Negative photosensitive resin composition, method for producing cured film using the same, and touch panel

By using a negative photosensitive resin composition in the touch panel, including a silicone resin and a specific photoradical polymerization initiator, the problem of insufficient hardness and weather resistance of the cured film at low temperatures is solved, and high resolution and low gas emissions are achieved. emissions effects.

CN113474730BActive Publication Date: 2024-10-01TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080016528.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-05
Filing Date
2020-03-02
Publication Date
2024-10-01
Estimated Expiration
2040-03-02

AI Technical Summary

Technical Problem

The cured film of existing touch panels cured at low temperatures has problems such as insufficient pencil hardness, insufficient weather resistance, and low resolution. In particular, during electrode or wiring processing, it is easy to generate outgassing, which affects its performance.

Method used

A negative photosensitive resin composition is used, which contains a silicone resin with a radical polymerizable group, a monomer with a radical polymerizable group, and a photoradical polymerization initiator with an absorption peak in the wavelength range of 350 nm to 370 nm. The agent promotes free radical reactions through light irradiation, improves cross-linking density and resolution, and cures at low temperatures below 150°C.

Benefits of technology

It achieves the formation of a cured film with high pencil hardness, excellent chemical resistance and weather resistance at low temperatures, suppresses the generation of external gases during electrode or wiring processing, and improves the overall performance of the touch panel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003228333380000121
    Figure BDA0003228333380000121
  • Figure BDA0003228333380000321
    Figure BDA0003228333380000321
  • Figure BDA0003228333380000331
    Figure BDA0003228333380000331
Patent Text Reader

Abstract

The present invention aims to provide a negative photosensitive resin composition which has high resolution and can form a cured film having high pencil hardness, excellent chemical resistance and weather resistance, and can suppress the generation of outgassing during electrode or wiring processing even when cured at a low temperature of 150°C or lower. The present invention is a negative photosensitive resin composition comprising: (A) a siloxane resin having a free radical polymerizable group; (B) a monomer having a free radical polymerizable group; and (C) a photo radical polymerization initiator, which has an absorption peak in the wavelength region of 350 to 370, and an absorbance at a wavelength of 400 is less than 10% of the absorbance at a wavelength of 365.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a negative photosensitive resin composition containing a siloxane resin having a radical polymerizable group, a monomer having a radical polymerizable group, and a photoradical polymerization initiator, a method for producing a cured film using the negative photosensitive resin composition, and a touch panel. Background Art

[0002] In recent years, touch panels have been widely used as input means. The touch panel includes a display unit such as a liquid crystal panel, and a touch panel sensor for detecting information input to a specific position. The touch panel method is roughly divided into a resistive film method, an electrostatic capacitance method, an optical method, an electromagnetic induction method, an ultrasonic method, etc. according to the detection method of the input position. Among them, the electrostatic capacitance method touch panel is widely used due to reasons such as optical brightness, excellent appearance design, simple structure and excellent function. The display unit of the touch panel uses a transparent electrode substrate with a transparent electrode formed on a substrate. As a transparent electrode, indium oxide doped with tin (indium tin oxide (Indium Tin Oxide, ITO)) and the like have been used previously. In order to make the touch panel large-screen or based on pen touch detection possible, further low resistance is required, but the high resistivity of ITO has become a subject. Therefore, in recent years, a touch panel having an electrode called a so-called metal mesh in which a conductor line formed of a conductive metal such as copper or a copper alloy is configured in a mesh shape has been proposed. However, copper is easily oxidized under high temperature conditions to form an oxide film, which increases the resistance value. Therefore, as a material for the insulating layer or protective layer of the touch panel, a material that can be cured at a low temperature of 150° C. or less is required.

[0003] Therefore, as a photosensitive resin composition that has excellent pattern processability and provides sufficient chemical resistance and substrate adhesion even when cured at a low temperature below 150°C, for example, a photosensitive resin composition comprising a photoreactive resin containing an ethylenically unsaturated group and a carboxyl group, a specific epoxy compound, a specific polyfunctional epoxy compound and a photopolymerization initiator has been proposed (for example, refer to Patent Document 1).

[0004] In addition, as a raw material composition for an insulating coating having excellent adhesion or chemical resistance, a composition for an insulating material containing a siloxane oligomer having a cross-linking functional group, a photopolymerization initiator, and a adhesion promoter containing a coordination compound of aluminum and / or zirconium has been proposed (for example, refer to Patent Document 2).

[0005] On the other hand, as photoradical polymerization initiators, benzoic acid-based, benzophenone-based, thioxanthone-based, acetophenone-based, and acylphosphine-based initiators are known, and oxime ester-based photoradical polymerization initiators have also been introduced recently (see Patent Documents 3 and 4).

[0006] [Prior art literature]

[0007] [Patent Document]

[0008] [Patent Document 1] International Publication No. 2017 / 110689

[0009] [Patent Document 2] International Publication No. 2014 / 185435

[0010] [Patent Document 3] Japanese Patent Publication No. 2009-519991

[0011] [Patent Document 4] Japanese Patent Publication No. 2014-522394 Summary of the invention

[0012] Problems to be solved by the invention

[0013] According to the technology described in Patent Document 1, even when cured at low temperature, a cured film with excellent chemical resistance and substrate adhesion can be obtained, but there are problems such as insufficient pencil hardness and weather resistance of the cured film, and generation of outgassing during wiring processing due to the remaining unreacted free radical polymerizable groups. In addition, according to the technology described in Patent Document 2, a cured film with excellent pencil hardness can be obtained, but there is a problem of insufficient resolution. In addition, due to insufficient crosslinking density of the cured film, there is a problem of insufficient chemical resistance such as etching solution penetrating into the insulating film when forming an electrode on the insulating film.

[0014] The present invention has been conceived in view of the problems of the above-mentioned prior art, and its object is to provide a negative photosensitive resin composition, which has high resolution and can form a cured film with high pencil hardness, excellent chemical resistance and weather resistance even when cured at a low temperature of 150° C. or below, and can suppress the generation of outgassing during electrode or wiring processing.

[0015] Means of solving problems

[0016] The object of the present invention is achieved by the following means.

[0017] First, the following negative photosensitive resin composition is provided. A negative photosensitive resin composition comprises: (A) a siloxane resin having a free radical polymerizable group, (B) a monomer having a free radical polymerizable group, and (C) a photoradical polymerization initiator, wherein the photoradical polymerization initiator (C) has a light absorption peak in the region of wavelengths of 350 nm to 370 nm, and the absorbance at a wavelength of 400 nm is less than 10% of the absorbance at a wavelength of 365 nm.

[0018] Furthermore, the characteristics of the negative photosensitive resin composition disclosed in the present invention also include the following inventions.

[0019] A method for producing a cured film comprises the steps of applying the negative photosensitive resin composition of the present invention on a substrate, exposing the composition to light, and curing the exposed composition at a temperature of 150° C. or less.

[0020] A touch panel comprises a substrate, electrodes and / or wirings containing copper, and a cured film formed by curing the negative photosensitive resin composition of the present invention.

[0021] Effects of the Invention

[0022] The negative photosensitive resin composition of the present invention has a high resolution. Even when cured at a low temperature of 150° C. or lower, a cured film having high pencil hardness, excellent chemical resistance and weather resistance and capable of suppressing the generation of outgassing during electrode or wiring processing can be obtained. DETAILED DESCRIPTION

[0023] Hereinafter, the present invention will be described in more detail.

[0024] The negative photosensitive resin composition of the present invention is characterized in that it contains at least: (A) a siloxane resin having a free radical polymerizable group (hereinafter sometimes simply described as "(A) siloxane resin"); (B) a monomer having a free radical polymerizable group; and (C) a photoradical polymerization initiator (hereinafter sometimes simply described as "(C) photoradical polymerization initiator"), wherein the (C) photoradical polymerization initiator has an absorption peak in the region of wavelengths of 350nm to 370nm, and the absorbance at a wavelength of 400nm is less than 10% of the absorbance at a wavelength of 365nm. By containing (A) siloxane resin and (C) photoradical polymerization initiator, free radical polymerization of the free radical polymerizable group of (A) siloxane resin and the monomer having (B) free radical polymerizable group proceeds in the light irradiation part, thereby enabling negative pattern processing that does not dissolve the light irradiation part. The (A) siloxane resin includes a siloxane skeleton having high heat resistance and weather resistance and a free radical polymerizable group in the main chain. In addition, the silanol condensation reaction proceeds even at 150° C. or lower, thereby increasing the crosslinking density of the cured film, thereby improving chemical resistance and weather resistance, and increasing pencil hardness.

[0025] On the other hand, in the case of the negative photosensitive resin composition known in the past, there is a problem that crosslinking cannot be fully carried out at a curing temperature below 150°C, and the chemical resistance of the film decreases. In contrast, in the exposure of the present invention using a common ultra-high pressure mercury lamp or light-emitting diode (LED) with a strong bright line emission spectrum in i-rays (wavelength 365nm) as a light source, by using a photo-radical polymerization initiator having an absorption peak in the region of wavelength 350nm to 370nm in the present invention, the concentration of free radicals generated in the light irradiation portion increases, thereby promoting the reaction of free radical polymerizable groups. Therefore, the crosslinking density of the film obtained by photocuring can be increased, thereby improving the pencil hardness or chemical resistance. Moreover, since the remaining unreacted free radical polymerizable groups can be suppressed, the weather resistance can be improved and the released gas during electrode or wiring processing can be reduced.

[0026] Furthermore, the photoradical polymerization initiator of the present invention, whose absorbance at a wavelength of 400 nm is 10% or less of the absorbance at a wavelength of 365 nm, suppresses absorption of long-wavelength light which is a major factor in reducing resolution, thereby improving resolution.

