A coarse grinding honing oilstone and its preparation method and application
By using coarse grinding and honing oilstones prepared from pure copper, tin, bronze and abrasive materials, combined with ball milling and sintering processes, the problems of low efficiency and poor accuracy of oilstones in the existing technology are solved, and an efficient and high-precision engine block is achieved Rough grinding ensures processing quality and reliability.
Patent Information
- Application Number
- CN202110717146.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-06-28
AI Technical Summary
The oil stone used in the rough grinding process of the engine block in the prior art has low efficiency and poor accuracy, resulting in poor surface integrity of the workpiece, uneven inner hole texture, large internal stress, and low reliability.
Using a coarse honing oil stone composed of pure copper, tin, bronze, abrasives and wetting agents, it is prepared through pre-mixed powder, ball milling and sintering processes to ensure the material particle size and purity, and is combined with a fully automatic hot press imported from Germany for sintering to improve Powder surface activity and crystal quality, add diamond powder for mixing and sintering.
It achieves efficient and high-precision rough grinding of the engine cylinder, ensures the integrity of the processed surface and the uniformity of the texture, and improves the reliability of the honing process.
Smart Images

Figure BDA0003135419620000031 
Figure BDA0003135419620000041
Abstract
Description
Technical Field
[0001] The invention belongs to the field of abrasive moulds, and in particular relates to a rough grinding and honing oilstone and a preparation method and application thereof. Background Art
[0002] Whetstone is a strip-shaped bonded abrasive made of abrasives and binders. It is embedded in the honing rod or honing head to finish the surface of the finished workpiece. It can process the inner and outer surfaces of cylindrical holes, planes, spherical surfaces, etc. It has the characteristics of high processing accuracy, good surface integrity, and a wide range of processing. Whetstone is one of the important factors affecting processing quality, and its quality directly affects the quality of the product.
[0003] For workpieces of different materials or machining precision, targeted oilstones need to be selected for machining. For engine cylinder honing, rough grinding is usually performed first, and then fine grinding. Rough grinding refers to grinding to remove the excess when the workpiece has a large allowance. Usually, when the allowance is 5-20 threads, rough grinding should be used first to control the allowance below 3-5 threads; fine grinding refers to the grinding method used when the workpiece has a small machining allowance and high precision requirements. Fine grinding removes less allowance, leaves less residual stress on the workpiece surface, has good surface integrity, low roughness, and high precision. Therefore, two different oilstones are used for rough grinding and fine grinding.
[0004] However, the oilstones currently used in the rough grinding process of engine cylinder blocks on the market have low efficiency and poor precision, poor surface integrity of the workpiece, uneven pore patterns in the cylinder body, large internal stress and low reliability. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a rough grinding honing oilstone with high efficiency and high precision for rough grinding of engine cylinder blocks and a preparation method thereof.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A rough grinding and honing oil stone, the raw material formula of the oil stone includes pure copper, tin, bronze, abrasive and wetting agent, wherein the tin accounts for 10-20% of the total mass of the raw material formula, the bronze accounts for 8-13% of the total mass of the raw material formula, the abrasive accounts for 10-15% of the total mass of the raw material formula, the wetting agent accounts for 1-5% of the total mass of the raw material formula, and the balance is the pure copper.
[0008] According to some preferred aspects of the present invention, the raw material formula of the oilstone consists of the following components in percentage by mass: 55-65% pure copper, 10-20% tin, 8-13% bronze, 10-15% abrasive and 1-5% wetting agent.
[0009] According to some implementation aspects of the present invention, the abrasive is diamond powder with a particle size of 0.1 to 0.15 mm.
[0010] According to some implementation aspects of the present invention, the bronze is bronze 663 powder, with a particle size of 0.04-0.06 mm and a purity greater than or equal to 99.8%.
[0011] According to some implementation aspects of the present invention, the pure copper is pure copper powder, the particle size of which is 0.01-0.02 mm and the purity is greater than or equal to 99.9%.
