Sulfide solid electrolyte
By heating the sulfide electrolyte raw material and lithium halide hydrate under vacuum, a sulfide solid electrolyte with specific diffraction peaks is formed, which solves the problem of hydrogen sulfide generation in the water reaction of sulfide solid electrolyte and improves lithium-ion conductivity and battery performance.
Patent Information
- Application Number
- CN202080017561.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-11
- Filing Date
- 2020-09-03
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-09-03
AI Technical Summary
Existing sulfide solid electrolytes are prone to producing hydrogen sulfide when they react with moisture in the atmosphere, which affects their performance and safety.
By heating the sulfide electrolyte raw material with lithium halide hydrate under vacuum, a sulfide solid electrolyte with specific diffraction peaks is formed, which suppresses the generation of hydrogen sulfide and optimizes its composition and structure to improve lithium-ion conductivity.
It effectively suppressed the generation of hydrogen sulfide, reduced the reaction resistance between active materials, and improved the discharge capacity and safety of solid-state batteries.
Smart Images

Figure CN113508484B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a sulfide solid electrolyte. In addition, the present invention relates to an electrode mixture and a solid battery having the solid electrolyte. Furthermore, the present invention relates to a method for producing the solid electrolyte. Background Art
[0002] Solid batteries do not use flammable organic solvents, so safety devices can be simplified, and not only can manufacturing costs and productivity be excellent, but also have the characteristics of being stacked in series in a unit cell to achieve high voltage. Sulfide solid electrolytes have been studied as one of the solid electrolytes for solid batteries. For example, Patent Document 1 discloses a sulfide solid electrolyte compound for lithium-ion batteries, which contains a cubic argyrodite-type crystal layer, and has a composition formula of: Li 7-x+y P S6-x Cl x+y In the above composition formula, x and y satisfy 0.05≤y≤0.9 and -3.0x+1.8≤y≤-3.0x+5.7.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent document 1: US2017 / 352916A1 Summary of the invention
[0006] It is known that sulfide solid electrolytes easily react with moisture in the atmosphere to generate hydrogen sulfide. The sulfide solid electrolyte described in Patent Document 1 above can satisfy lithium ion conductivity, but there is room for improvement in preventing the generation of hydrogen sulfide.
[0007] Therefore, an object of the present invention is to improve a sulfide solid electrolyte, and more specifically, to provide a sulfide solid electrolyte capable of suppressing the generation of hydrogen sulfide.
[0008] The present invention provides a sulfide solid electrolyte having a peak A at 2θ=20.7°±0.5° in an X-ray diffraction pattern obtained by X-ray diffraction measurement using CuKα1 rays.
[0009] In addition, the present invention provides a method for producing a sulfide solid electrolyte, which is a preferred method for producing the above-mentioned sulfide solid electrolyte, comprising: a mixing step of mixing a sulfide electrolyte raw material and a lithium halide hydrate to obtain a mixture; and a heating step of heating the mixture to 80° C. or higher under vacuum. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1It is a graph showing the results of X-ray diffraction measurement of the sulfide solid electrolytes obtained in Examples and Comparative Examples. DETAILED DESCRIPTION
[0011] The present invention is described below based on a preferred embodiment of the present invention. The present invention relates to a sulfide solid electrolyte. The sulfide solid electrolyte of the present invention (hereinafter also referred to as "solid electrolyte") has lithium ion conductivity. The degree of lithium ion conductivity of the solid electrolyte of the present invention will be described later.
[0012] The solid electrolyte of the present invention contains sulfur as its constituent element. The lithium ion conductivity of the solid electrolyte of the present invention is caused by the sulfide solid electrolyte. As for the sulfide solid electrolyte with lithium ion conductivity, various sulfide solid electrolytes are known in the technical field, and in the present invention, these various sulfide solid electrolytes can be used without particular restrictions. In particular, from the aspect of reducing the reaction resistance between the active material, it is advantageous for the sulfide solid electrolyte to contain lithium (Li) element, phosphorus (P) element, sulfur (S) element and halogen (X) element. As the halogen element, it is advantageous to use at least one of chlorine, bromine and iodine from the aspect of further reducing the reaction resistance with the active material. The sulfide solid electrolyte may contain elements other than lithium, phosphorus, sulfur and halogen elements. For example, a part of the lithium element can be replaced by other alkali metal elements, or a part of the phosphorus element can be replaced by other phosphorus elements, or a part of the sulfur element can be replaced by other sulfide elements.