[0027] In the present invention, as a photo-radical polymerization initiator having selective absorption in the wavelength region of i-rays, the absorbance at each wavelength is focused on, and the absorbance at a wavelength of 400nm is selected as an indicator of the absorbance in the wavelength region such as h-rays (405nm) or g-rays (436nm) having a long-wavelength emission spectrum compared to i-rays. The absorbance at a wavelength of 400nm being 10% or less of the absorbance at a wavelength of 365nm means that light in the wavelength region of i-rays is selectively absorbed.

[0028] The negative photosensitive resin composition of the present invention contains (A) a siloxane resin. The siloxane resin refers to a polymer containing a repeating unit having a siloxane skeleton. The (A) siloxane resin in the present invention has a free radical polymerizable group, and is preferably a hydrolysis condensate of an organic silane compound having a free radical polymerizable group. For the hydrolysis condensation reaction, it is preferred that a hydrolyzable group is directly bonded to the silicon atom of the organic silane compound. Examples of the hydrolyzable group include an alkoxy group and a carboxyl group.

[0029] From the viewpoint of further improving chemical resistance, the weight average molecular weight (Mw) of the siloxane resin (A) is preferably 500 or more, and more preferably 1,000 or more. On the other hand, from the viewpoint of improving solubility in a developer during pattern formation, the Mw of the siloxane resin (A) is preferably 10,000 or less, and more preferably 5,000 or less. Here, the Mw of the siloxane resin (A) refers to a polystyrene conversion value measured by gel permeation chromatography (GPC).

[0030] Examples of the radical polymerizable group include a vinyl group, an α-methylvinyl group, an allyl group, a styryl group, and a (meth)acryloyl group. From the viewpoint of further improving the pencil hardness of the cured film or the sensitivity during pattern processing, a (meth)acryloyl group is preferred.

[0031] From the viewpoint of improving the adhesion with the substrate as the base, the double bond equivalent of the siloxane resin (A) is preferably 150 g / mol or more, and more preferably 200 g / mol or more. On the other hand, from the viewpoint of further improving the crosslinking density of the cured film, further improving the chemical resistance, and further improving the pencil hardness, the double bond equivalent of the siloxane resin (A) is preferably 2,000 g / mol or less, and more preferably 1,500 g / mol or less. As described above, it is preferably a (meth)acryloyl group, so although it is not necessarily two functional groups, the total double bond equivalent of the acryloyl group and the methacryloyl group is preferably 2,000 g / mol or less, and more preferably 1,500 g / mol or less, from the viewpoint of further improving the crosslinking density of the cured film, further improving the chemical resistance, and further improving the pencil hardness. Here, the double bond equivalent of the siloxane resin can be calculated by measuring the iodine value.

[0032] Examples of the organosilane compound having a radical polymerizable group include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(methoxyethoxy)silane, vinylmethyldimethoxysilane, vinylmethyldiethoxysilane, vinylmethylbis(methoxyethoxy)silane, allyltrimethoxysilane, allyltriethoxysilane, allyltri(methoxyethoxy)silane, allylmethyldimethoxysilane, allylmethyldiethoxysilane, allylmethylbis(methoxyethoxy)silane, styryltrimethoxysilane, styryltriethoxysilane, styryltri(methoxyethoxy)silane, styrylmethyldimethoxysilane, styrylmethyl Diethoxysilane, styrylmethylbis(methoxyethoxy)silane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-acryloxypropyltri(methoxyethoxy)silane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropyltri(methoxyethoxy)silane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-acryloxypropylmethyldimethoxysilane, 3-acryloxypropylmethyldiethoxysilane, 3-methacryloxypropyl(methoxyethoxy)silane, etc. Two or more of these may be used. Among these, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-methacryloxypropyltriethoxysilane are preferred from the viewpoint of further improving the pencil hardness of the cured film or the sensitivity during pattern processing.

[0033] (A) The siloxane resin may also be a hydrolysis condensate of the above-mentioned organosilane compound having a free radical polymerizable group and another organosilane compound. The latter organosilane compound also preferably has a hydrolyzable group directly bonded to the silicon atom. Examples of the hydrolyzable group include an alkoxy group and a carboxyl group.

[0034] Examples of other organosilane compounds include methyltrimethoxysilane, methyltriethoxysilane, methyltri(methoxyethoxy)silane, methyltripropoxysilane, methyltriisopropoxysilane, methyltributoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, hexyltrimethoxysilane, octadecyltrimethoxysilane, octadecyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-chloropropyltrimethoxysilane, 3-(N,N-diglycidyl)aminopropyltrimethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 3-Aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 2-cyanoethyltriethoxysilane, glycidyloxymethyltrimethoxysilane, glycidyloxymethyltriethoxysilane, 1-glycidyloxyethyltrimethoxysilane, 1-glycidyloxyethyltriethoxysilane, 2-glycidyloxyethyltrimethoxysilane, 2-glycidyloxyethyltriethoxysilane, 1-glycidyloxypropyltrimethoxysilane, 1-glycidyloxypropyltriethoxysilane, 2-glycidyloxypropyltrimethoxysilane, 2-glycidyloxypropyltriethoxysilane, 3-glycidyl 2-glycidyloxybutyl trimethoxysilane, 2-glycidyloxybutyl trimethoxysilane, 2-glycidyloxybutyl triethoxysilane, 3-glycidyloxypropyl tripropoxysilane, 3-glycidyloxypropyl triisopropoxysilane, 3-glycidyloxypropyl tributoxysilane, 3-glycidyloxypropyl tri(methoxyethoxy)silane, 1-glycidyloxybutyl trimethoxysilane, 1-glycidyloxybutyl triethoxysilane, 2-glycidyloxybutyl trimethoxysilane, 3-glycidyloxybutyl trimethoxysilane, 3-glycidyloxybutyl triethoxysilane, 4-glycidyloxybutyl trimethoxysilane, 4-glycidyloxybutyl triethoxysilane silane, (3,4-epoxycyclohexyl)methyltrimethoxysilane, (3,4-epoxycyclohexyl)methyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltripropoxysilane, 2-(3,4-epoxycyclohexyl)ethyltributoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriphenoxysilane, 3-(3,4-epoxycyclohexyl)propyltrimethoxysilane, 3-(3,4-epoxycyclohexyl)propyltriethoxysilane, 4-(3,4-epoxycyclohexyl)butyltrimethoxysilane, 4-(3,4-epoxycyclohexyl)butyltrimethoxysilane,4-epoxycyclohexyl)butyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, glycidoxymethyldimethoxysilane, glycidoxymethylmethyldiethoxysilane, 1-glycidoxyethylmethyldimethoxysilane, 1-glycidoxyethylmethyldiethoxysilane, 2-glycidoxyethylmethyldimethoxysilane, 2-glycidoxyethylmethyl Diethoxysilane, 1-glycidoxypropylmethyldimethoxysilane, 1-glycidoxypropylmethyldiethoxysilane, 2-glycidoxypropylmethyldimethoxysilane, 2-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropylmethyldipropoxysilane, 2-glycidoxypropylmethyldibutoxysilane, 3-glycidoxypropylmethylbis(methoxyethoxy)silane, 3-glycidoxypropylethyldimethoxysilane, 3-glycidoxypropylethyl Diethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropylmethyldiethoxysilane, cyclohexylmethyldimethoxysilane, octadecylmethyldimethoxysilane, tetramethoxysilane, tetraethoxysilane, trifluoromethyltrimethoxysilane, trifluoromethyltriethoxysilane, trifluoropropyltrimethoxysilane, trifluoropropyltriethoxysilane, perfluoropropyltrimethoxysilane, perfluoropropyltriethoxysilane, perfluoropentyltrimethoxysilane, perfluoropentyltriethoxysilane, tridecafluorooctyltrimethoxysilane, tridecafluorooctyltriethoxysilane, tridecafluorooctyltripropoxysilane, tridecafluorooctyltriisopropoxysilane, heptadecafluorodecyl Trimethoxysilane, heptadecafluorodecyl triethoxysilane, bis(trifluoromethyl)dimethoxysilane, bis(trifluoropropyl)dimethoxysilane, bis(trifluoropropyl)diethoxysilane, trifluoropropylmethyldimethoxysilane, trifluoropropylmethyldiethoxysilane, trifluoropropylethyldimethoxysilane, trifluoropropylethyldiethoxysilane, heptadecafluorodecylmethyldimethoxysilane, 3-trimethoxysilylpropyl succinic anhydride, 3-triethoxysilylpropyl succinic anhydride, 3-triphenoxysilylpropyl succinic anhydride, 3-trimethoxysilylpropyl cyclohexyl dicarboxylic anhydride, 3-trimethoxysilylpropyl phthalic anhydride, etc. Two or more of these may also be used. Among these, methyltrimethoxysilane, phenyltrimethoxysilane, tetraethoxysilane, 3-glycidoxypropyltrimethoxysilane, etc. are preferred.

[0035] The siloxane resin (A) of the present invention can be obtained by subjecting the organosilane compound to hydrolysis and condensation, for example, by hydrolyzing an organosilane compound having a hydrolyzable group and then subjecting the resulting silanol compound to a condensation reaction in the presence of an organic solvent or in the absence of a solvent.

[0036] Regarding the negative photosensitive resin composition of the present invention, since it is intended to be cured after pattern processing, it is preferred that the siloxane resin (A) is not completely condensed, but has residual hydrolyzable groups or silanol groups. If these functional groups disappear, the molecular weight will be increased and cross-linking will occur, making it difficult to dissolve or disperse in a solvent or mix with other additives.

