Thermoplastic elastomer composition

By using ethylene rubber and propylene polymers in thermoplastic elastomer compositions, combined with specific molding conditions and hierarchical chromatography, the problem of thermoplastic elastomer compositions losing pattern and shape under harsh conditions is solved, and molding is achieved The product has excellent appearance and formability.

CN113444311BActive Publication Date: 2024-10-29SUMITOMO CHEM CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202110301070.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-22
Publication Date
2024-10-29
Estimated Expiration
2041-03-22

AI Technical Summary

Technical Problem

Existing thermoplastic elastomer compositions tend to lose their embossed patterns and shapes under harsh conditions such as vacuum forming, resulting in poor appearance of molded products.

Method used

Using a thermoplastic elastomer composition of 10% to 90% ethylene rubber and 10% to 90% propylene polymer, the sinking temperature is controlled by hot pressing at 200°C and cold pressing at 23°C. Above 115°C, cross-fractionation chromatography and gel permeation chromatography are combined to adjust the ingredient ratio and molecular weight distribution to ensure excellent embossing retention and appearance of molded products.

Benefits of technology

Even under harsh conditions such as vacuum forming, the embossed pattern and shape can be maintained to ensure excellent appearance and formability of molded products. It is suitable for areas with high requirements such as skin materials for automotive interiors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002986270410000441
    Figure BDA0002986270410000441
  • Figure BDA0002986270410000471
    Figure BDA0002986270410000471
Patent Text Reader

Abstract

The present invention provides a thermoplastic elastomer composition which can maintain a pattern and shape such as embossing even by processing under relatively harsh conditions such as vacuum forming, and has excellent moldability and appearance of the molded product. A thermoplastic elastomer composition, comprising 10% to 90% by mass of (A) an ethylene-based rubber and 10% to 90% by mass of (B) a propylene-based polymer (wherein the total amount of the thermoplastic elastomer composition is 100% by mass), wherein the sinking temperature of a pressed sheet obtained by press-molding the thermoplastic elastomer composition under the following molding conditions is 115° C. or higher, the sinking temperature being measured in accordance with JIS K7196-1991 and being defined as the temperature at which the indenter penetrates 100 μm from the sheet surface. Molding conditions: The thermoplastic elastomer composition is hot-pressed at a temperature of 200° C. and a maximum pressure of 10 MPa for 5 minutes, and then cold-pressed at a temperature of 23° C. and a maximum pressure of 10 MPa for 5 minutes to produce a pressed sheet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to thermoplastic elastomer compositions. Background Art

[0002] Thermoplastic elastomer compositions such as olefin-based thermoplastic elastomer compositions have advantages such as easy processing and are suitably used in a wide range of fields such as automobile parts (see, for example, Patent Document 1).

[0003] Prior art literature

[0004] [Patent Document]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 2001-335641 Summary of the invention

[0006] Problems to be solved by the invention

[0007] Automobile parts such as door trims, instrument panels and other automobile interior skin materials are often preferably provided with patterns and shapes such as embossing (patterns with concave and convex) on the surface in view of appearance. When a thermoplastic elastomer composition is processed into an embossed sheet, the embossing may disappear depending on the processing conditions after embossing, for example, when vacuum forming is performed, and a solution to this problem is required.

[0008] Under such circumstances, an object of the present invention is to provide a thermoplastic elastomer composition which can maintain a pattern and shape such as embossing even when processed under severe conditions such as vacuum forming and has excellent moldability and appearance of molded products.

[0009] Means used to solve problems

[0010] The present inventors conducted intensive studies in view of such background and finally completed the present invention.

[0011] That is, the first invention of this application is: [1]

[0013] A thermoplastic elastomer composition comprising 10% to 90% by mass of (A) an ethylene-based rubber and 10% to 90% by mass of (B) a propylene-based polymer (wherein the total amount of the thermoplastic elastomer composition is 100% by mass), wherein:

[0014] The pressed sheet obtained by press-molding the thermoplastic elastomer composition under the following molding conditions has a sinking temperature (sinking temperature) of 115° C. or more, the sinking temperature being measured in accordance with JIS K7196-1991 and being defined as the temperature at which the indenter penetrates 100 μm from the sheet surface,

[0015] Molding conditions: The thermoplastic elastomer composition was hot-pressed at a temperature of 200° C. and a maximum pressure of 10 MPa for 5 minutes, and then cold-pressed at a temperature of 23° C. and a maximum pressure of 10 MPa for 5 minutes to prepare a pressed sheet.

[0016] The following [2] and [3] are respectively preferred modes or embodiments of the first invention of the present application. [2]

[0018] The thermoplastic elastomer composition according to [1], wherein at least a part of the (A) ethylene-based rubber is crosslinked. [3]

[0020] The thermoplastic elastomer composition as described in [1] or [2], wherein the thermoplastic elastomer composition further contains 1% by mass to 60% by mass of (E) mineral oil, and the content of (A) ethylene-based rubber is 10% by mass to 89% by mass, and the content of (B) propylene-based polymer is 10% by mass to 89% by mass (wherein the total amount of the thermoplastic elastomer composition is 100% by mass).

[0021] The second invention of this application is: [4]

[0023] A sheet comprising 10% to 90% by mass of (A) an ethylene-based rubber and 10% to 90% by mass of (B) a propylene-based polymer (wherein the total amount of the sheet is set to 100% by mass), wherein:

[0024] The sinking temperature of the sheet is 115° C. or higher, which is measured in accordance with JIS K7196-1991 and is defined as the temperature at which the indenter penetrates 100 μm from the sheet surface.

[0025] The following [5] and [6] are respectively preferred modes or implementation modes of the second invention of the present application. [5]

[0027] The sheet according to [4], wherein at least a portion of the (A) ethylene-based rubber is cross-linked. [6]

[0029] A sheet as described in [4] or [5], wherein the sheet further contains 1% to 60% by mass of (E) mineral oil, and the content of (A) ethylene rubber is 10% to 89% by mass, and the content of (B) propylene polymer is 10% to 89% by mass (wherein the total amount of the sheet is set to 100% by mass).

[0030] The third invention of this application is: [7]

[0032] A thermoplastic elastomer composition, wherein the ratio of component (X) eluted in the range of elution temperature of more than 100° C. and less than or equal to 140° C. relative to the total elution amount (100% by mass) measured under the following conditions (1) to (3) by cross-fractionation chromatography using an apparatus having a temperature-elution fractionation section and a gel permeation chromatography section is 1% by mass to 50% by mass,

[0033] The proportion of the component (X1) having a molecular weight M in terms of polystyrene logM of 5.6 or more in the component (X) is 6.0% to 45.0% by mass relative to the total eluted amount (100% by mass), and

[0034] The gel fraction of the thermoplastic elastomer composition is 5.0% to 50% by mass.

[0035] (1) the temperature-eluting fractionation section into which the o-dichlorobenzene solution of the thermoplastic elastomer composition (the concentration of the thermoplastic elastomer composition in the solution was 1 mg / mL) was injected was maintained at 100° C. for 10 minutes;

[0036] (2) The temperature of the temperature-elution fractionation section was lowered to -5°C at a rate of 2.0°C / min, then maintained at -5°C for 30 minutes, and the elution amount at -5°C was measured;

[0037] (3) The following operation is repeated at three reaching temperatures of 50°C, 100°C and 140°C: the temperature of the temperature-eluting fractionation section is raised at a rate of 40°C / min to the reaching temperature, then maintained at the reaching temperature for 30 minutes, and then the elution amount at the reaching temperature is measured.

[0038] The following [8] to

[10] are respectively preferred modes or implementation modes of the third invention of the present application. [8]

[0040] The thermoplastic elastomer composition according to [7], wherein the ratio of the component (α) eluted at an elution temperature of -5°C is 70% by mass or less relative to 100% by mass of the total elution amount in cross fractionation chromatography. [9]

[0042] The thermoplastic elastomer composition according to [7] or [8], wherein the ratio of the component (β) eluted at an elution temperature in the range of greater than -5°C and less than or equal to 50°C is 1% by mass to 39% by mass relative to 100% by mass of the total elution amount in cross fractionation chromatography.

[10]

[0044] The thermoplastic elastomer composition according to any one of [7] to [9], wherein in cross fractionation chromatography, the ratio of the component (γ) eluted in the elution temperature range of more than 50°C and less than or equal to 100°C is 0.1% by mass to 39% by mass relative to the total elution amount (100% by mass).

[0045] Effects of the Invention

[0046] According to the present invention, it is possible to provide a thermoplastic elastomer composition which can maintain a pattern and shape such as embossing even when processed under relatively severe conditions such as vacuum forming and which has excellent moldability and appearance of a molded product. DETAILED DESCRIPTION

[0047] (First invention of this application)

[0048] The first invention of the present application is a thermoplastic elastomer composition, which contains 10% by mass to 90% by mass of (A) ethylene-based rubber and 10% by mass to 90% by mass of (B) propylene-based polymer (wherein the total amount of the thermoplastic elastomer composition is set to 100% by mass), wherein the sinking temperature of a pressed sheet obtained by press-molding the thermoplastic elastomer composition under the following molding conditions is 115° C. or higher, and the sinking temperature is measured in accordance with JIS K7196-1991 and is defined as the temperature when the indenter penetrates 100 μm from the surface of the pressed sheet.

[0049] Here, the molding conditions of the pressed tablets are as follows.

[0050] Molding conditions: The thermoplastic elastomer composition was hot-pressed at a temperature of 200° C. and a maximum pressure of 10 MPa for 5 minutes, and then cold-pressed at a temperature of 23° C. and a maximum pressure of 10 MPa for 5 minutes to prepare a pressed sheet.

[0051] Sinking temperature

[0052] The penetration temperature measured according to JIS K7196-1991 and defined as the temperature when the indenter penetrates 100 μm from the sheet surface can be specifically measured using a thermomechanical analyzer according to the method defined in JIS K7196 “Softening temperature measurement”, and more specifically can be measured by the following method.

[0053] A plate-shaped test piece with a length of 5.0 mm, a width of 5.0 mm, and a thickness of 0.50 mm was cut from the center of the pressed sheet produced under the above molding conditions, and the measurement was performed in the thickness direction. As for the tip of the indenter, a cylindrical tip with a diameter of 1.0 mm and a length of 2 mm was used, and a force of 780 mN was applied to the indenter. The temperature when the indenter was sunk to 100 μm was taken as the sinking temperature. As more detailed conditions, for example, the conditions described in the examples of the present application can be adopted.

[0054] The first invention of the present application can provide a thermoplastic elastomer composition that can maintain a pattern and shape such as embossing even by processing under severe conditions such as vacuum forming, and has excellent moldability and appearance of a molded product by having a sinking temperature of 115°C or higher and satisfying the other conditions specified in the first invention of the present application. The sinking temperature is preferably 125°C to 170°C, more preferably 130°C to 165°C, and even more preferably 135°C to 160°C.

[0055] In many cases, it is effective to use the thermoplastic elastomer composition of the third invention of the present application as a means for adjusting the sinking temperature to 115° C. or higher. More specifically, in the third invention of the present application, the sinking temperature can be increased by increasing the amount of the component (X1).

[0056] The first invention of the present application is a thermoplastic elastomer composition containing 10% to 90% by mass of (A) ethylene-based rubber and 10% to 90% by mass of (B) propylene-based polymer. Here, the total amount of the thermoplastic elastomer composition is set to 100% by mass.

[0057] The content of (A) ethylene rubber is usually 10% to 90% by mass, preferably 26% to 70% by mass, and more preferably 36% to 55% by mass. From the viewpoint of rubber elasticity and flexibility suitable for use as an inner skin material, the content of (A) ethylene rubber is usually set to 10% by mass or more. In addition, from the viewpoint of moldability and embossing retention during processing under harsh high temperature conditions, the content of (A) ethylene rubber is usually set to 90% by mass or less.

[0058] The content of the (B) propylene polymer is usually 10% to 90% by mass, preferably 16% to 45% by mass, and more preferably 26% to 40% by mass. From the viewpoint of moldability and embossing retention, the content of the (B) propylene polymer is usually set to 10% by mass or more. In addition, from the viewpoint of flexibility suitable for use as an inner skin material, the content of the (B) propylene polymer is usually set to 90% by mass or less.