[0013] When the solid electrolyte of the present invention is subjected to X-ray diffraction (hereinafter also referred to as "XRD") measurement using CuKα1 rays, a diffraction peak A is observed in the range of 2θ=20.7°±0.5° in the XRD diffraction pattern. As for the solid electrolyte in which the diffraction peak A is observed, the inventors' research results show that the generation of hydrogen sulfide can be further suppressed compared with the existing solid electrolyte.
[0014] From the viewpoint of making the above advantageous effects more significant, the solid electrolyte of the present invention is preferred because it can further suppress the generation of hydrogen sulfide if a diffraction peak A is observed in the range of 2θ=20.7°±0.4°, particularly at 20.7°±0.3°, more particularly at 20.7°±0.2°, and particularly at 20.7°±0.1° in XRD measurement using CuKα1 rays.
[0015] It is not clear what crystal structure the diffraction peak A observed in the range of 2θ=20.7°±0.5° in the XRD measurement using CuKα1 rays comes from. However, even if the attribution of the diffraction peak A cannot be determined, the inventors' research results show that the sulfide solid electrolyte in which the diffraction peak A is observed in the above-mentioned range of 2θ can suppress the generation of hydrogen sulfide compared to the sulfide solid electrolyte in which the diffraction peak A is not observed. This is exemplified in the examples described later.
[0016] The solid electrolyte of the present invention is also preferably observed in the XRD diffraction pattern in the range of 2θ=25.4°±1.0° in addition to the above-mentioned angle range when performing XRD measurement using CuKα1 rays. Diffraction peak B is also observed in the range of 2θ=25.4°±1.0°. Such a solid electrolyte further suppresses the generation of hydrogen sulfide. In addition, the reaction resistance between such a solid electrolyte and the active material is reduced. As a result, a solid battery containing the solid electrolyte of the present invention becomes a solid battery with a high discharge capacity. From the viewpoint of making these effects more significant, the solid electrolyte of the present invention is more preferably observed in the range of 2θ=25.4°±0.8°, wherein the diffraction peak B is preferably observed in the range of 25.4°±0.6°, especially in the range of 25.4°±0.4°, and especially in the range of 25.4°±0.2°.
[0017] When both the diffraction peak A and the diffraction peak B are observed in the solid electrolyte of the present invention, when the intensity of the diffraction peak A is set to 1 A , set the intensity of diffraction peak B to I B When A with I B I A / I B If the value of is greater than 0, the generation of hydrogen sulfide can be further suppressed, so it is preferred. In addition, the reaction resistance between the solid battery containing the solid electrolyte and the active material is further reduced, and the discharge capacity is further increased, so it is preferred. From the viewpoint of making these advantageous effects more significant, I A / I B The value of is, for example, more preferably 0.05 or more, and further preferably 0.1 or more. A / I B The value of is, for example, preferably 1.0 or less, more preferably 0.7 or less, further preferably 0.5 or less, and further preferably 0.4 or less.
[0018] The solid electrolyte of the present invention is also preferably observed in the XRD diffraction pattern in addition to the above-mentioned diffraction peak A or in addition to the diffraction peaks A and B in the range of 2θ=22.0°±0.5°. Such a solid electrolyte further suppresses the generation of hydrogen sulfide. In addition, the reaction resistance between such a solid electrolyte and the active material is further reduced. As a result, a solid battery containing the solid electrolyte of the present invention becomes a solid battery with a higher discharge capacity. From the viewpoint of making these effects more significant, the solid electrolyte of the present invention is more preferably observed in the range of 2θ=22.0°±0.4°, wherein the diffraction peak C is preferably observed in the range of 22.0°±0.3°, especially in the range of 22.0°±0.2°, and especially in the range of 22.0°±0.1°.
