14 L of HCl-treated BSR-1 resin
[0033] 9. Load 14 L of HCl-treated BSR-1 resin into a 20 L glass column (5.5 in diameter)
[0034] 10. Allow 80°C DI water to flow through the column at 6.6 BV / hr (1540 ml / min) for 13 hours
[0035] 11. Allow ambient temperature DI water to flow down the column at 6.6 BV / hr (1540 ml / min) for 13 hours
[0036] 12. Pass 21 liters of 4% NaOH through the column at 350 ml / min for 60 min.
[0037] 13. Stop flow and allow the resin to soak in 4% NaOH for 30 minutes
[0038] 14. Repeat steps 12 and 13
[0039] 15. Allow ambient temperature DI water to flow down the column at 6.6 BV / hr (1540 ml / min) for 6.5 hr
[0040] 16. Disassemble and drain water with a siphon
[0041] The final resin was analyzed for baseline delta-TOC and resistivity using an Anatel A-1000 at 50 BV / hr. The baseline delta-TOC was flushed down to 2.0-2.1 ppb and the resistivity was flushed up to 18.1 MOhm-cm. The static boron capacity was measured before the above flush to be 3.8 g boron / kg resin. The static boron capacity was measured after flushing to be 3.5 g boron / kg resin (92% of the original capacity)
[0042] The general properties were not affected by the flushing process.
[0043]
[0044] Comparative Example 2 (PWA10 cross processing)
[0045] 1. Add 500 ml of Amberlite TMPWA10 to a beaker. The resin was determined to have a 7% expansion (OH to HCl)
[0046] 2. Add 500ml MilliQ water and soak overnight
[0047] 3. Remove liquid with a siphon
[0048] 4. Add 500 ml 1N HCl and leave in contact for 30 seconds.
[0049] 5. Remove liquid with a siphon
[0050] 6. Repeat steps 3-4
[0051] 7. Transfer the resin to the glass column
[0052] 8. Pass 1N HCl through the resin at 4 BV / hr (33 ml / min) at ambient temperature for 1.4 hr
[0053] 9. Pass MilliQ water through the resin at 4 BV / hr (33 ml / min) at ambient temperature for 1.0 hr
[0054] 10. Pass 1N NaOH through the resin at 4 BV / hr (33 ml / min) at ambient temperature for 1.3 hr
[0055] 11. Pass MilliQ water through the resin at 4 BV / hr (33 ml / min) at ambient temperature for 1.0 hr
[0056] 12. Repeat steps 10-11
[0057] The final resin was analyzed for baseline delta-TOC and resistivity using an Anatel A-1000 at 25 BV / hr. The baseline delta-TOC was flushed down to 34.5 ppb and the resistivity was flushed up to 18.2 MOhm-cm.
[0058] Comparative Example 3 (BSR-1 Crossover Processing)
[0059] 1. Add 500 ml of DowexTM BSR-1 chelating resin to a beaker. The resin was measured to have a 22% expansion (OH to Cl)
[0060] 2. Add 500ml MilliQ water and soak overnight
[0061] 3. Remove liquid with a siphon
[0062] 4. Add 500 ml 1N HCl and leave in contact for 30 seconds.
[0063] 5. Remove liquid with a siphon
[0064] 6. Repeat steps 3-4
[0065] 7. Transfer the resin to the glass column
[0066] 8. Pass 1N HCl through the resin at 4 BV / hr (33 ml / min) at ambient temperature for 1.4 hr
[0067] 9. Pass MilliQ water through the resin at 4 BV / hr (33 ml / min) at ambient temperature for 1.0 hr
[0068] 10. Pass 1N NaOH through the resin at 4 BV / hr (33 ml / min) at ambient temperature for 1.3 hr
[0069] 11. Pass MilliQ water through the resin at 4 BV / hr (33 ml / min) at ambient temperature for 1.0 hr
[0070] 12. Repeat steps 10-11
[0071] The final resin was analyzed for baseline delta-TOC and resistivity using an Anatel A-1000 at 25 BV / hr. The baseline delta-TOC was flushed down to 9.8 ppb and the resistivity was flushed up to 18.2 MOhm-cm.
[0072] Comparative Example 4 (rinsed with PWA10 at 90°C) - PAC-BSR-11
[0073] 1. Load 150 ml of Amberlite into a 2-inch diameter jacketed glass column. TM PWA10.
[0074] 2. Allow 90°C DI water to flow downward through the column at 6.6 BV / hr (16 ml / min) for 6.5 hr
[0075] 3. Allow ambient temperature DI water to flow down the column at 13 BV / hr (33 ml / min) for 1.9 hr
[0076] 4. Disassemble and drain water with a siphon
[0077] The final resin was analyzed for baseline delta-TOC and resistivity using an Anatel A-1000 at 50 BV / hr. The baseline delta-TOC was flushed down to 2.5 ppb and the resistivity was flushed up to 17.7 MOhm-cm. The static boron capacity was measured to be 4.2 g boron / L resin before the above flush. The static boron capacity was measured to be 3.2 g boron / L resin after flushing (77% of the original capacity).
[0078] This rinse changed the % Base from 34.5% to 13.9%.
[0079]
Claims
1. A method for producing an ion exchange resin; the method comprising the following steps: (a) providing a basic ion exchange resin in acid form produced by adding an aqueous solution of an acid to a resin in base form and allowing the resin to soak, the resin comprising amino polyol groups and having a swell volume of 15% to 30% upon conversion from the base form to the acid form, (b) washing the resin with water or an aqueous acid solution, and (c) converting the resin back to the base form by contacting the resin with an aqueous base solution, Wherein, the resin has a large network structure, Wherein, the water used in step (b) is deionized water with a temperature of 50°C to 100°C.
2. The method of claim 1, wherein: The resin contains 2.0 to 3.2 equivalents / kg of active sites.
3. The method of claim 1, wherein: The resin contains 2.5 to 3 equivalents / kg of amino polyol groups.
4. The method of claim 1, wherein: The resin contains 2 to 4 wt% polymerized crosslinker units.
5. The method of claim 1, wherein: The water used in step (b) is deionized water having a temperature of 50°C to 85°C.
6. The method of claim 1, wherein: The resin includes 96 to 98 wt % of styrene-based monomers.
7. The method of claim 1, wherein: The amino polyol is N-methylglucamine.
8. An ion exchange resin produced by the process according to any one of claims 1 to 7.
Citation Information
Patent Citations
Water-treatment resin and pure water production method using the same
JP2016141738A
Arsenic removal
WO2005023409A2
Cited By
Hydrophobized ion exchange resins and methods of making
WO2026156241A1