[0059] (A) Ethylene rubber

[0060] The (A) ethylene rubber constituting the thermoplastic elastomer composition according to the embodiment of the first invention of the present application is a polymer having 50% by mass to 90% by mass of monomer units derived from ethylene and monomer units derived from at least one monomer selected from the group consisting of propylene and α-olefins having 4 to 15 carbon atoms (wherein the total amount of the ethylene rubber is 100% by mass). The (A) ethylene rubber may have monomer units derived from monomers other than ethylene and at least one monomer selected from the group consisting of propylene and α-olefins having 4 to 15 carbon atoms.

[0061] Examples of propylene and α-olefins having 4 to 15 carbon atoms include propylene, 1-butene, 2-methylpropylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 1-octene, etc. In the preparation of (A) ethylene-based rubber, propylene and α-olefins having 4 to 15 carbon atoms may be used alone or in combination of two or more. The monomer unit derived from at least one monomer selected from the group consisting of propylene and α-olefins having 4 to 15 carbon atoms is preferably a monomer unit derived from propylene, a monomer unit derived from 1-butene, or a monomer unit derived from 1-octene, and more preferably a monomer unit derived from propylene.

[0062] The content of monomer units derived from ethylene in the (A) ethylene-based rubber is 50 to 90% by mass, preferably 55 to 85% by mass, and more preferably 60 to 75% by mass (wherein the total amount of the ethylene-based rubber is 100% by mass).

[0063] (A) The content of monomer units derived from at least one monomer selected from the group consisting of propylene and α-olefins having 4 to 15 carbon atoms in the ethylene-based rubber is 10% to 50% by mass, preferably 15% to 45% by mass, and more preferably 25% to 40% by mass (wherein the total amount of the ethylene-based rubber is 100% by mass).

[0064] The content of monomer units derived from ethylene and the content of monomer units derived from at least one monomer selected from the group consisting of propylene and α-olefins having 4 to 15 carbon atoms in the (A) ethylene-based rubber can be obtained by infrared spectroscopy. Specifically, the infrared absorption spectrum of the (A) ethylene-based rubber is measured using an infrared spectrophotometer, and the content of monomer units derived from ethylene and the content of monomer units derived from at least one monomer selected from the group consisting of propylene and α-olefins having 4 to 15 carbon atoms are calculated according to the method described in "Characterization of Polyethylene by Infrared Absorption Spectroscopy" (written by Takayama, Usami et al.) or "Die Makromolekulare Chemie, 177, 461 (1976) (written by McRae, MA, Madam S, WF et al.)".

[0065] (A) The ethylene rubber may have monomer units derived from monomers other than ethylene and at least one monomer selected from the group consisting of propylene and α-olefins having 4 to 15 carbon atoms. Examples of the other monomers include conjugated dienes having 4 to 8 carbon atoms such as 1,3-butadiene, 2-methyl-1,3-butadiene, 1,3-pentadiene, and 2,3-dimethyl-1,3-butadiene; non-conjugated dienes having 5 to 15 carbon atoms such as dicyclopentadiene, 5-ethylidene-2-norbornene, 1,4-hexadiene, 1,5-cyclooctadiene, 7-methyl-1,6-octadiene, and 5-vinyl-2-norbornene; carboxylic acid vinyl esters such as vinyl acetate; unsaturated carboxylic acid esters such as methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, and ethyl methacrylate; and unsaturated carboxylic acids such as acrylic acid and methacrylic acid. The other monomer is preferably a non-conjugated diene having 5 to 15 carbon atoms, and more preferably 5-ethylidene-2-norbornene or dicyclopentadiene. The (A) ethylene-based rubber may contain two or more monomer units derived from the other monomer.

[0066] In the case where (A) ethylene rubber has monomer units derived from monomers other than ethylene and at least one monomer selected from the group consisting of propylene and α-olefins having 4 to 15 carbon atoms, the content of the monomer units derived from the other monomers is preferably 1% to 30% by mass, more preferably 2% to 20% by mass, and further preferably 3% to 15% by mass (wherein the total amount of the ethylene rubber is set to 100% by mass). The content of the monomer units derived from the other monomers can be obtained by infrared spectroscopy. Specifically, an infrared spectrophotometer is used to measure the peak intensity of the peak generated by the other monomers in the (A) ethylene rubber, and the content of the monomer units derived from the other monomers in the (A) ethylene rubber is calculated based on the peak intensity.

[0067] As (A) ethylene rubber, there can be listed: ethylene-propylene copolymer, ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-1-octene copolymer, ethylene-propylene-1-butene copolymer, ethylene-propylene-1-hexene copolymer, ethylene-propylene-1-octene copolymer, ethylene-propylene-5-ethylidene-2-norbornene copolymer, ethylene-propylene-dicyclopentadiene copolymer, ethylene-propylene-1,4-hexadiene copolymer, ethylene-propylene-5-vinyl-2-norbornene copolymer, etc. (A) ethylene rubber can be used alone or in combination of two or more. As (A) ethylene rubber, ethylene-propylene copolymer and ethylene-propylene-5-ethylidene-2-norbornene copolymer are preferred.

[0068] As a method for producing (A) ethylene rubber, there can be mentioned a method of copolymerizing ethylene with at least one monomer selected from the group consisting of propylene and α-olefins having 4 to 15 carbon atoms in the presence of a known complex catalyst such as a Ziegler-Natta catalyst, a metallocene complex or a non-metallocene complex. As a polymerization method, there can be mentioned a slurry polymerization method, a solution polymerization method, a bulk polymerization method, a gas phase polymerization method and the like.

[0069] It is preferred that at least a part of the (A) ethylene-based rubber is crosslinked.

[0070] (A) Mooney viscosity of ethylene rubber measured at 100°C (ML 1+4 100°C) is preferably 5 to 300, more preferably 10 to 200. It should be noted that the Mooney viscosity (ML 1+4 100℃) according to JIS K6300, "ML 1+4 100°C” has the following meanings.

[0071] M: Mooney viscosity

[0072] L: Use a large rotor

[0073] 100℃: Measurement temperature

[0074] 1+4: The value measured when the sample is heated for 1 minute and then the rotor is rotated at 2 rpm for 4 minutes

[0075] (A) The density of ethylene rubber is usually 0.850 g / cm 3 ~0.900g / cm 3 , preferably 0.870 g / cm 3 ~0.890g / cm 3 .

[0076] (B) Propylene polymer

[0077] The (B) propylene-based polymer constituting the thermoplastic elastomer composition of the embodiment of the first invention of the present application is a polymer having a content of monomer units derived from propylene of more than 50% by mass (wherein the total amount of the propylene-based polymer is 100% by mass). Examples of the (B) propylene-based polymer include propylene homopolymers, propylene random copolymers, and propylene polymer materials, preferably propylene homopolymers or propylene polymer materials. The (B) propylene-based polymer may be composed of only one type, or may contain two or more types.

[0078] Examples of the propylene random copolymer include:

[0079] (1) a propylene-ethylene polymer having a content of 90% to 99.5% by mass of monomer units derived from propylene and a content of 0.5% to 10% by mass of monomer units derived from ethylene (wherein the total content of the monomer units derived from propylene and the monomer units derived from ethylene is taken as 100% by mass);

[0080] (2) a propylene-ethylene-α-olefin random copolymer containing 81% to 99% by mass of monomer units derived from propylene, 0.5% to 9.5% by mass of monomer units derived from ethylene, and 0.5% to 9.5% by mass of monomer units derived from α-olefins having 4 to 10 carbon atoms (the total content of monomer units derived from propylene, monomer units derived from ethylene, and monomer units derived from α-olefins having 4 to 10 carbon atoms being 100% by mass); and

[0081] (3) A propylene-α-olefin random copolymer having a content of 90% by mass to 99.5% by mass of monomer units derived from propylene and a content of 0.5% by mass to 10% by mass of monomer units derived from α-olefins having 4 to 10 carbon atoms (wherein the total content of the monomer units derived from propylene and the monomer units derived from α-olefins having 4 to 10 carbon atoms is taken as 100% by mass).

[0082] Examples of the α-olefin having 4 to 10 carbon atoms in the propylene-ethylene-α-olefin random copolymer and the propylene-α-olefin random copolymer include 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 3-methyl-1-butene, 3-methyl-1-pentene, 4-methyl-1-pentene, 2-ethyl-1-hexene, and 2,2,4-trimethyl-1-pentene.

[0083] Examples of the method for producing the propylene homopolymer and the propylene random copolymer include known polymerization methods using known olefin polymerization catalysts, for example, slurry polymerization methods, solution polymerization methods, bulk polymerization methods, gas phase polymerization methods, etc. using complex catalysts such as Ziegler-Natta catalysts, metallocene complexes or non-metallocene complexes.

[0084] The propylene polymer material is a polymer material comprising a propylene homopolymer portion (I) and an ethylene copolymer portion (II), wherein the ethylene copolymer portion (II) has a monomer unit derived from at least one monomer selected from the group consisting of propylene and an α-olefin having 4 to 10 carbon atoms and a monomer unit derived from ethylene. The content of the propylene homopolymer portion (I) in the propylene polymer material is usually 70 to 95% by mass, preferably 75 to 95% by mass, and the content of the ethylene copolymer portion (II) is usually 5 to 30% by mass, preferably 5 to 25% by mass (wherein the total amount of the propylene polymer material is 100% by mass).

[0085] Examples of the α-olefin having 4 to 10 carbon atoms in the ethylene copolymer portion (II) include 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 4-methyl-1-pentene, 2-ethyl-1-hexene, 2,2,4-trimethyl-1-pentene, etc. The α-olefin having 4 to 10 carbon atoms is preferably 1-butene, 1-hexene, and 1-octene. The α-olefin having 4 to 10 carbon atoms may be used alone or in combination of two or more.

[0086] The content of monomer units derived from ethylene in the ethylene copolymer part (II) is usually 22% to 80% by mass, preferably 25% to 70% by mass, and more preferably 27% to 60% by mass. The content of monomer units derived from at least one monomer selected from the group consisting of propylene and α-olefins having 4 to 10 carbon atoms in the ethylene copolymer part (II) is usually 20% to 78% by mass, preferably 30% to 75% by mass, and more preferably 40% to 73% by mass (wherein the total content of monomer units derived from at least one monomer selected from the group consisting of propylene and α-olefins having 4 to 10 carbon atoms and monomer units derived from ethylene is set to 100% by mass). The content of monomer units derived from at least one monomer selected from the group consisting of propylene and α-olefins having 4 to 10 carbon atoms and the content of monomer units derived from ethylene can be determined by infrared spectroscopy.

[0087] Examples of the ethylene copolymer portion (II) include propylene-ethylene copolymers, ethylene-(1-butene) copolymers, ethylene-(1-hexene) copolymers, ethylene-(1-octene) copolymers, propylene-ethylene-(1-butene) copolymers, propylene-ethylene-(1-hexene) copolymers, propylene-ethylene-(1-octene) copolymers, and the like, preferably propylene-ethylene copolymers and propylene-ethylene-(1-butene) copolymers. The ethylene copolymer portion (II) may be a random copolymer or a block copolymer.

[0088] The propylene polymer material can be produced by multi-step polymerization using a polymerization catalyst. For example, the propylene polymer material can be produced by producing a propylene homopolymer fraction (I) in a previous polymerization step and producing an ethylene copolymer fraction (II) in a subsequent polymerization step.

[0089] Examples of the polymerization catalyst used in the production of the propylene polymer include a Ziegler-type catalyst system, a Ziegler-Natta-type catalyst system, a catalyst system comprising a transition metal compound of Group 4 of the periodic table having a cyclopentadienyl ring and an alkylaluminoxane, a catalyst system comprising a transition metal compound of Group 4 of the periodic table having a cyclopentadienyl ring, a compound that forms an ionic complex by reacting with the transition metal compound, and an organic aluminum compound, and the like.