[0019] In the case where both diffraction peak B and diffraction peak C are observed in addition to diffraction peak A in the solid electrolyte of the present invention, when the intensity of diffraction peak C is set to 1 C , set the intensity of diffraction peak B to I B When C with I B I C / I B If the value of is greater than 0 and less than 2.0, the generation of hydrogen sulfide can be further suppressed, so it is preferred. In addition, the reaction resistance between the solid battery containing the solid electrolyte and the active material is further reduced, resulting in a solid battery with a higher discharge capacity, so it is preferred. From the viewpoint of making these advantageous effects more significant, I C / I B The value of is, for example, more preferably 0.01 or more, and further preferably 0.02 or more. C / I B The value of is, for example, preferably 1.7 or less, more preferably 1.3 or less, further preferably 1.0 or less, and further preferably 0.7 or less.
[0020] In the solid electrolyte of the present invention, in order to observe the diffraction peak A, for example, the following method can be used: a sulfide electrolyte raw material is mixed with a hydrate of a lithium halide to obtain a mixture, and the mixture is heated to 80°C or more under vacuum. In the case of adopting this method, for the mixing ratio of the sulfide electrolyte raw material and the hydrate of the lithium halide, the amount of the hydrate of the lithium halide relative to the total amount of the two is preferably, for example, 5% by mass or more, more preferably 10% by mass or more, particularly preferably 20% by mass or more, and further preferably 40% by mass or more. On the other hand, the amount of the above-mentioned lithium halide hydrate is, for example, preferably 90% by mass or less, more preferably 80% by mass or less, particularly preferably 70% by mass or less, and further preferably 60% by mass or less. In this case, the obtained solid electrolyte preferably contains lithium (Li) element, phosphorus (P) element, sulfur (S) element, halogen (X) element and oxygen (O) element. In addition, it is also preferred that the halogen (X) element is, for example, at least one of a fluorine (F) element, a chlorine (Cl) element, a bromine (Br) element and an iodine (I) element. The sulfide electrolyte raw material preferably contains lithium (Li) element, phosphorus (P) element, sulfur (S) element, and halogen (X) element.
[0021] The reason why the generation of hydrogen sulfide is suppressed in the solid electrolyte of the present invention obtained by heating a mixture of a sulfide electrolyte raw material and a hydrate of a lithium halide under vacuum has not been fully understood. As one reason, the present inventors believe that it is because a layer capable of suppressing the generation of hydrogen sulfide is formed on the surface of the sulfide electrolyte raw material. However, the scope of the present invention is not limited to this theory.
[0022] As the hydrate of the above-mentioned lithium halide, for example, a hydrate of lithium chloride, a hydrate of lithium bromide and a hydrate of lithium iodide etc. can be listed. These hydrates can be used alone or in combination of two or more. The hydrate of the lithium halide can be a monohydrate, or can be more than a dihydrate. From the viewpoint of effectively suppressing the generation of hydrogen sulfide, the hydrate of the lithium halide is preferably a monohydrate.
[0023] The mixing of the sulfide electrolyte raw material and the lithium halide hydrate is advantageously accompanied by pulverization. For pulverization, for example, a known pulverization means such as a ball mill or a bead mill can be used. The mixing is preferably performed in an atmosphere without the presence of water.
[0024] The heating of the mixture of the sulfide electrolyte raw material and the lithium halide hydrate is performed under vacuum as described above. The degree of vacuum is represented by the gauge pressure when the atmospheric pressure is set to 0 Pa, and is preferably -0.01 MPa or less, more preferably -0.05 MPa or less, and further preferably -0.1 MPa or less.
[0025] Diffraction peak A can be observed in the solid electrolyte of the present invention obtained by heating a mixture of a sulfide electrolyte raw material and a hydrate of a lithium halide under vacuum. The so-called "heating" refers to raising the temperature of an object to above room temperature. In the present invention, it is preferred to raise the temperature until the diffraction peak A is observed. The temperature when the mixture is heated under vacuum can be appropriately adjusted according to other conditions such as the heating time, and is not particularly limited. For example, it is preferably above 50°C, more preferably above 80°C, and particularly preferably above 120°C. On the other hand, the above-mentioned heating temperature can be, for example, below 200°C, below 180°C, or below 150°C. As far as the heating time is concerned, with the heating temperature being in the above-mentioned range as a condition, it is preferably 20 minutes or more and 4 hours or less, more preferably 40 minutes or more and 3 hours or less, and further preferably 1 hour or more and 2 hours or less. By heating under this condition, it becomes easy to observe the diffraction peak A in the solid electrolyte of the present invention, and the solid electrolyte becomes a solid electrolyte that suppresses the generation of hydrogen sulfide.
