Electrode active material for secondary battery, electrode and secondary battery comprising the same, and method for preparing the electrode active material

By forming an internal silicon layer on the carbon-based material of the secondary battery and controlling the particle size of the silicon particle, the problem of deterioration of cycle characteristics caused by silicon volume expansion is solved, and the battery capacity and performance are improved.

CN113302764BActive Publication Date: 2024-11-12LIVENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980002868.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-06
Publication Date
2024-11-12
Estimated Expiration
2039-12-06

AI Technical Summary

Technical Problem

The existing electrode active materials for secondary batteries have deteriorated cycle characteristics due to the volume expansion and contraction of silicon during charging and discharging, which cannot effectively improve battery capacity and performance.

Method used

By forming a silicon layer on a carbon-based material, the silicon layer is located inside the carbon-based material and not exposed to the outer surface, or partially exposed to a portion of the outer surface, and contains both silicon and carbon in the silicon layer, formed by chemical vapor deposition The silicon layer controls the silicon particle size in the range of 0.1 nm to 10 nm to buffer the expansion and contraction of silicon.

Benefits of technology

It significantly improves the capacity and performance of the secondary battery, reduces the risk of electrical short circuits and side reactions between the electrode active material and the electrode, and extends the battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113302764B_ABST
    Figure CN113302764B_ABST
Patent Text Reader

Abstract

According to one embodiment of the present invention, an electrode active material for a secondary battery is provided. The electrode active material according to one embodiment of the present invention can be formed by using a composite having a silicon layer formed on a carbon-based material as a unit powder. According to one embodiment of the present invention, the composite can be configured so that the silicon layer is located inside the carbon-based material and the silicon is not exposed to the outer surface of the carbon-based material or is partially exposed to a part of the outer surface of the carbon-based material, and the silicon layer can include both silicon and carbon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrode active material for a secondary battery, an electrode and a secondary battery including the electrode active material, and a method for preparing the electrode active material. More specifically, it relates to an electrode active material that can provide high-capacity and high-efficiency charge and discharge characteristics by mixing carbon-based materials and silicon, an electrode and a secondary battery including the electrode active material, and a method for preparing the electrode active material. Background Art

[0002] Recently, lithium secondary batteries have attracted attention as power sources for driving electronic devices, and the use of such lithium secondary batteries in various fields ranging from IT equipment such as mobile phones to electric vehicles and energy storage devices has been increasing.

[0003] At present, with the increase in the application fields and demand for lithium secondary batteries, a variety of lithium secondary battery structures have been developed, and various research and development are actively carried out to improve the capacity, life, performance and safety of the battery.

[0004] As an example, in the past, graphite-based materials have been mainly used as electrode active materials (negative electrode active materials) of lithium secondary batteries. However, since the capacity per unit mass of graphite is only 372 mAh / g, there are limitations to increasing the capacity, making it difficult to fully improve the performance of secondary batteries. Therefore, research has recently been conducted on replacing graphite-based materials with materials that form electrochemical alloys with lithium, such as silicon (Si), tin (Sn), antimony (Sb) and aluminum (Al).

[0005] However, these materials have the characteristics of volume expansion and contraction during the process of charging and discharging by forming electrochemical alloys with lithium, and the volume change caused by this charging and discharging causes the volume expansion of the electrode, thereby deteriorating the cycle characteristics of the secondary battery. Therefore, electrode active materials prepared using these materials have not yet been substantially commercialized.

[0006] For example, silicon has attracted much attention as an electrode active material for secondary batteries that can replace graphite-based materials, and can provide high capacity because each silicon can absorb a maximum of 4.4 lithiums. However, in the process of absorbing lithium ions, the volume of silicon expands by about four times (for reference, graphite, which has been commonly used as an electrode active material, exhibits an expansion rate of about 1.2 times during charge and discharge). Therefore, if the secondary battery continues to charge and discharge, the expansion of the electrode intensifies, causing the cycle characteristics of the secondary battery to deteriorate rapidly.

[0007] As a method for solving this problem, a technology for forming an electrode active material by mixing silicon with a carbon-based material such as graphite has recently been proposed. For example, referring to Patent Documents 1 and 2, it discloses a technology for improving the performance of a secondary battery by forming a silicon layer on a carbon-based material such as graphite.

[0008] Specifically, Patent Document 1 discloses a solution for forming a silicon coating on the surface of a carbon-based material such as graphite to ensure a higher capacity than an existing electrode active material formed of a graphite material, while reducing the degradation of the cycle performance of a secondary battery caused by the expansion and contraction of silicon. However, since the electrode active material disclosed in Patent Document 1 has a structure including a silicon layer on the outer surface of the carbon-based material, the outer silicon layer greatly expands and contracts during the charge and discharge process, thereby causing the electrode active material to be electrically short-circuited with the electrode or the surface of the electrode active material to be micronized to accelerate the side reaction with the electrolyte, etc., and the problem of secondary battery performance degradation cannot be avoided.

[0009] On the other hand, Patent Document 2 discloses a technology for improving the performance of electrode active materials by forming a silicon coating inside a carbon-based material such as graphite. Specifically, Patent Document 2 discloses a technology for depositing a silicon coating by chemical vapor deposition (CVD) after spheroidizing a carbon-based material to form a cavity inside it, thereby forming a silicon coating in the cavity inside the carbon-based material. However, the technology disclosed in Patent Document 2 is also due to the process of placing a carbon-based material having a cavity formed inside it by spheroidization into a reaction chamber and injecting a raw material gas to deposit a silicon coating, and the silicon coating is not only formed in the cavity inside the carbon-based material, but also naturally formed outside the carbon-based material, so that the silicon coating formed outside the carbon-based material repeatedly expands and contracts during the charge and discharge process, thereby becoming a reason for reducing the cycle characteristics of the secondary battery similar to Patent Document 1.

[0010] Therefore, in the field of secondary batteries, there is still a need to develop an electrode active material and a preparation method thereof that can improve battery capacity and ensure good cycle characteristics.

[0011] (Prior art literature)

[0012] Patent Document 1: Korean Patent No. 10-1628873 (grant date: 2016.06.02)

[0013] Patent Document 2: Korean Patent No. 10-1866004 (grant date: 2018.06.01.) Summary of the invention

[0014] Technical issues

[0015] The present invention is proposed to solve the above-mentioned problems of existing electrode active materials for secondary batteries, and its purpose is to provide an electrode active material for secondary batteries that can improve the capacity of secondary batteries and provide good cycle characteristics, an electrode and a secondary battery including the same, and a method for preparing the above-mentioned electrode active material.