[0090] In addition, in the presence of the above-mentioned polymerization catalyst, a prepolymerized catalyst can be used. As the prepolymerized catalyst, for example, the catalyst system recorded in Japanese Unexamined Patent Publication No. 61-218606, Japanese Unexamined Patent Publication No. 61-287904, Japanese Unexamined Patent Publication No. 5-194685, Japanese Unexamined Patent Publication No. 7-216017, Japanese Unexamined Patent Publication No. 9-316147, Japanese Unexamined Patent Publication No. 10-212319, Japanese Unexamined Patent Publication No. 2004-182981 can be enumerated.

[0091] As the polymerization method in the manufacture of propylene polymer materials, bulk polymerization, solution polymerization, slurry polymerization, gas phase polymerization, etc. can be listed. As the inert hydrocarbon solvent used in solution polymerization and slurry polymerization, propane, butane, isobutane, pentane, hexane, heptane, octane, etc. can be listed. These polymerization methods can be combined in two or more, and can be any of intermittent or continuous. As the polymerization method in the manufacture of propylene polymer materials, continuous gas phase polymerization, bulk-gas phase polymerization in which bulk polymerization and gas phase polymerization are continuously carried out, is preferred.

[0092] The intrinsic viscosity ([ηcxs]) of the 20°C xylene soluble matter (CXS portion) of the (B) propylene-based polymer is preferably 1.0 dl / g to 8.0 dl / g, more preferably 2.0 dl / g to 7.0 dl / g, and still more preferably 3.0 dl / g to 6.5 dl / g. In addition, the ratio of [ηcxs] to the intrinsic viscosity ([ηcxis]) of the 20°C xylene insoluble matter (CXIS portion) is preferably 2.0 to 12.0.

[0093] The intrinsic viscosity was determined by the following procedure: The reduced viscosity was measured in tetralin at 135° C. using an Ubbelohde viscometer, and the intrinsic viscosity was determined from the obtained reduced viscosity by extrapolation according to the calculation method described in “Polymer Solutions, Polymer Experiments 11” (published by Kyoritsu Publishing Co., Ltd. in 1982), page 491.

[0094] Here, the CXS portion and the CXIS portion were obtained by the following method.

[0095] About 5 g of (B) propylene polymer is completely dissolved in 500 ml of boiling xylene. The obtained xylene solution is slowly cooled to 20° C., conditioned at 20° C. for more than 4 hours, and the precipitate is separated from the solution by filtration. The precipitate is the CXIS portion, and the substance obtained by removing the solvent from the solution is the CXS portion.

[0096] The melt flow rate of the (B) propylene-based polymer measured at 230°C and a load of 21.18N according to JIS K7210 is preferably 0.1 g / 10 min to 30 g / 10 min, more preferably 0.2 g / 10 min to 12 g / 10 min, further preferably 0.3 g / 10 min to 7 g / 10 min, and particularly preferably 0.4 g / 10 min to 3 g / 10 min. From the viewpoint of embossing retention at high temperatures, the melt flow rate of the (B) propylene-based polymer is preferably 0.1 g / 10 min or more. From the viewpoint of moldability, the melt flow rate of the (B) propylene-based polymer is preferably 30 g / 10 min or less.

[0097] The isotactic pentad fraction of the propylene-based polymer (B) measured by 13C-NMR is usually 0.95 or more, preferably 0.98 or more.

[0098] Here, the fraction of isotactic pentads refers to the fraction of propylene monomer units located at the center of the isotactic chain in terms of pentads in the molecular chain of the (B) propylene-based polymer, in other words, the fraction of propylene monomer units located in a chain (mmmm) formed by continuous meso-bonding of 5 propylene monomer units. The fraction of isotactic pentads is determined by the method described by A. Zambelli et al. in Macromolecules, 6, 925 (1973), i.e., by 13C-NMR.

[0099] Specifically, the ratio of the area of ​​the NMR peak attributed to mmmm measured by 13C-NMR spectrum to the area of ​​the absorption peak in the methyl carbon region is the fraction of the isotactic pentad.

[0100] The melting temperature of the (B) propylene-based polymer is usually 100°C or higher. The melting temperature of a propylene homopolymer or a propylene polymer material is preferably 155°C or higher, more preferably 160°C or higher. The melting temperature of a propylene random copolymer is preferably 130°C or higher, more preferably 135°C or higher. In addition, the melting temperature of the (B) propylene-based polymer is usually 175°C or lower. In the present invention, the melting temperature is the peak temperature of the endothermic peak with the largest peak temperature in the differential scanning calorimetry curve during the temperature increase operation measured by a differential scanning calorimeter. The measurement conditions of the differential scanning calorimetry curve using a differential scanning calorimeter are as follows.

[0101] <Measurement conditions>

[0102] Temperature reduction operation: (B) the propylene-based polymer was melted at 220°C, and then the temperature was reduced from 220°C to -90°C at a temperature reduction rate of 5°C / min.

[0103] Temperature increase operation: After cooling from 220°C to -90°C, immediately increase the temperature from -90°C to 200°C at 5°C / min.

[0104] (C) Ethylene polymers having more than 90% by mass of monomer units derived from ethylene

[0105] The thermoplastic elastomer composition of the present embodiment may contain (C) an ethylene polymer having more than 90% by mass of monomer units derived from ethylene (wherein the total amount of the ethylene polymer is 100% by mass). (C) The ethylene polymer having more than 90% by mass of monomer units derived from ethylene may have monomer units derived from a monomer other than ethylene.

[0106] Examples of monomers other than ethylene include: α-olefins having 3 to 10 carbon atoms; conjugated dienes having 4 to 8 carbon atoms, such as 1,3-butadiene, 2-methyl-1,3-butadiene, 1,3-pentadiene, and 2,3-dimethyl-1,3-butadiene; non-conjugated dienes having 5 to 15 carbon atoms, such as dicyclopentadiene, 5-ethylidene-2-norbornene, 1,4-hexadiene, 1,5-cyclooctadiene, 7-methyl-1,6-octadiene, and 5-vinyl-2-norbornene; carboxylic acid vinyl esters, such as vinyl acetate; unsaturated carboxylic acid esters, such as methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, and ethyl methacrylate; and unsaturated carboxylic acids, such as acrylic acid and methacrylic acid.

[0107] As (C) ethylene polymers having more than 90% by mass of monomer units derived from ethylene, there can be mentioned: ethylene homopolymers, and ethylene copolymers having monomer units derived from ethylene and monomer units derived from monomers other than ethylene. The ethylene copolymer as (C) ethylene polymer having more than 90% by mass of monomer units derived from ethylene may have only one monomer unit derived from a monomer other than ethylene, or may have two or more monomer units derived from monomers other than ethylene. (C) Ethylene polymers having more than 90% by mass of monomer units derived from ethylene are preferably ethylene homopolymers, ethylene-propylene copolymers, ethylene-1-butene copolymers, ethylene-1-pentene copolymers, ethylene-4-methyl-1-pentene copolymers, ethylene-1-hexene copolymers, and ethylene-1-octene copolymers, and more preferably ethylene homopolymers, ethylene-1-butene copolymers, and ethylene-1-hexene copolymers.

[0108] The melt flow rate of (C) an ethylene polymer having more than 90% by mass of monomer units derived from ethylene, measured under the conditions of a temperature of 190°C and a load of 21.18 N according to JIS K7210, is not limited and is preferably 0.01 g / 10 min to 200 g / 10 min, more preferably 0.05 g / 10 min to 100 g / 10 min, and more preferably 1.0 g / 10 min to 20 g / 10 min.

[0109] The density of (C) the ethylene polymer having more than 90% by mass of monomer units derived from ethylene as measured in accordance with JIS K7112 is not limited, but is preferably 0.91 g / cm 3 ~0.97g / cm 3 .

[0110] (C) The ethylene polymer having more than 90% by mass of monomer units derived from ethylene can be produced by polymerizing ethylene in the presence of a polymerization catalyst such as a Ziegler-Natta catalyst or a metallocene catalyst. Examples of the polymerization method include solution polymerization, bulk polymerization, slurry polymerization, and gas phase polymerization, and two or more of these methods may be combined.

[0111] The amount of (C) the ethylene polymer having more than 90% by mass of monomer units derived from ethylene is not particularly limited. When the thermoplastic elastomer composition is taken as 100% by mass, the content of (C) the ethylene polymer having more than 90% by mass of monomer units derived from ethylene in the thermoplastic elastomer composition is preferably 30% by mass or less, more preferably 20% by mass or less.

[0112] (D) Cross-linking agent

[0113] The thermoplastic elastomer composition of the present embodiment may contain (D) a crosslinking agent. Examples of the crosslinking agent (D) include organic peroxides, sulfur-containing compounds, and alkylphenol resins, and organic peroxides are preferred.

[0114] Examples of the organic peroxide include ketone peroxides, diacyl peroxides, hydroperoxides, dialkyl peroxides, peroxyketals, alkyl peresters, percarbonates, peroxydicarbonates, and peroxyesters. Specific examples of the organic peroxide include dicumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne, 1,3-bis(tert-butylperoxyisopropyl)benzene, tert-butylcumyl peroxide, di-tert-butyl peroxide, 2,2,4-trimethylpentyl-2-hydroperoxide, diisopropylbenzene hydroperoxide, isopropylbenzene peroxide, tert-butyl peroxide, 1,1-di(tert-butylperoxy)-3,5,5-trimethylcyclohexane, 1,1-di(tert-butylperoxy)cyclohexane, isobutyl peroxide, 2,4-dichlorobenzoyl peroxide, o-methylbenzoyl peroxide, di(3,5,5-trimethylhexanoyl) peroxide, lauroyl peroxide, benzoyl peroxide, and p-chlorobenzoyl peroxide. The organic peroxide may be used alone or in combination of two or more.

[0115] The amount of the crosslinking agent (D) used is not particularly limited. When the thermoplastic elastomer composition is taken as 100% by mass, the content of the crosslinking agent (D) in the thermoplastic elastomer composition is preferably 0.01% by mass to 3.0% by mass, more preferably 0.05% by mass to 2% by mass, and even more preferably 0.1% by mass to 1% by mass.

[0116] In order to increase the crosslinking degree of the above-mentioned (A) ethylene-based rubber, (D) a crosslinking agent may be used in combination with a crosslinking aid. A preferred crosslinking aid is a compound having two or more double bonds.

[0117] As crosslinking aids, there can be listed: peroxide crosslinking aids such as N,N-phenylene bismaleimide, toluene bismaleimide, p-benzoquinone dioxime, nitrosobenzene, diphenylguanidine, and trimethylolpropane; divinylbenzene, triallyl cyanurate, triallyl isocyanurate, ethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, allyl methacrylate, etc., preferably trimethylolpropane trimethacrylate.

[0118] The amount of the crosslinking aid used is not particularly limited, but the content of the crosslinking aid in the thermoplastic elastomer composition is preferably 0.01 to 10% by mass, more preferably 0.1 to 2% by mass, based on 100% by mass of the thermoplastic elastomer composition.

[0119] (E) Mineral oil

[0120] The thermoplastic elastomer composition of the present invention may contain (E) mineral oil. Examples of the mineral oil (E) include high boiling point fractions of petroleum having an average molecular weight of 300 to 1500 and a pour point of 0°C or less, such as aromatic mineral oil, naphthenic mineral oil, and paraffinic mineral oil, and paraffinic mineral oil is preferred.

[0121] (E) Mineral oil can be added as an extender oil for (A) ethylene rubber. Examples of methods for adding (E) mineral oil to (A) ethylene rubber include: a method of mechanically mixing (A) ethylene rubber and (E) mineral oil using a mixing device such as a roll or a Banbury mixer; a method of adding a predetermined amount of (E) mineral oil to a solution of (A) ethylene rubber to obtain a mixed solution, and then removing the solvent from the mixed solution by a spray drying method, a steam stripping method, a supercritical drying method using carbon dioxide, etc.; a method of directly adding mineral oil to latex-state rubber and stirring it, and then coagulating the rubber; and the like.