[0026] The diffraction peak B in the present invention is a peak derived from the argyrodite type crystal structure. Therefore, in order to observe the diffraction peak B, it is preferred to adjust the composition of the sulfide solid electrolyte raw material. In addition, the diffraction peak C in the present invention is a peak derived from a hydrate of a lithium halide. Therefore, in order to observe the diffraction peak C, it is preferred to adjust the heating temperature under vacuum and the amount of the hydrate of a lithium halide.
[0027] From the viewpoint of further suppressing the generation of hydrogen sulfide and further improving the discharge capacity of the solid battery containing the solid electrolyte of the present invention, the solid electrolyte of the present invention is preferably observed to reduce weight in thermogravimetric measurement. It is particularly preferred to observe weight reduction when heated from 25°C to 400°C. The weight reduction rate in the above-mentioned temperature range in thermogravimetric measurement is, for example, preferably 1.6% or more, more preferably 2.0% or more, particularly preferably 3.5% or more, and more preferably 4.0% or more. On the other hand, the above-mentioned weight reduction rate is, for example, preferably 20% or less, more preferably 10% or less, particularly preferably 8.0% or less, and more preferably 6.0% or less. In the present invention, the generation of hydrogen sulfide can be further suppressed by the above-mentioned weight reduction rate being within the above-mentioned range. In addition, the discharge capacity of the solid battery containing the solid electrolyte of the present invention is further improved. Thermogravimetric measurement is performed at a heating rate of 10°C / min. The atmosphere is set to Ar. For example, TG-DTA2000SA (trade name) manufactured by MAC science Co., Ltd. can be used in the measurement.
[0028] The weight reduction rate was calculated by the following formula (1).
[0029] Weight reduction rate (wt%) = (W 25 -W 400 ) / W25 ×100 (1)
[0030] Where W 25 Indicates the weight of the sample at 25°C (g), W 400 It shows the weight (g) of the sample at 400°C.
[0031] From the viewpoint of further reducing the reaction resistance with the active material to further increase the discharge capacity of the solid battery containing the solid electrolyte, the particularly preferred sulfide solid electrolyte used in the present invention is a material containing a crystal phase having an argyrodite-type crystal structure. The so-called argyrodite-type crystal structure is a crystal structure possessed by a compound group derived from a mineral represented by the chemical formula: Ag8GeS6. From the viewpoint of further reducing the reaction resistance with the active material, it is particularly preferred that the sulfide solid electrolyte having an argyrodite-type crystal structure has a crystal structure belonging to a cubic crystal.
[0032] In the sulfide solid electrolyte including a crystal phase having an argyrodite-type crystal structure, as the halogen element contained therein, for example, one or more elements selected from the group consisting of F element, Cl element, Br element and I element can be used. From the viewpoint of improving ion conductivity, it is particularly preferable to use the Cl element and the Br element in combination as the halogen element.
[0033] From the viewpoint of further improving ion conductivity, a sulfide solid electrolyte containing a crystal phase having an argyrodite-type crystal structure is particularly preferred, for example, a sulfide solid electrolyte having a composition formula (I): Li a PS b X c A compound represented by (X is at least one of fluorine (F) element, chlorine (Cl) element, bromine (Br) element, and iodine (I) element). X is preferably one or two of chlorine (Cl) element and bromine (Br) element.
[0034] In the above composition formula (I), a, which represents the molar ratio of the Li element, is preferably 3.0 or more and 6.5 or less, more preferably 3.5 or more and 6.3 or less, and further preferably 4.0 or more and 6.0 or less. As long as a is within this range, the cubic argyrodite-type crystal structure near room temperature (25° C.) is stable, and the conductivity of lithium ions can be improved.
[0035] In the above composition formula (I), b is a value indicating how much less the Li2S component is relative to the stoichiometric composition. From the viewpoint of stabilizing the argyrodite-type crystal structure near room temperature (25°C) and improving the conductivity of lithium ions, b is preferably 3.5 or more and 5.5 or less, more preferably 4.0 or more and 5.3 or less, and further preferably 4.2 or more and 5.0 or less.
