Mask blank, phase-shift mask, method for manufacturing mask blank, and method for manufacturing phase-shift mask
By optimizing the composition and position of the phase shift layer, etching stop layer, and light-shielding layer in the mask blank, the problem of optical property changes and shape abnormalities caused by molybdenum silicide film etching is solved, and high-definition mask manufacturing and static electricity suppression are achieved. .
Patent Information
- Application Number
- CN202110268167.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-16
- Filing Date
- 2021-03-12
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-03-12
AI Technical Summary
In liquid crystal displays and organic EL displays, the existing technology causes the quartz substrate to be etched and the optical properties of the phase shift mask to change when etching using a molybdenum silicide film, and the etching stop film is over-etched during patterning, resulting in shape abnormalities and static electricity destroy.
The mask blank structure is adopted, and the composition and position arrangement of the phase shift layer, etching stop layer and light shielding layer ensure that the nitrogen concentration of the etching stop layer is close to the light shielding layer in the film thickness direction to reach the peak area, and the resistivity is set to 1.0×10 -3Ωcm or more, the nitrogen concentration is 30 atomic % or more, the silicon concentration is 35 atomic % or less, the molybdenum concentration is 30 atomic % or less, and the etching stop layer is formed by controlling the partial pressure of the nitrogen-containing gas.
It improves the chemical resistance and adhesion of the etching stop layer, enhances the shape accuracy of the pattern, shortens the etching time, reduces the impact on the glass substrate, and suppresses electrostatic damage and pinhole generation.
Smart Images

Figure CN113406856B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a technique suitable for use in a mask blank, a phase shift mask, a method for manufacturing a mask blank, and a method for manufacturing a phase shift mask. Background Art
[0002] In recent years, in flat panel displays (FPDs) such as liquid crystal displays and organic EL displays, the panels have been greatly improved in terms of resolution. As the panels have become more precise, the photomasks have also been miniaturized. Therefore, the necessity of the mask using a light-shielding film, which has been used so far, has increased, and the necessity of the edge-enhanced phase-shift mask has also increased.
[0003] In FPD and the like, both line and space and contact hole patterns are required to be miniaturized, and a phase shift mask is required to form fine patterns.
[0004] For example, for a contact hole pattern, a large contrast is required during exposure, and a flange type phase shift mask is sometimes used. The flange type phase shift mask is constructed by forming a phase shift layer using a chromium compound on a quartz substrate, forming an etching stop layer using a molybdenum silicide compound on the upper part of the phase shift layer, and forming a light shielding layer using a metal film such as a chromium film on the upper part of the etching stop layer.
[0005] WET etching is generally used for patterning of large masks used in FPDs, etc. As an etching stopper film used in such WET etching, an etching stopper film formed of a silicide film such as a molybdenum silicide film is known (Patent Document 1).
[0006] Patent Document 1: International Publication No. 2013 / 190786
[0007] When the etching stop film is formed of a silicide film such as a molybdenum silicide film, the etching solution for the molybdenum silicide film contains fluoric acid, so that the quartz substrate is etched during WET etching of the molybdenum silicide film and the optical characteristics of the phase shift mask are changed.
[0008] Furthermore, if an appropriate etching stopper film is not used, etching is excessively performed at the interface between the etching stopper film and the light shielding film during patterning. Therefore, it is also clear that there is a problem that the etching stopper film disappears after etching and the cross-sectional shape becomes abnormal. Summary of the invention
[0009] The present invention has been made in view of the above circumstances, and intends to achieve the following objects.
[0010] 1. It has good etching stop properties in etching of a layer above the etching stop layer.
[0011] 2. During the etching of the etching stop layer, suppress the influence on other parts.
[0012] 3. Suppress electrostatic damage.
[0013] 4. Improve the accuracy of shapes in patterning.
[0014] 5. It can achieve high precision in mask manufacturing.
[0015] The mask blank of the present invention is a mask blank having a layer that becomes a phase shift mask, comprising: a phase shift layer laminated on a transparent substrate; an etching stop layer provided at a position farther from the transparent substrate than the phase shift layer; and a light shielding layer provided at a position farther from the transparent substrate than the etching stop layer, wherein the phase shift layer contains chromium, the light shielding layer contains chromium and oxygen, the etching stop layer contains molybdenum silicide and nitrogen, and has a peak region where the nitrogen concentration reaches a peak at a position close to the light shielding layer in the film thickness direction. Thus, the above-mentioned problem is solved.
[0016] In the mask blank of the present invention, the etching stop layer may have the peak region on an upper surface close to the light shielding layer in a film thickness direction.
[0017] In the mask blank of the present invention, the resistivity in the peak region of the etch stop layer may be set to 1.0×10 -3 Ωcm or more.
[0018] In the present invention, it is preferable that the nitrogen concentration in the peak region of the etching stop layer is set to 30 atomic % or more.
[0019] In the mask blank of the present invention, a method in which the silicon concentration in the peak region of the etching stop layer is set to 35 atomic % or less can be adopted.
[0020] In the mask blank of the present invention, the molybdenum concentration in the peak region of the etching stop layer may be set to 30 atomic % or less.
[0021] In the mask blank of the present invention, the film thickness of the peak region may be set within a range not greater than 1 / 3 of the film thickness of the etching stop layer.
[0022] In the mask blank of the present invention, the resistivity of the etching stop layer excluding the peak region may be set to 1.0×10 -3 Ωcm or less.
[0023] In the mask blank of the present invention, the nitrogen concentration of the etching stop layer excluding the peak region may be set to 25 atomic % or less.
[0024] In the mask blank of the present invention, a composition ratio of molybdenum to silicon in the etching stop layer excluding the peak region may be set to 1≤Si / Mo.
[0025] In the mask blank of the present invention, the film thickness of the etching stop layer can be set in a range of 10 nm to 100 nm.
[0026] The manufacturing method of the mask blank of the present invention is the manufacturing method of the mask blank described in any of the above items, and may include: a phase-shift layer forming process, stacking the phase-shift layer containing chromium on the transparent substrate; an etching stop layer forming process, stacking the etching stop layer containing molybdenum silicide and nitrogen at a position farther away from the transparent substrate than the phase-shift layer; and a shading layer forming process, stacking the shading layer containing chromium and oxygen at a position farther away from the transparent substrate than the etching stop layer, in which the etching stop layer forming process is formed by setting the partial pressure of the nitrogen-containing gas used as the supply gas in sputtering to control the nitrogen concentration in the peak region in the film thickness direction.
[0027] In the method for manufacturing a mask blank of the present invention, in the etching stop layer forming step, the partial pressure of the nitrogen-containing gas may be set so that the sheet resistance in the etching stop layer increases with an increase in nitrogen content.
[0028] In the method for manufacturing a mask blank of the present invention, the peak region may be formed by setting the partial pressure ratio of the nitrogen-containing gas to a range of 30% or more in the etching stop layer forming step.
[0029] In the method for manufacturing a mask blank of the present invention, in the etching stop layer forming step, the nitrogen-containing gas may be N 2 .
[0030] In the method for manufacturing a mask blank of the present invention, in the etching stop layer forming step, a target in which a composition ratio of molybdenum to silicon is set to 2.3≤Si / Mo≤3.0 may be used.
[0031] The phase-shift mask of the present invention can be manufactured from any of the mask blanks described above.
[0032] The manufacturing method of the phase shift mask blank of the present invention is the manufacturing method of the above-mentioned phase shift mask, which comprises: a phase shift pattern forming step, forming a pattern on the phase shift layer; an etching stop pattern forming step, forming a pattern on the etching stop layer; and a light shielding pattern forming step, forming a pattern on the light shielding layer, and the etching liquid in the phase shift pattern forming step and the light shielding pattern forming step is different from the etching liquid in the etching stop pattern forming step.
[0033] The mask blank of the present invention is a mask blank having a layer to be a phase shift mask, comprising: a phase shift layer laminated on a transparent substrate, an etching stop layer provided at a position farther from the transparent substrate than the phase shift layer; and a light shielding layer provided at a position farther from the transparent substrate than the etching stop layer. The phase shift layer contains chromium, the light shielding layer contains chromium and oxygen, the etching stop layer contains molybdenum silicide and nitrogen, and has a peak region where the nitrogen concentration reaches a peak at a position close to the light shielding layer in the film thickness direction.
[0034] Thus, the chemical resistance on the surface of the etching stop layer can be improved during the etching of the light shielding layer. Therefore, the adhesion between the light shielding layer and the etching stop layer can be improved, and the accuracy of the cross-sectional shape can be improved during the etching of the light shielding layer, thereby improving the shape accuracy of the mask pattern.