[0122] When (E) mineral oil is blended as an extender oil for (A) ethylene-based rubber, the Mooney viscosity (ML) of the composition containing (E) mineral oil and (A) ethylene-based rubber measured at 100°C is 1+4 100°C) is preferably 5 to 300, more preferably 40 to 200, and even more preferably 50 to 100. It should be noted that the Mooney viscosity (ML 1+4 100°C) was measured according to JIS K6300.

[0123] The amount of (E) mineral oil used is not particularly limited. When the thermoplastic elastomer composition is set to 100% by mass, the content of (E) mineral oil in the thermoplastic elastomer composition is preferably 1% to 60% by mass, more preferably 10% to 50% by mass, and further preferably 15% to 45% by mass. At this time, according to the amount of (E) mineral oil used, the content of (A) ethylene rubber and / or the content of (B) propylene polymer is reduced accordingly. For example, when the content of (E) mineral oil is 1% to 60% by mass, the content of (A) ethylene rubber is 10% to 89% by mass, and the content of (B) propylene polymer is 10% to 89% by mass.

[0124] other

[0125] The thermoplastic elastomer composition of the first invention of the present application may contain other additives and other thermoplastic resins in addition to the above (A) to (E) (wherein the essential components are only (A) ethylene rubber and (B) propylene polymer). Examples of other additives include inorganic fillers, organic fillers, fatty acid derivatives, antioxidants, weathering stabilizers, ultraviolet absorbers, heat stabilizers, light stabilizers, antistatic agents, nucleating agents, colorants (inorganic pigments, organic pigments, pigment dispersants, etc.), adsorbents, metal chlorides, flame retardants, organosilicon compounds, friction reducers, antibacterial agents, mildew inhibitors, neutralizers, foaming agents, foaming nucleating agents, etc. These additives may be used alone or in combination of two or more.

[0126] Examples of the antioxidant include phenolic antioxidants, sulfur-containing antioxidants, phosphorus-containing antioxidants, lactone antioxidants, and vitamin-based antioxidants.

[0127] Examples of the ultraviolet absorber include benzotriazole ultraviolet absorbers, triazine ultraviolet absorbers, anilide ultraviolet absorbers, and benzophenone ultraviolet absorbers.

[0128] Examples of the light stabilizer include hindered amine light stabilizers and benzoate light stabilizers.

[0129] Production of thermoplastic elastomer compositions

[0130] The thermoplastic elastomer composition of the first invention of the present application can be manufactured by mixing (A) ethylene rubber and (B) propylene polymer and various additives as required by conventional methods, for example, using a conventional extruder, Banbury mixer, roll, Brabender plastometer, Brabender kneader, etc. It is preferably manufactured using an extruder, especially a twin-screw extruder. In addition, all the components to be mixed can be melt-mixed together, or a part of the components can be mixed, and then the remaining components are added and melt-mixed, and melt-mixing can be performed once or twice or more. The temperature during melt mixing is preferably 150°C to 300°C, and more preferably 180°C to 250°C. The time during melt mixing is preferably 20 seconds to 30 minutes, and more preferably 30 seconds to 20 minutes. The components to be mixed can be added in any order or at the same time.

[0131] When producing the thermoplastic elastomer composition of the present invention, it is preferred to crosslink the (A) ethylene rubber and other crosslinkable resin components from the viewpoint of achieving sufficient rubber elasticity.

[0132] When crosslinking is performed, it is preferred that various crosslinking agents and crosslinking aids are introduced into an extruder, particularly a twin-screw extruder, in addition to the raw material resin, and melt-kneaded to perform crosslinking.

[0133] When the thermoplastic elastomer composition of the first invention of the present application is produced, in the case of carrying out the above-mentioned cross-linking step, a step of further adding other resins may be added after the above-mentioned cross-linking step. In this case, the above-mentioned cross-linking step is also referred to as "step 1", and the step of further adding other resins after step 1 is also referred to as "step 2". According to the conditions of step 1, the cross-linking agent (D) such as organic peroxide is almost completely consumed in step 1, so step 2 can be carried out under the condition that the organic peroxide and the like are substantially absent. In this case, since cross-linking and decomposition of the resin component do not substantially occur in step 2, the resin composition, molecular weight distribution, gel fraction, etc. of the thermoplastic elastomer composition can be adjusted with a high degree of freedom. In particular, by adding a desired amount of (B) propylene-based polymers that are easily decomposed by organic peroxides, etc., a desired molecular weight distribution can be achieved.

[0134] In the case of adopting such a method, the resin composition obtained in step 1 may have a composition, physical properties, etc. different from those of the desired thermoplastic elastomer composition, and therefore is also referred to as a "thermoplastic elastomer composition precursor".

[0135] The conditions of step 2 are not particularly limited, and step 2 can be carried out by introducing the thermoplastic elastomer composition precursor obtained in step 1 and other resins into the same extruder as in step 1, particularly a twin-screw extruder, and melt-kneading. The temperature during melt-kneading in step 2 is preferably 150° C. to 300° C., more preferably 180° C. to 250° C. The time during melt-kneading is not particularly limited, but is preferably 10 seconds to 30 minutes, more preferably 20 seconds to 10 minutes.

[0136] From the viewpoint of performing step 2 in the substantial absence of a crosslinking agent such as an organic peroxide, the temperature during melt kneading in step 1 is preferably 150° C. to 300° C., more preferably 190° C. to 250° C. The time during melt kneading is not particularly limited, but is preferably 10 seconds to 30 minutes, more preferably 20 seconds to 10 minutes.

[0137] The thermoplastic elastomer composition is preferably produced by a production method comprising the following step 1' and step 2'.

[0138] Step 1': a step of melt-kneading (A) an ethylene-based rubber and (B1) a propylene-based polymer in the presence of (D) a crosslinking agent to obtain a thermoplastic elastomer precursor;

[0139] Step 2': a step of melt-kneading a thermoplastic elastomer composition precursor and (B2) a propylene-based polymer having a melt flow rate of 0.3 g / 10 min to 2 g / 10 min to obtain a thermoplastic elastomer composition.

[0140] By producing the composition using the production method including the step 1' and the step 2', the sinking temperature of the thermoplastic elastomer composition can be adjusted to 115°C or higher.

[0141] The (A) ethylene-based rubber used in step 1' is usually an uncrosslinked ethylene-based rubber. It is preferred that at least a part of the (A) ethylene-based rubber is crosslinked in step 1'.

[0142] Examples of the (B1) propylene-based polymer include the above-mentioned (B) propylene-based polymer.

[0143] In order to adjust the sinking temperature of the thermoplastic elastomer composition to 115° C. or higher, the propylene-based polymer (B2) having a melt flow rate of 0.3 to 2 g / 10 min is preferably a propylene homopolymer and / or a propylene polymer material.

[0144] In order to adjust the sinking temperature of the thermoplastic elastomer composition to 115° C. or higher, it is preferred that 11% to 29% by mass of the (B1) propylene-based polymer and 5% to 16% by mass of the (B2) propylene-based polymer having a melt flow rate of 0.3 g / 10 min to 2 g / 10 min are used, based on 100% by mass of the total amount of the thermoplastic elastomer composition.

[0145] In order to adjust the sinking temperature of the thermoplastic elastomer composition to 115° C. or more, the amount of the crosslinking agent (D) used in step 2′ is preferably 0.01% to 3.0% by mass, more preferably 0.05% to 2% by mass, and further preferably 0.1% to 1% by mass, when the total amount of the thermoplastic elastomer composition is 100% by mass. The obtained thermoplastic elastomer composition may or may not contain the crosslinking agent (D). When the crosslinking agent (D) used in step 2′ is an organic peroxide, the organic peroxide is almost completely consumed in step 2′, and the obtained thermoplastic elastomer composition may not contain the organic peroxide.

[0146] The thermoplastic elastomer composition of the first invention of the present application may correspond to the thermoplastic elastomer composition of the third invention of the present application, which will be described in detail later. Depending on the application and the required properties, the thermoplastic elastomer composition of the first invention of the present application preferably has all or part of the requirements and / or preferred technical matters of the thermoplastic elastomer composition of the third invention of the present application.

[0147] The shape of the thermoplastic elastomer composition of the first invention of the present application when used is not particularly limited, and it can be processed and molded into a desired shape according to the application, etc., and can be molded into a sheet for use. The sheet containing such a thermoplastic elastomer composition of the first invention of the present application can be equivalent to the sheet of the second invention of the present application, which will be described in detail later. Depending on the application and the required characteristics, it is preferred that the sheet containing the thermoplastic elastomer composition of the first invention of the present application has all or part of the requirements and / or preferred technical matters of the sheet of the second invention of the present application.

[0148] (Second invention of this application)

[0149] The second invention of the present application is a sheet containing 10% to 90% by mass of (A) ethylene rubber and 10% to 90% by mass of (B) propylene polymer (wherein the total amount of the sheet is set to 100% by mass), wherein the sinking temperature of the sheet is above 115°C, and the sinking temperature is measured according to JIS K7196-1991 and is defined as the temperature when the pressure head penetrates 100 μm from the surface of the sheet.

[0150] The (A) ethylene-based rubber and (B) propylene-based polymer constituting the sheet of the second invention of the present application and their preferred embodiments are the same as those described above in connection with the first invention of the present application.

[0151] The composition of the sheet of the second invention, the production method, and components that may be contained other than (A) the ethylene rubber and (B) the propylene polymer are the same as those described above with respect to the first invention.

[0152] The definition, measurement method and preferred range of the penetration temperature of the sheet of the second invention of the present application, which is measured according to JIS K7196-1991 and is defined as the temperature when the indenter penetrates 100 μm from the sheet surface, are the same as those described above for the first invention of the present application.

[0153] The sheet of the second invention of the present application is preferably produced using the thermoplastic elastomer composition of the first invention of the present application or the third invention of the present application described later.

[0154] The molding method of the sheet of the second invention of the present application is not particularly limited, and the sheet can be appropriately molded by a method used in the technical field, such as press molding, extrusion molding, compression molding, injection molding, calendar molding, blow molding, etc.

[0155] The sheet of the second invention of the present application is not limited to a flat sheet, but may be a so-called shaped sheet. When manufacturing a shaped sheet, a flat sheet may be first formed, and then the sheet may be shaped by vacuum forming or the like.

[0156] The thickness of the sheet of the second invention of the present application is not particularly limited and may be appropriately set depending on the intended use, but is usually 0.01 mm to 50 mm, preferably 0.1 mm to 20 mm, and more preferably 0.2 mm to 10 mm.

[0157] The surface of the sheet of the second invention of the present application may be a smooth surface, or may be a surface processed to have projections and recesses such as by embossing, matte processing, or sandblasting.

[0158] In particular, when used for automotive interior surface materials, embossing is preferably performed. Here, the shape of the embossing is not particularly limited, and is not limited to the narrow sense of embossing that imparts a leather-like appearance. It can be appropriately selected from pear skin patterns (pear ground), wood grain, rock grain, sand grain, cloth grain and silk grain (cloth pattern), geometric patterns, etc. in consideration of the purpose, etc. In the case of automotive interior surface materials, embossing in the narrow sense of imparting a leather-like appearance is preferably used in consideration of imparting a sense of luxury, etc.

[0159] Sometimes the ten-point average roughness (R zjis) It is appropriate to control the surface unevenness when embossing is performed. In this case, R zjis It is preferably 10 μm to 1000 μm, and more preferably 50 μm to 500 μm.

[0160] In the case of a surface material for automobile interior, after the sheet is embossed, the sheet can be shaped into the shape of a desired interior part by vacuum forming or the like. In this case, there is a problem that the pattern of the embossing processed on the sheet surface becomes lighter and / or larger or disappears compared to the desired pattern of the embossing, and it is desired to suppress this problem. Since the sheet of the second invention of the present application and the sheet obtained from the elastomer resin composition of the first invention and the third invention of the present application are excellent in moldability and appearance of the molded product, they are particularly suitable for use as a surface material for automobile interior.