[0016] Solutions to the problem

[0017] To achieve the above-mentioned object, the representative structure of the present invention is as follows.

[0018] According to one embodiment of the present invention, an electrode active material for a secondary battery is provided. The electrode active material according to one embodiment of the present invention can be formed by using a composite having a silicon layer formed on a carbon-based material as a unit powder. According to one embodiment of the present invention, the composite can be configured so that the silicon layer is located inside the carbon-based material and the silicon is not exposed to the outer surface of the carbon-based material or is partially exposed to a part of the outer surface of the carbon-based material, and the silicon layer can include both silicon and carbon.

[0019] According to an embodiment of the present invention, the composite may be configured such that the silicon layer is only located inside the carbon-based material, and the silicon is not exposed to the outer surface of the carbon-based material.

[0020] According to an embodiment of the present invention, the silicon layer may be configured such that the carbon content is 17 wt % to 27 wt % relative to the total weight of the silicon layer.

[0021] According to an embodiment of the present invention, silicon contained in the silicon layer may have a particle size of 0.1 nm to 10 nm.

[0022] According to an embodiment of the present invention, silicon contained in the silicon layer may have a grain size of 2 nm to 5 nm.

[0023] According to an embodiment of the present invention, the silicon layer may be formed in a form using SiC as a substrate and silicon particles are distributed in the SiC substrate.

[0024] According to an embodiment of the present invention, the content of silicon in the composite may be greater than 10 wt % relative to the total weight of the composite.

[0025] According to an embodiment of the present invention, the content of silicon in the composite may be greater than 15 wt % relative to the total weight of the composite.

[0026] According to an embodiment of the present invention, the silicon layer may be formed by simultaneously supplying a first raw material gas containing silicon and a second raw material gas containing carbon to deposit the silicon layer on the carbon-based material.

[0027] According to one embodiment of the present invention, the first silicon-containing raw material gas may include at least one of SiH4, Si2H6, Si3H8, SiCl4, SiHCl3, Si2Cl6, SiH2Cl2, and SiH3Cl, and the second carbon-containing raw material gas may include at least one of C2H4, C2H2, and CH4.

[0028] According to an embodiment of the present invention, the composite further includes a surface layer on the outer peripheral surface.

[0029] According to an embodiment of the present invention, the surface layer may be formed of at least one carbon-based material selected from coal tar pitch, petroleum pitch, epoxy resin, phenolic resin, polyvinyl alcohol, polyvinyl chloride, ethylene, acetylene and methane.

[0030] According to an embodiment of the present invention, a negative electrode for a secondary battery including the electrode active material for a secondary battery may be provided.

[0031] According to one embodiment of the present invention, a secondary battery can be provided, characterized in that it includes: a positive electrode; the negative electrode mentioned above; and an electrolyte located between the positive electrode and the negative electrode.

[0032] According to one embodiment of the present invention, a method for preparing an electrode active material for a secondary battery can be provided. The method for preparing an electrode active material according to one embodiment of the present invention may include: a base material preparation step of preparing a carbon-based material used as a base material; a silicon layer formation step of forming a silicon layer on the surface of the above-mentioned carbon-based material; and a spheroidization step of reassembling the carbon-based material formed with the silicon layer. According to one embodiment of the present invention, in the silicon layer formation step, the silicon layer may be formed so that the silicon layer includes both silicon and carbon, the silicon layer may be positioned inside the carbon-based material by the spheroidization step, and the silicon may not be exposed to the outer surface of the carbon-based material or may be partially exposed to a portion of the outer surface of the carbon-based material.

[0033] According to an embodiment of the present invention, in the step of forming the silicon layer, the silicon layer may be formed by depositing the silicon layer in the form of a thin film layer on the carbon-based material by chemical vapor deposition.

[0034] According to an embodiment of the present invention, in the silicon layer forming step, the silicon layer may be formed by simultaneously supplying a first raw material gas containing silicon and a second raw material gas containing carbon to be deposited in the form of a thin film layer on the carbon-based material.

[0035] According to one embodiment of the present invention, the first silicon-containing raw material gas may include at least one of SiH4, Si2H6, Si3H8, SiCl4, SiHCl3, Si2Cl6, SiH2Cl2, and SiH3Cl, and the second carbon-containing raw material gas may include at least one of C2H4, C2H2, and CH4.

[0036] According to an embodiment of the present invention, in the step of forming the silicon layer, the silicon layer may be formed such that the content of carbon is 17 wt % to 27 wt % relative to the total weight of the silicon layer.

[0037] According to an embodiment of the present invention, silicon contained in the silicon layer may have a particle size of 0.1 nm to 10 nm.

[0038] According to an embodiment of the present invention, silicon contained in the silicon layer may have a grain size of 2 nm to 5 nm.

[0039] According to an embodiment of the present invention, the content of silicon may be greater than 10 wt % relative to the total weight of the composite forming the electrode active material.

[0040] According to an embodiment of the present invention, the content of silicon may be greater than 15 wt % relative to the total weight of the composite forming the electrode active material.

[0041] According to one embodiment of the present invention, in the spheroidization step, the carbon-based material formed with a silicon layer can be put into a spheroidization device, and then polished while rotating at a high speed, and the fragments that fall through the polishing are reassembled to achieve spheroidization, or the carbon-based material formed with a silicon layer is edge cut, or the carbon-based material formed with a silicon layer is bent to wrinkle the material to reassemble the structure and achieve spheroidization.

[0042] According to an embodiment of the present invention, after the spheroidizing step, a surface layer forming step of forming a surface layer on the outer peripheral surface may be further included.

[0043] According to an embodiment of the present invention, a modification step of modifying the surface characteristics of the carbon-based material used as the base material may be further included between the base material preparation step and the silicon layer formation step.

[0044] In addition, the electrode active material for a secondary battery, the electrode (negative electrode) including the same, and the method for preparing a secondary battery and the electrode active material according to the present invention may further include other additional structures within the scope not departing from the technical concept of the present invention.