[0035] In addition, during the etching of the etching stop layer, the etching rate (ER) in the etching stop layer can be increased. Therefore, the etching time in the etching stop layer can be shortened, and the influence of etching on the transparent substrate used as the glass substrate can be reduced. This is because when the etching stop layer is etched, the glass substrate is sometimes exposed, and sometimes the etchant of the etching stop layer containing molybdenum silicon acts on the exposed portion. At the same time, the etching stop layer can be effectively removed by etching.
[0036] In the mask blank of the present invention, the etching stop layer has the peak region on an upper surface close to the light shielding layer in a film thickness direction.
[0037] Thus, the chemical resistance on the surface of the etching stop layer can be improved during the etching of the light shielding layer. Therefore, the adhesion between the light shielding layer and the etching stop layer can be improved, and the accuracy of the cross-sectional shape can be improved during the etching of the light shielding layer, thereby improving the shape accuracy of the mask pattern.
[0038] In addition, in the etching of the etching stop layer, the etching rate (ER) in the etching stop layer can be increased after removing the peak region. Therefore, the etching time in the etching stop layer can be shortened, and the influence of etching on the transparent substrate used as the glass substrate can be reduced.
[0039] In the mask blank of the present invention, the resistivity in the peak region of the etching stop layer is set to 1.0×10 -3 Ωcm or more.
[0040] Thus, during the etching of the light shielding layer, the chemical resistance on the surface of the etching stop layer can be improved, so that a mask having a good cross-sectional shape can be formed.
[0041] In addition, the number of particles adhering to the surface of the etching stop layer can be reduced, thereby suppressing the generation of pinholes.
[0042] In the present invention, the nitrogen concentration in the peak region of the etching stop layer is set to 30 atomic % or more.
[0043] Thus, by setting the sheet resistance in the peak region to the above range, the chemical resistance on the surface of the etching stop layer can be improved during etching of the light shielding layer, thereby forming a mask having a good cross-sectional shape.
[0044] In addition, the number of particles adhering to the surface of the etching stop layer can be reduced, thereby suppressing the generation of pinholes.
[0045] Furthermore, in the mask blank of the present invention, the silicon concentration in the peak region of the etching stop layer is set to 35 atomic % or less.
[0046] This makes it possible to provide a mask blank having sufficient etching stop capability and capable of forming a phase shift mask having a good cross-sectional shape.
[0047] In the mask blank of the present invention, the molybdenum concentration in the peak region of the etching stop layer is set to 30 atomic % or less.
[0048] This makes it possible to provide a mask blank having sufficient etching stop capability and capable of forming a phase shift mask having a good cross-sectional shape.
[0049] In the mask blank of the present invention, the film thickness of the peak region is set to be within a range not greater than 1 / 3 of the film thickness of the etching stop layer.
[0050] Thus, it is possible to achieve both sufficient etching stop properties in the etching stop layer and a large etching rate (ER) in the etching stop layer. Therefore, in etching the light shielding layer, the chemical resistance on the surface of the etching stop layer can be improved, and in etching the etching stop layer, the etching rate (ER) in the etching stop layer can be increased after removing the peak region.
[0051] In the mask blank of the present invention, the resistivity of the etching stop layer excluding the peak region is set to 1.0×10 -3 Ωcm or less.
[0052] Thus, in the etching of the etching stop layer, after removing the peak region, the etching rate (ER) in the etching stop layer can be increased. Therefore, the etching time in the etching stop layer can be shortened, and the influence of etching on the transparent substrate used as the glass substrate can be reduced.
[0053] Furthermore, by using a molybdenum silicide film having a low resistivity as an etching stopper layer, electrostatic breakdown can be suppressed.
[0054] In the mask blank of the present invention, the nitrogen concentration of the etching stop layer excluding the peak region is set to 25 atomic % or less.
[0055] Thus, the etching rate (ER) can be increased in the etching stop layer closer to the phase shift layer than the peak region, so that the etching time in the etching stop layer can be shortened, and the influence of etching on the transparent substrate used as the glass substrate can be reduced.
[0056] Furthermore, by using a molybdenum silicide film having a low resistivity as an etching stopper layer, electrostatic breakdown can be suppressed.
[0057] In the mask blank of the present invention, the composition ratio of molybdenum to silicon in the etching stop layer excluding the peak region is set to 1≤Si / Mo.
[0058] This makes it possible to provide a mask blank having sufficient etching stop capability and capable of forming a phase shift mask having a good cross-sectional shape.
[0059] In the mask blank of the present invention, the film thickness of the etching stop layer is set to be in the range of 10 nm to 100 nm.
[0060] This makes it possible to provide a mask blank having sufficient etching stop capability and capable of forming a phase shift mask having a good cross-sectional shape.
[0061] The manufacturing method of the mask blank of the present invention is the manufacturing method of the mask blank described in any one of the above items, comprising: a phase shift layer forming step of stacking the phase shift layer containing chromium on the transparent substrate; an etching stop layer forming step of stacking the etching stop layer containing molybdenum silicide and nitrogen at a position farther from the transparent substrate than the phase shift layer; and a light shielding layer forming step of stacking the light shielding layer containing chromium and oxygen at a position farther from the transparent substrate than the etching stop layer. In the etching stop layer forming step, the etching stop layer is formed by controlling the nitrogen concentration in the peak region in the film thickness direction by setting the partial pressure of the nitrogen-containing gas as the supply gas in sputtering.
[0062] In the method for manufacturing a mask blank of the present invention, in the etching stop layer forming step, the partial pressure of the nitrogen-containing gas is set so that the sheet resistance in the etching stop layer increases with an increase in nitrogen content.
[0063] Thus, it is possible to manufacture a mask blank having an etching stop layer having a higher nitrogen concentration at a position closer to the light shielding layer than at a position closer to the phase shift layer in the film thickness direction.
[0064] In addition, a peak region where the nitrogen concentration reaches a peak can be formed on the etching stop layer near the interface with the light shielding layer. In addition, in the etching stop layer, the nitrogen concentration at a position close to the phase shift layer can be lowered compared to the nitrogen concentration in the peak region. Furthermore, during the formation of the etching stop layer by sputtering, the etching stop layer having such a structure can be realized by controlling the partial pressure of the nitrogen-containing gas in the atmosphere gas.
[0065] Therefore, it is possible to manufacture a mask blank that has a sufficient etching stop capability and can form a phase shift mask with a good cross-sectional shape.
[0066] In the method for manufacturing a mask blank of the present invention, in the etching stop layer forming step, the peak region is formed by setting the partial pressure ratio of the nitrogen-containing gas to a range of 30% or more.
[0067] Thereby, the peak region in the etching stop layer can be set to a predetermined nitrogen concentration and formed so as to achieve the above-mentioned sheet resistance.
[0068] In the method for manufacturing a mask blank of the present invention, in the etching stop layer forming step, the nitrogen-containing gas is N 2 .
[0069] Thereby, the peak region in the etching stop layer can be set to a predetermined nitrogen concentration, and the etching stop layer can be formed to have the above-mentioned resistivity.
[0070] In the method for manufacturing a mask blank of the present invention, in the etching stop layer forming step, a target whose composition ratio of molybdenum to silicon is set to 2.3≤Si / Mo≤3.0 is used.
[0071] Thus, it is possible to manufacture a mask blank capable of setting the peak region in the etching stop layer to a predetermined nitrogen concentration, forming the mask blank to have the above-mentioned sheet resistance, having a sufficient etching stop capability, and being able to form a phase shift mask with a good cross-sectional shape.
[0072] The phase shift mask of the present invention is manufactured from any of the mask blanks described above. Thus, it is possible to provide a phase shift mask having a sufficient etching stop capability and a good cross-sectional shape.
[0073] The manufacturing method of the phase shift mask blank of the present invention is the manufacturing method of the phase shift mask described above, comprising: a phase shift pattern forming step of forming a pattern on the phase shift layer; an etching stop pattern forming step of forming a pattern on the etching stop layer; and a light shielding pattern forming step of forming a pattern on the light shielding layer. The etching liquid in the phase shift pattern forming step and the light shielding pattern forming step is different from the etching liquid in the etching stop pattern forming step. Thus, a phase shift mask having a sufficient etching stop capability and a good cross-sectional shape can be formed.
[0074] According to the present invention, it is possible to provide a mask blank capable of reducing the influence on the surface of a glass substrate and forming a phase shift mask having a good cross-sectional shape. BRIEF DESCRIPTION OF THE DRAWINGS
[0075] Figure 1 It is a cross-sectional view showing a mask blank according to the first embodiment of the present invention.
[0076] Figure 2 It is a cross-sectional view showing a method for manufacturing a mask blank according to the first embodiment of the present invention.
[0077] Figure 3 The diagram is a cross-sectional view showing the steps of the method for manufacturing the phase shift mask according to the first embodiment of the present invention.
[0078] Figure 4 The diagram is a cross-sectional view showing the steps of the method for manufacturing the phase shift mask according to the first embodiment of the present invention.
[0079] Figure 5 The diagram is a cross-sectional view showing the steps of the method for manufacturing the phase shift mask according to the first embodiment of the present invention.