[0012] According to some implementation aspects of the present invention, the tin is tin powder, the particle size of which is 0.02-0.03 mm and the purity is greater than or equal to 99.9%.
[0013] According to some implementation aspects of the present invention, the wetting agent is a combination of one or more of paraffin, PVA, and ethanol.
[0014] Another technical solution adopted by the present invention: The preparation method of the above-mentioned rough grinding honing oilstone includes the steps of mixing pure copper, tin and bronze, adding a wetting agent for ball milling, then adding abrasive and mixing evenly, sintering at 600-700°C and a pressure of 8-12MPa to obtain the oilstone.
[0015] Furthermore, the ball milling is carried out in a ball mill for 1 to 3 hours; and the adding of abrasives and mixing are carried out in a mixer for 1 to 3 hours.
[0016] The present invention adopts specific metal (pure copper, tin, bronze) powder premixing, the particle size and purity of each powder are strictly controlled, a wetting agent is added after the premixed powder is mixed, ball milling is performed to improve the surface activity of the powder, promote sintering crystallization, and facilitate sintering, and then abrasive is added to mix, and then sintering is performed.
[0017] The sintering was performed using a fully automatic hot press DSP510 imported from Germany.
[0018] Another technical solution adopted by the present invention is the application of the rough grinding honing oilstone in the honing process of the engine cylinder block, which can realize the controllable parameters of the cylinder block platform reticulation and meet the requirements of high-speed, high-efficiency and high-precision honing rough grinding process.
[0019] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0020] The present invention utilizes a mixture of pure copper, tin and bronze, in combination with abrasives and wetting agents, to prepare a rough grinding oilstone which is not only highly efficient but also highly precise during honing. The rough grinding oilstone is used in the honing of an engine cylinder block to ensure the surface integrity and the uniformity of the mesh pattern of the honing cylinder block. DETAILED DESCRIPTION
[0021] The specific implementation of the present invention is further described in detail below in conjunction with specific embodiments, but the implementation and protection scope of the present invention are not limited thereto.
[0022] Example 1
[0023] The rough honing oilstone for rough honing of engine cylinder block provided in this embodiment is composed of the following components: 60% pure copper, 15% tin, 10% bronze 663, 13% diamond and 2% wetting agent, wherein the pure copper is pure copper powder with a particle size of 0.01mm and a purity of 99.9%; the tin is atomized tin powder with a particle size of 0.02mm and a purity of 99.9%; the bronze 663 is powder with a particle size of 0.04mm and a purity of 99.8%; the diamond is powder with a particle size of 0.1-0.12mm; and the wetting agent is liquid paraffin.
[0024] The preparation method of oilstone is: mix pure copper powder, tin powder and bronze powder evenly, then add a wetting agent and ball mill in a ball mill for 2 hours to increase the surface activity of the powder, then add abrasive diamond, mix in a mixer for 2 hours, then weigh, transfer and sinter to obtain the oilstone. The sintering machine uses the fully automatic hot press DSP510 imported from Germany, with precise temperature control and uniform heating. The sintering temperature is 660℃ and the pressure is 10MPa.
[0025] Example 2
[0026] The rough honing oilstone for rough honing of the engine cylinder block provided in this embodiment is composed of the following components: 62% pure copper, 12% tin, 12% bronze 663, 12% diamond and 2% wetting agent, wherein the particle size of the pure copper is 0.015 mm, the particle size of the tin is 0.015 mm, and the particle size of the bronze is 0.05 mm.
[0027] Others are the same as in Example 1
[0028] Example 3
[0029] The rough grinding oilstone for honing and rough grinding of the engine cylinder block provided in this embodiment is composed of the following components: 58% pure copper, 18% tin, 11% bronze 663, 10% diamond and 3% wetting agent, and the rest is the same as in Example 1.