[0045] Effects of the Invention

[0046] According to one embodiment of the present invention, the electrode active material is formed by a composite formed by mixing a carbon-based material and silicon, so that the silicon contained in the composite is located inside the carbon-based material, and the silicon is not exposed to the outer surface of the carbon-based material, or the silicon is locally located on a part of the outer surface of the composite. Therefore, by including the silicon material in the electrode active material, the capacity and performance of the secondary battery can be improved, and at the same time, the volume expansion of the electrode caused by the expansion and contraction of silicon can be reduced, and the risk of electrical short circuit between the electrode active material and the electrode can be significantly suppressed. Moreover, the phenomenon of accelerating the side reaction between the silicon exposed on the outer surface of the electrode active material and the electrolyte solution can be reduced, thereby greatly improving the performance and life of the secondary battery.

[0047] Furthermore, the electrode active material according to one embodiment of the present invention is configured so that silicon and carbon are located in a carbon-based material used as a matrix material, and therefore, the volume expansion of silicon particles is buffered in the silicon layer formed together with the carbon to further prevent the degradation of the life and performance of the secondary battery due to the expansion and contraction of the silicon particles, and a silicon layer including both silicon and carbon is formed by simultaneously supplying a first raw material gas containing silicon and a second raw material gas containing carbon, so that the particle size of silicon contained in the silicon layer can be formed to be smaller within a predetermined range to more effectively prevent the problem of volume expansion of silicon. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 A transmission electron microscope (TEM) photograph of an electrode active material for a secondary battery (a composite of a carbon-based material and silicon) according to an embodiment of the present invention is schematically shown.

[0049] Figure 2 A scanning electron microscope (SEM) photograph and an energy dispersive spectrometer (EDS) photograph of an electrode active material for a secondary battery according to an embodiment of the present invention are schematically shown.

[0050] Figure 3 Schematically illustrating half-cell performance and related component ratios of an electrode active material for a secondary battery according to an embodiment of the present invention according to a heat treatment state.

[0051] Figure 4 The change in battery performance according to the carbon content contained in the silicon layer is schematically shown.

[0052] Figure 5 Performance experiment results of a case where a silicon layer is formed only inside a carbon-based material and a case where a silicon layer is formed both inside and outside of the carbon-based material are schematically shown.

[0053] Figure 6 The thickness and formation degree of electrolyte decomposition byproducts formed on the surface of the electrode material observed by TEM are schematically shown in the case where the silicon layer is formed only inside the carbon-based material and the case where the silicon layer is formed both inside and outside the carbon-based material.

[0054] Figure 7 The difference in electrode expansion observed by SEM is schematically shown after electrodes are formed using a sample in which a silicon layer is formed only inside a carbon-based material and a sample in which a silicon layer is formed both inside and outside the carbon-based material and charged and discharged 50 times.

[0055] Figure 8The change in the specific surface area characteristics of the carbon-based material (graphite) occurring before and after the modification process is schematically shown. DETAILED DESCRIPTION

[0056] Hereinafter, with reference to the accompanying drawings, preferred embodiments of the present invention will be described in detail to an extent that can be easily implemented by a person skilled in the art to which the present invention belongs.

[0057] In order to clearly illustrate the present invention, the parts irrelevant to the description are omitted. In the full text of the specification, the same figure numerals are marked for the same or similar structural elements. In addition, for the convenience of explanation, the size of each structure shown in the drawings is arbitrarily shown, so the present invention is not limited to the drawings shown. That is, it is necessary to understand that, without departing from the idea and scope of the present invention, the specific shape, structure and characteristic recorded in the specification can be changed from one embodiment to another embodiment, and the position or configuration of individual structural elements can also be changed without departing from the idea and scope of the present invention. Therefore, the detailed description described below is not used to limit the present invention, and the scope of protection of the present invention includes the scope to be protected by the claims in the claims and all scopes equivalent thereto.

[0058] Electrode active material, electrode including the same and secondary battery according to the present invention

[0059] One embodiment of the present invention can provide an electrode active material (negative electrode active material) for a secondary battery formed by mixing a carbon-based material and silicon.

[0060] As described above, graphite-based materials that have been used as negative electrode active materials for lithium secondary batteries have limited capacity and problems such as deterioration of output characteristics during rapid charging, while silicon materials that have attracted much attention as materials to replace graphite have problems in that they have low electrical conductivity and undergo significant volume expansion during charge and discharge, thereby severely damaging the electrode active material and the electrode plate, resulting in a significant reduction in the cycle characteristics of the secondary battery, and therefore are difficult to commercialize.

[0061] In contrast, the electrode active material of one embodiment of the present invention has a structure in which a carbon-based material and silicon are mixed, and thus the battery capacity can be significantly improved compared to existing graphite-based electrode active materials. As will be described below, most of the silicon contained in the electrode active material is located on the inner side of the carbon-based material while the silicon is locally exposed to a portion of the outer surface of the carbon-based material (preferably, the silicon is not exposed to the outer surface of the carbon-based material). Therefore, the problem of silicon being exposed to the electrolyte and causing side reactions during the process of forming an electrode from the electrode active material through a calendering process can be prevented. Moreover, the silicon only expands and contracts inside the carbon-based material, thereby suppressing the problem of reduced life and performance of the secondary battery due to the volume expansion of silicon.

[0062] Furthermore, according to one embodiment of the present invention, the electrode active material is configured so that the silicon layer formed on the carbon-based material contains both silicon and carbon, so that in the process of depositing the silicon layer containing both silicon and carbon by chemical vapor deposition, etc., the silicon particles are formed to be smaller within a predetermined range, thereby reducing the problem of volume expansion of silicon. In addition, the volume expansion of silicon can be reduced by a carbon-containing material (for example, C, SiC, etc.) located around the silicon, thereby more effectively suppressing the problem of degradation of the performance and life of the secondary battery due to the volume expansion of silicon.

[0063] Specifically, the electrode active material according to one embodiment of the present invention can be formed into a composite material in which silicon is mixed in a carbon-based material by using a carbon-based material as a matrix material. The composite material is used as a unit powder for forming an electrode active material for a secondary battery, and a plurality of the composite materials are aggregated to form an electrode active material according to the capacity of the secondary battery.

[0064] According to an embodiment of the present invention, a composite electrode active material may be formed by forming a silicon layer containing silicon on a carbon-based material to form a composite electrode active material containing silicon on a carbon-based material (eg, natural graphite, artificial graphite, hard carbon, etc.).

[0065] According to one embodiment of the present invention, a silicon layer may be formed by being deposited on a carbon-based material by methods such as chemical vapor deposition (CVD), and the silicon layer may be located only inside the carbon-based material while the silicon layer is not exposed on the outer surface of the carbon-based material (even if exposed, it is only partially exposed to a portion of the outer surface).