[0161] When a practical automotive interior skin material is manufactured by vacuum forming or the like, it is preferred that the sheet of the second invention of the present application or the sheet obtained from the elastomer resin composition of the first invention of the present application or the third invention of the present application be vacuum formed in a state of being laminated with a polyolefin foam such as polyethylene foam. It should be noted that the above description of the thickness of the sheet is a description of the thickness of the sheet of the second invention of the present application or the sheet (surface layer) obtained from the elastomer resin composition of the first invention of the present application or the third invention of the present application that does not contain a polyolefin foam.

[0162] The sheet of the second invention of the present application is preferably at least partially crosslinked with the (A) ethylene rubber constituting the sheet. The crosslinking agent, crosslinking aid, and conditions of the crosslinking step used in the crosslinking are the same as those described above for the first invention of the present application.

[0163] The sheet of the second invention of the present application preferably contains (E) mineral oil. When the mass of the entire sheet is set to 100 mass%, the content of (E) mineral oil is preferably 1 mass% to 60 mass%, more preferably 10 mass% to 50 mass%, and further preferably 15 mass% to 45 mass%. The details of (E) mineral oil, its addition method, etc. are the same as those described above for the first invention of the present application.

[0164] The sheet of the second invention of the present application is preferably manufactured using the thermoplastic elastomer composition of the first invention of the present application or the thermoplastic elastomer composition of the third invention of the present application described later. Depending on the application and the required characteristics, the sheet of the second invention of the present application is preferably manufactured using a thermoplastic elastomer composition having all or part of the requirements and / or preferred technical matters of the thermoplastic elastomer composition of the first invention of the present application and / or the thermoplastic elastomer composition of the third invention of the present application. Alternatively, the sheet of the second invention of the present application preferably has all or part of such requirements and / or preferred technical matters.

[0165] (Third invention of this application)

[0166] The third invention of the present application is a thermoplastic elastomer composition, wherein:

[0167] The ratio of component (X) eluted in the range of elution temperature greater than 100° C. and less than or equal to 140° C. relative to the total elution amount (100% by mass) as measured by cross fractionation chromatography (CFC) using an apparatus having a temperature rising elution fractionation (TREF) section and a gel permeation chromatography (GPC) section under the following conditions (1) to (3) is 1% by mass to 50% by mass,

[0168] The proportion of the component (X1) having a molecular weight M in terms of polystyrene logM of 5.6 or more in the component (X) is 6.0% to 45.0% by mass relative to the total eluted amount (100% by mass), and

[0169] The thermoplastic elastomer composition has a gel fraction of 5.0% by mass to 50% by mass.

[0170] (1) The TREF section into which an o-dichlorobenzene solution of a thermoplastic elastomer composition (the concentration of the thermoplastic elastomer composition in the solution was 1 mg / mL) was injected was maintained at 100° C. for 10 minutes.

[0171] (2) The temperature of the TREF section was lowered to -5°C at a rate of 2.0°C / min, then maintained at -5°C for 30 minutes, and the elution amount at -5°C was measured.

[0172] (3) The following operation is repeated at three reaching temperatures of 50°C, 100°C and 140°C: the temperature of the TREF portion is raised to the reaching temperature at a rate of 40°C / min, then maintained at the reaching temperature for 30 minutes, and then the elution amount at the reaching temperature is measured.

[0173] Gel fraction

[0174] The thermoplastic elastomer composition of the third invention of the present application has a gel fraction of 5.0% by mass to 50% by mass.

[0175] The gel fraction is the ratio of components insoluble in o-dichlorobenzene at 140°C, and indicates the ratio of the crosslinked portion (substantially most of which is crosslinked (A) ethylene-based rubber) in the thermoplastic elastomer composition. When the gel fraction is 5.0% to 50% by mass, the ratio of the crosslinked portion to the non-crosslinked portion is appropriate, and the thermoplastic elastomer composition can achieve an appropriate balance between rubber elasticity and moldability, and the embossing retention during processing under severe conditions is excellent, and the appearance of the sheet, especially the matte property, is excellent. The gel fraction is preferably 10% to 45% by mass, and more preferably 15% to 30% by mass.

[0176] The thermoplastic elastomer composition of the third invention of the present application preferably contains (A) an ethylene-based rubber and (B) a propylene-based polymer.

[0177] The gel fraction can be measured by a method generally used in the technical field. From the viewpoint of accuracy, it is preferably measured by a GPC method, and more preferably measured by the following method.

[0178] A predetermined amount of a thermoplastic elastomer composition (solid) is sealed in a metal mesh bag, heated and stirred in a predetermined amount of a dissolving solvent (o-dichlorobenzene) to dissolve it, thereby preparing a sample solution for GPC measurement. As a result, the cross-linked components insoluble in the solvent remain in the metal mesh, and only the components soluble in the solvent are measured by GPC. The peak area of ​​the GPC chromatogram obtained by measuring the sample solution using GPC using a refractive index detector is set to P, and the peak area of ​​the GPC chromatogram obtained by measuring an equal amount of a polyethylene standard substance under the same conditions is set to Q, and the gel fraction is calculated according to the following formula (1).

[0179] Gel fraction (mass %) = 100 (QP) / Q ... (1)

[0180] More specifically, the gel fraction can be determined more accurately by the method described in Examples of the present application.

[0181] The reason for obtaining the gel fraction by the above method is as follows.

[0182] This GPC uses a refractive index detector, so the peak area of ​​the GPC chromatogram is proportional to the sample concentration (sample amount), and basically, if it is a hydrocarbon, the same amount is detected with the same intensity. Here, the polyethylene standard substance is completely dissolved in the solvent (o-dichlorobenzene), while in the thermoplastic elastomer composition, the crosslinked part is insoluble in the solvent, so it does not dissolve and remains in the metal mesh bag and is removed, so only the solution of the part soluble in the solvent becomes the sample solution of GPC.

[0183] That is, the sample concentration of the GPC sample solution of the thermoplastic elastomer composition having a crosslinked portion becomes lower and the amount of lowering corresponds to the amount of the crosslinked portion.

[0184] The peak area Q of the solution of the polyethylene standard substance is proportional to the total amount dissolved, and the peak area P of the sample solution of the thermoplastic elastomer composition becomes smaller and the amount of decrease corresponds to the amount of the crosslinked part. Therefore, the difference between P and Q calculated according to formula (1) is equivalent to the amount of the crosslinked component contained in the thermoplastic elastomer composition.

[0185] The gel fraction can be appropriately adjusted by adjusting the content and molecular weight of (A) ethylene rubber, the content of monomer units derived from at least one monomer selected from the group consisting of propylene and α-olefins having 4 to 15 carbon atoms, the content of monomer units derived from non-conjugated dienes, or adjusting the amount of (D) crosslinking agent and crosslinking aid, and crosslinking conditions.

[0186] If the content of (A) the ethylene-based rubber is increased, the gel fraction can be increased.

[0187] If the content of the non-conjugated diene in the (A) ethylene-based rubber is increased, the gel fraction can be increased.

[0188] If the amount of the (D) crosslinking agent or the crosslinking auxiliary agent is increased, the gel fraction can be increased.

[0189] In order to adjust the gel fraction of the thermoplastic elastomer composition to 5.0 to 50% by mass, the content of the (A) ethylene-based rubber in the thermoplastic elastomer composition is preferably 26 to 70% by mass, more preferably 36 to 55% by mass (here, the total amount of the thermoplastic elastomer composition is 100% by mass).

[0190] In order to adjust the gel fraction of the thermoplastic elastomer composition to 5.0% by mass to 50% by mass, the content of the monomer units derived from the non-conjugated diene in the (A) ethylene-based rubber in the thermoplastic elastomer composition is preferably 1% by mass to 30% by mass, more preferably 2% by mass to 20% by mass, and further preferably 3% by mass to 15% by mass (wherein the total amount of the ethylene-based rubber is set to 100% by mass).

[0191] In order to adjust the gel fraction of the thermoplastic elastomer composition to 5.0 to 50% by mass, the amount of the crosslinking agent (D) used during the production of the thermoplastic elastomer composition is preferably 0.01 to 3.0% by mass, more preferably 0.05 to 2% by mass, and even more preferably 0.1 to 1% by mass, based on 100% by mass of the thermoplastic elastomer composition.

[0192] Component (X) eluted within the range of elution temperature greater than 100°C and less than or equal to 140°C

[0193] The proportion of the component (X) eluted in the range of an elution temperature of more than 100° C. and less than or equal to 140° C. in the thermoplastic elastomer composition of the third invention of the present application relative to the total eluted amount of 100 mass %, is usually 1 to 50 mass %, preferably 10 to 45 mass %, and more preferably 15 to 40 mass %.

[0194] When the ratio of component (X) satisfies the above conditions and has other conditions specified in the third invention of the present application, the thermoplastic elastomer composition of the third invention of the present application is excellent in moldability, embossing retention in a wide temperature range from low to high temperatures, and sheet appearance.

[0195] The proportion of the component (X) can be appropriately adjusted by adjusting the content, molecular weight, content of monomer units derived from propylene, and the like of the non-crosslinkable resin component, for example, the propylene-based polymer (B).

[0196] When the content of the propylene-based polymer (B) is increased, the proportion of the component (X) can be increased.

[0197] In order to adjust the proportion of the component (X) to 1 to 50% by mass, the content of the propylene-based polymer (B) in the thermoplastic elastomer composition is preferably 16 to 45% by mass, more preferably 26 to 40% by mass.

[0198] The ratio of the component (X) can be measured by CFC, and more specifically, can be measured by the method described in the Examples of the present application.

[0199] When measuring by CFC, it is preferred to seal a sample (solid) of the thermoplastic elastomer composition in a metal mesh bag, heat and stir it in a solvent (o-dichlorobenzene), and prepare a sample solution. Thus, the crosslinked components insoluble in the solvent remain in the metal mesh, and only the components soluble in the solvent are measured by CFC. Therefore, the proportion of component (X) can be calculated based on the total eluted amount (100% by mass).

[0200] Component (X1) having a molecular weight M logarithm logM of 5.6 or more in terms of polystyrene

[0201] The proportion of the component (X1) having a molecular weight M (logM) of 5.6 or more in terms of polystyrene is 6.0% to 45.0% by mass, preferably 7.0% to 40.0% by mass, more preferably 8.0% to 35.0% by mass, and further preferably 9.0% to 30.0% by mass, relative to the total eluted amount of 100% by mass. When the proportion of the component (X1) satisfies the above conditions and has other conditions specified in the third invention of the present application, the thermoplastic elastomer composition of the third invention of the present application is excellent in moldability and embossing retention in a severe high temperature range, and has an excellent sheet appearance.

[0202] In order to adjust the ratio of the component (X1) to 6.0% by mass to 45.0% by mass, it is preferred to produce the thermoplastic elastomer composition by the production method comprising the above-mentioned steps 1' and 2'.

[0203] Preferred embodiments of the (A) ethylene rubber, (B1) propylene polymer, (B2) propylene polymer having a melt flow rate of 0.3 g / 10 min to 2 g / 10 min, and (D) crosslinking agent used in step 1' and step 2' are the same as those described above. The proportion of component (X1) can be increased by increasing the amount of (B2) propylene polymer having a melt flow rate of 0.3 g / 10 min to 2 g / 10 min used in step 2'. In order to adjust the proportion of component (X1) to 6.0% by mass to 45.0% by mass, it is preferred that (B2) propylene polymer having a melt flow rate of 0.3 g / 10 min to 2 g / 10 min is a propylene homopolymer and / or a propylene polymer material, and when the total amount of the thermoplastic elastomer composition is set to 100% by mass, its usage amount is 7% by mass to 15% by mass.

[0204] Component (X2) having a molecular weight M logarithm logM of 4.6 or less in terms of polystyrene

[0205] The proportion of the component (X2) having a molecular weight M (logM) of 4.6 or less in terms of polystyrene is preferably 10.0% by mass or less, more preferably 0.1% by mass to 5.0% by mass, and further preferably 0.1% by mass to 2.5% by mass, relative to the total eluted amount of 100% by mass. When the component (X2) is in the above proportion, the thermoplastic elastomer composition of this embodiment is excellent in moldability and embossing retention, and the appearance of the sheet is excellent.