[0037] The various conditions of the hydrolysis reaction can be appropriately set in consideration of the reaction scale, the size and shape of the reaction vessel, etc. For example, it is preferred that the reaction is carried out at room temperature to 110° C. for 1 minute to 180 minutes after adding an acid catalyst and water to the organosilane compound in a solvent. By carrying out the hydrolysis reaction under such conditions, a rapid reaction can be suppressed. The reaction temperature is more preferably 30° C. to 105° C.

[0038] The hydrolysis reaction is preferably carried out in the presence of an acid catalyst. As the acid catalyst, an acidic aqueous solution containing formic acid, acetic acid, phosphoric acid, or nitric acid is preferred. The amount of the acid catalyst added is preferably 0.05 to 5 parts by weight relative to 100 parts by weight of all the organosilane compounds used during the hydrolysis reaction. By making the amount of the acid catalyst within the above range, the hydrolysis reaction can be carried out more efficiently.

[0039] Preferably, after obtaining the silanol compound by hydrolysis of the organosilane compound to generate silanol groups, the reaction solution is directly heated at 50° C. or higher and below the boiling point of the solvent for 1 to 100 hours to carry out the condensation reaction. Further heating or addition of an alkali catalyst may be performed to increase the degree of polymerization of the polysiloxane.

[0040] Examples of the organic solvent used in the hydrolysis reaction of the organosilane compound and the condensation reaction of the silanol compound include alcohols such as methanol, ethanol, propanol, isopropanol, butanol, isobutanol, tert-butanol, pentanol, 4-methyl-2-pentanol, 3-methyl-2-butanol, 3-methyl-3-methoxy-1-butanol, 1-tert-butoxy-2-propanol, and diacetone alcohol; glycols such as ethylene glycol and propylene glycol; and ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, and diethyl ether. Ketones such as methyl ethyl ketone, acetylacetone, methyl propyl ketone, methyl butyl ketone, methyl isobutyl ketone, diisobutyl ketone, cyclopentanone, and 2-heptanone; amides such as dimethylformamide and dimethylacetamide; acetates such as ethyl acetate, propyl acetate, butyl acetate, isobutyl acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, methyl lactate, ethyl lactate, and butyl lactate; aromatic or aliphatic hydrocarbons such as toluene, xylene, hexane, and cyclohexane, γ-butyrolactone, N-methyl-2-pyrrolidone, and dimethyl sulfoxide. Two or more of these may be used. In terms of transmittance and crack resistance of the cured film, diacetone alcohol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether, propylene glycol mono-tert-butyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, γ-butyrolactone, etc. are preferably used.

[0041] In the case where a solvent is generated by the hydrolysis reaction, the hydrolysis can also be carried out without a solvent. It is also preferred that a solvent is further added after the reaction is completed to adjust the concentration to be appropriate for the resin composition. In addition, it is also possible to distill and remove an appropriate amount of generated alcohol etc. under heating and / or reduced pressure after the hydrolysis according to the purpose, and then add a preferred solvent.

[0042] The amount of the solvent used in the hydrolysis reaction is preferably 80 parts by mass or more and 500 parts by mass or less relative to 100 parts by mass of the total organosilane compound. When the amount of the solvent is within the above range, the hydrolysis reaction can be performed more efficiently.

[0043] The water used in the hydrolysis reaction is preferably ion-exchanged water, and the amount of water is preferably 1.0 mol to 4.0 mol per 1 mol of silicon atoms.

[0044] From the viewpoint of increasing the crosslinking density of the cured film by the silanol condensation reaction to further increase the pencil hardness of the cured film and further suppressing the generation of outgassing during electrode or wiring processing, the content of the siloxane resin (A) having a free radical polymerizable group in the negative photosensitive resin composition of the present invention is preferably 30% by mass or more, more preferably 40% by mass or more, and further preferably 50% by mass or more in the solid content. On the other hand, from the viewpoint of further improving the chemical resistance of the cured film, the content of the siloxane resin (A) is preferably 70% by mass or less, more preferably 60% by mass or less in the solid content.

[0045] The negative photosensitive resin composition of the present invention contains (B) a monomer having a free radical polymerizable group. As the free radical polymerizable group, the group exemplified as the free radical polymerizable group possessed by the (A) siloxane resin is preferred, and a (meth)acryloyl group is more preferred. From the viewpoint of further improving the chemical resistance by further improving the crosslinking density and hydrophobicity of the cured film, it is preferred that the monomer (B) having a free radical polymerizable group contains (B1) a multifunctional monomer and (B2) a monomer having an aromatic ring and / or an alicyclic carbon ring.

[0046] (B1) The multifunctional monomer refers to a compound having two or more free radical polymerizable groups, preferably having two or more (meth)acryloyl groups. Examples of the compound having two (meth)acryloyl groups include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, glycerol di(meth)acrylate, tripropylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, and 1,10-decanediol di(meth)acrylate. As compounds having three or more (meth)acryloyl groups, for example, glycerol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, tripentaerythritol octa(meth)acrylate, four-season pentaerythritol nine(meth)acrylate, four-season pentaerythritol ten(meth)acrylate, pentaerythritol eleven(meth)acrylate, pentaerythritol twelve(meth)acrylate, etc. may be included. Two or more of these may also be included. In addition, if it is a compound having two or more free radical polymerizable groups, even if it contains an aromatic ring or an alicyclic carbon ring, it is classified as a (B1) multifunctional monomer.

[0047] Examples of the monomer (B2) having an aromatic ring and / or an alicyclic carbon ring include acrylates such as 2,2-[9H-fluorene-9,9-diylbis(1,4-phenylene)bisoxy]diethanol di(meth)acrylate, dimethyloltricyclodecane di(meth)acrylate, and ethoxylated bisphenol A di(meth)acrylate. Two or more of these may be contained.

[0048] From the viewpoint of improving the hydrophobicity of the cured film to further enhance the chemical resistance, the content of the monomer having an aromatic ring and / or an alicyclic carbon ring (B2) in the negative photosensitive resin composition of the present invention is preferably 10% by mass or more, more preferably 15% by mass or more in the solid content. On the other hand, from the viewpoint of improving the solubility in the developer during pattern formation to further enhance the resolution, the content of the monomer having an aromatic ring and / or an alicyclic carbon ring (B2) in the solid content is preferably 35% by mass or less, more preferably 25% by mass or less.

[0049] From the viewpoint of increasing the crosslinking density and hydrophobicity of the cured film to further enhance chemical resistance, the total content of the monomers having a radical polymerizable group (B) is preferably 20% by mass or more, more preferably 30% by mass or more in the solid content.

[0050] The negative photosensitive resin composition of the present invention contains (C) a photoradical polymerization initiator having an absorption peak in the wavelength region of 350 nm to 370 nm, and an absorbance at a wavelength of 400 nm being 10% or less of the absorbance at a wavelength of 365 nm. Examples of such (C) photoradical polymerization initiators include TR-PBG-326, TR-PBG-331, TR-PBG-345 (trade names, all manufactured by TRONLY), "Irgacure" (registered trademark) OXE03 (trade name, manufactured by BASF), and NCI-738 (trade name, manufactured by ADEKA Co., Ltd.). Two or more of these may be contained. Among these photopolymerization initiators, those containing two or more ketoxime ester groups in one molecule represented by the following general formula (1), such as TR-PBG-345, are particularly preferred. By containing more than two oxime ester groups in one molecule, the free radicals are cracked by light irradiation, and the free radicals are generated at more than two positions, so the free radical concentration can be further improved. Thus, the reaction of the free radical polymerizable group is promoted, so the crosslinking density of the film based on the photocuring can be improved, thereby further improving the pencil hardness or chemical resistance. In addition, since the unreacted free radical polymerizable group can be suppressed from remaining in the cured film, the weather resistance can be further improved, and the outgoing gas during the electrode or wiring processing can be reduced. Furthermore, since the oxime ester group is a ketone oxime ester group, high transparency can also be maintained after light irradiation.

[0051]

[0052] In the general formula (1), m is 0 or 1. n is an integer of 2 or more. n is preferably 6 or less, more preferably 4 or less or 3 or less. 1 R represents a hydrogen atom, an alkyl group or a phenyl group, and from the viewpoint of reactivity, a methyl group which generates a methyl radical having little steric hindrance and high reactivity is most preferred. 2 represents an alkyl group, a cycloalkyl group or a cycloalkylalkyl group, and preferably has 1 to 7 carbon atoms from the viewpoint of solubility in a solvent. 1 and R 2 There are multiple R 1 Can be the same or different. 2 They may be the same or different. Ar represents an aromatic group. Ar may contain nitrogen, oxygen, sulfur, or a carbonyl group as disclosed in Patent Documents 3 and 4. Furthermore, Ar also includes the following structures and bonds between these structures, as well as groups formed by bonding other functional groups to these structures.

[0053] 9H-fluorene, 9H-carbazole, dibenzo[b,d]furan, dibenzo[b,d]thiophene, 9H-fluorene-9-one, 9,10-dihydroanthracene, 9H-thioxanthene, 9,10-dihydroacridine, 9H-xanthene-9,10H-one, 9H-thioxanthene-9-one, 9H-xanthene-9-one, acridine-9,10H-one, 10H-phene Oxazine, phenanthracene Phenoxathiin, 10H-phenothiazine, dibenzo-p-diphenylamine Oxanthrene, 5,10-dihydrophenazine, thianthrene, anthracene-9,10-dione.

[0054] 1H-Indene, 1H-Indole, 1-Benzofuran, 1-Benzothiophene, 1H-inden-1-one.