[0080] Figure 6 The diagram is a cross-sectional view showing the steps of the method for manufacturing the phase shift mask according to the first embodiment of the present invention.
[0081] Figure 7 The diagram is a cross-sectional view showing the steps of the method for manufacturing the phase shift mask according to the first embodiment of the present invention.
[0082] Figure 8 The diagram is a cross-sectional view showing the steps of the method for manufacturing the phase shift mask according to the first embodiment of the present invention.
[0083] Fig. 9 The diagram is a cross-sectional view showing the steps of the method for manufacturing the phase shift mask according to the first embodiment of the present invention.
[0084] Fig.10 It is a cross-sectional view showing a phase shift mask according to the first embodiment of the present invention.
[0085] Fig.11 It is a schematic diagram showing a film forming apparatus in the method for manufacturing a mask blank according to the first embodiment of the present invention.
[0086] Fig.12 This is a graph showing the relationship between the etching rate (ER) and the nitrogen concentration of the etching stop layer in the mask blank and the method for manufacturing the phase shift mask according to the first embodiment of the present invention.
[0087] Fig.13This is a graph showing the composition ratio in the film thickness direction of the etching stop layer in the mask blank and the phase shift mask according to the first embodiment of the present invention. DETAILED DESCRIPTION
[0088] Hereinafter, a mask blank, a phase shift mask, and a manufacturing method according to a first embodiment of the present invention will be described with reference to the drawings.
[0089] Figure 1 is a cross-sectional view showing a mask blank in this embodiment, Figure 2 is a cross-sectional view showing a mask blank in this embodiment. Figure 1 and Figure 2 In the figure, reference numeral 10B is a mask blank.
[0090] The mask blank 10B according to the present embodiment is provided to a phase shift mask (photomask) used in a range of about 365 nm to 436 nm in wavelength of exposure light. Figure 1 As shown, the mask blank 10B according to the present embodiment includes: a glass substrate (transparent substrate) 11 ; a phase shift layer 12 formed on the glass substrate 11 ; an etching stop layer 13 formed on the phase shift layer 12 ; and a light shielding layer 14 formed on the etching stop layer 13 .
[0091] That is, the etching stop layer 13 is provided at a position farther from the glass substrate 11 than the phase shift layer 12. In addition, the light shielding layer 14 is provided at a position farther from the glass substrate 11 than the etching stop layer 13.
[0092] These phase shift layer 12 , etching stop layer 13 , and light shielding layer 14 configure a mask layer which is a stacked film having optical characteristics required for a photomask.
[0093] In addition, if Figure 2 As shown, the mask blank 10B involved in this embodiment can also be Figure 1 As shown in the figure, a mask layer having a phase shift layer 12, an etching stop layer 13, and a light shielding layer 14 stacked thereon has been previously formed a photoresist layer 15.
[0094] In addition, the mask blank 10B according to the present embodiment may have a structure in which, in addition to the phase shift layer 12, the etching stop layer 13 and the light shielding layer 14, an anti-reflection layer, a chemical resistance layer, a protective layer, a sealing layer and the like are laminated. Figure 2 As shown, a photoresist layer 15 may be formed on these laminated films.
[0095] As the glass substrate 11, a material having excellent transparency and optical isotropy, such as a quartz glass substrate, can be used. The size of the glass substrate 11 is not particularly limited and can be appropriately selected according to the substrate (such as a FPD substrate for an LCD (liquid crystal display), a plasma display, an organic EL (electroluminescence) display, etc.) to be exposed using the mask.
[0096] In this embodiment, as the glass substrate 11, a rectangular substrate with a side of about 100 mm to a side of more than 2000 mm can be used, and a substrate with a thickness of less than 1 mm, a substrate with a thickness of several millimeters, or a substrate with a thickness of more than 10 mm can also be used.
[0097] In addition, the flatness of the glass substrate 11 can be reduced by grinding the surface of the glass substrate 11. The flatness of the transparent substrate 11 can be, for example, 20 μm or less. As a result, the depth of focus of the mask becomes deeper, which can make a great contribution to the formation of a fine and high-precision pattern. In addition, the flatness is preferably a small value of 10 μm or less.
[0098] The phase shift layer 12 is a layer containing Cr (chromium) as a main component, and contains C (carbon), O (oxygen), and N (nitrogen).
[0099] The phase shift layer 12 may have different compositions in the thickness direction. In this case, the phase shift layer 12 may be constructed by stacking one or more selected from Cr alone and Cr oxides, nitrides, carbides, oxynitrides, carbonitrides, and oxycarbonitrides.
[0100] As described later, the thickness of the phase shift layer 12 and the composition ratio (atomic %) of Cr, N, C, O, etc. are set so as to obtain predetermined optical characteristics and resistivity.
[0101] The film thickness of the phase shift layer 12 is set according to the optical characteristics required for the phase shift layer 12 and varies according to the composition ratio of Cr, N, C, O, etc. The film thickness of the phase shift layer 12 can be 50 nm to 150 nm.
[0102] For example, the composition ratio in the phase shift layer 12 can be set to a carbon content (carbon concentration) of 2.3 atomic % to 10.3 atomic %, an oxygen content (oxygen concentration) of 8.4 atomic % to 72.8 atomic %, a nitrogen content (nitrogen concentration) of 1.8 atomic % to 42.3 atomic %, and a chromium content (chromium concentration) of 20.3 atomic % to 42.4 atomic %.
[0103] Therefore, when the refractive index is about 2.4 to 3.1 and the extinction coefficient is 0.3 to 2.1 in the wavelength range of about 365 nm to 436 nm, the phase shift layer 12 can be set to have a film thickness of about 90 nm.
[0104] In addition, the composition ratio and film thickness of the phase shift layer 12 are set according to the optical characteristics required for the phase shift mask 10 to be manufactured, and are not limited to the above-mentioned values.
[0105] The etching stop layer 13 is made of a material different from that of the phase shift layer 12, and may be a metal silicide film, for example, a film containing a metal such as Ta (tantalum), Ti (titanium), W (tungsten), Mo (molybdenum), Zr (zirconium), or an alloy of these metals and silicon. In particular, among the metal silicide films, molybdenum silicide films are preferably used, and examples thereof include MoSi X (X≥2) film (for example, MoSi2 film, MoSi3 film or MoSi4 film, etc.).
[0106] As the etching stop layer 13, a molybdenum silicide film containing O (oxygen), N (nitrogen), and C (carbon) is preferable.
[0107] In addition, the etching stop layer 13 may contain C (carbon).
[0108] In the etching stop layer 13, the oxygen content (oxygen concentration) can be set in the range of 2.6 atomic % to 10.9 atomic %, the nitrogen content (nitrogen concentration) can be set in the range of 1.5 atomic % to 40.9 atomic %, and the carbon content (carbon concentration) can be set in the range of 2.4 atomic % to 4.3 atomic %.
[0109] The film thickness of the etching stop layer 13 can be set in the range of 10 nm to 100 nm.
[0110] The etching stop layer 13 has a peak region 13A where the nitrogen concentration reaches a peak at a position close to the light shielding layer 14 in the film thickness direction.
[0111] The etching stop layer 13 has a nitrogen concentration lower than the nitrogen concentration in the peak region 13A at a position close to the phase shift layer 12 in the film thickness direction.
[0112] Peak region 13A may be formed in etching stop layer 13 to be exposed on the upper surface close to light shielding layer 14 in the film thickness direction. That is, peak region 13A is formed at the interface between etching stop layer 13 and light shielding layer 14.
[0113] The resistivity in the peak region 13A of the etching stop layer 13 is set to 1.0×10 -3 Ωcm or more.
[0114] The nitrogen concentration in peak region 13A of etching stop layer 13 is set to 30 atomic % or more.
[0115] The silicon concentration in peak region 13A of etching stop layer 13 is set to be in the range of 20 atomic % to 70 atomic %.
[0116] The molybdenum concentration in peak region 13A of etching stop layer 13 is set to be in the range of 20 atomic % to 40 atomic %.
[0117] The film thickness of peak region 13A is set to be within a range not greater than 1 / 3 of the film thickness of etching stop layer 13 .
[0118] The resistivity of the etching stop layer 13 other than the peak region 13A, that is, at a position closer to the phase shift layer 12 than the peak region 13A, is set to 1.0×10 -3 Ωcm or less.
[0119] The nitrogen concentration of the etching stop layer 13 excluding the peak region 13A, that is, at a position closer to the phase shift layer 12 than the peak region 13A, is set to 25 atomic % or less.
[0120] The composition ratio of molybdenum to silicon in the etching stop layer 13 excluding the peak region 13A, that is, at a position closer to the phase shift layer 12 than the peak region 13A, is set to satisfy 1≤Si / Mo.