[0206] In order to adjust the proportion of component (X2) to 10.0% by mass or less, it is preferred to produce the thermoplastic elastomer composition by the production method comprising the aforementioned steps 1' and 2'. The proportion of component (X2) can be reduced by reducing the amount of the (B1) propylene-based polymer used in step 1'. In order to adjust the proportion of component (X2) to 10.0% by mass or less, it is preferred that the amount of the (B1) propylene-based polymer used is 15% to 20% by mass when the total amount of the thermoplastic elastomer composition is 100% by mass.

[0207] Component eluted at -5°C (α)

[0208] The ratio of the component (α) eluted at an elution temperature of -5°C is preferably 70% by mass or less, more preferably 20% to 65% by mass, and further preferably 30% to 60% by mass, relative to the total eluted amount of 100% by mass. When the component (α) is in the above ratio, the thermoplastic elastomer composition of this embodiment is excellent in moldability and embossing retention, and the appearance of the sheet is excellent.

[0209] The proportion of the component (α) can be appropriately adjusted by adjusting the proportions of (A) ethylene rubber and (E) mineral oil, or by adjusting the amounts of (D) a crosslinking agent or a crosslinking aid and the crosslinking conditions.

[0210] If the proportion of the (E) mineral oil is increased, the proportion of the component (α) can be increased.

[0211] In order to adjust the proportion of the component (α) to 70 mass % or less, the content of the mineral oil (E) in the thermoplastic elastomer composition is preferably 1 to 60 mass %, more preferably 10 to 50 mass %, further preferably 15 to 45 mass %.

[0212] The component (α) is presumably derived from the (E) mineral oil and the uncrosslinked component having a low ethylene content and a small molecular weight in the (A) ethylene-based rubber.

[0213] The ratio of the component (α) can be measured by CFC, and more specifically, can be measured by the method described in the Examples of the present application.

[0214] It should be noted that the component (α) herein is intended to include all components eluted at -5°C, which is the lowest temperature during measurement, and the component (α) also includes components that can be eluted at a temperature lower than -5°C.

[0215] Components eluting in the range of elution temperature greater than -5°C and less than or equal to 50°C (β)

[0216] The ratio of the component (β) eluted at an elution temperature of greater than -5°C and less than or equal to 50°C is preferably 1% to 39% by mass, more preferably 3% to 20% by mass, and further preferably 5% to 14% by mass, relative to the total eluted amount of 100% by mass. When the component (β) is in the above ratio, the thermoplastic elastomer composition of this embodiment does not contain an excessive amount of uncrosslinked (A) ethylene-based rubber and the like, and thus has excellent embossing retention and excellent sheet appearance.

[0217] The proportion of component (β) can be appropriately adjusted by adjusting the amount of (A) ethylene rubber, or adjusting the molecular weight of (C) ethylene polymer having more than 90% by mass of monomer units derived from ethylene, the content of monomer units derived from ethylene, density, etc., or adjusting (D) the amount of crosslinking agent, crosslinking aid, and crosslinking conditions.

[0218] If the proportion of the (A) ethylene-based rubber is increased, the proportion of the component (β) can be increased.

[0219] If the amount of the crosslinking agent or the crosslinking auxiliary (D) is reduced, the proportion of the component (β) can be increased.

[0220] In order to adjust the ratio of the component (β) to 1 to 39 mass%, the content of the crosslinking agent (D) in the thermoplastic elastomer composition is preferably 0.01 to 3.0 mass%, more preferably 0.05 to 2 mass%, and even more preferably 0.1 to 1 mass%, based on 100 mass% of the thermoplastic elastomer composition.

[0221] The component (β) is presumably derived from the uncrosslinked (A) ethylene-based rubber and the low molecular weight ethylene copolymer portion (II) when the (B) propylene-based polymer is a propylene polymer material.

[0222] The ratio of the component (β) can be measured by CFC, and more specifically, can be measured by the method described in the examples of the present application.

[0223] Components eluting in the range of elution temperature greater than 50°C and less than or equal to 100°C (γ)

[0224] The ratio of the component (γ) eluted in the range of elution temperature of more than 50° C. and less than or equal to 100° C. is preferably 0.1% by mass to 39% by mass, more preferably 5% by mass to 30% by mass, and further preferably 8% by mass to 25% by mass, relative to the total eluted amount of 100% by mass. When the component (γ) is in the above ratio, the thermoplastic elastomer composition of this embodiment is excellent in moldability and embossing retention in a low temperature range, and the appearance of the sheet is excellent.

[0225] The proportion of component (γ) can be appropriately adjusted by adjusting the amount, molecular weight, content of monomer units derived from propylene of (B) the propylene-based polymer, or adjusting the content of (C) the ethylene polymer having more than 90% by mass of monomer units derived from ethylene.

[0226] If the molecular weight of (C) the ethylene polymer having more than 90% by mass of monomer units derived from ethylene is increased, the proportion of the component (γ) can be increased.

[0227] Component (γ) is presumed to be derived from (B) a low molecular weight propylene-based polymer, the ethylene copolymer portion (II) when the (B) propylene-based polymer is a propylene polymer material, (C) an ethylene polymer having more than 90% by mass of monomer units derived from ethylene, and the like.

[0228] The ratio of the component (γ) can be measured by CFC, and more specifically, can be measured by the method described in the Examples of the present application.

[0229] The material constituting the thermoplastic elastomer composition of the third invention of the present application is not particularly limited, and a part or all of the material constituting the thermoplastic elastomer composition of the first invention of the present application may be used as appropriate.

[0230] The thermoplastic elastomer composition of the third invention of the present application preferably has all or part of the requirements and / or preferred technical matters of the thermoplastic elastomer composition of the first invention of the present application, depending on the application and the required properties.

[0231] The shape of the thermoplastic elastomer composition of the third invention of the present application when used is not particularly limited, and it can be processed and molded into a desired shape according to the application, etc., and can be molded into a sheet for use. A sheet containing such a thermoplastic elastomer composition of the third invention of the present application can be equivalent to the sheet of the second invention of the present application. Depending on the application and the required characteristics, it is preferred that the sheet containing the thermoplastic elastomer composition of the third invention of the present application has all or part of the requirements and / or preferred technical matters of the sheet of the second invention of the present application.

[0232] use

[0233] The thermoplastic elastomer compositions of the first and third inventions of the present application and the sheet of the second invention of the present application can be used in various applications, and are particularly suitable for applications that require high levels of moldability and appearance of molded products. For example, they are suitable for automobile parts, sporting goods, leisure goods, household goods, electrical and electronic equipment, building interior materials, exterior materials, etc., and are particularly suitable for automobile interior skin materials such as door trims and instrument panels, especially skin materials with patterns such as embossing on the surface, etc.

[0234] [Example]

[0235] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples. It should be noted that the technical scope of the present invention is not limited to these Examples in any sense.

[0236] Evaluation of physical properties in Examples and Comparative Examples was performed by the following methods.

[0237] (1) Melt flow rate (MFR, unit: g / 10 minutes)

[0238] (C) MFR of an ethylene polymer having more than 90% by mass of monomer units derived from ethylene is measured under the conditions of a temperature of 190° C. and a load of 21.18 N by method B in accordance with JIS K7210.

[0239] (B) MFR of the propylene-based polymer was measured under the conditions of a temperature of 230° C. and a load of 21.18 N by method B in accordance with JIS K7210.

[0240] The MFR of the thermoplastic elastomer composition is measured under the conditions of a temperature of 230° C. and a load of 98.07 N by method B in accordance with JIS K7210.

[0241] (2) Mooney viscosity (ML) 1+4 100℃)

[0242] (A) The Mooney viscosity of the ethylene-based rubber was measured at 100°C in accordance with JIS K6300.

[0243] (3) (A) Contents of monomer units derived from ethylene, monomer units derived from propylene, and monomer units derived from 5-ethylidene-2-norbornene contained in ethylene-based rubber (unit: mass %)

[0244] (A) The contents of monomer units derived from ethylene, monomer units derived from propylene, and monomer units derived from 5-ethylidene-2-norbornene contained in the ethylene-based rubber were measured by infrared spectroscopy. Specifically, an ethylene-propylene-5-ethylidene-2-norbornene copolymer was formed into a film having a thickness of about 0.5 mm, and then the peak (1688 cm-1) derived from 5-ethylidene-2-norbornene of the film was measured using an infrared spectrophotometer. -1The intensity of the absorption peak of the absorption peak (A) was used to calculate the content of the monomer unit derived from 5-ethylidene-2-norbornene in the (A) ethylene-based rubber. Next, the ethylene-propylene-5-ethylidene-2-norbornene copolymer was remolded into a film with a thickness of about 0.1 mm, and then the infrared absorption spectrum of the film was measured using an infrared spectrophotometer. The content of the monomer unit derived from ethylene and the content of the monomer unit derived from propylene were calculated according to the method described in the literature (Characterization of Polyethylene by Infrared Absorption Spectroscopy, Takayama, Usami, etc.; or Die Makromolekulare Chemie, 177, 461 (1976) Mc Rae, MA, Madam S, WF, etc.).

[0245] (4) Content of monomer units derived from ethylene and content of monomer units derived from at least one monomer selected from the group consisting of propylene and α-olefins having 4 to 10 carbon atoms contained in each polymer (unit: mass %)

[0246] The content of monomer units derived from ethylene and the content of monomer units derived from at least one monomer selected from the group consisting of propylene and α-olefins having 4 to 10 carbon atoms contained in each polymer used in the examples were determined by infrared absorption spectroscopy (manufactured by JASCO Corporation, FT-IR5200 model) according to the method specified in ASTM D 3900.

[0247] (5) Intrinsic viscosity ([ηcxs], [ηcxis]) (unit: dl / g)

[0248] The reduced viscosity was measured in tetralin at 135° C. using an Ubbelohde viscometer, and the intrinsic viscosity was determined by extrapolation according to the calculation method described in “Polymer Solutions, Polymer Experiments 11” (published by Kyoritsu Publishing Co., Ltd. in 1982), p. 491.

[0249] In this embodiment, for the heterophasic propylene polymer material, the intrinsic viscosity of the xylene insoluble matter at 20°C ([ηcxis]) is regarded as the intrinsic viscosity ([ηA]) of the propylene homopolymer component contained in the heterophasic propylene polymer material, and the intrinsic viscosity of the xylene soluble matter at 20°C ([ηcxs]) is regarded as the intrinsic viscosity ([ηB]) of the ethylene-propylene copolymer component contained in the heterophasic propylene polymer material.

[0250] (6) Separation of CXIS and CXS

[0251] About 5 g of the sample was completely dissolved in 500 ml of boiling xylene, and the resulting xylene solution was slowly cooled to room temperature, kept at 20° C. for more than 4 hours, and the precipitate and the solution were separated by filtration. The precipitate was taken as the CXIS fraction, and the substance obtained by removing the solvent from the solution was taken as the CXS fraction.

[0252] (7) Density (unit: g / cm 3 )

[0253] The measurement was performed without annealing according to the method specified in JIS K7112.

[0254] (8) Method for producing compressed tablets

[0255] The thermoplastic elastomer composition was hot-pressed at a temperature of 200°C and a maximum pressure of 10 MPa for 5 minutes using a compression molding machine F-37 manufactured by Shinto Metal Industries, Ltd., and then cold-pressed at a temperature of 23°C and a maximum pressure of 10 MPa for 5 minutes to produce a pressed sheet (length 50 mm, width 50 mm, thickness 0.50 mm).

[0256] (9) Method for manufacturing extruded sheet

[0257] The thermoplastic elastomer compositions of Examples and Comparative Examples were melt-extruded from a T-die using a USV 25 mm Φ extruder manufactured by Union Plastics having a T-die with a width of 100 mm, at a barrel temperature of 220° C., a full-flight screw, and a screw speed of 40 rpm. The extruded molten film was air-cooled and molded along a metal roll to obtain an extruded sheet (width of about 95 mm, thickness of 1.0 mm).

[0258] In the measurement of gloss, a raw material obtained by blending 1 part by mass of a black pigment masterbatch (manufactured by Sumika Masterbatch Co., Ltd., trade name "PEM8020") described later in the form of pellets with 100 parts by mass of the thermoplastic elastomer composition was used to obtain an extruded sheet under the above conditions.