[0055] The absorption peak wavelength and absorbance of the photo-radical polymerization initiator can be obtained by the following method. First, the photo-radical polymerization initiator is diluted to a concentration of 0.001% by weight using propylene glycol methyl ether acetate. For the obtained dilution, the absorbance at a wavelength of 300nm to 400nm is measured using an ultraviolet-visible spectrophotometer UV-2600 (manufactured by Shimadzu Corporation (stock)). From the obtained absorbance spectrum, the absorption peak wavelength, the absorbance at a wavelength of 365nm, and the absorbance at a wavelength of 400nm can be obtained respectively.

[0056] From the viewpoint of sufficiently performing radical curing, further improving chemical resistance, further improving pencil hardness, and further suppressing generation of outgassing during electrode or wiring processing, the content of the (C) photoradical polymerization initiator in the negative photosensitive resin composition of the present invention is preferably 0.1% by weight or more, more preferably 1% by weight or more, and further preferably 4% by weight or more in the solid content. On the other hand, from the viewpoint of suppressing the residue of the (C) photoradical polymerization initiator and further improving chemical resistance, and suppressing the generation of excess radicals and further improving resolution, the content of the (C) photoradical polymerization initiator is preferably 20% by weight or less, more preferably 10% by weight or less, and further preferably 6% by weight or less in the solid content.

[0057] The negative photosensitive resin composition of the present invention may further contain a photoradical polymerization initiator other than the photoradical polymerization initiator represented by the general formula (1), for example, an alkylphenone-based photoradical polymerization initiator, an acylphosphine oxide-based photoradical polymerization initiator, an oxime ester-based photoradical polymerization initiator in one molecule, a benzophenone-based photoradical polymerization initiator, a thioxanthone-based photoradical polymerization initiator, an imidazole-based photoradical polymerization initiator, a benzothiazole-based photoradical polymerization initiator, a benzo Azole-based photoradical polymerization initiators, carbazole-based photoradical polymerization initiators, triazine-based photoradical polymerization initiators, benzoate-based photoradical polymerization initiators, phosphorus-based photoradical polymerization initiators, inorganic photoradical polymerization initiators such as titanate, etc. Two or more of these may be contained.

[0058] The negative photosensitive resin composition of the present invention may contain an adhesion improver such as a silane coupling agent. Examples of the silane coupling agent include silane coupling agents having a functional group such as a vinyl group, an epoxy group, a styryl group, a methacryloxy group, an acryloxy group, and an amino group.

[0059] Specifically, preferred are 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(2-methoxyethoxy)silane, N-(2-aminoethyl)-3-amino 3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, 3-mercaptopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, 3-isocyanatepropyltriethoxysilane, p-phenylenetrimethoxysilane, etc.

[0060] The negative photosensitive resin composition of the present invention may contain various curing agents, which can promote or facilitate the curing of the negative photosensitive resin composition. Examples of curing agents include nitrogen-containing organic substances, silicone resin curing agents, metal alkoxides, metal chelates, isocyanate compounds and polymers thereof, epoxy compounds and polymers thereof, methylolated melamine derivatives, methylolated urea derivatives, and the like. Two or more of these may also be contained. Among them, metal chelate compounds, methylolated melamine derivatives, and methylolated urea derivatives may be preferably used in terms of the stability of the curing agent, the processability of the obtained coating film, and the like.

[0061] (A) Since the curing of the siloxane resin is accelerated by acid, the negative photosensitive resin composition of the present invention may also contain a curing catalyst such as a thermal acid generator. Examples of the thermal acid generator include aromatic diazonium salts, sulfonium salts, diaryliodonium salts, and the like. Salts, triarylsulfonium salts, triarylselenium salts, etc. Salt compounds, sulfonate esters, halogen compounds, etc.

[0062] The negative photosensitive resin composition of the present invention may also contain a polymerization inhibitor. By containing a polymerization inhibitor, the storage stability and resolution of the negative photosensitive resin composition can be further improved. Examples of the polymerization inhibitor include phenol, catechol, resorcinol, hydroquinone, 4-tert-butylcatechol, 2,6-di(tert-butyl)-p-cresol, phenothiazine, and 4-methoxyphenol.

[0063] The content of the polymerization inhibitor in the negative photosensitive resin composition of the present invention is preferably 0.01% by mass or more, more preferably 0.05% by mass or more in the solid content. On the other hand, from the viewpoint of further improving the pencil hardness of the cured film, the content of the polymerization inhibitor is preferably 5% by mass or less, more preferably 1% by mass or less in the solid content.

[0064] The negative photosensitive resin composition of the present invention may contain an ultraviolet absorber as long as it does not hinder the effect of the present invention. By containing an ultraviolet absorber, the resolution of the negative photosensitive resin composition and the weather resistance of the cured film can be further improved. As the ultraviolet absorber, benzotriazole compounds, benzophenone compounds, and triazine compounds can be preferably used in terms of transparency and non-coloring properties.

[0065] Examples of the benzotriazole compound include 2-(2H-benzotriazol-2-yl)phenol, 2-(2H-benzotriazol-2-yl)-4,6-tert-amylphenol, 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol, 2(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol, 2-(2'-hydroxy-5'-methacryloyloxyethylphenyl)-2H-benzotriazole, and RUVA-93 (trade name, manufactured by Otsuka Chemical Co., Ltd.).

[0066] Examples of the benzophenone-based compound include 2-hydroxy-4-methoxybenzophenone.

[0067] Examples of the triazine compound include 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol and Tinuvin 477 (trade name, manufactured by BASF).

[0068] The content of the ultraviolet absorber in the negative photosensitive resin composition of the present invention is preferably 10 wt % or less, more preferably 5 wt % or less in the solid content from the viewpoint of improving adhesion to a substrate such as glass serving as a base of the cured film.

[0069] The negative photosensitive resin composition of the present invention may also contain a solvent. By containing a solvent, each component can be uniformly dissolved. As the solvent, for example, aliphatic hydrocarbons, carboxylates, ketones, ethers, alcohols, etc. can be listed. Two or more of these can also be contained. From the viewpoint of uniformly dissolving each component and improving the transparency of the obtained coating film, a compound having an alcoholic hydroxyl group and a cyclic compound having a carbonyl group are preferred.

[0070] Examples of the compound having an alcoholic hydroxyl group include acetol, 3-hydroxy-3-methyl-2-butanone, 4-hydroxy-3-methyl-2-butanone, 5-hydroxy-2-pentanone, 4-hydroxy-4-methyl-2-pentanone (diacetone alcohol), ethyl lactate, butyl lactate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, propylene glycol mono-tert-butyl ether, 3-methoxy-1-butanol, and 3-methyl-3-methoxy-1-butanol.

[0071] Specific examples of the cyclic compound having a carbonyl group include γ-butyrolactone, γ-valerolactone, δ-valerolactone, propylene carbonate, N-methylpyrrolidone, cyclohexanone, cycloheptanone, etc. Among these, γ-butyrolactone can be particularly preferably used.

[0072] Examples of the aliphatic hydrocarbon include xylene, ethylbenzene, and solvent naphtha.

[0073] Examples of the carboxylic acid ester include benzyl acetate, ethyl benzoate, γ-butyrolactone, methyl benzoate, diethyl malonate, 2-ethylhexyl acetate, 2-butoxyethyl acetate, 3-methoxy-3-methyl-butyl acetate, diethyl oxalate, ethyl acetoacetate, cyclohexyl acetate, 3-methoxy-butyl acetate, methyl acetoacetate, ethyl-3-ethoxypropionate, 2-ethylbutyl acetate, isopentyl propionate, propylene glycol monomethyl ether propionate, propylene glycol monoethyl ether acetate, ethyl acetate, butyl acetate, isopentyl acetate, amyl acetate, and propylene glycol monomethyl ether acetate.

[0074] Examples of the ketone include cyclopentanone and cyclohexanone.

[0075] Examples of the ether include aliphatic ethers such as propylene glycol derivatives such as propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol tert-butyl ether, and dipropylene glycol monomethyl ether.

[0076] The negative photosensitive resin composition of the present invention may also contain a surfactant. By containing a surfactant, the fluidity during coating can be improved. Examples of the surfactant include: fluorine-based surfactants; silicone-based surfactants; fluorine-containing thermally decomposable surfactants; polyether-modified siloxane-based surfactants; polyalkylene oxide-based surfactants; poly(meth)acrylate-based surfactants; anionic surfactants such as ammonium lauryl sulfate and triethanolamine polyoxyethylene alkyl ether sulfate; cationic surfactants such as stearylamine acetate and lauryl trimethylammonium chloride; lauryl dimethylamine oxide, lauryl carboxymethyl hydroxyethyl imidazole; Amphoteric surfactants such as betaine, nonionic surfactants such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, sorbitan monostearate, etc. Two or more of these may be contained.

[0077] Examples of commercially available fluorine-based surfactants include Megafac (registered trademark) F142D, Megafac (registered trademark) F172, Megafac (registered trademark) F173, Megafac (registered trademark) F183, Megafac (registered trademark) F445, Megafac (registered trademark) F470, Megafac (registered trademark) F475, Megafac (registered trademark) F477 (all manufactured by DIC Corporation), NBX-15, and FTX-218 (manufactured by Neos Corporation). Examples of commercially available silicone surfactants include BYK (registered trademark)-333, BYK-301, BYK-331, BYK-345, and BYK-307 (manufactured by BYK-Chemie Japan Co., Ltd.). Examples of commercially available fluorinated thermally decomposable surfactants include Megafac (registered trademark) DS-21 (manufactured by DIC Co., Ltd.). Examples of commercially available polyether-modified silicone surfactants include BYK (registered trademark)-345, BYK-346, BYK-347, BYK-348, and BYK-349 (all manufactured by Beck Chemical Industries, Ltd.), SILFACE (registered trademark) SAG002, SILFACE (registered trademark) SAG005, SILFACE (registered trademark) SAG503A, and SILFACE (registered trademark) SAG008 (all manufactured by Nissin Chemical Industries, Ltd.).