[0121] The nitrogen concentration of the etching stop layer 13 other than the peak region 13A, i.e., at a position closer to the phase shift layer 12 than the peak region 13A, may be a uniform constant value, have a gradient, or have a predetermined change in the film thickness direction as long as it is lower than the nitrogen concentration in the peak region 13A.
[0122] In addition, regarding the etching stop layer 13, as long as the peak region 13A has a portion with a high nitrogen concentration, it is preferred that the nitrogen concentration is as low as possible and the etching rate (ER) is large in the other portions. In addition, regarding the etching stop layer 13, as long as the peak region 13A has a portion with a high nitrogen concentration, it is preferred that the nitrogen concentration is as low as possible and the resistivity is low in the other portions.
[0123] The light shielding layer 14 is a layer containing Cr (chromium) and O (oxygen) as main components, and also contains C (carbon) and N (nitrogen).
[0124] In this case, the light shielding layer 14 may be constructed by laminating one or more selected from oxides, nitrides, carbides, oxynitrides, carbonitrides, and oxycarbonitrides of Cr. The light shielding layer 14 may have different compositions in the thickness direction.
[0125] As described later, the thickness of the light shielding layer 14 and the composition ratio (atomic %) of Cr, N, C, O, Si, etc. are set so as to obtain predetermined adhesion (hydrophobicity) and predetermined optical characteristics.
[0126] The film thickness of the light shielding layer 14 is set according to the conditions required for the light shielding layer 14, that is, the film characteristics such as the adhesion (hydrophobicity) and optical characteristics of the photoresist layer 15 described later and the light shielding layer 14. The film characteristics in these light shielding layers 14 vary according to the composition ratio of Cr, N, C, O, etc. In particular, the film thickness of the light shielding layer 14 can be set according to the optical characteristics required for the phase shift mask 10.
[0127] By setting the film thickness and composition of the light shielding layer 14 in the above manner, the adhesion between the photoresist layer 15 used for, for example, chromium-based materials and the light shielding layer 14 can be improved during pattern formation in the photolithography method. As a result, etching liquid does not intrude into the interface between the photoresist layer 15 and the light shielding layer 14. Therefore, a good pattern shape can be obtained, and a desired pattern can be formed.
[0128] In addition, if the light shielding layer 14 is not set as described above, the adhesion between the photoresist layer 15 and the light shielding layer 14 cannot be in a predetermined state, and the etching solution intrudes into the interface due to the peeling of the photoresist layer 15, and pattern formation cannot be performed, which is not preferred. In addition, if the film thickness of the light shielding layer 14 is not set as described above, it is difficult to set the optical properties of the photomask to the desired conditions, or the cross-sectional shape of the mask pattern may not be in a desired state, which is not preferred.
[0129] The light shielding layer 14 can reduce hydrophilicity and increase hydrophobicity and adhesion by increasing the oxygen concentration and nitrogen concentration in the chromium compound.
[0130] Meanwhile, for the light shielding layer 14, the values of the refractive index and the extinction coefficient can be lowered by increasing the oxygen concentration and the nitrogen concentration in the chromium compound, or the values of the refractive index and the extinction coefficient can be increased by decreasing the oxygen concentration and the nitrogen concentration in the chromium compound.
[0131] In the method for manufacturing the mask blank in the present embodiment, the phase shift layer 12 is formed on the glass substrate 11 , the etching stop layer 13 is formed, and then the light shielding layer 14 is formed.
[0132] When a protective layer, a light shielding layer, a chemical resistant layer, an antireflection layer, etc. are stacked in addition to the phase shift layer 12, the etching stop layer 13, and the light shielding layer 14, the method for manufacturing the mask blank may include a stacking step of these layers.
[0133] As an example, an adhesion layer containing chromium can be mentioned.
[0134] Figure 3 It is a cross-sectional view showing the manufacturing process of the phase shift mask in this embodiment. Figure 4 It is a cross-sectional view showing the manufacturing process of the phase shift mask in this embodiment. Figure 5It is a cross-sectional view showing the manufacturing process of the phase shift mask in this embodiment. Figure 6 It is a cross-sectional view showing the manufacturing process of the phase shift mask in this embodiment. Figure 7 It is a cross-sectional view showing the manufacturing process of the phase shift mask in this embodiment. Figure 8 It is a cross-sectional view showing the manufacturing process of the phase shift mask in this embodiment. Fig. 9 It is a cross-sectional view showing the manufacturing process of the phase shift mask in this embodiment. Fig.10 It is a cross-sectional view showing a phase shift mask in this embodiment.
[0135] like Fig.10 As shown, the phase shift mask (photomask) 10 in this embodiment is obtained by forming patterns on the phase shift layer 12, the etching stop layer 13, and the light shielding layer 14 stacked as a mask blank 10B.
[0136] Next, a method for manufacturing the phase shift mask 10 from the mask blank 10B of the present embodiment will be described.
[0137] As a resist pattern forming process, Figure 2 As shown, a photoresist layer 15 is formed on the outermost surface of the mask blank 10B. Alternatively, a mask blank 10B having a photoresist layer 15 formed on the outermost surface may be prepared in advance. The photoresist layer 15 may be a positive type or a negative type. As a material for the photoresist layer 15, a material that can cope with etching of chromium-based materials and etching of molybdenum silicide-based materials may be used. As the photoresist layer 15, a liquid resist may be used.
[0138] Next, the photoresist layer 15 is exposed and developed to form a resist pattern 15P1 outside the light shielding layer 14. The resist pattern 15P1 functions as an etching mask used for etching the phase shift layer 12, the etching stop layer 13, and the light shielding layer 14.
[0139] The shape of the resist pattern 15P1 is appropriately determined according to the etching patterns of the phase shift layer 12, the etching stop layer 13, and the light shielding layer 14. As an example, it is set to have a shape similar to that of the light-transmitting region 10L (see Figure 6 to Figure 10 )'s opening width dimension corresponds to the shape of the opening width.
[0140] Next, as a light shielding pattern forming step, the light shielding layer 14 is wet-etched using an etching solution via the resist pattern 15P1. Figure 3 As shown, a light shielding pattern 14P1 is formed.
[0141] As the etching solution in the light shielding pattern forming step, an etching solution containing ammonium cerium nitrate can be used as an etching solution for chromium-based materials. For example, ammonium cerium nitrate containing an acid such as nitric acid or perchloric acid is preferably used.
[0142] In the light shielding pattern forming step, the etching stopper layer 13 composed of molybdenum silicide is hardly etched by the above-mentioned chromium-based etching solution.
[0143] At this time, since the peak region 13A is provided on the etching stop layer 13, the etching resistance to the chromium-based etching solution can be improved. At the same time, since the peak region 13A is provided on the etching stop layer 13, the adhesion between the light shielding layer 14 and the etching stop layer 13 can be improved, and the etched shape can be prevented from collapsing.
[0144] Next, as an etching stop pattern forming step, the etching stop layer 13 is wet-etched using an etching solution via the light shielding pattern 14P1. Figure 4 As shown, an etch stop pattern 13P1 is formed.
[0145] As the etching liquid in the etching stop pattern forming step, an etching liquid capable of etching the etching stop layer 13 composed of molybdenum silicide can be used. As such an etching liquid, an etching liquid containing at least one fluorine compound selected from hydrofluoric acid, hydrofluoric acid and ammonium bifluoride and at least one oxidant selected from hydrogen peroxide, nitric acid and sulfuric acid is preferably used.
[0146] At this time, since the peak region 13A is provided in the etching stop layer 13, the etching rate (ER) of the molybdenum silicide etching solution is reduced, but since the film thickness of the peak region 13A is set to be small, it is possible to prevent the etching time from being prolonged. In addition, since the nitrogen concentration at the position below the peak region 13A of the etching stop layer 13, that is, close to the phase shift layer 12, is set to be low, the etching rate (ER) of the molybdenum silicide etching solution is increased, and the etching time can be shortened.
[0147] This can shorten the etching time and suppress the influence of the etching liquid on the glass substrate 11 .
[0148] Next, as a phase shift pattern forming step, the phase shift layer 12 is wet-etched via the patterned etching stop pattern 13P1, the light shielding pattern 14P1, and the resist pattern 15P1. Figure 5 As shown, a phase shift pattern 12P1 is formed.
[0149] Thereby, the light-transmitting region 10L in which the surface of the glass substrate 11 is exposed can be formed.
[0150] As the etching solution in the phase shift pattern forming step, similarly to the light shielding pattern forming step, an etching solution containing ammonium cerium nitrate can be used. For example, ammonium cerium nitrate containing an acid such as nitric acid or perchloric acid is preferably used.
[0151] For example, the molybdenum silicide compound constituting the etching stop layer 13 can be etched with a mixed solution of ammonium bifluoride and hydrogen peroxide. On the other hand, the chromium compound constituting the light shielding layer 14 and the phase shift layer 12 can be etched with a mixed solution of ammonium cerium nitrate and perchloric acid.