[0259] (10) Appearance of extruded sheet

[0260] The USV type 25mmΦ extruder manufactured by Union Plastic was used to produce an extruded sheet with a thickness of 0.2mm under the conditions of a barrel temperature of 220°C, a full-thread screw, and a screw speed of 20rpm. The lumps (しこり) with a diameter of 0.5mm or more in the extruded sheet were judged as bumps, and the appearance of the extruded sheet was visually determined based on the number of bumps confirmed in the randomly selected area of ​​the extruded sheet with a length of 40cm and a width of 80mm. The situation where the epidermis of the sheet is good and the number of bumps is less than 10 is judged as "0", the situation where the epidermis of the sheet is slightly rough and the number of bumps is greater than 10 and less than or equal to 20 is judged as "△", and the situation where the epidermis of the sheet is poor and the number of bumps is greater than 20 is judged as "×".

[0261] (11) Gel fraction

[0262] The gel fraction is the ratio of the component insoluble in o-dichlorobenzene at 140° C. and is determined by GPC. GPC measurement and calculation of the gel fraction were performed under the following conditions.

[0263] (GPC measurement conditions)

[0264] GPC device: HLC-8321GPC / HT (manufactured by Tosoh Corporation)

[0265] GPC column: Tosoh TSKgel GMH HR -H(S)HT2 inner diameter 7.8mm×300mm (manufactured by Tosoh Corporation) 3 pieces

[0266] Mobile phase: o-dichlorobenzene (special grade, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added with 0.1 weight / volume % of 2,6-di-tert-butyl-4-methylphenol (BHT) (special grade, purity 98%) as an antioxidant to inhibit decomposition of the polymer.

[0267] Flow rate: 1ml / min

[0268] Column thermostat temperature: 140°C

[0269] Autosampler temperature: 140°C

[0270] System thermostat temperature: 40°C

[0271] Detection: Refractive Index Detector (RID)

[0272] RID sample cell temperature: 140°C

[0273] Sample solution injection volume: 300μl

[0274] Dissolving solvent: Same as mobile phase

[0275] Automatic oscillator for dissolution: DF-8020 (manufactured by Tosoh Corporation)

[0276] Dissolution step: 20.0 mg of the thermoplastic elastomer composition and 20.0 ml of the dissolving solvent were added to a 30 ml screw bottle and sealed, and the bottle was placed on an automatic shaker for dissolution and stirred at 140° C. for 120 minutes. Next, the obtained solution was filtered through a filter having a pore size of 0.8 μm or more. Here, the filtration was performed at 140° C. or higher and within 20 minutes to avoid concentration changes caused by evaporation of the solvent. Through these operations, a sample solution for GPC measurement was prepared.

[0277] <Calculation of gel fraction>

[0278] The gel fraction was calculated by the following formula (1).

[0279] Gel fraction (mass %) = 100 (QP) / Q ... (1)

[0280] In formula (1), P is the peak area obtained by performing the above-mentioned measurement using GPC on the sample solution and drawing the baseline of the peak in the obtained chromatogram. In addition, Q is the peak area obtained by performing the above-mentioned measurement using GPC on the polyethylene standard substance NIST1475a and drawing the baseline of the peak in the obtained chromatogram. The definition of the baseline is based on the description of ISO16014-1.

[0281] (12) Identification of extracted components (ratio of components eluted within a specified temperature range)

[0282] The amount of each component in the sample is measured by CFC. 20 mg of the sample is sealed in a 2300-mesh SUS metal mesh bag, and heated and stirred at 145°C for 60 minutes in 20 ml of o-dichlorobenzene containing 0.05 wt% BHT to prepare a sample solution with a concentration of 1.0 mg / ml. 0.5 ml of the sample solution is injected into a TREF column maintained at 145°C in a CFC device and maintained for 20 minutes. Then, the temperature of the TREF column is cooled to 100°C at a rate of 40°C / min and maintained at 100°C for 10 minutes. Then, the temperature of the TREF column is cooled to -5°C at a rate of 2.0°C / min and maintained at -5°C for 30 minutes. Then, the temperature of the TREF column is increased to 50°C at a rate of 40°C / min and maintained at 50°C for about 30 minutes. Then, the temperature of the TREF column is increased to 100°C at a rate of 40°C / min and maintained for about 30 minutes. Next, the temperature of the TREF column was raised to 140°C at a rate of 40°C / min and maintained for about 30 minutes, and then the elution amount at 140°C was measured using a GPC (built-in CFC) with an infrared spectrophotometer. The ratio (mass %) of the elution amount at -5°C in the total elution amount was taken as component (α), the ratio of the elution amount at 50°C in the total elution amount (equivalent to the component eluted in the range of elution temperature greater than -5°C and less than or equal to 50°C, mass %) was taken as component (β), the ratio of the elution amount at 100°C in the total elution amount (equivalent to the component eluted in the range of elution temperature greater than 50°C and less than or equal to 100°C, mass %) was taken as component (γ), and the ratio of the elution amount at 140°C in the total elution amount (equivalent to the component eluted in the range of elution temperature greater than 100°C and less than or equal to 140°C, mass %) was taken as component (X). In addition, the molecular chain length distribution of (X) in the sample as a component soluble in o-dichlorobenzene at 140°C was determined, and the ratio (mass %) of the component having a logM (M is a molecular weight calculated as polystyrene) of 5.6 or more as an elution at 140°C was taken as component (X1), and the ratio (mass %) of the component having a logM of 4.6 or less as an elution at 140°C was taken as component (X2).

[0283] (i) Equipment: Automated 3D analyzer CFC-2 manufactured by Polymer ChAR

[0284] (ii) TREF column: manufactured by Polymer ChAR, stainless steel microsphere packed column (outer diameter 3 / 8" × 150 mm)

[0285] (iii) Solvent, GPC mobile phase: o-dichlorobenzene (special grade, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added with 0.05 weight / volume % of 2,6-di-tert-butyl-4-methylphenol (BHT) (special grade, purity 98%) as an antioxidant to inhibit the decomposition of the polymer.

[0286] (iv) Sample solution concentration: add 20 ml of solvent to 20 mg of sample

[0287] (v) Sample dissolution: Heat and stir at 145°C for 60 minutes

[0288] (vi) Injection volume into TREF column: 0.5 mL

[0289] (vii) GPC mobile phase flow rate: 1.0 ml / min

[0290] (viii)GPC column: Tosoh TSKgel GMH HR -H(S)HT2 inner diameter 7.8mm×300mm (manufactured by Tosoh Corporation) 3 pieces

[0291] (ix) Detector: Polymer ChAR, infrared spectrophotometer IR5 (built-in CFC device)

[0292] (x) Calibration of GPC column: 1 mg of each standard polystyrene manufactured by Tosoh Corporation was weighed according to the combination shown in the table below, and 20 ml of o-dichlorobenzene (with the same composition as the GPC mobile phase) was added to each solution. The solution was dissolved at 145°C for 1 hour. The resulting solutions were subjected to GPC analysis. A calibration curve was prepared based on the relationship between the molecular chain length of each standard polystyrene and the peak elution time, and calibration was performed.

[0293] Combination 1 F850, F80, F1

[0294] Combination 2 F288, F10, A2500

[0295] Combination 3 F80, F4, A1000

[0296] Combination 4 F40, F2, A500

[0297] (13) Immersion temperature

[0298] The softening point was measured using a thermomechanical analyzer according to the method specified in JIS K7196. A plate-shaped test piece having a length of 5.0 mm, a width of 5.0 mm, and a thickness of 0.50 mm was cut from the center of the pressed sheet obtained in (8), and the measurement was performed in the thickness direction. As for the tip of the indenter, a cylindrical tip having a diameter of 1.0 mm was used, and a force of 780 mN was applied to the indenter. The temperature at which the indenter was sunk 100 μm was taken as the sinking temperature.

[0299] (i) Device: Hitachi High-Technology Co., Ltd., TMA / SS6200

[0300] (ii) Indenter: 1mmΦ

[0301] (iii) Atmosphere: Nitrogen, 100 ml per minute

[0302] (iv) Temperature program: from 30°C to 190°C at a rate of 5°C / min

[0303] (v) Load: 780mN

[0304] (vi) Calculation method of sinking temperature: The temperature at which the displacement of the indenter starts when it sinks into the sample is taken as the softening point. The temperature at which the displacement reaches 100 μm is taken as the sinking temperature.

[0305] (14) Matting

[0306] The gloss value of the extruded sheet produced by the method of (9) above was measured in accordance with JIS K-7105 (1981) under the conditions of an incident angle and a light receiving angle of 60 degrees using a digital variable angle gloss meter (model UGV-5DP) manufactured by Suga Test Instruments Co., Ltd. The smaller the value, the better the matte property.

[0307] (15) Method for manufacturing extruded sheet for vacuum forming

[0308] An extruded sheet T containing a thermoplastic elastomer composition having a width of about 450 mm and a thickness of 0.5 mm was obtained using an S550-V4 sheet manufacturing apparatus (40 mm Φ extruder, L / D=26, Dulmadge screw, coat hanger die) manufactured by Tanabe Plastic Machinery Co., Ltd. at a die temperature of 190° C., a screw speed of 33 rpm, and a pulling speed of 0.4 m / min. It should be noted that the extruded sheet T was prepared using a raw material obtained by blending 1 part by mass of a black pigment masterbatch (manufactured by Sumika Masterbatch Co., Ltd., trade name “PEM8020”) described later in the form of pellets with 100 parts by mass of the thermoplastic elastomer compositions of Examples and Comparative Examples.

[0309] The extruded sheet T obtained was given a geometric pattern (each embossing had a checkered pattern with a length of 4.0 mm, a width of 4.0 mm, and a depth of 300 μm) by an embossing roll, thereby obtaining an extruded sheet T with embossing.

[0310] (16) Vacuum forming method

[0311] The vacuum forming was performed using a vacuum forming machine model TF-16-VP manufactured by Nakakura Co., Ltd.

[0312] First, the embossed extruded sheet T produced by the method of (15) above was fixed with a clamp. Then, the sheet was heated so that the surface temperature reached 150°C and vacuum-formed using a box-shaped male mold (a convex (convex) vacuum forming mold with a quadrangular prism shape having a convex portion with a bottom surface of 145 mm × 140 mm, an upper surface of 90 mm × 90 mm, and a height of 55 mm).

[0313] (17) Embossing retention

[0314] The embossing retention of the present application was evaluated by two methods as described below.

[0315] (17-1) Quantitative evaluation

[0316] The embossing retention rate of the molded article obtained in the above (16) can be determined by measuring the amount of change in embossing height using an optical microscope. Observation using an optical microscope and calculation of the amount of change in embossing height are performed under the following conditions.

[0317] (i) Optical microscope observation conditions

[0318] Microscope: Digital microscope RH2000 (HiROX)

[0319] Program used: Hirox RH2000

[0320] Measurement mode: 3D automatic stitching

[0321] Multiple: 200 times

[0322] Image processing: smoothing, tilt correction

[0323] Cut-off value: 25 μm (using roughness curve)

[0324] Observation steps: The image is acquired in the range of 80 mm × 80 mm in the 3D automatic stitching mode in such a way that the part with the worst embossing retention falls into the field of view when visually observed. The average height is calculated from the acquired image using the above procedure. Select 5 rows of concave and convex in the horizontal direction of the image and 5 rows of concave and convex in the vertical direction, calculate the average height difference between the convex part and the concave part of the embossing, and calculate the average value.

[0325] (ii) Calculation of the change in embossing height

[0326] The change in embossing height is calculated according to the following formula (2).

[0327] Embossing retention rate = h / H × 100……(2)

[0328] In formula (2), H represents the average embossing height difference between the convex part and the concave part of the embossing before vacuum forming, and h represents the average embossing height difference between the convex part and the concave part of the embossing after vacuum forming.

[0329] (17-2) Qualitative evaluation by visual inspection

[0330] The embossing retention property of the molded article obtained in the above (16) was evaluated by the following 5 levels when visually inspected.