[0078] The negative photosensitive resin composition of the present invention may contain a dispersant. Examples of the dispersant include polyacrylic acid-based dispersants, polycarboxylic acid-based dispersants, phosphoric acid-based dispersants, and silicone-based dispersants.

[0079] The negative photosensitive resin composition of the present invention may contain a resin other than the (A) siloxane resin, and may contain, for example, a siloxane resin having no radical polymerizable group.

[0080] Next, the method for producing the negative photosensitive resin composition of the present invention is described. The method for producing the negative photosensitive resin composition of the present invention is generally a method of stirring and mixing (A) a siloxane resin, (B) a monomer having a radical polymerizable group, (C) a photoradical polymerization initiator, and other components as required.

[0081] The negative photosensitive resin composition of the present invention is cured to obtain a cured film. The method for producing the cured film preferably comprises the steps of applying the negative photosensitive resin composition of the present invention on a substrate, exposing the substrate to light, and curing the substrate at a temperature of 180° C. or less.

[0082] Next, a method for producing a cured film from the negative photosensitive resin composition of the present invention will be described with examples.

[0083] A negative photosensitive resin composition is applied on a substrate to obtain a coating. As the substrate, a glass substrate or a resin film can be cited. These substrates can also form ITO or electrodes or wiring containing metals such as copper and copper alloys on their surfaces. As coating methods, for example, spin coating using a spinner, spray coating, inkjet coating, die coating, roller coating, etc. can be cited. The film thickness of the coating can be appropriately selected according to the coating method, etc. Generally, the film thickness after drying is set to 0.1μm to 10μm.

[0084] The obtained coating film is dried to obtain a dried film. Examples of drying methods include heating drying, air drying, reduced pressure drying, infrared irradiation, and the like. Examples of heating drying devices include ovens, hot plates, and the like. The drying temperature is preferably 50° C. to 150° C., and the drying time is preferably 1 minute to several hours.

[0085] The obtained dried film is irradiated with actinic rays (exposure) through a mask having a desired pattern to obtain an exposed film. Examples of the actinic rays to be irradiated include ultraviolet rays, visible rays, electron beams, and X-rays. The negative photosensitive resin composition of the present invention is preferably irradiated with i-rays (365 nm) of a mercury lamp or light containing i-rays.

[0086] The obtained exposed film is developed using an alkaline developer, etc., and the unexposed portion is removed to obtain a pattern. Examples of the alkaline compound used in the alkaline developer include inorganic bases such as sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium silicate, sodium metasilicate, and ammonia water; primary amines such as ethylamine and n-propylamine; secondary amines such as diethylamine and di-n-propylamine; tertiary amines such as triethylamine and methyldiethylamine; tetraalkylammonium hydroxides such as tetramethylammonium hydroxide (TMAH), quaternary ammonium salts such as choline; alcohol amines such as triethanolamine, diethanolamine, monoethanolamine, dimethylaminoethanol, and diethylaminoethanol; organic bases such as cyclic amines such as pyrrole, piperidine, 1,8-diazabicyclo[5,4,0]-7-undecene, 1,5-diazabicyclo[4,3,0]-5-nonane, and morpholine.

[0087] The concentration of the alkaline compound in the alkaline developer is generally 0.01 wt% to 50 wt%, preferably 0.02 wt% to 1 wt%. In addition, in order to make the pattern shape after development better, 0.1 wt% to 5 wt% of a surfactant such as a nonionic surfactant may be added. Furthermore, when the developer is an alkaline aqueous solution, a water-soluble organic solvent such as ethanol, γ-butyrolactone, dimethylformamide, N-methyl-2-pyrrolidone, etc. may be added to the developer.

[0088] Examples of the developing method include an immersion method, a spray method, and a liquid coating method. The obtained pattern may be rinsed and cleaned using pure water or the like.

[0089] The obtained pattern is heat-treated (post-baked) to cure the pattern, thereby obtaining a patterned cured film. The heat treatment can be performed in air, nitrogen atmosphere, or vacuum. The heating temperature is preferably 80° C. to 180° C., and the heating time is preferably 0.25 to 5 hours. The heating temperature can be changed continuously or in stages.

[0090] When the cured film does not need to be patterned, it is also preferred to expose the entire surface of the dried film to light cure the cured film and then heat treat it. By light curing before heat treatment, rapid film shrinkage during heat treatment can be suppressed, thereby further improving the adhesion between the cured film and the substrate.

[0091] Next, the touch panel of the present invention is described. The touch panel of the present invention comprises a substrate, electrodes and / or wirings containing copper, and a cured film formed by curing the negative photosensitive resin composition of the present invention. For example, it is preferred that an X-axis electrode conduction wiring and a Y-axis electrode conduction wiring are provided on the substrate, and a transparent insulating film comprising the cured film is provided at the intersection of these wirings.

[0092] Examples of the substrate include a glass substrate and a resin film.

[0093] As electrodes and wiring, for example, thin films or laminated films of metals such as copper, copper alloys, gold, silver, aluminum, molybdenum, and molybdenum-niobium alloys can be cited. The negative photosensitive resin composition of the present invention can be cured at a low temperature of 150° C. or less. Therefore, it can be preferably used in combination with electrodes and / or wiring containing copper. The electrodes and wiring preferably have a pattern called a so-called metal grid in which the conductor wires are arranged in a mesh shape.

[0094] Next, the manufacturing method of the touch panel of the present invention is described by taking the touch panel having the above structure as an example. First, an electrode film containing copper is formed on a substrate. As a method for forming an electrode film, for example, physical methods such as vacuum evaporation, sputtering, ion plating, and ion beam evaporation can be listed; chemical vapor deposition method, etc. Next, a resist material is coated on the electrode film, and after pattern processing by photolithography technology, the electrode film is etched with an etching solution, and the resist is stripped with a stripping solution, thereby forming an X-axis electrode conduction wiring. Subsequently, a cured film is formed by the method at the intersection of the X-axis electrode conduction wiring and the Y-axis electrode conduction wiring formed thereafter, thereby forming a transparent insulating film. Thereafter, wiring connected to the IC driver and Y-axis electrode conduction wiring are formed in the same manner as the X-axis electrode conduction wiring. Finally, a cured film is formed by the method at a portion other than the portion connected to the IC driver at the end of the substrate, thereby forming a transparent protective film, so that a touch panel can be obtained.

[0095] The negative photosensitive resin composition of the present invention can be preferably used as various protective films such as a protective film for a touch panel or a protective film for metal wiring, an insulating film for a touch panel, a glass-reinforced resin layer, an insulating film for a thin film transistor (TFT), various insulating films such as an interlayer insulating film, various hard coating materials, a flattening film for TFT, an outer coating for a color filter, a passivation film, an anti-reflection film, an optical filter, an optical spacer for a color filter, and a microlens. Because it has negative photosensitivity, it can be preferably used for a flattening film, an insulating film, an anti-reflection film, an outer coating for a color filter, a column material, etc. for a liquid crystal or organic electroluminescent (EL) display. Among these, even if it is cured at a low temperature below 180°C, the chemical resistance is high, and the generation of external gas during electrode or wiring processing can be suppressed, so it can be preferably used as an insulating film, a protective film, and a glass-reinforced resin layer for a touch panel having electrodes and / or wiring containing copper.

[0096] Example

[0097] Hereinafter, the present invention will be described in more detail using Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0098] <Evaluation Method>

[0099] Absorbance

[0100] The photoradical polymerization initiator used in each example and comparative example was diluted to a concentration of 0.001% by mass using propylene glycol methyl ether acetate (hereinafter referred to as "PGMEA"). The absorbance at a wavelength of 300 nm to 400 nm was measured using an ultraviolet-visible spectrophotometer UV-2600 (manufactured by Shimadzu Corporation). From the absorbance spectrum obtained, the absorption peak wavelength, the absorbance at a wavelength of 365 nm, and the absorbance at a wavelength of 400 nm were respectively obtained.

[0101] "Double bond equivalent"

[0102] The siloxane resin obtained by Synthesis Examples 1 and 2 was measured for iodine value by Wijs method using a potentiometric automatic titrator (AT-510; manufactured by Kyoto Electronics Co., Ltd.), an ICl solution (a mixed solution of ICl3=7.9 g, I2=8.9 g, and AcOH (acetic acid)=1,000 mL) as an iodine supply source, a 100 g / L KI aqueous solution as an aqueous solution for capturing unreacted iodine, and a 0.1 mol / L Na2S2O3 aqueous solution as a titration reagent, in accordance with the method described in "Item 6 Iodine Value" of Japanese Industrial Standards (JIS) K0070:1992 "Test methods for acid value, saponification value, ester value, iodine value, hydroxyl value, and unsaponifiable matter of chemicals". The double bond equivalent (in g / mol) was calculated from the measured iodine value (in gI / 100 g).

[0103] "Acid Value"

[0104] For the acrylic resin obtained by Synthesis Example 4 and the cardo-based resin obtained by Synthesis Example 5, a potentiometric automatic titrator (AT-510; manufactured by Kyoto Electronics Industries, Ltd.) was used, a 0.1 mol / L NaOH / ethanol solution was used as a titration reagent, and xylene / N,N-dimethylformamide (DMF) = 1 / 1 (mass ratio) was used as a titration solvent. The acid value (unit: mgKOH / g) was determined by potentiometric titration based on "JIS K2501 (2003)".