[0066] As described above, when the composite of the unit powder used to form the electrode active material is configured so that silicon exists only inside and silicon is not exposed on the outer surface, the electrode plate can be prevented from being damaged by the expansion and contraction of the silicon exposed to the outside and the problem of the silicon exposed to the outside contacting the electrolyte and accelerating the side reactions can be prevented, thereby greatly improving the performance and life of the secondary battery.

[0067] According to an embodiment of the present invention, the silicon layer may be formed by injecting a first raw material gas containing silicon and a second raw material gas containing carbon into a reaction chamber where a carbon-based material serving as a mother material is located to deposit the silicon layer in the form of a thin film layer on the carbon-based material.

[0068] For example, a silicon layer can be formed by simultaneously injecting a first silicon-containing raw material gas (e.g., raw material gases of SiH4, Si2H6, Si3H8, SiCl4, SiHCl3, Si2Cl6, SiH2Cl2, SiH3Cl, etc.) and a second carbon-containing raw material gas (e.g., raw material gases of C2H4, C2H2, CH4, etc.) into a reaction chamber heated to a temperature of 400°C to 700°C and depositing them.

[0069] As described above, when a silicon layer is formed by simultaneously supplying a first raw material gas containing silicon and a second raw material gas containing carbon, the silicon layer can be formed in such a way that silicon and carbon exist together in the silicon layer. The volume expansion of silicon that occurs during charging and discharging is alleviated by the carbon present in the silicon layer, thereby suppressing the life and performance degradation of the secondary battery caused by the volume expansion of silicon.

[0070] Furthermore, as described above, when a silicon layer is formed by simultaneously supplying a first raw material gas containing silicon and a second raw material gas containing carbon, the silicon particles contained in the silicon layer can be prevented from agglomerating with each other and coarsening, so that the silicon contained in the silicon layer can be formed to have a small particle size of less than 10 nm (preferably a small particle size of less than 5 nm), and by making the silicon have a small particle size as described above, the problem of shortened life of the secondary battery electrode caused by damage to the volume expansion of silicon can be more effectively prevented.

[0071] According to one embodiment of the present invention, the silicon included in the silicon layer can be formed to have a particle size of 1nm to 10nm, preferably a particle size of 2nm to 5nm. When silicon particles with a large particle size are included in the silicon layer, the stress of the silicon particles increases and the volume expansion of the silicon particles during charging and discharging greatly increases, which may cause the performance and life of the secondary battery to deteriorate. On the contrary, when silicon with an excessively small particle size is included in the silicon layer, the resistance will increase during charging and discharging, which may reduce the performance of the secondary battery. Therefore, preferably, the silicon included in the silicon layer can be formed to have a particle size within the above numerical range.

[0072] According to one embodiment of the present invention, the silicon and carbon contained in the silicon layer may exist in the form of Si, C, and SiC. Preferably, the silicon and carbon formed in the silicon layer exist mostly in the form of Si and SiC and are formed in a form partially containing C. For example, according to one embodiment of the present invention, the silicon layer may be formed to have a structure in which SiC is used as a substrate and Si particles are dispersed on the SiC substrate.

[0073] Generally, since SiC does not contribute substantially to the capacity of a secondary battery, it may be advantageous to have as little SiC as possible in terms of the capacity of the secondary battery. However, in the case where the carbon present in the silicon layer is formed in the form of a mixture of a considerable amount of C and SiC (for example, the case where the silicon layer is deposited at a low temperature below 500°C without sufficiently producing SiC, etc.), when a composite formed by mixing a carbon-based material and silicon is manufactured, the capacity characteristics may be different each time it is produced. Therefore, preferably, in the electrode active material according to one embodiment of the present invention, most of the carbon (C) present in the silicon layer is in a state of reacting with Si to form SiC.

[0074] For example, according to one embodiment of the present invention, a silicon layer can be deposited at a relatively low temperature of 400°C to 700°C using a first raw material gas containing silicon and a second raw material gas containing carbon, and then heat treatment can be performed at a high temperature above 700°C (preferably, above 900°C) to stabilize the silicon layer.

[0075] According to an embodiment of the present invention, the content of carbon (C) contained in the silicon layer may be 17 wt% to 27 wt% relative to the total weight of the silicon layer (in this specification, unless otherwise specified, the content of carbon contained in the silicon layer is the sum of the carbon contents of all particles contained in the silicon layer such as C and SiC). If less than 17 wt% of carbon is contained in the silicon layer, a low capacity retention rate of less than 90% may be exhibited, and if more than 27 wt% of carbon is contained, there is a risk of a sharp decrease in discharge capacity and initial coulombic efficiency.

[0076] For example, Figure 4 Experimental data of discharge capacity, capacity retention rate, initial coulombic efficiency, etc. according to the carbon content formed in the silicon layer in the electrode active material according to one embodiment of the present invention are schematically shown.

[0077] Specifically, Figure 4 It is shown that a silicon thin film layer is deposited on a carbon-based material using a first raw material gas containing silicon and a second raw material gas containing carbon, and then heat treated at a high temperature above 900°C to form a silicon layer with Si and SiC. The experiment provides experimental data on discharge capacity, capacity retention rate, initial coulomb efficiency, etc. based on the content of SiC material.

[0078] Refer to Figure 4 As shown in the experimental results, when the SiC content in the silicon layer is less than 34wt% relative to the total weight of the silicon layer (that is, when the C content in the silicon layer is less than 17% relative to the total weight of the silicon layer), as shown in Figure 4 As shown in parts (a) and (b) of FIG. 1 , it can be confirmed that the capacity retention rate has a low value of less than 90%. In addition, when the SiC content in the silicon layer is greater than 54% relative to the total weight of the silicon layer (that is, when the C content in the silicon layer is greater than 27% relative to the total weight of the silicon layer), as shown in parts (a) and (b) of FIG. Figure 4 As shown in part (a) of FIG. 1 , it can be confirmed that the discharge capacity is greatly reduced, or as Figure 4 As shown in part (b) of FIG. 1 , it can be confirmed that the initial coulombic efficiency is greatly reduced. Therefore, as described above, the carbon content contained in the silicon layer is preferably 17 wt % to 27 wt % relative to the total weight of the silicon layer.

[0079] According to an embodiment of the present invention, the content of silicon contained in the composite constituting the electrode active material may be greater than 10 wt %, preferably greater than 15 wt %, relative to the total weight of the composite.