[0036] In the above composition formula (I), c is preferably 0.1 or more and 3.0 or less, more preferably 0.5 or more and 2.5 or less, and further preferably 1.0 or more and 1.8 or less.
[0037] In addition, the sulfide solid electrolyte including a crystal phase having an argyrodite-type crystal structure may be, for example, a sulfide solid electrolyte having a composition formula (II): Li 7-d PS 6-d X d The composition represented by the composition formula (II) is the stoichiometric composition of the argyrodite type crystal phase. In the composition formula (II), X has the same meaning as in the composition formula (I).
[0038] In the above composition formula (II), d is preferably 0.4 or more and 2.2 or less, more preferably 0.8 or more and 2.0 or less, and further preferably 1.2 or more and 1.8 or less.
[0039] Furthermore, the sulfide solid electrolyte including a crystal phase having an argyrodite-type crystal structure may be, for example, a sulfide solid electrolyte having a composition formula (III): Li 7-d-2e PS 6-d-e X d The argyrodite-type crystal phase having a composition represented by formula (III) is generated, for example, by the reaction of the argyrodite-type crystal phase having a composition represented by formula (II) with P2S5 (phosphorus pentasulfide). The reaction formula is shown below.
[0040] Li 7-d PS 6-d X d +y / 3P2S5→Li 7-d-2e PS 6-d-e X d +2y / 3Li3PS4
[0041] As shown in the above reaction formula, Li3PS4 phase is generated together with the argyrodite-type crystal phase represented by the composition formula (III). In addition, a trace amount of LiX phase (X is at least one of fluorine (F) element, chlorine (Cl) element, bromine (Br) element, and iodine (I) element) is sometimes generated. In the composition formula (III), X and d have the same meaning as in the composition formula (II).
[0042] In the composition formula (III), e is a value indicating the deviation of the Li2S component from the stoichiometric composition represented by the composition formula (II). e is preferably greater than -0.9 and less than (-d+2), more preferably greater than -0.6 and less than (-d+1.6), and further preferably greater than -0.3 and less than (-d+1.0).
[0043] In the composition formula (I), (II) or (III), a part of P may be replaced by at least one or more elements selected from Si, Ge, Sn, Pb, B, Al, Ga, As, Sb and Bi. In this case, the composition formula (I) becomes Li a (P 1-y M y )S b X c , the composition formula (II) becomes Li 7-d (P 1-y M y )S 6-d X d , the composition formula (III) becomes Li 7-d-2e (P 1-y M y )S 6-d-e X d M is one or more elements selected from Si, Ge, Sn, Pb, B, Al, Ga, As, Sb and Bi. y is preferably 0.01 to 0.7, more preferably 0.02 to 0.4, and further preferably 0.05 to 0.2.
[0044] Whether the sulfide solid electrolyte has an argyrodite-type crystal structure can be confirmed, for example, by XRD measurement. That is, in XRD measurement using an X-ray diffraction device (XRD) using CuKα1 rays, the argyrodite-type crystal phase has characteristic peaks at 2θ=15.34°±1.00°, 17.74°±1.00°, 25.19°±1.00°, 29.62°±1.00°, 30.97°±1.00°, 44.37°±1.00°, 47.22°±1.00°, and 51.70°±1.00°. In addition, for example, characteristic peaks are present at 2θ=54.26°±1.00°, 58.35°±1.00°, 60.72°±1.00°, 61.50°±1.00°, 70.46°±1.00°, and 72.61°±1.00°. On the other hand, the fact that the sulfide solid electrolyte does not contain a crystalline phase of an argyrodite structure can be confirmed by the fact that it does not have a peak characteristic of a crystalline phase of an argyrodite structure.