[0105] "Chemical resistance"

[0106] A substrate was prepared by sequentially stacking molybdenum-niobium / copper / molybdenum-niobium on an alkali-free glass substrate (glass thickness 0.55 mm). Hereinafter, it is referred to as a "metal laminated substrate". The respective film thicknesses of the laminated molybdenum-niobium / copper / molybdenum-niobium are 20 nm, 300 nm, and 20 nm. On the metal laminated substrate, a negative photosensitive resin composition obtained by each embodiment and comparative example was spin-coated using a spin coater (MS-A150 manufactured by Mikasa Co., Ltd.). The metal laminated substrate coated with the negative photosensitive resin composition was pre-baked at 90°C for 2 minutes using a heating plate (HHP-230SQ manufactured by ASONE Co., Ltd.) to produce a pre-baked film with a film thickness of 2.3 μm. A mask aligner (LA-610 manufactured by San-Yeung Electric Co., Ltd.) was used with an ultra-high pressure mercury lamp as the light source and an exposure dose of 100 mJ / cm 2 (i-ray conversion), the obtained pre-baked film was exposed. Thereafter, an automatic developing device (AD-1200 manufactured by Takizawa Sangyo Co., Ltd.) was used to perform shower development for 60 seconds using a 0.5 wt% potassium hydroxide aqueous solution (manufactured by Mitsubishi Gas Chemical Co., Ltd.), followed by rinsing with water for 30 seconds. Finally, an oven (DHS-42 manufactured by Espec Co., Ltd.) was used to cure at 130°C in air for 30 minutes to produce a cured film with a film thickness of 2.0 μm. The obtained cured film was immersed in "hydrogen peroxide water (30%) (trade name)" (manufactured by Fuji Film and Kou Jun Pharmaceutical Co., Ltd.) as a metal etching solution at 30°C for 2 minutes, and then the metal under the cured film was visually observed for discoloration. If no discoloration is confirmed, an additional immersion is performed for 3 minutes (a total of 5 minutes), and the metal is visually observed for discoloration. If no discoloration is confirmed, an additional immersion is performed for 2 minutes (a total of 7 minutes), and the metal is visually observed for discoloration. If no discoloration is confirmed, an additional immersion is performed for 3 minutes (a total of 10 minutes), and the metal is visually observed for discoloration. According to the relationship between the immersion time and the discoloration, the chemical resistance is evaluated according to the following criteria. In addition, when the black color derived from the molybdenum-niobium alloy layer before the test changes to the red color derived from the copper layer due to the corrosion of the molybdenum-niobium alloy after the test, it is judged to be discolored.

[0107] A: After 10 minutes of testing, no discoloration was observed on the metal under the cured film.

[0108] B: After 10 minutes of testing, the metal under the cured film changed color.

[0109] C: After 7 minutes of testing, the metal under the cured film changed color.

[0110] D: After 5 minutes of testing, the metal under the cured film changed color.

[0111] E: After 2 minutes of testing, the metal under the cured film changed color.

[0112] "Pencil Hardness"

[0113] On an alkali-free glass substrate (glass thickness 0.55 mm), a cured film having a film thickness of 2.0 μm was prepared using the negative photosensitive resin composition obtained in each Example and Comparative Example in the same manner as described in the evaluation of "chemical resistance". The pencil hardness of the obtained cured film was measured in accordance with JIS "K5600-5-4 (established on April 20, 1999)".

[0114] "Resolution"

[0115] On an alkali-free glass substrate (glass thickness 0.55 mm), a negative photosensitive resin composition obtained by each embodiment and comparative example was spin-coated using a spin coater (MS-A150 manufactured by Mikasa Co., Ltd.). The alkali-free glass substrate coated with the negative photosensitive resin composition was pre-baked for 2 minutes at 90°C using a hot plate (HHP-230SQ manufactured by ASONE Co., Ltd.) to produce a pre-baked film with a film thickness of 2.3 μm. A mask aligner (LA-610 manufactured by Sanei Electric Co., Ltd.) was used, with an ultra-high pressure mercury lamp as the light source, and a mask with a 1-to-1 line and space (L&S) pattern of 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, and 50 μm widths, and a mask gap (mask gap) of 200 μm was used to expose the obtained pre-baked film. Thereafter, shower development was performed for 60 seconds using an automatic developer (AD-1200 manufactured by Takizawa Sangyo Co., Ltd.) using a 0.5 wt% potassium hydroxide aqueous solution (manufactured by Mitsubishi Gas Chemical Co., Ltd.), followed by rinsing with water for 30 seconds. The minimum pattern size after development was measured and taken as the resolution.

[0116] "Weather resistance"

[0117] On an alkali-free glass substrate (glass thickness 0.55 mm), a negative photosensitive resin composition obtained by each embodiment and comparative example was used to prepare a cured film with a film thickness of 2.0 μm in the same manner as described in the evaluation of "chemical resistance". The obtained cured film was subjected to a weathering tester (trade name "Q-Sun", manufactured by Q-Lab) at 0.55 W / m 2 The simulated sunlight was irradiated for 300 hours under the conditions of 340 nm and 63 ° C. The UV-visible spectrophotometer UV-2600 (manufactured by Shimadzu Corporation) was used to calculate Δb* from the b* values ​​before and after the test to evaluate the weather resistance. Based on Δb*, the weather resistance was evaluated according to the following criteria. A or above was considered acceptable.

[0118] A: Δb* is less than 1.

[0119] B: Δb* is 1 or more and less than 3.

[0120] C: Δb* is 3 or more.

[0121] "External gas"

[0122] On a silicon wafer substrate, a cured film with a film thickness of 2.0 μm was prepared using the negative photosensitive resin composition obtained by each embodiment and comparative example in the same manner as described in the evaluation of "chemical resistance". The obtained cured film was heated from room temperature to 400°C at a heating rate of 10°C / min in a helium gas environment of 50 mL / min, and the amount of gas generated from the cured film was measured using a mass spectrometer (MS) device (GC / MS QP2010 (8), manufactured by Shimadzu Corporation). Based on the amount of gas generated, the gas generation weight was calculated according to (generation weight of each gas / sample weight) × 10 6 The concentration was calculated by the calculation formula, and the released gas was evaluated according to the following criteria. B or above was considered acceptable.

[0123] A: less than 250 wtppm.

[0124] B: 250 wtppm or more and less than 500 wtppm.

[0125] C: 500 wtppm or more and less than 750 wtppm.

[0126] D: 750 wtppm or more and less than 1000 wtppm.

[0127] E: 1000wtppm or more.

[0128] [Synthesis example 1]

[0129] In a 500 mL three-necked flask, 40.86 g (0.30 mol) of methyltrimethoxysilane, 59.49 g (0.30 mol) of phenyltrimethoxysilane, 20.83 g (0.10 mol) of tetraethoxysilane, 23.63 g (0.10 mol) of 3-glycidyloxypropyltrimethoxysilane, 49.68 g (0.20 mol) of 3-methacryloxypropyltrimethoxysilane, and 220.99 g of PGMEA were placed. The flask was immersed in a 40° C. oil bath, and while stirring the contents, a nitric acid aqueous solution obtained by dissolving 3.1 g (0.1 parts by weight relative to the charged monomer) of 1 mol / L nitric acid in 55.8 g of water was added using a dropping funnel over 10 minutes. After stirring at 40° C. for 1 hour, the oil bath temperature was set to 70° C. and stirred for 1 hour, and the oil bath was further heated to 115° C. over 30 minutes. One hour after the start of the temperature increase, the internal temperature of the solution reached 100°C, and then heated and stirred at an internal temperature of 100°C to 120°C for 2 hours. A total of 120 g of methanol and water were distilled as by-products in the reaction. PGMEA was added to the obtained PGMEA solution of siloxane resin in such a manner that the polymer concentration became 30% by weight to obtain a siloxane resin solution (PS-1). In addition, the weight average molecular weight (hereinafter, "Mw") of the obtained siloxane resin was measured by GPC, and the result was 2,000 (polystyrene conversion). Moreover, the double bond equivalent measured by the method described is 630 g / mol.

[0130] [Synthesis example 2]

[0131] In a 500 mL three-necked flask, 40.86 g (0.30 mol) of methyltrimethoxysilane, 59.49 g (0.30 mol) of phenyltrimethoxysilane, 20.83 g (0.10 mol) of tetraethoxysilane, 23.63 g (0.10 mol) of 3-glycidyloxypropyltrimethoxysilane, 46.86 g (0.20 mol) of 3-acryloxypropyltrimethoxysilane, and 216.98 g of PGMEA were placed. The flask was immersed in a 40° C. oil bath, and while stirring the contents, a nitric acid aqueous solution obtained by dissolving 3.0 g (0.1 parts by weight relative to the charged monomer) of 1 mol / L nitric acid in 55.8 g of water was added using a dropping funnel over 10 minutes. After stirring at 40° C. for 1 hour, the oil bath temperature was set to 70° C. and stirred for 1 hour, and the oil bath temperature was further raised to 115° C. over 30 minutes. One hour after the start of the temperature rise, the internal temperature of the solution reached 100°C, and then heated and stirred at an internal temperature of 100°C to 120°C for 2 hours. A total of 120 g of methanol and water were distilled as by-products in the reaction. PGMEA was added to the obtained PGMEA solution of siloxane resin in such a way that the polymer concentration became 30% by weight to obtain a siloxane resin solution (PS-2). In addition, the Mw of the obtained siloxane resin was measured by GPC, and the result was 2,000 (polystyrene conversion). Moreover, the double bond equivalent measured by the method was 610 g / mol.