[0080] Since silicon can provide a larger capacity than graphite, the greater the silicon content in the electrode active material, the higher the capacity of the secondary battery, but the silicon contained in the electrode active material may significantly reduce the cycle characteristics of the secondary battery due to expansion that occurs during charge and discharge, so there may be limitations to increasing the amount of silicon added to the electrode active material.

[0081] For example, in a silicon-graphite composite electrode active material known in the prior art, the electrode active material actually contains a small amount of silicon due to the problem of deterioration of the cycle characteristics of a secondary battery caused by expansion and contraction of silicon.

[0082] However, in the electrode active material of one embodiment of the present invention, most of the silicon is located inside the carbon-based material and the silicon is not exposed to the outer surface of the carbon-based material. Therefore, even if more than 10wt% (preferably more than 15wt%) of silicon is included in the electrode active material, surface cracking due to expansion and contraction of silicon can be suppressed, thereby enabling more silicon and carbon-based materials such as graphite to be mixed to form a composite to further increase the capacity of the secondary battery.

[0083] According to one embodiment of the present invention, a surface layer may be further included on the outer circumference of the composite of the carbon-based material and silicon. The surface layer formed on the outer circumference of the composite may improve the conductivity by providing an electron transfer path and suppress the volume change of silicon during charge and discharge to perform the function of improving the stability of the electrode plate.

[0084] According to one embodiment of the present invention, the surface layer formed on the outer peripheral surface of the composite can be formed by a heterogeneous carbon material (for example, at least one carbon material selected from coal tar pitch, petroleum asphalt, epoxy resin, phenolic resin, polyvinyl alcohol, polyvinyl chloride, ethylene, acetylene and methane) that is different from the carbon-based material (parent material) constituting the composite.

[0085] However, the surface layer is not necessarily provided, and the electrode active material may be formed by omitting the surface layer, or an additional coating layer (conductive coating layer, etc.) may be formed in addition to the above-mentioned carbon material surface layer.

[0086] On the other hand, according to an embodiment of the present invention, an electrode (negative electrode) and a secondary battery including the electrode active material may be provided.

[0087] Specifically, an electrode and a secondary battery of one embodiment of the present invention may include an electrode active material formed by a composite of the above-mentioned carbon-based material and silicon, and the composite of the carbon-based material and silicon forming the electrode active material may be formed in a structure in which silicon is mixed inside the carbon-based material as described above, and the silicon may be configured to be positioned together with the carbon.

[0088] According to this structure, the silicon-graphite composite can be formed into a mixed structure in which silicon is located inside the carbon-based material, which can increase the battery capacity through silicon and effectively suppress the problem of reducing the performance and life of the secondary battery due to the volume expansion of silicon and contact with the electrolyte. The volume expansion of silicon is alleviated by the carbon material around the silicon, so as to further solve the problem of battery performance degradation caused by the volume expansion of silicon.

[0089] For example, Figures 5 to 7 Performance comparison between a case where a silicon layer is formed only inside a carbon-based material (eg, graphite) and a case where a silicon layer is formed both inside and outside of a carbon-based material (eg, graphite) is schematically shown.

[0090] Specifically, if Figure 5 As shown, as in the electrode active material according to one embodiment of the present invention, when the silicon layer is located only on the inner side of the carbon-based material, compared with the case where the silicon layer is formed on both the inner side and the outer side of the carbon-based material, when the electrode active material is formed in a manner having the same battery capacity, as shown in FIG. Figure 5 As shown in (b), it can be confirmed that the coulombic efficiency is higher [for example, when the silicon layer is located only inside the carbon-based material, a coulombic efficiency of 99.8% is exhibited after 50 charge and discharge cycles].

[0091] Furthermore, as in the case of the electrode active material according to one embodiment of the present invention, when the silicon layer is located only on the inner side of the carbon-based material, compared with the case where the silicon layer is formed on both the inner side and the outer side of the carbon-based material, as shown in FIG. Figure 6 As shown, it can be confirmed that less side reaction by-products are formed by the reaction with the electrolyte [ Figure 6 The sample in which the silicon layer is formed inside and outside the carbon-based material shown in part (b) is different from the sample in which the silicon layer is formed inside and outside the carbon-based material. Figure 6 Compared with the sample in which only a silicon layer is formed inside the carbon-based material as shown in part (a) of , a thicker side reaction by-product layer (a layer containing impurities such as F, P, etc.) is formed].

[0092] Furthermore, as in the case of the electrode active material according to one embodiment of the present invention, when the silicon layer is only located inside the carbon-based material, if the electrode is formed and charged and discharged 50 times, Figure 7 The electrode expansion shown occurs less than in the case where the silicon layer is formed both inside and outside the carbon-based material. Figure 7 As shown in part (a) of FIG. 1 , in the case where a silicon layer is formed inside the carbon-based material, the electrode expansion rate is 40% after 50 cycles of charge and discharge, but Figure 7 As shown in part (b), when silicon layers are formed on both the inside and outside of the carbon-based material, the electrode expansion rate is 66% after 50 cycles of charge and discharge.

[0093] On the other hand, the electrode active material of one embodiment of the present invention can be used not only alone to form a secondary battery, but also mixed with an existing electrode active material (for example, an electrode active material formed of a graphite-based material) to form an electrode active material for a secondary battery.

[0094] As described above, the electrode active material of one embodiment of the present invention can stably control problems such as electrode damage caused by the volume expansion of silicon. Therefore, compared with the past, a larger amount of silicon is included in the electrode active material to be able to fully amplify the battery capacity. Therefore, even if mixed with conventional electrode active materials, it can provide a capacity improvement effect that is substantially improved compared with the past. On the contrary, the volume expansion problem caused by silicon is more effectively controlled by conventional electrode active materials such as electrode active materials formed of graphite-based materials.

[0095] Preparation method of electrode active material according to the present invention

[0096] One embodiment of the present invention provides a method for preparing an electrode active material (specifically, a composite of a carbon-based material and silicon) formed by mixing silicon into a carbon-based material.

[0097] According to one embodiment of the present invention, a method for preparing an electrode active material (a 'composite of a carbon-based material and silicon' constituting the electrode active material) may include: a base material preparation step of preparing a carbon-based material (e.g., plate-like graphite); a silicon layer formation step of forming a silicon layer on the prepared carbon-based material; and a spheroidization step of reassembling the carbon-based material having a silicon layer by mechanically crushing or polishing the carbon-based material having a silicon layer or by edge cutting or bending the carbon-based material.