[0030] Example 4
[0031] The rough honing oilstone for rough honing of the engine cylinder block provided in this embodiment is composed of the following components: 60% pure copper, 13% tin, 13% bronze 663, 12% diamond and 2% wetting agent, and the rest is the same as in Example 1.
[0032] The rest is the same as in Example 1.
[0033] Comparative Example 1
[0034] The coarse grinding honing oilstone provided in this comparative example is the same as that in Example 1, except that no wetting agent is added.
[0035] Its specific raw material composition is: 62% pure copper, 15% tin, 10% bronze 663 and 13% diamond.
[0036] Comparative Example 2
[0037] The rough grinding honing oil stone provided in this comparative example has a specific raw material composition of: 70% pure copper, 15% tin, 2% bronze 663, 10% diamond and 2% wetting agent.
[0038] The rest is the same as in Example 1.
[0039] Comparative Example 3
[0040] The rough grinding honing oilstone provided in this comparative example has a specific raw material composition of: 62% pure copper, 17% tin, 13% bronze 663, 5% diamond and 3% wetting agent.
[0041] The rest is the same as in Example 1.
[0042] Comparative Example 4
[0043] The particle size of the pure copper powder in the rough grinding honing oilstone provided in this comparative example is 0.01 mm, the particle size of the tin powder is 0.01 mm, and the particle size of the bronze powder is 0.08 mm. Others are the same as in Example 1.
[0044] Performance Testing
[0045] The oilstones of Examples 1 to 4 and Comparative Examples 1 to 4 were used to perform a grinding test on the same engine cylinder block. The results are shown in Table 1.
[0046] Table 1 shows the performance test results of the oilstones of Examples 1 to 4 and Comparative Examples 1 to 4
[0047]
[0048]
[0049] In Table 1, the test method for relative density is: GB / T 4472-2011.
[0050] The test method for Rockwell hardness is: GB / T 230.1-2004.
[0051] The test method for flexural strength is: GB / T232-2010.
[0052] The test method for grinding efficiency test is: GB / T 10155-1999.
[0053] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A rough grinding honing oilstone for honing engine cylinder block, It is characterized in that The raw material formula of the oilstone is composed of the following components by mass percentage: 55-65% pure copper, 10-20% tin, 8-13% bronze, 10-15% abrasive and 1-5% wetting agent; The abrasive is diamond powder; The bronze is bronze 663 powder with a particle size of 0.04 to 0.06 mm and a purity greater than or equal to 99.8%; The pure copper is pure copper powder with a particle size of 0.01 to 0.02 mm and a purity greater than or equal to 99.9%; The tin is tin powder with a particle size of 0.02 to 0.03 mm and a purity greater than or equal to 99.9%; The wetting agent is a combination of one or more of paraffin, PVA, and ethanol; The preparation method of the rough grinding honing oilstone comprises the steps of mixing pure copper, tin and bronze, adding a wetting agent for ball milling, adding abrasive and mixing evenly, sintering at 600-700° C. and a pressure of 8-12 MPa to obtain the oilstone.
2. The method for preparing the rough grinding honing oilstone according to claim 1, Features: The method comprises the steps of mixing pure copper, tin and bronze, adding a wetting agent for ball milling, adding abrasive and mixing evenly, sintering at 600-700° C. and a pressure of 8-12 MPa to prepare the oilstone.
3. The method for preparing the rough grinding honing oilstone according to claim 2, Features: The ball milling is carried out in a ball mill for 1 to 3 hours; the adding of abrasives and mixing is carried out in a mixer for 1 to 3 hours.
4. Use of the rough grinding honing oilstone according to claim 1 in the honing process of engine cylinder block.
Citation Information
Patent Citations
Large-diameter diamond grinding wheel special for coarse grinding of silicon nitride ceramic ball and manufacturing method thereof
CN104907941A
Honing oilstone and preparation method and application thereof
CN108115546A