[0132] [Synthesis example 3]

[0133] In a 500 mL three-necked flask, 47.67 g (0.35 mol) of methyltrimethoxysilane, 69.41 g (0.35 mol) of phenyltrimethoxysilane, 31.25 g (0.15 mol) of tetraethoxysilane, 35.45 g (0.15 mol) of 3-glycidyloxypropyltrimethoxysilane, and 204.83 g of PGMEA were placed. The flask was immersed in a 40°C oil bath, and while stirring the contents, a nitric acid aqueous solution obtained by dissolving 2.9 g (0.1 weight part relative to the charged monomer) of 1 mol / L nitric acid in 56.7 g of water was added using a dropping funnel over 10 minutes. After stirring at 40°C for 1 hour, the oil bath temperature was set to 70°C and stirred for 1 hour, and the oil bath was further heated to 115°C over 30 minutes. One hour after the start of the heating, the internal temperature of the solution reached 100°C, and then heated and stirred at an internal temperature of 100°C to 120°C for 2 hours. In the reaction, 120 g of methanol and water were distilled as byproducts. PGMEA was added to the obtained siloxane resin PGMEA solution so that the polymer concentration became 30% by weight to obtain a siloxane resin solution (PS-3). In addition, the Mw of the obtained siloxane resin was measured by GPC, and the result was 2,000 (polystyrene conversion).

[0134] [Synthesis example 4]

[0135] 3 g of 2,2'-azobis(isobutyronitrile) and 50 g of PGMEA were placed in a 500 ml flask. Then, 30 g of methacrylic acid, 35 g of benzyl methacrylate, and tricyclo[5.2.1.0 2,6 ] 35g of decane-8-yl methacrylate was added, stirred at room temperature for a while, and after nitrogen substitution in the flask, heated and stirred at an internal temperature of 70°C for 5 hours. Secondly, 15g of glycidyl methacrylate, 1g of dimethylbenzylamine, 0.2g of p-methoxyphenol, and 100g of PGMEA were added to the obtained solution, and heated and stirred at 90°C for 4 hours. PGMEA was added to the obtained PGMEA solution of acrylic resin in such a way that the solid content concentration became 30% by weight to obtain an acrylic resin solution (PA-1). The Mw of the obtained acrylic resin was measured by GPC, and the result was 10,000. Moreover, the acid value of the obtained acrylic resin was 118mgKOH / g.

[0136] [Synthesis Example 5]

[0137] In a 500 ml flask, 92.2 g of 9,9-bis(4-glycidyloxyphenyl)fluorene ("PG-100 (trade name)" manufactured by Osaka Gaschem Co., Ltd.), 14.4 g of acrylic acid, 0.32 g of tetrabutylammonium acetate, 0.26 g of 2,6-di-tert-butylcatechol and 110 g of PGMEA were placed, and stirred at an internal temperature of 120°C for 9 hours. Next, 34.8 g of biphenyltetracarboxylic dianhydride and 50 g of PGMEA were added, and the mixture was further stirred at 120°C for 5 hours. PGMEA was added to the obtained PGMEA solution of cardo resin in such a manner that the solid content concentration became 30% by weight, and a cardo resin solution (PA-2) was obtained. The Mw of the obtained cardo resin was measured by GPC, and the result was 5,700. Moreover, the acid value of the obtained cardo resin was 100 mgKOH / g.

[0138] [Example 1]

[0139] Under a yellow light, 0.71 g of "TR-PBG-345 (trade name)" (manufactured by TRONLY) and 0.014 g of 4-tert-butylcatechol (hereinafter referred to as TBC) were dissolved in 62.12 g of PGMEA, and 0.18 g of "Tinuvin (registered trademark) 477 (trade name)" (manufactured by BASF) and "BYK (registered trademark)-333 (trade name)" (manufactured by BYK-Chemie Japan Co., Ltd.) as a silicone surfactant were added to PGMEA. 0.30 g of a 10 mass % solution (equivalent to a concentration of 300 ppm), 2.82 g of dipentaerythritol hexaacrylate ("Kayarad" (registered trademark) DPHA (trade name) manufactured by Nippon Kayaku Co., Ltd.), 5.64 g of a PGMEA 50 mass % solution of 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene "OGSOL" (registered trademark) EA-0250P (trade name) (manufactured by Osaka Gas Chemika Co., Ltd.), and 28.22 g of the siloxane resin solution (PS-1) obtained in Synthesis Example 1 were stirred. Subsequently, the mixture was filtered using a 0.20 μm filter to prepare a negative photosensitive resin composition C-1 having a solid content concentration of 15 wt %. A cured film was prepared for the obtained negative photosensitive resin composition C-1 in the same manner as the evaluation method described in the above-mentioned “chemical resistance” or “resolution”, and each item was evaluated by the above-mentioned method.

[0140] [Example 2]

[0141] A negative photosensitive resin composition C-2 was prepared in the same manner as in Example 1 except that pentaerythritol tetraacrylate ("Light Acrylate" (registered trademark) PE-4A (trade name) manufactured by Kyoeisha Chemical Co., Ltd.) was added instead of ("Kayarad" DPHA (trade name)). Using the obtained negative photosensitive resin composition C-2, evaluation was performed in the same manner as in Example 1.

[0142] [Example 3]

[0143] Under a yellow light, 0.71 g of "TR-PBG-345 (trade name)" and 0.014 g of TBC were dissolved in 64.79 g of PGMEA, and 0.30 g of a 10 wt% solution of "BYK"-333 (trade name)" in PGMEA, 2.85 g of "Kayarad" DPHA (trade name), 2.85 g of dimethylol-tricyclodecane diacrylate ("Light Acrylate" DCP-A (trade name) manufactured by Kyoeisha Chemical Co., Ltd.), and 28.49 g of the siloxane resin solution (PS-1) obtained in Synthesis Example 1 were added and stirred. Subsequently, the mixture was filtered using a 0.20 μm filter to prepare a negative photosensitive resin composition C-3 having a solid content concentration of 15% by mass. Evaluation was performed in the same manner as in Example 1 using the obtained negative photosensitive resin composition C-3.

[0144] [Example 4]

[0145] Under a yellow light, 0.43 g of "TR-PBG-345 (trade name)" and 0.014 g of TBC were dissolved in 61.69 g of PGMEA, and 0.18 g of "Tinuvin" 477 (trade name), 0.30 g of a 10 wt% solution of "BYK"-333 (trade name)", 2.88 g of "Kayarad" DPHA (trade name), 5.75 g of "OGSOL" EA-0250P (trade name), and 28.76 g of the siloxane resin solution (PS-1) obtained in Synthesis Example 1 were added and stirred. Subsequently, the mixture was filtered using a 0.20 μm filter to prepare a negative photosensitive resin composition C-4 having a solid content concentration of 15% by mass. Evaluation was performed in the same manner as in Example 1 using the obtained negative photosensitive resin composition C-4.

[0146] [Example 5]

[0147] Under a yellow light, 1.10 g of "TR-PBG-345 (trade name)" and 0.014 g of TBC were dissolved in 62.74 g of PGMEA, and 0.17 g of "Tinuvin" 477 (trade name), 0.30 g of a 10 mass % solution of "BYK"-333 (trade name)", 2.74 g of "Kayarad" DPHA (trade name), 5.49 g of "OGSOL" EA-0250P (trade name), and 27.44 g of the siloxane resin solution (PS-1) obtained in Synthesis Example 1 were added and stirred. Subsequently, the mixture was filtered with a 0.20 μm filter to prepare a negative photosensitive resin composition C-5 having a solid content concentration of 15 wt%. Evaluation was performed in the same manner as in Example 1 using the obtained negative photosensitive resin composition C-5.

[0148] [Example 6]

[0149] Under a yellow light, 0.71 g of "TR-PBG-345 (trade name)" and 0.014 g of TBC were dissolved in 63.39 g of PGMEA, and 0.18 g of "Tinuvin" 477 (trade name), 0.30 g of a 10 wt% solution of "BYK"-333 (trade name) in PGMEA, 4.09 g of "Kayarad" DPHA (trade name), 3.10 g of "OGSOL" EA-0250P (trade name), and 28.22 g of the siloxane resin solution (PS-1) obtained in Synthesis Example 1 were added and stirred. Subsequently, the mixture was filtered using a 0.20 μm filter to prepare a negative photosensitive resin composition C-6 having a solid content concentration of 15 wt%. Evaluation was performed in the same manner as in Example 1 using the obtained negative photosensitive resin composition C-6.

[0150] [Example 7]

[0151] Under a yellow light, 0.71 g of "TR-PBG-345 (trade name)" and 0.014 g of TBC were dissolved in 60.71 g of PGMEA, and 0.18 g of "Tinuvin" 477 (trade name), 0.30 g of a 10 wt% solution of "BYK"-333 (trade name) in PGMEA, 1.41 g of "Kayarad" DPHA (trade name), 8.47 g of "OGSOL" EA-0250P (trade name), and 28.22 g of the siloxane resin solution (PS-1) obtained in Synthesis Example 1 were added and stirred. Subsequently, the mixture was filtered using a 0.20 μm filter to prepare a negative photosensitive resin composition C-7 having a solid content concentration of 15 wt%. Evaluation was performed in the same manner as in Example 1 using the obtained negative photosensitive resin composition C-7.

[0152] [Example 8]

[0153] Under a yellow light, 0.71 g of "TR-PBG-345 (trade name)" and 0.014 g of TBC were dissolved in 64.71 g of PGMEA, and 0.18 g of "Tinuvin" 477 (trade name), 0.30 g of a 10 wt% solution of "BYK"-333 (trade name) in PGMEA, 3.53 g of "Kayarad" DPHA (trade name), 7.05 g of "OGSOL" EA-0250P (trade name), and 23.52 g of the siloxane resin solution (PS-1) obtained in Synthesis Example 1 were added and stirred. Subsequently, the mixture was filtered using a 0.20 μm filter to prepare a negative photosensitive resin composition C-8 having a solid content concentration of 15 wt%. Evaluation was performed in the same manner as in Example 1 using the obtained negative photosensitive resin composition C-8.