[0152] Therefore, the selectivity when etching each wafer becomes very large. Therefore, after the light shielding pattern 14P1, the etching stop pattern 13P1, and the phase shift pattern 12P1 are formed by etching, the cross-sectional shape of the phase shift mask 10 can be a good cross-sectional shape close to vertical.
[0153] In the phase shift pattern forming step, the etching rate is reduced by setting the oxygen concentration of the light shielding layer 14 higher than that of the phase shift layer 12. Therefore, the etching progress of the light shielding pattern 14P1 is delayed compared to the etching of the phase shift layer 12.
[0154] Based on these circumstances, the angle (taper angle) θ formed by the wall surface formed by etching the light shielding pattern 14P1 , the etching stop pattern 13P1 , and the phase shift pattern 12P1 and the surface of the glass substrate 11 is close to a right angle, for example, about 90°.
[0155] Furthermore, by forming the peak region 13A on the etching stop pattern 13P1 so as to be in contact with the light shielding pattern 14P1, the adhesion between the light shielding pattern 14P1 and the etching stop pattern 13P1 is improved. Thus, in the phase shift pattern forming step, the etching liquid does not penetrate into the interface between the light shielding pattern 14P1 and the etching stop pattern 13P1. Therefore, reliable pattern formation can be performed.
[0156] In addition, in this embodiment, as a resist pattern forming step, Figure 6 As shown, a resist pattern 15P2 is formed outside the light shielding pattern 14P1 by exposing and developing the photoresist layer 15. The resist pattern 15P2 functions as an etching mask for the etching stop pattern 13P1 and the light shielding pattern 14P1.
[0157] The shape of the resist pattern 15P2 is appropriately determined according to the etching pattern of the etching stop pattern 13P1 and the light shielding pattern 14P1. As an example, it is set to have a shape corresponding to the phase shift region 10P2 and the exposure region 10P1 (see Figure 8 to Figure 10 )'s opening width dimension corresponds to the shape of the opening width.
[0158] Next, as a pattern forming step for a light shielding pattern, the light shielding pattern 14P1 is wet-etched using an etching solution via the resist pattern 15P2. Figure 7 As shown, a light shielding pattern 14P2 is formed.
[0159] As the etching solution in the light shielding pattern forming step, an etching solution containing ammonium cerium nitrate can be used as an etching solution for chromium-based materials. For example, ammonium cerium nitrate containing an acid such as nitric acid or perchloric acid is preferably used.
[0160] In the light shielding pattern forming step, the etching stopper pattern 13P1 made of molybdenum silicide is hardly etched by the chromium-based etching solution.
[0161] At this time, since the peak region 13A is provided in the etching stop pattern 13P1, the etching resistance to the chromium-based etching solution can be improved. At the same time, since the peak region 13A is provided in the etching stop pattern 13P1, the adhesion between the light shielding pattern 14P2 and the etching stop pattern 13P1 can be improved, and the etched shape can be prevented from collapsing.
[0162] Next, as an etching stop pattern forming step, the etching stop pattern 13P1 is wet-etched using an etching liquid via the light shielding pattern 14P2. Figure 8 As shown, an etching stop pattern 13P2 is formed.
[0163] Thus, the etching stop pattern 13P2 in which the surface of the phase shift pattern 12P1 is exposed can be formed corresponding to the exposure region 10P1.
[0164] As the etching liquid in the etching stop pattern forming step, an etching liquid capable of etching the etching stop pattern 13P1 composed of molybdenum silicide can be used. As such an etching liquid, an etching liquid containing at least one fluorine compound selected from hydrofluoric acid, hydrofluoric acid and ammonium bifluoride and at least one oxidant selected from hydrogen peroxide, nitric acid and sulfuric acid is preferably used.
[0165] At this time, since the peak region 13A is provided in the etching stop pattern 13P1, the etching rate (ER) of the molybdenum silicide etching solution is reduced. On the other hand, since the film thickness of the peak region 13A is set to be small, the etching time for forming the etching stop pattern 13P2 can be prevented from being prolonged. In addition, the nitrogen concentration at the position of the etching stop pattern 13P1 that is lower than the peak region 13A, that is, close to the phase shift pattern 12P1, is set to be low. Therefore, by increasing the etching rate (ER) of the molybdenum silicide etching solution, the etching time for forming the etching stop pattern 13P2 can be shortened.
[0166] This can shorten the etching time and suppress the influence of the etching solution on the glass substrate 11 exposed in the light-transmitting region 10L and other regions.
[0167] Next, as a phase shift pattern forming step, the phase shift pattern 12P1 is wet-etched using an etching solution via the resist pattern 15P2, the light shielding pattern 14P2, and the etching stop pattern 13P2. Fig. 9 As shown, a phase shift pattern 12P2 is formed.
[0168] As the etching solution in the phase shift pattern forming step, similarly to the light shielding pattern forming step, an etching solution containing ammonium cerium nitrate can be used. For example, ammonium cerium nitrate containing an acid such as nitric acid or perchloric acid is preferably used.
[0169] At this time, while the phase shift pattern 12P1 is wet-etched, the exposed surface of the light shielding pattern 14P2 is wet-etched. The exposed surface of the light shielding pattern 14P2 is wet-etched in the lateral direction of the figure. Fig. 9 As shown, a light shielding pattern 14P3 having a larger opening width than the phase shift pattern 12P2 is formed.
[0170] The selectivity during wet etching is very large in the molybdenum silicide compound constituting the etching stop layer 13 and the chromium compound forming the light shielding layer 14 and the phase shift layer 12. Therefore, the phase shift pattern 12P1 covered by the etching stop layer 13 is not etched. On the other hand, the light shielding pattern 14P2 exposed in the pattern section and the phase shift pattern 12P1 in the region where the etching stop layer 13 is removed are etched.
[0171] Here, the light shielding pattern 14P2 is etched in the direction along the surface of the glass substrate 11 , and the phase shift pattern 12P1 in the region where the etching stop layer 13 is removed is etched in the thickness direction.
[0172] Thereby, a pattern including the phase shift pattern 12P2 which protrudes toward the exposure region 10P1 more than the light shielding pattern 14P3 and has the phase shift region 10P2 can be formed as required for the cross-sectional shape of the phase shift mask 10 .
[0173] In this case, as the cross-sectional shape of the phase shift mask 10 , a favorable cross-sectional shape close to vertical can be obtained.
[0174] In the phase shift pattern forming step, the etching rate is reduced by setting the oxygen concentration of the light shielding layer 14 higher than that of the phase shift layer 12. Therefore, the etching progress of the light shielding pattern 14P2 is set to a predetermined state with respect to the etching of the phase shift pattern 12P1, and the width dimension of the phase shift region 10P2 is set.
[0175] Based on these circumstances, in the light shielding pattern 14P3, the etching stop layer 13P2 and the phase shift pattern 12P2, the angle (taper angle) θ formed by the wall surface formed by each etching and the surface of the glass substrate 11 is close to a right angle, for example, can be about 90°.
[0176] Furthermore, by forming the peak region 13A on the etching stop pattern 13P1 in contact with the light shielding pattern 14P2, the adhesion between the light shielding pattern 14P2 and the etching stop pattern 13P2 is improved. Thus, in the phase shift pattern forming step, the etching liquid does not penetrate into the interface between the light shielding pattern 14P2 and the etching stop pattern 13P1. Therefore, reliable pattern formation can be performed.
[0177] Next, as a resist removal step, the resist pattern 15P2 is removed, as shown in FIG. Fig.10 As shown, a phase-shift mask 10 is manufactured.
[0178] Next, a method for manufacturing a mask blank in the present embodiment will be described with reference to the drawings.
[0179] Fig.11 It is a schematic diagram which shows the manufacturing apparatus of the mask blank in this embodiment.
[0180] The mask blank 10B in this embodiment is formed by Fig.11 The manufacturing device shown is used to manufacture.
[0181] Fig.11 The manufacturing device S10 shown is a reciprocating (inner bag type) sputtering device. The manufacturing device S10 has a loading chamber S11, an unloading chamber S16 and a film forming chamber (vacuum processing chamber) S12. The film forming chamber S12 is located between the loading chamber S11 and the unloading chamber S16. The film forming chamber S12 is connected to the loading chamber S11 through a sealing mechanism S17, and is connected to the unloading chamber S16 through a sealing mechanism S18.
[0182] The loading chamber S11 is provided with a transport mechanism S11a for transporting the glass substrate 11 brought in from outside the manufacturing apparatus S10 to the film forming chamber S12 and an exhaust mechanism S11f such as a rotary pump for roughly evacuating the inside of the loading chamber S11.
[0183] The unloading chamber S16 is provided with a conveying mechanism S16a for conveying the glass substrate 11 after film formation from the film forming chamber S12 to the outside of the manufacturing apparatus S10 and an exhaust mechanism S16f such as a rotary pump for roughly evacuating the inside of the unloading chamber S16.