[0045] The so-called sulfide solid electrolyte has a argyrodite crystal structure, which means that the sulfide solid electrolyte has at least a crystalline phase of the argyrodite structure. In the present invention, it is preferred that the sulfide solid electrolyte has a crystalline phase of the argyrodite structure as the main phase. The so-called "main phase" refers to the phase that accounts for the largest proportion relative to the total amount of all crystalline phases constituting the sulfide solid electrolyte. Therefore, with respect to the proportion of the crystalline phase of the argyrodite structure contained in the sulfide solid electrolyte, relative to all crystalline phases constituting the sulfide solid electrolyte, for example, it is preferably 60% by mass or more, more preferably 70% by mass or more, particularly preferably 80% by mass or more, and further preferably 90% by mass or more. The proportion of the crystalline phase can be confirmed, for example, by XRD.
[0046] The solid electrolyte of the present invention is made of a powder as a particle aggregate. From the viewpoint of improving ion conductivity, the solid electrolyte of the present invention preferably has a volume cumulative particle diameter D at a cumulative volume of 50% by volume obtained by laser diffraction scattering particle size distribution measurement. 50 For example, it is 0.1 μm or more, more preferably 0.3 μm or more, and even more preferably 0.5 μm or more. 50 For example, it is preferably 20 μm or less, more preferably 10 μm or less, and further preferably 5 μm or less. The volume cumulative particle size D of the solid electrolyte 50 By making the particle size D of the solid electrolyte larger than 0.1 μm, the surface area of the solid electrolyte powder as a whole can be prevented from increasing excessively, and the unfavorable situation that the resistance increases and the mixing with the active material becomes difficult can be effectively prevented. 50 When the solid electrolyte of the present invention is used in combination with other solid electrolytes, for example, the solid electrolyte of the present invention becomes easy to enter the gap of the other solid electrolytes, etc. Therefore, the contact points between the solid electrolytes increase and the contact area increases, which can effectively improve the ion conductivity.
[0047] The solid electrolyte of the present invention can be used as a material constituting a solid electrolyte layer, an electrode mixture constituting a solid electrolyte layer containing an active substance. Specifically, it can be used as a positive electrode mixture constituting a positive electrode layer containing a positive electrode active substance, or a negative electrode mixture constituting a negative electrode layer containing a negative electrode active substance. Therefore, the solid electrolyte of the present invention can be used in a battery having a solid electrolyte layer, a so-called solid battery. More specifically, it can be used in a lithium solid battery. A lithium solid battery can be a primary battery or a secondary battery, and is preferably used in a lithium secondary battery. It should be noted that the so-called "solid battery", in addition to including solid batteries that do not contain any liquid substance or gel-like substance as an electrolyte, also includes a form containing, for example, less than 50% by mass, less than 30% by mass, or less than 10% by mass of a liquid substance or gel-like substance as an electrolyte.
[0048] The solid electrolyte layer of the present invention can be manufactured by, for example, the following methods: dripping a slurry containing the solid electrolyte, a binder and a solvent onto a substrate, using a method of flattening with a scraper, or using a method of cutting the substrate with an air knife after contacting the slurry, or using a method of forming a coating by screen printing, etc., and then removing the solvent by heating and drying. Alternatively, it can also be manufactured by appropriately processing the powder of the solid electrolyte of the present invention after press molding. In the solid electrolyte layer of the present invention, in addition to the solid electrolyte of the present invention, other solid electrolytes may be included. The thickness of the solid electrolyte layer in the present invention is typically preferably 5 μm or more and 300 μm or less, more preferably 10 μm or more and 100 μm or less.
[0049] The solid battery has a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer, and has the solid electrolyte of the present invention. Examples of the shape of the battery include a laminated body, a cylindrical shape, and a square shape.
[0050] As the active material contained in the above-mentioned positive electrode mixture, for example, an active material used as a positive electrode active material of a lithium secondary battery can be appropriately used. As the positive electrode active material, for example, spinel-type lithium transition metal compounds, lithium metal oxides with a layered structure, etc. can be listed. The particles of the positive electrode active material may have a coating layer on their surface that can reduce the reaction resistance of the solid electrolyte and the positive electrode active material. In particular, according to the present invention, it is possible to expect the same effect as the case where a coating layer is formed on the surface of the particles of the active material, so even an active material without a coating layer can be preferably used. In addition to the positive electrode active material, the positive electrode mixture may also include other materials headed by a conductive auxiliary agent.
