Method for manufacturing semiconductor device and semiconductor device
By forming a fin structure embedded in an isolation insulating layer in a semiconductor device and forming an epitaxial source/drain structure at a merge point thereon, the challenges of high-density and low-cost manufacturing in the prior art are solved, and high-performance source electrodes are achieved /drain structure and improved short channel effect.
Patent Information
- Application Number
- CN202110073377.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-25
- Filing Date
- 2021-01-20
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-01-20
AI Technical Summary
In the process of manufacturing semiconductor devices, it is difficult for the prior art to effectively form high-performance source/drain structures, especially under high-density and low-cost nanotechnology process nodes. The challenge of three-dimensional design makes fin field effect transistors (FinFETs) ) and high K material metal gate structures have difficulties in manufacturing.
By forming the first and second fin structures on the substrate and forming an isolation insulating layer thereon, the lower part of the fin structure is embedded and the upper part is exposed, and then a gate structure is formed on the channel region of the fin structure, recessed into the source The electrode/drain region is formed at the recess, and an epitaxial source/drain structure with a merge point is formed, with the bottom of the merge point being 50% or more from the upper surface of the isolation insulating layer.
A high-performance source/drain structure is achieved, short channel effect is improved, and overall device performance and manufacturing efficiency are improved.
Smart Images

Figure CN113539960B_ABST
Abstract
Description
Technical Field
[0001] Embodiments of the present application relate to a method for manufacturing a semiconductor device and a semiconductor device. Background Art
[0002] The present invention relates to semiconductor integrated circuits, and more specifically to semiconductor devices having epitaxial source / drain (S / D) structures with holes and processes for manufacturing the same. As the semiconductor industry has evolved into nanotechnology process nodes in pursuit of higher device density, higher performance, and lower cost, challenges from manufacturing and design issues have led to the development of three-dimensional designs, such as fin field effect transistors (FinFETs) and the use of metal gate structures with high-K (dielectric constant) materials. Metal gate structures are often manufactured using gate replacement techniques, and the source and drain are formed using epitaxial growth methods. Summary of the invention
[0003] According to an embodiment of the present application, a method for manufacturing a semiconductor device is provided, the method comprising: forming a first fin structure and a second fin structure above a substrate; forming an isolation insulating layer above the substrate so that the lower portions of the first fin structure and the second fin structure are embedded in the isolation insulating layer and the upper portions of the first fin structure and the second fin structure are exposed to the isolation insulating layer; forming a gate structure above the channel region of the first fin structure and the second fin structure; recessing the source / drain region of the first fin structure and the second fin structure; and forming an epitaxial source / drain structure above the recessed first fin structure and the second fin structure, wherein the epitaxial source / drain structure is a merged structure having a merge point, and the height of the bottom of the merge point from the upper surface of the isolation insulating layer is 50% or more of the height of the channel region of the first fin structure and the second fin structure from the upper surface of the isolation insulating layer.
[0004] According to another embodiment of the present application, a method for manufacturing a semiconductor device is provided, the method comprising: forming a first fin structure and a second fin structure above a substrate; forming an isolation insulating layer above the substrate so that the lower portions of the first fin structure and the second fin structure are embedded in the isolation insulating layer and the upper portions of the first fin structure and the second fin structure are exposed to the isolation insulating layer; forming fin sidewalls on opposite sides of the source / drain regions of the first fin structure and the second fin structure; recessing the source / drain regions of the first fin structure and the second fin structure; at a first temperature, forming a first epitaxial layer above the recessed first fin structure and the second fin structure, respectively; at a second temperature, performing an etching operation on the first epitaxial layer; at a third temperature, forming a second epitaxial layer having a composition different from that of the first epitaxial layer, respectively, above the first epitaxial layer; at a fourth temperature, forming a third epitaxial layer having a composition different from that of the second epitaxial layer above the second epitaxial layer; at a fifth temperature, performing an etching operation on the third epitaxial layer, and at a sixth temperature, forming a fourth epitaxial layer having a composition different from that of the third epitaxial layer above the third epitaxial layer.