[0184] The film forming chamber S12 is provided with a substrate holding mechanism S12 a and three-stage film forming mechanisms S13 , S14 , and S15 as mechanisms for three film forming processes.
[0185] The substrate holding mechanism S12a holds the glass substrate 11 conveyed by the conveying mechanism S11a so that the glass substrate 11 faces the targets S13b, S14b, and S15b during film formation. The substrate holding mechanism S12a can convey the glass substrate 11 from the loading chamber S11 and convey the glass substrate 11 to the unloading chamber S16.
[0186] Among the three stages of film forming mechanisms S13 , S14 , and S15 in the film forming chamber S12 , a film forming mechanism S13 for supplying a first stage of film forming material is provided at a position closest to the loading chamber S11 .
[0187] The film forming mechanism S13 includes: a cathode electrode (back plate) S13c having a target S13b; and a power supply S13d for applying a negative potential sputtering voltage to the back plate S13c.
[0188] The film forming mechanism S13 comprises: a gas introduction mechanism S13e, which is used to introduce gas into the vicinity of the cathode electrode (back plate) S13c in the film forming chamber S12; and a high vacuum exhaust mechanism S13f such as a turbomolecular pump, which is used to draw a high vacuum into the vicinity of the cathode electrode (back plate) S13c in the film forming chamber S12.
[0189] In addition, a film forming mechanism S14 is provided at an intermediate position between the loading chamber S11 and the unloading chamber S16 in the film forming chamber S12. The film forming mechanism S14 is used to supply film forming materials to the second film forming mechanism among the three film forming mechanisms S13, S14, and S15.
[0190] The film forming mechanism S14 includes: a cathode electrode (back plate) S14c having a target S14b; and a power supply S14d for applying a negative potential sputtering voltage to the back plate S14c.
[0191] The film forming mechanism S14 comprises: a gas introduction mechanism S14e, which is used to introduce gas into the vicinity of the cathode electrode (back plate) S14c in the film forming chamber S12; and a high vacuum exhaust mechanism S14f such as a turbomolecular pump, which is used to draw a high vacuum into the vicinity of the cathode electrode (back plate) S14c in the film forming chamber S12.
[0192] Furthermore, a film forming mechanism S15 is provided at a position closest to the unloading chamber S16 among the three film forming mechanisms S13 , S14 , and S15 of the film forming chamber S12 . The film forming mechanism S15 is used to supply the film forming material to the third film forming mechanism.
[0193] The film forming mechanism S15 includes: a cathode electrode (back plate) S15c having a target S15b; and a power supply S15d for applying a negative potential sputtering voltage to the back plate S15c.
[0194] The film forming mechanism S15 comprises: a gas introduction mechanism S15e, which is used to introduce gas into the vicinity of the cathode electrode (back plate) S15c in the film forming chamber S12; and a high vacuum exhaust mechanism S15f such as a turbomolecular pump, which is used to draw a high vacuum into the vicinity of the cathode electrode (back plate) S15c in the film forming chamber S12.
[0195] In the film forming chamber S12, gas barriers S12g for suppressing gas flow are respectively provided near the cathode electrodes (back plates) S13c, S14c, and S15c, so that the gases respectively supplied by the gas introduction mechanisms S13e, S14e, and S15e are not mixed into the adjacent film forming mechanisms S13, S14, and S15. These gas barriers S12g are constructed so that the substrate holding mechanism S12a can move between the respectively adjacent film forming mechanisms S13, S14, and S15.
[0196] In the film forming chamber S12 , each of the three-stage film forming mechanisms S13 , S14 , and S15 has a composition required for sequentially forming a film on the glass substrate 11 , and can form a film under conditions required for film formation.
[0197] In the present embodiment, the film forming mechanism S13 is used to form the phase shift layer 12 , the film forming mechanism S14 is used to form the etching stop layer 13 , and the film forming mechanism S15 is used to form the light shielding layer 14 .
[0198] Specifically, in the film forming mechanism S13 , the target S13 b is formed of a material containing chromium, which is a composition necessary for forming the phase shift layer 12 on the glass substrate 11 .
[0199] At the same time, in the film forming mechanism S13 , corresponding to the film formation of the phase shift layer 12 , the process gas supplied by the gas introduction mechanism S13 e contains carbon, nitrogen, oxygen, etc., and is conditioned to a predetermined gas partial pressure together with a sputtering gas such as argon or nitrogen.
[0200] In addition, according to the film forming conditions, the high vacuum exhaust mechanism S13f is exhausted.
[0201] In addition, in the film forming mechanism S13 , a sputtering voltage applied from the power supply S13 d to the back plate S13 c is set in accordance with the film forming of the phase shift layer 12 .
[0202] In the film forming mechanism S14 , the target S14 b is formed of a material having molybdenum silicide, which is a composition required for forming the etching stop layer 13 on the phase shift layer 12 .
[0203] At the same time, in the film forming mechanism S14 , corresponding to the film formation of the etching stop layer 13 , the process gas supplied from the gas introduction mechanism S14 e contains carbon, nitrogen, oxygen, etc., and is set to a predetermined gas partial pressure together with a sputtering gas such as argon or an inert gas.
[0204] The gas supplied by the gas introduction mechanism S14 e is configured to be able to adjust the partial pressure of the nitrogen-containing gas or the like so as to vary by a predetermined amount in accordance with the film thickness of the etching stop layer 13 to be formed.
[0205] In addition, according to the film forming conditions, exhaust is performed by the high vacuum exhaust mechanism S14f.
[0206] In addition, in the film forming mechanism S14 , a sputtering voltage applied from the power supply S14 d to the backing plate S14 c is set in accordance with the film formation of the etching stop layer 13 .
[0207] In the film forming mechanism S15 , the target S15 b is formed of a material containing chromium, which is a composition necessary for forming the light shielding layer 14 on the etching stop layer 13 .
[0208] At the same time, in the film forming mechanism S15, corresponding to the film formation of the light shielding layer 14, the process gas supplied by the gas introduction mechanism S15e contains carbon, nitrogen, oxygen, etc., and together with the sputtering gas such as argon, nitrogen, etc. which is an inert gas, the conditions are set to a specified gas partial pressure.
[0209] In addition, according to the film forming conditions, the high vacuum exhaust mechanism S15f is exhausted.
[0210] In addition, in the film forming mechanism S15 , a sputtering voltage applied from the power supply S15 d to the back plate S15 c is set in accordance with the film forming of the light shielding layer 14 .
[0211] right Fig.11 As for the manufacturing apparatus S10 shown, a glass substrate 11 transported from a loading chamber S11 by a transport mechanism S11a is transported by a substrate holding mechanism S12a in a film forming chamber S12, and three-stage sputtering film forming is performed. Then, the glass substrate 11 after film forming is transported from an unloading chamber S16 to the outside of the manufacturing apparatus S10 by a transport mechanism S16a.
[0212] In the phase shift layer forming process, in the film forming mechanism S13, a sputtering gas and a reaction gas are supplied as supply gas from a gas introduction mechanism S13e to the vicinity of a back plate S13c of the film forming chamber S12. In this state, a sputtering voltage is applied to the back plate (cathode electrode) S13c from an external power supply. In addition, a predetermined magnetic field can also be formed on the target S13b by a magnetron magnetic circuit.
[0213] Sputtering gas ions are excited by plasma near the back plate S13c in the film forming chamber S12, and the ions collide with the target S13b of the cathode electrode S13c to cause particles of the film forming material to fly out. Furthermore, since the flying particles are combined with the reaction gas and then attached to the glass substrate 11, a phase shift layer 12 with a predetermined composition is formed on the surface of the glass substrate 11.
[0214] Similarly, for the etching stop layer formation process, in the film forming mechanism S14, a sputtering gas and a reaction gas are supplied as supply gas from a gas introduction mechanism S14e to the vicinity of a back plate S14c of the film forming chamber S12. In this state, a sputtering voltage is applied to the back plate (cathode electrode) S14c from an external power supply. In addition, a predetermined magnetic field can also be formed on the target S14b by a magnetron magnetic circuit.
[0215] Sputtering gas ions are excited by plasma near the back plate S14c in the film forming chamber S12, and the ions collide with the target S14b of the cathode electrode S14c to cause particles of the film forming material to fly out. The flying particles are combined with the reaction gas and then attached to the glass substrate 11, thereby being stacked on the surface of the glass substrate 11 with a predetermined composition on the phase shift layer 12 and forming an etching stop layer 13.
[0216] Similarly, in the light shielding layer forming step, in the film forming mechanism S15, a sputtering gas and a reaction gas are supplied as supply gas from a gas introduction mechanism S15e to the vicinity of a back plate S15c of the film forming chamber S12. In this state, a sputtering voltage is applied to the back plate (cathode electrode) S15c from an external power supply. In addition, a predetermined magnetic field can also be formed on the target S15b by a magnetron magnetic circuit.