[0051] As the active material contained in the above-mentioned negative electrode mixture, for example, an active material used as a negative electrode active material of a lithium secondary battery can be appropriately used. As the negative electrode active material, for example, carbon materials such as lithium metal, artificial graphite, natural graphite and difficult graphitization carbon (hard carbon), silicon, silicon compounds, tin and tin compounds can be listed. In addition to the negative electrode active material, the negative electrode mixture may also include other materials headed by a conductive auxiliary agent.
[0052] Example
[0053] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to the examples.
[0054] [Example 1]
[0055] (1) Manufacturing of solid electrolyte
[0056] To become Li 5.4 PS 4.4 Cl 0.8 Br 0.8 Li2S powder, P2S5 powder, LiCl powder and LiBr powder were weighed in a manner of composition so that the total amount reached 75 g. These powders were crushed and mixed using a ball mill to obtain a mixed powder. The mixed powder was sintered to obtain a sintered product of the above composition. The sintering was carried out using a tubular electric furnace. During the sintering, 100% pure hydrogen sulfide gas was circulated in the electric furnace at 1.0 L / min. The sintering temperature was set to 500°C and sintering was performed for 4 hours. The sintered product was crushed using a mortar and pestle, and then pulverized using a wet bead mill to obtain a sulfide electrolyte raw material. The results of XRD measurement confirmed that the sulfide electrolyte raw material had a crystalline phase of a argyrodite-type structure.
[0057] The obtained sulfide electrolyte raw material and LiBr·H2O were mixed under an Ar atmosphere to obtain a mixture. The amount of LiBr·H2O added was 10% by mass relative to the total amount of the sulfide electrolyte raw material and LiBr·H2O. The obtained mixture was heated at 120°C for 1 hour under a vacuum of -0.1 MPa at a gauge pressure when the atmospheric pressure was set to 0 Pa. In this way, the target solid electrolyte was obtained.
[0058] [Example 2]
[0059] A solid electrolyte was obtained in the same manner as in Example 1 except that the amount of LiBr·H 2 O added was 40 mass %.
[0060] [Example 3]
[0061] A solid electrolyte was obtained in the same manner as in Example 1 except that the amount of LiBr·H 2 O added was 80 mass %.
[0062] [Comparative Example 1]
[0063] A solid electrolyte was obtained in the same manner as in Example 1 except that LiBr·H 2 O was not added.
[0064] [evaluate]
[0065] The solid electrolytes obtained in the examples and comparative examples were subjected to XRD measurements using the following method. The results are shown in Figure 1 The results are shown in Table 1. In addition, thermogravimetric measurement was performed at a heating rate of 10°C / min to measure the weight loss rate when heated from 25°C to 400°C. Furthermore, the amount of hydrogen sulfide generated was measured by the following method. The results are shown in Table 1.
[0066] [Conditions for XRD measurement]
[0067] The conditions for XRD measurement are as follows.
[0068] Equipment: SmartLab, a fully automatic multi-purpose X-ray diffraction device manufactured by Rigaku Co., Ltd.
[0069] Tube voltage: 40kV
[0070] Tube current: 30mA
[0071] X-ray source: CuKα1
[0072] Incident optics: Confocal mirror (CMF)
[0073] Incident side slit composition: Collimator size 1.4mm×1.4mm
[0074] Light receiving side slit composition: Parallel slit analyzer 0.114 degrees, light receiving slit 20mm
[0075] Detector: Scintillation counter
[0076] Scan axis: 2θ / θ
[0077] Measuring range: 2θ = 20 degrees to 40 degrees
[0078] Step width: 0.01 degree
[0079] Scanning speed: 1 degree / minute
[0080] Department of Optics: Concentration Method
[0081] Incident monochromator: Johnson type
[0082] Non-exposed fixture
[0083] Maximum intensity: 5000 counts or more
[0084] The analysis of peak intensity was performed using PDXL2 (version 2.8.4.0). XRD data was read using PDXL2, and "Calculate and Determine" was performed in the form of "Data Processing" - "Automatic", "Peak Search" - "σ Cutoff 3.00". Then, the "2θ (degrees)" and "Height (count)" published in the "Peak List" were set to "Peak Position" and "Peak Intensity", respectively. However, in the case where the peak existing at the peak position described later is decomposed by multiple peaks, it is edited as a single peak ("Delete Peak" or "Add Peak"), and in the dialogue of "Information" - "Optimization", the check box of "Refine Background" is removed, and "Execute" optimization. Then, the results published in the "Peak List" are used.