[0331] “5”: The embossing is almost gone

[0332] “4”: The embossing is slightly disappeared

[0333] “3”: The embossing pattern has obviously disappeared

[0334] “2”: The embossing is almost completely gone

[0335] “1”: The embossing has completely disappeared

[0336] The starting materials used in the examples are as follows. In addition, in the tables and the like, these materials may be represented by only symbols.

[0337] Oil-extended ethylene rubber (composition comprising (A) ethylene rubber and (E) mineral oil)

[0338] A product obtained by adding 40 parts by mass of paraffin-based mineral oil (E-1) (manufactured by Idemitsu Kosan Co., Ltd., trade name "PW-380") to 100 parts by mass of the ethylene-propylene-5-ethylidene-2-norbornene copolymer (A-1)

[0339] Mooney viscosity (ML) of (A-1)+(E-1) 1+4 100°C) = 79, the content of monomer units derived from ethylene in (A-1) = 67.9% by mass, the content of monomer units derived from propylene in (A-1) = 27.8% by mass, the content of monomer units derived from 5-ethylidene-2-norbornene in (A-1) = 4.3% by mass, density: 0.884 g / cm 3 .

[0340] (B): Propylene polymer

[0341] (B-1) Propylene homopolymer

[0342] MFR (230°C, 21.18N) = 0.5 g / 10 min, [ηcxis] = 3.0 dl / g.

[0343] (B-2) Propylene homopolymer

[0344] MFR (230°C, 21.18N) = 20 g / 10 min, [ηcxis] = 1.3 dl / g.

[0345] (B-3) Propylene random copolymer

[0346] MFR (230°C, 21.18N) = 1.5 g / 10 min, content of monomer units derived from ethylene = 5% by mass, [ηcxs] = 0.88 dl / g, [ηcxis] = 2.24 dl / g.

[0347] (B-4) Propylene polymer material

[0348] MFR (230°C, 21.18N) = 3 g / 10 min, content of ethylene-propylene copolymer component = 20% by mass, content of monomer units derived from ethylene in the ethylene-propylene copolymer component = 37% by mass, [ηcxs] = 3.80 dl / g, [ηcxis] = 1.79 dl / g.

[0349] (B-5) Propylene polymer material

[0350] MFR (230°C, 21.18N) = 0.5 g / 10 min, content of ethylene-propylene copolymer component = 16% by mass, content of monomer units derived from ethylene in the ethylene-propylene copolymer component = 40% by mass, [ηcxs] = 3.20 dl / g, [ηcxis] = 2.77 dl / g.

[0351] (C): Ethylene polymer having more than 90% by mass of monomer units derived from ethylene

[0352] (C-1) Sumitomo Chemical Co., Ltd., trade name “SUMIKATHEN E G201” (low-density polyethylene), MFR (190°C, 21.18 N) = 2 g / 10 min, density: 0.919 g / cm 3 .

[0353] Composition comprising (D) a crosslinking agent and (E) a mineral oil

[0354] (D-1+E-2) Manufactured by AKZO Co., Ltd., trade name "APO-10DL"

[0355] (a composition comprising 10% by mass of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (D-1) and 90% by mass of paraffin-based mineral oil (E-2) (manufactured by Idemitsu Kosan Co., Ltd., trade name "PW-100") (wherein the total amount of (D-1) and (E-2) is 100% by mass)).

[0356] other

[0357] Antioxidant: BASF Japan Ltd., trade name "Irganox 1010"

[0358] Crosslinking aid: manufactured by Seiko Chemical Industries, Ltd., trade name "Hi-Cross MP" (trimethylolpropane trimethacrylate diluted to 66.7% with silicon oxide)

[0359] Black pigment masterbatch: manufactured by Sumika Masterbatch Co., Ltd., trade name "PEM8020"

[0360] In the following Examples and Comparative Examples, the thermoplastic elastomer composition was produced by melt-kneading the materials at 200°C±20°C for 40 seconds±20 seconds using a twin-screw kneading extruder (TEX-44HCT manufactured by The Nippon Steel Works, Ltd.).

[0361] [Example 1]

[0362] A thermoplastic elastomer composition precursor was prepared by melt-kneading 62.6% by mass of an oil-extended ethylene rubber (44.7% by mass of (A-1) + 17.9% by mass of (E-1)), 26.8% by mass of a propylene polymer (B-4), 0.1% by mass of an antioxidant (Irganox 1010), 0.4% by mass of a crosslinking aid (Hi-Cross MP), and 2.1% by mass of a crosslinking agent ((D-1) + (E-2)). The obtained thermoplastic elastomer composition precursor and 8.0% by mass of the propylene polymer (B-1) were melt-kneaded under the above conditions to prepare a thermoplastic elastomer composition.

[0363] The gel fraction of the thermoplastic elastomer composition was 30.3% by mass. The content of the component (X) in the thermoplastic elastomer composition was 35.0% by mass, and the content of the component (X1) was 10.2% by mass.

[0364] The sinking temperature of a pressed sheet obtained by press-molding the obtained thermoplastic elastomer composition by the method (8) above was 128°C.

[0365] Table 1 shows the evaluation results of the extruded sheet obtained by extrusion molding the obtained thermoplastic elastomer composition by the method (9) above.

[0366] [Examples 2 to 5]

[0367] A thermoplastic elastomer composition was produced in the same manner as in Example 1 except that the type and / or amount of the starting material used was changed as shown in Table 1, and the properties thereof were evaluated.

[0368] Table 1 shows the results.

[0369]

[0370] [Comparative Example 1]

[0371] Except for changing the kind and / or amount of the starting materials used as shown in Table 2, a thermoplastic elastomer composition was produced in the same manner as in Example 1, and the properties thereof were evaluated.

[0372] The point that the sinking temperature is 111° C. is outside the scope of the first invention of the present application, and the point that the proportion of the component (X1) is 5.9 mass % is outside the scope of the third invention of the present application.

[0373] Table 2 shows the results.

[0374] [Comparative Example 2]

[0375] Except for changing the kind and / or amount of the starting materials used as shown in Table 2, a thermoplastic elastomer composition was produced in the same manner as in Example 1, and the properties thereof were evaluated.

[0376] The point that the sinking temperature is 111° C. is outside the scope of the first invention of the present application, and the point that the proportion of the component (X1) is 5.6% by mass is outside the scope of the third invention of the present application.

[0377] Table 2 shows the results.

[0378] [Comparative Example 3]

[0379] Except for changing the kind and / or amount of the starting materials used as shown in Table 2, a thermoplastic elastomer composition was produced in the same manner as in Example 1, and the properties thereof were evaluated.

[0380] The sinking temperature of 108° C. is outside the scope of the first invention of the present application, and the gel fraction of 4.7% by mass is outside the scope of the third invention of the present application.

[0381] Table 2 shows the results.

[0382] [Comparative Example 4]

[0383] A thermoplastic elastomer composition was produced in the same manner as in Example 1 except that the type and / or amount of the starting materials used was changed as shown in Table 2 and melt kneading with the propylene polymer (B1) was not performed, and the properties thereof were evaluated.

[0384] The sinking temperature is 92° C., which is outside the scope of the first invention of the present application, and the proportion of the component (X1) is 3.3% by mass, which is outside the scope of the third invention of the present application.

[0385] Table 2 shows the results.

[0386]

[0387] Industrial Applicability

[0388] The thermoplastic elastomer composition of the present invention has excellent moldability and appearance of molded articles. For example, even when processed under relatively severe conditions such as vacuum molding, the pattern and shape of the surface such as embossing applied can be maintained. Therefore, it can be suitably used for automobile interior surface materials such as door trims and instrument panels, and has high practical application in various fields of industries such as automobile and other transportation machinery industries, sporting goods industries, leisure goods industries, household goods industries, electrical and electronic equipment industries, and construction industries.

Claims

1. A thermoplastic elastomer composition, wherein: The total amount of the thermoplastic elastomer composition is 100 mass %, and the thermoplastic elastomer composition contains 10 mass % to 70 mass % of (A) ethylene-based rubber, 10 mass % to 89 mass % of (B) propylene-based polymer, and 1 mass % to 60 mass % of (E) mineral oil, wherein: The proportion of the component (X1) having a logarithm of molecular weight M (logM) of 5.6 or more in terms of polystyrene is 6.0% to 45.0% by mass relative to 100% by mass of the total eluted amount. (A) at least a portion of the ethylene-based rubber is crosslinked, The pressed sheet obtained by press-molding the thermoplastic elastomer composition under the following molding conditions has a sinking temperature of 125° C. or higher, the sinking temperature being measured in accordance with JIS K7196-1991 and being defined as the temperature at which the indenter penetrates 100 μm from the sheet surface, Molding conditions: The thermoplastic elastomer composition was hot-pressed at a temperature of 200° C. and a maximum pressure of 10 MPa for 5 minutes, and then cold-pressed at a temperature of 23° C. and a maximum pressure of 10 MPa for 5 minutes to prepare a pressed sheet. The thermoplastic elastomer composition has a gel fraction of 5.0% by mass to 50% by mass.

2. The thermoplastic elastomer composition according to claim 1, wherein The ratio of component (X) eluted in the range of elution temperature greater than 100°C and less than or equal to 140°C relative to the total elution amount (100% by mass) measured by cross-fractionation chromatography using an apparatus having a temperature-elution fractionation section and a gel permeation chromatography section under the following conditions (1) to (3) is 1% by mass to 50% by mass, The ratio of the component (X1) having a logarithm logM of a molecular weight M in terms of polystyrene of 5.6 or more in the component (X) is 6.0% by mass to 45.0% by mass relative to the total eluted amount (100% by mass), (1) maintaining the temperature-eluting fractionation section at 100° C. for 10 minutes, into which an o-dichlorobenzene solution of a thermoplastic elastomer composition is injected, wherein the concentration of the thermoplastic elastomer composition in the o-dichlorobenzene solution is 1 mg / mL; (2) The temperature of the temperature-elution fractionation section was lowered to -5°C at a rate of 2.0°C / min, then maintained at -5°C for 30 minutes, and the elution amount at -5°C was measured; (3) The following operation is repeated at three reaching temperatures of 50°C, 100°C and 140°C: the temperature of the temperature-eluting fractionation section is raised at a rate of 40°C / min to the reaching temperature, then maintained at the reaching temperature for 30 minutes, and then the elution amount at the reaching temperature is measured.

3. The thermoplastic elastomer composition according to claim 2, wherein In the cross-fractionation chromatography, the ratio of the component (α) eluted at an elution temperature of -5°C is 70% by mass or less relative to the total elution amount of 100% by mass.

4. The thermoplastic elastomer composition according to claim 2 or 3, wherein In the cross-fractionation chromatography, the ratio of the component (β) eluted in the elution temperature range of greater than -5°C and less than or equal to 50°C is 1% by mass to 39% by mass with respect to the total elution amount of 100% by mass.

5. The thermoplastic elastomer composition according to claim 2 or 3, wherein In the cross-fractionation chromatography, the ratio of the component (γ) eluted in the elution temperature range of more than 50° C. and less than or equal to 100° C. is 0.1% by mass to 39% by mass with respect to the total elution amount of 100% by mass.

6. A sheet produced using the thermoplastic elastomer composition according to claim 1, wherein: The total amount of the sheet is 100 mass %, and the sheet contains 10 mass % to 70 mass % of (A) ethylene rubber, 10 mass % to 89 mass % of (B) propylene polymer, and 1 mass % to 60 mass % of (E) mineral oil, wherein: The sinking temperature of the sheet is 125° C. or higher, which is measured in accordance with JIS K7196-1991 and is defined as the temperature at which the indenter penetrates 100 μm from the sheet surface.

Citation Information

Patent Citations

  • Production of alpha-olefin polymer

    JP1986218606A

  • Production of alpha-olefin polymer

    JP1986287904A

  • Ethylene-propylene block copolymer

    JP1993194685A

  • Catalyst for polymerizing alpha-olefin and production of alpha-olefin polymer

    JP1995216017A

  • Propylene / ethylene-alpha-olefin block copolymer and its production

    JP1997316147A