[0217] Sputtering gas ions are excited by plasma near the back plate S15c in the film forming chamber S12, and the ions collide with the target S15b of the cathode electrode S15c to cause particles of the film forming material to fly out. The flying particles are combined with the reaction gas and then attached to the glass substrate 11, thereby being stacked on the etching stop layer 13 with a predetermined composition on the surface of the glass substrate 11 and forming the light shielding layer 14.
[0218] At this time, during the film formation of the phase shift layer 12, the sputtering gas, oxygen-containing gas, etc. are supplied to a predetermined partial pressure from the gas introduction mechanism S13e and switched in a manner to control the partial pressure, thereby setting the composition of the phase shift layer 12 within a set range. At the same time, when the composition is changed in the film thickness direction to form the phase shift layer 12, the partial pressure of each gas in the atmosphere gas can also be changed according to the film thickness of the formed film.
[0219] In addition, during the formation of the etching stop layer 13, the sputtering gas, nitrogen-containing gas, etc. are supplied at a predetermined partial pressure from the gas introduction mechanism S14e, and the partial pressure of the nitrogen-containing gas is switched so as to control the partial pressure of the nitrogen-containing gas. Thus, the composition of the etching stop layer 13 is set to a predetermined concentration ratio or a variable concentration.
[0220] In particular, as described above, the partial pressure ratio of the nitrogen-containing gas is controlled so that the peak region 13A having a high nitrogen concentration and other regions having a lower nitrogen concentration than the peak region 13A are formed in the film thickness direction.
[0221] Specifically, when the molybdenum silicide compound film is formed, as the film thickness increases, the peak region 13A can be formed by increasing the partial pressure of nitrogen gas from the time when the film is formed to a predetermined film thickness such as 2 / 3 of the film thickness of the etching stop layer 13 .
[0222] At the same time, in order to set the etching stop ability in the etching stop layer 13 to a predetermined state, the composition ratio of molybdenum to silicon and the composition ratio of the contents other than molybdenum to silicon in the target S14b can be set to a predetermined state. In addition, it is preferred to appropriately select targets S14b having different composition ratios.
[0223] During the formation of the light shielding layer 14 , nitrogen gas, oxygen-containing gas, or the like is supplied at a predetermined partial pressure from the gas introduction mechanism S15 e and switched so as to control the partial pressure, thereby setting the composition of the light shielding layer 14 within a set range.
[0224] Here, examples of the oxygen-containing gas include CO 2 (carbon dioxide), O 2 (oxygen), N 2 O (nitrous oxide), NO (nitrogen monoxide), and CO (carbon monoxide).
[0225] In addition, examples of the carbon-containing gas include CO 2 (carbon dioxide), CH 4 (methane), C 2 H 6 (ethane), and CO (carbon monoxide).
[0226] In addition, examples of the nitrogen-containing gas include N 2 (nitrogen), N 2 O (nitrous oxide), NO (nitrogen monoxide), and NH 3 (ammonia).
[0227] In addition, during the film formation of the phase shift layer 12 , the etching stop layer 13 , and the light shielding layer 14 , the targets S13 b , S14 b , and S15 b may be replaced as necessary.
[0228] In addition, after forming the phase shift layer 12, the etching stop layer 13, and the light shielding layer 14, other films may be laminated on the glass substrate 11. In this case, the following method can be cited: this method uses a target corresponding to the material of the film laminated on the glass substrate 11, and sets the sputtering conditions of the gas, etc. to form the film by sputtering. Alternatively, the mask blank 10B of this embodiment may be obtained by laminating the film by a film forming method other than sputtering.
[0229] Next, the film properties of the phase shift layer 12 , the etching stop layer 13 , and the light shielding layer 14 in this embodiment, especially the film properties of the etching stop layer, will be described.
[0230] On the glass substrate 11 for forming the mask, a phase shift layer 12 constituting a chromium compound film is formed by sputtering or the like. The chromium compound film formed here is preferably a film containing chromium, oxygen, nitrogen, carbon, etc. By controlling the composition and film thickness of chromium, oxygen, nitrogen, and carbon contained in the film at this time, the phase shift layer 12 having a desired transmittance and phase can be formed.
[0231] Next, a molybdenum silicide compound film serving as the etching stopper layer 13 is formed by sputtering or the like. The molybdenum silicide compound film formed here is preferably a film containing molybdenum, silicon, oxygen, nitrogen, carbon, and the like.
[0232] Then, a chromium compound film serving as the light shielding layer 14 is formed by sputtering or the like. The chromium compound film formed here is preferably a film containing chromium, oxygen, nitrogen, carbon, and the like.
[0233] By forming the mask blank 10B having such a film structure, it is possible to form the phase shift mask 10 in which the phase shift layer 12 and the light shielding layer 14 are formed of a chromium compound.
[0234] When the molybdenum silicide film is used to form the etching stop layer 13, etching needs to be performed using an etching solution containing fluoric acid. Therefore, it is necessary to reduce the effect of etching on the glass substrate 11. Therefore, it is best to use the molybdenum silicide film with an etching rate (ER) as high as possible.
[0235] Fig.12 The relationship between the nitrogen concentration in the film and the etching rate when a molybdenum silicide film is formed using molybdenum silicide targets with different target compositions is shown. Fig.12 It is understood that a molybdenum silicide film having a high etching rate can be formed by using a molybdenum silicide target having a small silicon content in the target composition.
[0236] In addition, regarding the molybdenum silicide target, by mixing MoSi 2 which is a crystal of molybdenum silicide and Si materials, a target having a desired composition ratio can be formed.
[0237] Here, if silicon is not present in excess of MoSi2 at a constant level or above, it is difficult to form a target with a stable composition.
[0238] In contrast, the inventors have found that if the silicon composition is increased until the composition ratio of molybdenum to silicon is 1:2.3, a target with a high relative density can be stably formed. Therefore, by using a target with a composition ratio of molybdenum silicide of 1:2.3, a high-density target can be used while suppressing etching of the glass substrate 11.
[0239] Thus, it is possible to manufacture the mask blank 10B suitable for producing the phase shift mask 10 with reduced influence of defects as a product.
[0240] These manufacturing conditions and film characteristics of the etching stop layer 13 were verified.
[0241] First, a molybdenum silicide film is formed as the etching stopper layer 13 using a target having a composition ratio of molybdenum to silicon of 1:2.3, and the molybdenum silicide film is formed by changing the flow rates of argon and nitrogen during film formation.
[0242] In the manufacturing process of the phase shift mask 10 , chemical liquids such as acid and alkali are generally used, but it is necessary to suppress the change in transmittance during the process.
[0243] The present inventors have found that by increasing the nitrogen concentration of the molybdenum silicide film, the chemical resistance to acid and alkali liquids can be improved.
[0244] Thus, as the mask blank 10B, a peak region 13A composed of a molybdenum silicide film having a high nitrogen concentration is formed at the interface between the light shielding layer 14 and the etching stop layer 13. In addition, as the mask blank 10B, a molybdenum silicide film having a low nitrogen concentration is used in a portion of the etching stop layer 13 below the peak region 13A (a portion close to the glass substrate 11).
[0245] Thus, the etching time of the etching stopper film can be shortened and the influence of the contact between the glass substrate 11 and the etching liquid can be reduced, thereby forming an etching stopper film having high resistance to chemical liquids.
[0246] Furthermore, the present inventors have found that when etching the light shielding layer 14 which is a chromium film, the etching stopper layer 13 formed with a molybdenum silicide film having a high nitrogen concentration on the surface has a high etching stopper function with little penetration of etching solution.
[0247] Therefore, it is preferable to use a molybdenum silicide film having a nitrogen concentration as high as possible for the etching stop layer 13 .
[0248] Therefore, by forming the peak region 13A as a molybdenum silicide film with a high nitrogen concentration on the upper layer of the etching stop layer 13, there is also the following effect: that is, when etching the light shielding layer 14, the penetration of the etching solution near the interface between the light shielding layer 14 and the etching stop layer 13 is suppressed.
[0249] Furthermore, the present inventors investigated the relationship between the etching rate of the molybdenum silicide film and the sheet resistance, and found that the etching rate of the molybdenum silicide film increases as the sheet resistance decreases.
[0250] It can be seen that by using a resistivity of 1.0×10 -3 The invention also found that the use of a molybdenum silicide film with a resistivity of less than Ωcm as an etching stop layer can form an etching stop layer with a high etching rate. In addition, it was found that the use of a molybdenum silicide film with a low resistivity can suppress electrostatic damage.