[0098] The matrix material preparation step is a step of preparing a carbon-based material used as a basic matrix material of an electrode active material of one embodiment of the present invention, wherein the matrix material can be, for example, natural or artificial graphite, hard carbon, etc., for example, can be formed by a material having a particle size of 2μm to 20μm.

[0099] The silicon layer forming step is a step of forming a silicon layer on the carbon-based material serving as a matrix material in order to increase the capacity of the electrode active material. The silicon layer can be formed in a thin film shape on the surface of the carbon-based material by chemical vapor deposition or the like.

[0100] Specifically, the silicon layer can be formed by injecting a first raw material gas containing silicon and a second raw material gas containing carbon into a reaction chamber heated to a temperature of 400°C to 700°C and depositing the silicon layer on the surface of a carbon-based material used as a mother material, and can be formed by simultaneously supplying a first raw material gas containing silicon such as SiH4, Si2H6, Si3H8, SiCl4, SiHCl3, Si2Cl6, SiH2Cl2, SiH3Cl, etc. and a second raw material gas containing carbon such as C2H4, C2H2, CH4, etc. to a reaction chamber heated to a temperature of 400°C to 700°C to deposit the silicon layer in the form of a thin film layer on the surface of the carbon-based material.

[0101] According to the method as described above, by simultaneously supplying a first raw material gas containing silicon and a second raw material gas containing carbon for deposition, a silicon layer can be formed that contains both silicon and carbon. In this process, silicon particles in the silicon layer can be prevented from agglomerating and becoming coarse, so that the silicon particles can be formed to have a small particle size.

[0102] According to one embodiment of the present invention, the content of silicon contained in the composite forming the electrode active material may be greater than 10wt% relative to the total weight of the composite, preferably greater than 15wt%, and the silicon layer containing silicon may be formed in the form of a thin film layer having a thickness ranging from 20nm to 500nm. In addition, in the silicon layer, the content of carbon may be 17wt% to 27wt% relative to the total weight of the silicon layer.

[0103] The spheroidization step performs the function of spheroidizing the carbon-based material formed with the silicon layer and reassembling the structure. Through the above-mentioned spheroidization step, the silicon layer deposited on the surface of the carbon-based material can be reassembled in such a manner that it moves to the inside of the carbon-based material and is positioned.

[0104] For example, in the spheroidization step, the carbon-based material deposited with a silicon layer is injected into a machine equipped with a rotating rotor and blades, polished while rotating at a high speed, and the fragments fallen by the polishing are reassembled to achieve spheroidization, or the carbon-based material deposited with a silicon layer is reassembled by crushing and pressurizing it, or the carbon-based material deposited with a silicon layer is edge cut or bent to wrinkle the material and reassemble the structure to achieve spheroidization.

[0105] According to one embodiment of the present invention, in the spheroidization step, in order to prevent the carbon-based material or silicon from being oxidized due to the strong friction heat generated during the reassembly process of the carbon-based material having the silicon layer, the spheroidization can be performed while the internal atmosphere is replaced with an inert gas such as N2 or Ar. In order to improve the bonding force between the carbon-based material and the silicon layer, the spheroidization can be performed while adding coal tar pitch, petroleum pitch, epoxy resin, phenolic resin, polyvinyl alcohol, polyvinyl chloride, etc. as an adhesive.

[0106] On the other hand, according to one embodiment of the present invention, after preparing the carbon-based material used as the mother material, before forming the silicon layer on the carbon-based material, a modification step of modifying the surface characteristics of the carbon-based material may be further included. The modification is a step of preventing silicon from flowing into the micropores in the space where it is difficult to ensure silicon expansion by filling the micropores of the carbon-based material used as the mother material. When the modification process is performed, the micropores of 50 nm or less formed on the mother material of the carbon-based material are filled with different kinds of amorphous or crystalline carbon, so that the specific surface area of ​​the mother material of the carbon-based material is reduced (when the modification process is performed, the micropores inside the carbon-based material used as the mother material are filled with different kinds of amorphous or crystalline carbon, so that, as Figure 8 As shown, the specific surface area will be reduced to 2 to 10 m 2 / g to 1~5m 2 / g), whereby the silicon layer can be formed only in the large cavities existing inside the carbon-based material used as the base material and outside the carbon-based material. The silicon layer formed in the micropores may induce cracking of the carbon-based material such as graphite used as the base material because there is not enough space for silicon to expand. However, if the silicon layer is modified, the silicon layer is prevented from being formed in the above-mentioned micropores, thereby further suppressing the damage of the electrode active material and the electrode including the same.

[0107] According to one embodiment of the present invention, the modification process can be performed by coating the precursors of petroleum asphalt, coal tar pitch, resin, asphalt, methane, ethylene and acetylene on the surface of the carbon-based material used as the mother material. For example, the precursors of petroleum asphalt, coal tar pitch, resin, asphalt, etc. can be coated on the carbon-based material (mother material) by using a rotary furnace or an atmosphere furnace, etc., and the coating can be performed by keeping the material in a temperature range of 600°C to 1,000°C for 2 hours or more in an inert gas atmosphere such as N2, Ar, etc. On the other hand, precursors such as methane, ethylene and acetylene can be coated on the carbon-based material used as the mother material by using a vapor deposition device or a rotary furnace, etc., for example, the precursor is supplied to the carbon-based material at a flow rate of 3L to 8L per minute at a temperature of 800°C to 1,000°C to coat the precursor on the surface.

[0108] The electrode active material of one embodiment of the present invention prepared in the manner described above is formed in a state where silicon is stably located inside a carbon-based material such as graphite, thereby reducing the risk of silicon contacting the electrolyte to produce side reactions and further improving the performance and life of the electrode and secondary battery.

[0109] According to an embodiment of the present invention, after the reassembly step, the reassembled carbon-based material and silicon composite can be further integrated into a structure by heat treatment, thereby further improving the structural stability of the silicon layer containing silicon and carbon.

[0110] As described above, when a silicon layer is deposited on the surface of a carbon-based material at a temperature range of 400°C to 700°C in the silicon layer forming step, the first raw gas containing silicon is actively decomposed to perform deposition, but the second raw gas containing carbon may not be fully decomposed, and only a small amount is decomposed and deposited. During these processes, a small amount of carbon reacts with silicon to form a SiC compound.

[0111] However, when the silicon layer is formed in this manner, as a result of manufacturing samples and evaluating performance, non-uniform capacity is formed for each production, and there is a possibility that problems may arise in terms of suitability for large-scale production processes and commercialization.