[0085] [Amount of hydrogen sulfide produced]
[0086] The solid electrolytes obtained in Examples and Comparative Examples were weighed in metal containers in a glove box replaced with sufficiently dried Ar gas (dew point -60°C or lower), placed in a bag made of a laminated film, and then sealed.
[0087] A 1000 ml glass removable flask was placed in a constant temperature and humidity chamber maintained at room temperature (25°C) in an atmosphere with a dew point of -30°C adjusted by mixing dry air with the atmosphere, and kept until the interior of the removable flask became the same as the environment in the constant temperature and humidity chamber. Next, the sealed bag containing the solid electrolyte was opened in the constant temperature and humidity chamber, the solid electrolyte was quickly placed in the removable flask, and then the removable flask was sealed. For the hydrogen sulfide generated from just after sealing until 30 minutes had passed, 100 ml of the interior of the removable flask was sucked using a gas detector (GV-100 manufactured by GESTEC) and a gas detector (No. 4LL manufactured by GESTEC) after 30 minutes, and the hydrogen sulfide concentration was measured.
[0088] Table 1
[0089]
[0090] Depend on Figure 1 As can be seen from the results shown in , all of the diffraction peaks A, B, and C were observed in the solid electrolyte obtained in each example.
[0091] As can be seen from the results shown in Table 1, the solid electrolytes obtained in the respective Examples suppress the amount of hydrogen sulfide generated compared to the solid electrolytes obtained in the Comparative Examples.
[0092] Industrial Applicability
[0093] According to the present invention, a sulfide solid electrolyte capable of suppressing the generation of hydrogen sulfide can be provided.
Claims
1. A sulfide solid electrolyte having a peak A at 2θ=20.7°±0.5° in an X-ray diffraction pattern obtained by X-ray diffraction measurement using CuKα1 rays, In the X-ray diffraction pattern obtained by X-ray diffraction measurement using CuKα1 rays, there is a peak B at 2θ=25.4°±1.0°, In the X-ray diffraction pattern obtained by X-ray diffraction measurement using CuKα1 rays, there is a peak C at 2θ=22.0°±0.5°, When the intensity of the peak B is set to I B , the intensity of the peak C is set to I C When C with I B I C / I B The value of is greater than 0 and less than 2.0, The sulfide solid electrolyte contains lithium (Li) element, phosphorus (P) element, sulfur (S) element, halogen (X) element and oxygen (O) element.
2. The sulfide solid electrolyte according to claim 1, wherein The diffraction peak B is a peak derived from the argyrodite type crystal structure.
3. The sulfide solid electrolyte according to claim 2, wherein The halogen (X) element is at least one of chlorine (Cl), bromine (Br) and iodine (I).
4. The sulfide solid electrolyte according to claim 1 or 2, wherein When the intensity of the peak A is set to I A , the intensity of the peak B is set to I B When A with I B I A / I B The value of is greater than 0.
5. The sulfide solid electrolyte according to claim 1 or 2, wherein The diffraction peak C is a peak derived from a hydrate of a lithium halide. 6 . The sulfide solid electrolyte according to claim 1 , wherein the weight reduction rate when heated from 25° C. to 400° C. in a thermogravimetric measurement performed at a heating rate of 10° C. / min is 1.6% or more. 7 . An electrode mixture comprising the sulfide solid electrolyte according to claim 1 and an active material. 8 . A solid battery comprising a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer, wherein the solid electrolyte layer contains the sulfide solid electrolyte according to claim 1 .
9. The method for producing a sulfide solid electrolyte according to claim 1, comprising: a mixing step of mixing a sulfide electrolyte raw material and a hydrate of a lithium halide to obtain a mixture; and a heating step of heating the mixture to 50° C. or higher under vacuum, in, In the mixing step, the sulfide electrolyte raw material and the lithium halide hydrate are mixed in a ratio such that the amount of the lithium halide hydrate is 5 mass % or more and 90 mass % or less relative to the total amount of the sulfide electrolyte raw material and the lithium halide hydrate.