[0251] When a molybdenum silicide film is used as the etching stop layer 13, a target having a ratio of molybdenum to silicon of 1:3 or less is used. A nitrogen-containing gas is used as an atmospheric gas during sputtering. By controlling the gas partial pressure of the nitrogen-containing gas, a peak region 13A having a nitrogen concentration of 30% or more is formed at the interface between the light shielding layer 14 and the etching stop layer 13. In addition, the nitrogen concentration at the lower portion closer to the glass substrate 11 than the peak region 13A is set to 25% or less.
[0252] The thickness of the etching stop layer 13, which is a molybdenum silicide film, is set to be 10 nm to 100 nm, and the resistivity of the lower portion of the peak region 13A closer to the glass substrate 11 is set to 1.0×10 -3 By using such a molybdenum silicide film as the etching stopper layer 13, it is possible to form a phase shift mask 10 which has little influence on etching of the glass substrate 11 and has a good cross-sectional shape.
[0253] [Example]
[0254] Next, embodiments of the present invention will be described.
[0255] Furthermore, as a specific example of the etching stop layer 13 in the present invention, a confirmation test will be described.
[0256] <Example>
[0257] As Example 1, a molybdenum silicide compound film is formed as an etching stop layer on a glass substrate by sputtering or the like. The molybdenum silicide compound film formed here is a film containing molybdenum, silicon, oxygen, nitrogen, carbon, etc. The composition of the film is evaluated by Auger electron spectroscopy.
[0258] The results are shown in Fig.13 .
[0259] like Fig.13 As shown, it can be confirmed that a peak region with a high nitrogen concentration is formed on the left side of the figure.
[0260] Next, in sputtering for forming a molybdenum silicide compound film, a target having a ratio of molybdenum to silicon of 1:2.3 was used, and the film was formed by changing the nitrogen partial pressure within a range of 0 to 100%.
[0261] As the atmospheric gas during sputtering, carbon dioxide or argon was used in addition to nitrogen.
[0262] These were designated as Examples 1 to 4, and the composition ratios of the respective samples, the etching rates of molybdenum and silicon, and the ratio of the etching rates to the etching rates of glass were measured.
[0263] Table 1 shows the results.
[0264]
[0265] Likewise, in sputtering for forming a molybdenum silicide compound film, a target having a ratio of molybdenum to silicon of 1:3.7 was used, and the film formation was performed while changing the nitrogen partial pressure within a range of 0 to 100%.
[0266] As the atmospheric gas during sputtering, carbon dioxide or argon was used in addition to nitrogen.
[0267] These were designated as Examples 5 to 8, and their composition ratios, etching rates of molybdenum to silicon, and ratios of the etching rates to the etching rates of glass were measured.
[0268] The results are shown in Table 1.
[0269] Furthermore, in Examples 1 to 8, the relationship between the etching rate and the sheet resistance of the molybdenum silicide film was respectively examined.
[0270] These results show that the nitrogen concentration in the molybdenum silicide film can be controlled by the nitrogen partial pressure during film formation. In addition, by sputtering using a MoSi2.3 target with a composition ratio of Si / Mo=2.3, a molybdenum silicide film with a low resistivity can be formed. This shows that the influence of electrostatic damage can be reduced.
[0271] In addition, it was found that by using a stacked structure of a molybdenum silicide film having a high nitrogen concentration and a molybdenum silicide film having a low nitrogen concentration, a molybdenum silicide film suitable for use in a phase shift mask can be formed, the cross-sectional shape of the molybdenum silicide film is good, and the etching time can be shortened.
[0272] In addition, it is known that the chemical resistance to acid and alkali liquids is improved by increasing the nitrogen concentration of the molybdenum silicide film. It is known that the etching stop film using the molybdenum silicide film with a high nitrogen concentration has a high etching stop function with less infiltration of the etching liquid when etching the chromium film. The relationship between the etching rate and the sheet resistance of the molybdenum silicide film was investigated, and the result showed that if the sheet resistance becomes lower, the etching rate of the molybdenum silicide film is accelerated. In addition, it is also clear that by using a molybdenum silicide film with a low resistivity, electrostatic damage can be suppressed.
[0273] The inventors have completed the present invention based on these circumstances. Thus, it is possible to form a mask that has little effect on etching of the glass substrate and has a good cross-sectional shape.
[0274] Description of Reference Numerals
[0275] 10…Phase shift mask
[0276] 10B...Mask Blank
[0277] 10L…Light-transmitting area
[0278] 10P1…Exposure area
[0279] 10P2…Phase shift region
[0280] 11…Glass substrate (transparent substrate)
[0281] 12…Phase shift layer
[0282] 12P1…Phase shift pattern
[0283] 13…Etch stop layer
[0284] 13P1, 13P2…etch stop pattern
[0285] 14…Light-shielding layer
[0286] 14P1, 14P2…Shading pattern
[0287] 15…Photoresist layer
[0288] 15P1, 15P2…Resist pattern
Claims
1. A mask blank having a layer to be a phase shift mask, the mask blank having: A phase shift layer, laminated on a transparent substrate; an etching stop layer disposed at a position farther from the transparent substrate than the phase-shift layer; and a light shielding layer disposed at a position farther from the transparent substrate than the etching stop layer, The phase shift layer contains chromium, The light shielding layer contains chromium and oxygen, The etching stop layer contains molybdenum silicide and nitrogen, and has a peak region where the nitrogen concentration reaches a peak at a position close to the light shielding layer in the film thickness direction. The nitrogen concentration in the peak region of the etching stop layer is set to 30 atomic % or more.
2. The mask blank according to claim 1, wherein: The etching stop layer has the peak region on an upper surface close to the light shielding layer in a film thickness direction.
3. The mask blank according to claim 1, wherein: The resistivity of the etching stop layer in the peak region is set to 1.0×10 -3 Ωcm or more.
4. The mask blank according to claim 2, wherein: The resistivity of the etching stop layer in the peak region is set to 1.0×10 -3 Ωcm or more.
5. The mask blank according to any one of claims 1 to 4, wherein: The silicon concentration in the peak region of the etching stop layer is set to 35 atomic % or less.
6. The mask blank according to any one of claims 1 to 4, wherein: The molybdenum concentration in the peak region of the etching stop layer is set to 30 atomic % or less.
7. The mask blank according to any one of claims 1 to 4, wherein: The film thickness of the peak region is set in a range not greater than 1 / 3 of the film thickness of the etching stop layer.
8. The mask blank according to any one of claims 1 to 4, wherein: The resistivity of the etching stop layer except the peak region is set to 1.0×10 -3 Ωcm or less.
9. The mask blank according to any one of claims 1 to 4, wherein: The nitrogen concentration of the etching stop layer excluding the peak region is set to 25 atomic % or less.
10. The mask blank according to any one of claims 1 to 4, wherein: The composition ratio of molybdenum to silicon in the etching stop layer excluding the peak region is set to 1≤Si / Mo.
11. The mask blank according to any one of claims 1 to 4, wherein: The film thickness of the etching stop layer is set in the range of 10 nm to 100 nm.
12. A method for manufacturing a mask blank, the method being the method for manufacturing a mask blank according to any one of claims 1 to 11, comprising: a phase shift layer forming step of laminating the phase shift layer containing chromium on the transparent substrate; an etching stop layer forming step of laminating the etching stop layer containing molybdenum silicide and nitrogen at a position farther from the transparent substrate than the phase shift layer; and a light shielding layer forming step of stacking the light shielding layer containing chromium and oxygen at a position farther from the transparent substrate than the etching stop layer, In the etching stop layer forming step, the etching stop layer is formed by controlling the nitrogen concentration in the peak region in the film thickness direction by setting the partial pressure of a nitrogen-containing gas as a supply gas during sputtering.
13. The method for manufacturing a mask blank according to claim 12, wherein: In the etching stop layer forming step, the partial pressure of the nitrogen-containing gas is set so that the sheet resistance in the etching stop layer increases with an increase in nitrogen content.
14. The method for manufacturing a mask blank according to claim 13, wherein: In the etching stop layer forming step, the peak region is formed by setting the partial pressure ratio of the nitrogen-containing gas to a range of 30% or more.
15. The method for manufacturing a mask blank according to claim 14, wherein: In the etching stop layer forming process, the nitrogen-containing gas is N2.
16. The method for manufacturing a mask blank according to any one of claims 12 to 15, wherein: In the etching stop layer forming step, a target in which the composition ratio of molybdenum to silicon is set to 2.3≤Si / Mo≤3.0 is used.
17. A phase shift mask manufactured from the mask blank according to any one of claims 1 to 11.
18. A method for manufacturing a phase-shift mask, the method being the method for manufacturing a phase-shift mask according to claim 17, comprising: a phase-shift pattern forming step of forming a pattern on the phase-shift layer; An etch stop pattern forming step of forming a pattern on the etch stop layer; and a light shielding pattern forming step of forming a pattern on the light shielding layer, The etching liquid in the phase shift pattern forming step and the light shielding pattern forming step is different from the etching liquid in the etching stop pattern forming step.