[0112] In contrast, when an additional heat treatment process is performed at a temperature range of 700° C. or higher (preferably, 900° C. or higher) after forming the silicon layer, the silicon layer is stabilized, so that an electrode active material having uniform properties can be prepared.

[0113] For example, Figure 3 The experimental results show that after simultaneously supplying a first raw gas containing silicon and a second raw gas containing carbon to form a silicon layer under a temperature environment of 475°C, additional heat treatment is performed at temperatures of 650°C, 800°C, and 900°C, respectively, and then the capacity, composition, etc. of the electrode active material are analyzed.

[0114] like Figure 3 As shown in FIG. 1 , when heat treatment is performed at a high temperature after forming the silicon layer, silicon and carbon contained in the silicon layer react to form SiC. At this time, SiC cannot perform the function of generating capacity in the secondary battery, so when SiC is generated as described above, the performance of the secondary battery is reduced. For example, Figure 5 As shown, after the silicon layer is formed, the higher the temperature at which the heat treatment is performed, the more carbon reacts with silicon to form SiC, so that Si decreases and SiC increases, and thus the battery capacity gradually decreases.

[0115] However, when a heat treatment process is performed in a high temperature environment after forming the silicon layer, the silicon layer is stabilized, so that an electrode active material with the same performance can be manufactured when the electrode active material is repeatedly produced. Thus, for the commercialization of the electrode active material according to an embodiment of the present invention, even if the initial battery capacity is slightly reduced, it may be advantageous to stabilize the silicon layer by forming a silicon layer containing silicon and carbon under a temperature environment of 400° C. to 700° C. and then performing a heat treatment at a high temperature of 700° C. or above (more preferably, 900° C. or above).

[0116] On the other hand, according to one embodiment of the present invention, a surface layer forming step of forming a surface layer on the outer peripheral surface of the composite of carbon-based material and silicon formed by the process as described above can also be performed. These surface layers can improve electrical conductivity to perform the function of improving the performance and life of the electrode active material according to one embodiment of the present invention and the electrode and secondary battery including the same.

[0117] According to one embodiment of the present invention, the surface layer can be formed by forming a carbon material (for example, a heterogeneous carbon material different from the carbon-based material used as the parent material of the composite: coal tar pitch, petroleum pitch, epoxy resin, phenolic resin, polyvinyl alcohol, polyvinyl chloride, ethylene, acetylene and methane, etc.) on the surface of the above-mentioned composite formed by mixing carbon-based materials and silicon. However, the surface layer is not necessarily provided, and the surface coating can be omitted to form an electrode active material, or an additional coating (conductive coating, etc.) can be formed in addition to the above-mentioned carbon material surface layer.

[0118] Specific embodiments of the electrode active material according to the present invention

[0119] ① Embodiment 1 (GPS-1)

[0120] First, a carbon-based material is prepared in the form of a plate-like graphite material with an average particle size of 4 μm. Next, 10 g of the prepared carbon-based material is added to a rotary furnace, the vacuum inside the rotary furnace is replaced with a nitrogen atmosphere, the temperature is raised to 550°C, and then SiH4 and CH4 flow for about 20 minutes to coat the silicon layer on the carbon-based material. After that, the carbon-based material deposited with the silicon layer is placed in a spheroidizing device for reassembly. As for reassembly, the carbon-based material deposited with the silicon layer is placed in a spheroidizing device and bending is applied, so that the composite is mechanically reassembled in a manner that the silicon layer is moved to the inside of the carbon-based material and positioned.

[0121] ②Example 2 (GPS-2)

[0122] First, a carbon-based material is prepared in the form of a plate-like graphite material with an average particle size of 4 μm. Next, 10 g of the prepared carbon-based material is added to a rotary furnace, the vacuum inside the rotary furnace is replaced with a nitrogen atmosphere, the temperature is raised to 550°C, and then SiH4 and CH4 flow for about 20 minutes to coat the silicon layer on the carbon-based material. After that, the carbon-based material deposited with the silicon layer is placed in a spheroidizing device for reassembly. As for reassembly, the carbon-based material deposited with the silicon layer is placed in a spheroidizing device and bending is applied, so that the composite is mechanically reassembled in a manner that the silicon layer moves to the inside of the carbon-based material and is positioned. After reassembly, the reassembled composite is placed in a reaction chamber, the temperature is raised to 675°C for heat treatment, and then air-cooled.

[0123] ③Example 3 (GPS-3)

[0124] First, a carbon-based material is prepared in the form of a plate-like graphite material with an average particle size of 4 μm. Next, 10 g of the prepared carbon-based material is added to a rotary furnace, the vacuum inside the rotary furnace is replaced with a nitrogen atmosphere, the temperature is raised to 550°C, and then SiH4 and CH4 flow for about 20 minutes to coat the silicon layer on the carbon-based material. After that, the carbon-based material deposited with the silicon layer is placed in a spheroidizing device for reassembly. As for reassembly, the carbon-based material deposited with the silicon layer is placed in a spheroidizing device and bending is applied, so that the composite is mechanically reassembled in a manner that the silicon layer moves to the inside of the carbon-based material and is positioned. After reassembly, the reassembled composite is placed in a reaction chamber, the temperature is raised to 800°C for heat treatment, and then air-cooled.

[0125] ④ Embodiment 4

[0126] First, a carbon-based material is prepared in the form of a plate-like graphite material with an average particle size of 4 μm. Next, 10 g of the prepared carbon-based material is added to a rotary furnace, the vacuum inside the rotary furnace is replaced with a nitrogen atmosphere, the temperature is raised to 550°C, and then SiH4 and CH4 flow for about 20 minutes to coat the silicon layer on the carbon-based material. After that, the carbon-based material deposited with the silicon layer is placed in a spheroidizing device for reassembly. As for reassembly, the carbon-based material deposited with the silicon layer is placed in a spheroidizing device and bending is applied, so that the composite is mechanically reassembled in a manner that the silicon layer is moved to the inside of the carbon-based material and positioned. After reassembly, the reassembled composite is placed in a reaction chamber, the temperature is raised to 900°C for heat treatment, and then air-cooled.

[0127] According to the results of the performance test using the electrode active material prepared as described above, Figure 3As shown, the electrode active material of one embodiment of the present invention can ensure high capacity and provide good cycle characteristics as a whole, and the electrode active material according to one embodiment of the present invention is different from the prior art and can stably maintain a capacity retention rate of 90% or higher after 50 charge and discharge cycles.