[0154] [Example 9]

[0155] Under a yellow light, 0.71 g of "TR-PBG-345 (trade name)" and 0.014 g of TBC were dissolved in 59.53 g of PGMEA, and 0.18 g of "Tinuvin" 477 (trade name), 0.30 g of a 10 wt% solution of "BYK"-333 (trade name)", 2.11 g of "Kayarad" DPHA (trade name), 4.23 g of "OGSOL" EA-0250P (trade name), and 32.92 g of the siloxane resin solution (PS-1) obtained in Synthesis Example 1 were added and stirred. Subsequently, the mixture was filtered using a 0.20 μm filter to prepare a negative photosensitive resin composition C-9 having a solid content concentration of 15 wt%. Evaluation was performed in the same manner as in Example 1 using the obtained negative photosensitive resin composition C-9.

[0156] [Example 10]

[0157] A negative photosensitive resin composition C-10 having a solid content concentration of 15 wt % was prepared in the same manner as in Example 1, except that the siloxane resin solution (PS-2) obtained in Synthesis Example 2 was added instead of the siloxane resin solution (PS-1) obtained in Synthesis Example 1. The obtained negative photosensitive resin composition C-10 was used and evaluated in the same manner as in Example 1.

[0158] [Example 11]

[0159] A negative photosensitive resin composition C-11 having a solid content concentration of 15 wt % was prepared in the same manner as in Example 3 except that the siloxane resin solution (PS-2) obtained in Synthesis Example 2 was added instead of the siloxane resin solution (PS-1) obtained in Synthesis Example 1. The obtained negative photosensitive resin composition C-11 was evaluated in the same manner as in Example 1.

[0160] [Example 12]

[0161] A negative photosensitive resin composition C-12 having a solid content concentration of 15 wt % was prepared in the same manner as in Example 1 except that "TR-PBG-331 (trade name)" (manufactured by TRONLY) was added instead of "TR-PBG-345 (trade name)". The obtained negative photosensitive resin composition C-12 was used and evaluated in the same manner as in Example 1.

[0162] [Example 13]

[0163] A negative photosensitive resin composition C-12 having a solid content concentration of 15 wt % was prepared in the same manner as in Example 1 except that "Irgacure" (registered trademark) OXE03 (trade name) (manufactured by BASF) was added instead of "TR-PBG-345 (trade name)". The obtained negative photosensitive resin composition C-12 was used and evaluated in the same manner as in Example 1.

[0164] [Comparative Example 1]

[0165] A negative photosensitive resin composition C-14 was prepared in the same manner as in Example 1 except that "Irgacure" (registered trademark) OXE01 (trade name) (manufactured by BASF) was added instead of "TR-PBG-345 (trade name)". The negative photosensitive resin composition C-14 obtained was evaluated in the same manner as in Example 1.

[0166] [Comparative Example 2]

[0167] A negative photosensitive resin composition C-15 was prepared in the same manner as in Example 1 except that "Irgacure" OXE02 (trade name) (manufactured by BASF) was added instead of "TR-PBG-345 (trade name)". The negative photosensitive resin composition C-15 obtained was evaluated in the same manner as in Example 1.

[0168] [Comparative Example 3]

[0169] A negative photosensitive resin composition C-16 having a solid content concentration of 15 wt % was prepared in the same manner as in Example 1 except that "ADEKA ARKLS" (registered trademark) NCI-730 (trade name) (manufactured by ADEKA Co., Ltd.) was added instead of "TR-PBG-345 (trade name)". The obtained negative photosensitive resin composition C-16 was used and evaluated in the same manner as in Example 1.

[0170] [Comparative Example 4]

[0171] A negative photosensitive resin composition C-17 having a solid content concentration of 15 wt % was prepared in the same manner as in Example 1 except that "ADEKA ARKLS" (registered trademark) NCI-930 (trade name) (manufactured by ADEKA Co., Ltd.) was added instead of "TR-PBG-345 (trade name)". The obtained negative photosensitive resin composition C-17 was used and evaluated in the same manner as in Example 1.

[0172] [Comparative Example 5]

[0173] A negative photosensitive resin composition C-18 having a solid content concentration of 15 wt % was prepared in the same manner as in Example 1 except that "ADEKA ARKLS" (registered trademark) N-1919 (trade name) (manufactured by ADEKA Co., Ltd.) was added instead of "TR-PBG-345 (trade name)". The obtained negative photosensitive resin composition C-18 was used and evaluated in the same manner as in Example 1.

[0174] [Comparative Example 6]

[0175] A negative photosensitive resin composition C-19 was prepared in the same manner as in Example 1 except that "ADEKA ARKLS" (registered trademark) NCI-831 (trade name) (manufactured by ADEKA Co., Ltd.) was added instead of "TR-PBG-345 (trade name)". The negative photosensitive resin composition C-19 obtained was evaluated in the same manner as in Example 1.

[0176] [Comparative Example 7]

[0177] A negative photosensitive resin composition C-20 was prepared in the same manner as in Example 1 except that "Omnirad" (registered trademark) 819 (trade name) (manufactured by IGM) was added instead of "TR-PBG-345 (trade name)". The negative photosensitive resin composition C-20 obtained was evaluated in the same manner as in Example 1.

[0178] [Comparative Example 8]

[0179] A negative photosensitive resin composition C-21 was prepared in the same manner as in Example 1 except that the siloxane resin solution (PS-3) obtained in Synthesis Example 3 was added instead of the siloxane resin solution (PS-1) obtained in Synthesis Example 1. The negative photosensitive resin composition C-21 obtained was evaluated in the same manner as in Example 1.

[0180] [Comparative Example 9]

[0181] A negative photosensitive resin composition C-22 was prepared in the same manner as in Example 1 except that the acrylic resin solution (PA-1) obtained in Synthesis Example 4 was added instead of the siloxane resin solution (PS-1) obtained in Synthesis Example 1. The negative photosensitive resin composition C-22 obtained was evaluated in the same manner as in Example 1.

[0182] [Comparative Example 10]

[0183] Under a yellow light, 0.75 g of "Irgacure" OXE01 (trade name) (manufactured by BASF), 0.015 g of TBC, and 1.20 g of a multifunctional epoxy compound "TECHMORE" (registered trademark) VG-3101L (trade name) (manufactured by Printec Co., Ltd.) were dissolved in 69.03 g of PGMEA, and PGMEA of "BYK-333 (trade name)" was added. 0.30 g of a 10 wt% solution, 4.49 g of "Kayarad" DPHA (trade name), 1.79 g of 4-hydroxybutyl acrylate glycidyl ether ("4HBAGE (trade name)" manufactured by Nippon Chemical Industry Co., Ltd.), and 22.43 g of the cardo resin solution (PA-2) obtained in Synthesis Example 5 were stirred. Then, the mixture was filtered using a 0.20 μm filter to prepare a negative photosensitive resin composition C-23 having a solid content concentration of 15 wt%. The obtained negative photosensitive resin composition C-23 was evaluated in the same manner as in Example 1.

[0184] Table 1 shows the composition (excluding TBC, surfactant, and solvent) of the negative photosensitive resin composition in each Example and Comparative Example, and Table 2 shows the evaluation results.

[0185]

[0186]

[0187]

Table 2

[0188]

[0189] It is known that the negative photosensitive resin composition prepared in the examples has high resolution, and even when cured at 130° C., can form a cured film having high pencil hardness, excellent chemical resistance and weather resistance, and capable of suppressing the generation of outgassing during electrode or wiring processing.

[0190] Industrial Availability

[0191] The negative photosensitive resin composition of the present invention has high resolution, and even when cured at a low temperature of 150° C. or lower, a cured film having high pencil hardness, excellent chemical resistance and weather resistance, and capable of suppressing the generation of outgassing during electrode or wiring processing can be obtained. Therefore, the negative photosensitive resin composition of the present invention can be preferably used as an insulating film, a protective film, or a glass-reinforced resin layer for a touch panel having electrodes and / or wiring containing copper.

Claims

1. A negative photosensitive resin composition comprising: (A) a siloxane resin having a free radical polymerizable group; (B) a monomer having a free radical polymerizable group; and (C) a photoradical polymerization initiator having a light absorption peak in the wavelength range of 350 nm to 370 nm, wherein the absorbance at a wavelength of 400 nm is 10% or less of the absorbance at a wavelength of 365 nm, The (C) photoradical polymerization initiator is represented by the following general formula (1), and contains two or more ketoxime ester groups in one molecule. In the general formula (1), m is 0 or 1; n is an integer greater than 2; R 1 represents a hydrogen atom, an alkyl group or a phenyl group, R 2 represents an alkyl group, a cycloalkyl group or a cycloalkylalkyl group; Ar is an aromatic group. 2 . The negative photosensitive resin composition according to claim 1 , wherein the (B) monomer having a radical polymerizable group comprises (B1) a polyfunctional monomer and (B2) a monomer having an aromatic ring and / or an alicyclic carbon ring. 3 . The negative photosensitive resin composition according to claim 2 , comprising 10 wt % or more of the (B2) monomer having an aromatic ring and / or an alicyclic carbocyclic ring in a solid content.

4. A method for producing a cured film, comprising: applying the negative photosensitive resin composition according to any one of claims 1 to 3 on a substrate, exposing the composition to light, and curing the exposed composition at a temperature of 150°C or less. 5 . A touch panel comprising a substrate, electrodes and / or wirings containing copper, and a cured film formed by curing the negative photosensitive resin composition according to claim 1 .