[0128] The present invention is described above using specific details such as specific structural elements and limited embodiments and figures, but this is only provided to help understand the present invention more as a whole. The present invention is not limited to the above-mentioned embodiments. Any technician in the technical field to which the present invention belongs can make various modifications and changes based on such descriptions.

[0129] Therefore, the concept of the present invention is not limited to the embodiments described above. Not only the scope of the patent claims described below belongs to the concept of the present invention, but all scopes that are equal to or equivalent to the patent scope also belong to the concept of the present invention.

Claims

1. An electrode active material for a secondary battery, which is an electrode active material for a secondary battery, characterized in that the electrode active material for a secondary battery is formed by using a composite having a silicon layer formed on a carbon-based material as a unit powder, The composite is configured such that the silicon layer is located inside the carbon-based material and the silicon is not exposed to the outer surface of the carbon-based material or is partially exposed to a portion of the outer surface of the carbon-based material. The silicon layer includes both silicon and carbon. The silicon layer is formed by simultaneously supplying a first source gas containing silicon and a second source gas containing carbon to deposit the silicon layer on the carbon-based material.

2. The electrode active material for a secondary battery according to claim 1, It is characterized in that The composite is configured such that the silicon layer is only located inside the carbon-based material and the silicon is not exposed to the outer surface of the carbon-based material.

3. The electrode active material for a secondary battery according to claim 1, It is characterized in that The silicon layer is configured such that a carbon content is 17 wt % to 27 wt % relative to a total weight of the silicon layer.

4. The electrode active material for a secondary battery according to claim 3, It is characterized in that The silicon contained in the silicon layer has a particle size of 0.1 nm to 10 nm.

5. The electrode active material for a secondary battery according to claim 4, It is characterized in that The silicon contained in the silicon layer has a particle size of 2 nm to 5 nm.

6. The electrode active material for a secondary battery according to claim 4, It is characterized in that The silicon layer is formed using SiC as a base material and silicon particles are distributed in the SiC base material.

7. The electrode active material for a secondary battery according to claim 4, It is characterized in that The content of silicon in the composite is greater than 10 wt % relative to the total weight of the composite.

8. The electrode active material for a secondary battery according to claim 7, It is characterized in that The content of silicon in the composite is greater than 15 wt % relative to the total weight of the composite.

9. The electrode active material for a secondary battery according to claim 1, It is characterized in that The first silicon-containing raw material gas includes SiH 4 、Si 2 H 6 、Si 3 H 8 、SiCl 4 、SiHCl 3 、Si 2 Cl 6 、SiH 2 Cl 2 、SiH 3 Cl, the carbon-containing second raw material gas includes C 2 H 4 , C 2 H 2 , CH 4 At least one of .

10. The electrode active material for a secondary battery according to claim 9, It is characterized in that The composite further includes a surface layer on the outer peripheral surface.

11. The electrode active material for a secondary battery according to claim 10, It is characterized in that The surface layer is formed of at least one carbon-based material selected from coal tar pitch, petroleum pitch, epoxy resin, phenolic resin, polyvinyl alcohol, polyvinyl chloride, ethylene, acetylene and methane.

12. A negative electrode for a secondary battery, It is characterized in that The invention comprises the electrode active material for a secondary battery according to any one of claims 1 to 11.

13. A secondary battery, It is characterized in that include: positive electrode; The negative electrode as claimed in claim 12; and The electrolyte is located between the positive electrode and the negative electrode.

14. A method for preparing an electrode active material, which is a method for preparing an electrode active material for a secondary battery, wherein the method for preparing the electrode active material is characterized in that: include: a base material preparation step of preparing a carbon-based material to be used as a base material; A silicon layer forming step, forming a silicon layer on the carbon-based material; and The spheroidization step reassembles the carbon-based material formed with the silicon layer. In the silicon layer forming step, the silicon layer is formed so that the silicon layer includes both silicon and carbon, and the silicon layer is formed by simultaneously supplying a first raw material gas containing silicon and a second raw material gas containing carbon to deposit on the carbon-based material in the form of a thin film layer. The silicon layer is positioned inside the carbon-based material through the spheroidization step, and the silicon is not exposed to the outer surface of the carbon-based material or is partially exposed to a portion of the outer surface of the carbon-based material.

15. The method for preparing an electrode active material according to claim 14, It is characterized in that In the above-mentioned silicon layer forming step, the silicon layer is formed by being deposited in the form of a thin film layer on the carbon-based material by chemical vapor deposition.

16. The method for preparing an electrode active material according to claim 14, It is characterized in that The first silicon-containing raw material gas includes SiH 4 、Si 2 H 6 、Si 3 H 8 、SiCl 4 、SiHCl 3 、Si 2 Cl 6 、SiH 2 Cl 2 、SiH 3 Cl, the carbon-containing second raw material gas includes C 2 H 4 , C 2 H 2 , CH 4 At least one of .

17. The method for preparing an electrode active material according to claim 16, It is characterized in that In the above-mentioned silicon layer forming step, the silicon layer is formed so that the content of carbon is 17 wt % to 27 wt % with respect to the total weight of the silicon layer.

18. The method for preparing an electrode active material according to claim 17, It is characterized in that The silicon contained in the silicon layer has a particle size of 0.1 nm to 10 nm.

19. The method for preparing an electrode active material according to claim 18, It is characterized in that The silicon contained in the silicon layer has a particle size of 2 nm to 5 nm.

20. The method for preparing an electrode active material according to claim 18, It is characterized in that The content of silicon is greater than 10 wt % relative to the total weight of the composite forming the electrode active material.

21. The method for preparing an electrode active material according to claim 20, It is characterized in that The content of silicon is greater than 15 wt % relative to the total weight of the composite forming the electrode active material.

22. The method for preparing an electrode active material according to claim 18, It is characterized in that In the above-mentioned spheroidization step, the carbon-based material formed with the silicon layer is put into the spheroidization equipment, and then polished while rotating at a high speed, and the fragments fallen by polishing are reassembled to achieve spheroidization, or the carbon-based material formed with the silicon layer is trimmed, or the carbon-based material is bent to wrinkle the material to reassemble the structure and achieve spheroidization.

23. The method for preparing an electrode active material according to claim 22, It is characterized in that After the spheroidizing step, a surface layer forming step of forming a surface layer on the outer peripheral surface is further included.

24. The method for preparing an electrode active material according to claim 23, It is characterized in that A modification step of modifying the surface characteristics of the carbon-based material used as the base material is further included between the base material preparation step and the silicon layer formation step.