[0005] According to another embodiment of the present application, a semiconductor device is provided, including: an isolation insulating layer, arranged above a substrate; a first fin structure and a second fin structure, arranged above the substrate; a gate structure, arranged above the channel region of the first fin structure and the second fin structure; and a source / drain epitaxial layer, arranged above the source / drain region of the first fin structure and the second fin structure, wherein: the source / drain epitaxial layer has a merged structure, the merged structure has a merged point, and the height of the bottom of the merged point from the upper surface of the isolation insulating layer is 65% or more of the height of the channel region of the first fin structure and the second fin structure from the upper surface of the isolation insulating layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0006] Aspects of the present invention will be best understood from the following detailed description when read in conjunction with the accompanying drawings. It should be noted that, in accordance with standard practice in the industry, the various components are not drawn to scale. In fact, the dimensions of the various components may be arbitrarily increased or decreased for clarity of discussion.
[0007] Figure 1 A process flow diagram illustrating fabrication operations of a semiconductor device according to an embodiment of the present invention is shown.
[0008] Figure 2 A cross-sectional view is shown of one of the various stages of fabrication operations of a semiconductor device in accordance with an embodiment of the present invention.
[0009] Figure 3 A cross-sectional view is shown of one of the various stages of fabrication operations of a semiconductor device in accordance with an embodiment of the present invention.
[0010] Figure 4 A cross-sectional view is shown of one of the various stages of fabrication operations of a semiconductor device in accordance with an embodiment of the present invention.
[0011] Figure 5 A cross-sectional view is shown of one of the various stages of fabrication operations of a semiconductor device in accordance with an embodiment of the present invention.
[0012] Fig. 6A , Figure 6B and Figure 6C A diagram illustrating one of the various stages of fabrication operations for a semiconductor device according to an embodiment of the present invention.
[0013] Figure 7 A cross-sectional view is shown of one of the various stages of fabrication operations of a semiconductor device in accordance with an embodiment of the present invention.
[0014] Fig. 8A and Figure 8B A cross-sectional view is shown of one of the various stages of fabrication operations of a semiconductor device in accordance with an embodiment of the present invention.
[0015] Fig. 9A and Fig. 9B A cross-sectional view is shown of one of the various stages of fabrication operations of a semiconductor device in accordance with an embodiment of the present invention.
[0016] Fig. 10A and Fig. 10B A cross-sectional view is shown of one of the various stages of fabrication operations of a semiconductor device in accordance with an embodiment of the present invention.
[0017] Fig.11A and Fig. 11B A cross-sectional view is shown of one of the various stages of fabrication operations of a semiconductor device in accordance with an embodiment of the present invention.
[0018] Fig. 12A and Fig. 12B A cross-sectional view is shown of one of the various stages of fabrication operations of a semiconductor device in accordance with an embodiment of the present invention.
[0019] Fig.13A and Fig. 13B A cross-sectional view is shown of one of the various stages of fabrication operations of a semiconductor device in accordance with an embodiment of the present invention.
[0020] Fig.14 A cross-sectional view is shown of one of the various stages of fabrication operations of a semiconductor device in accordance with an embodiment of the present invention.
[0021] Fig.15 The process flow of forming a source / drain epitaxial layer according to an embodiment of the present invention is shown.
[0022] Fig.16A , Fig. 16B and Fig. 16C A cross-sectional view is shown of one of the various stages of fabrication operations of a semiconductor device in accordance with an embodiment of the present invention.
[0023] Fig.17 A cross-sectional view is shown of one of the various stages of fabrication operations of a semiconductor device in accordance with an embodiment of the present invention.
[0024] Fig.18 Element analysis results of the source / drain structure according to an embodiment of the present invention are shown. DETAILED DESCRIPTION
[0025] It should be understood that the following disclosure provides many different embodiments or examples of different components for realizing the provided subject matter. Specific examples of components and arrangements are described below to simplify the present invention. Of course, these are merely examples and are not intended to limit the present invention. For example, the size of the element is not limited to the disclosed range or value, but may depend on the desired properties of the process conditions and / or the device. In addition, in the following description, forming a first component above or on a second component may include an embodiment in which the first component and the second component are directly contacted, and may also include an embodiment in which an additional component may be formed between the first component and the second component, so that the first component and the second component may not be in direct contact. For the purpose of simplicity and clarity, various components may be drawn at will according to different scales. In the accompanying drawings, some layers / components may be omitted for simplicity.
[0026] Moreover, for ease of description, spatially relative terms such as "under...", "below...", "lower part", "above...", "upper part", etc. may be used herein to describe the relationship between one element or component and another (or other) elements or components as shown in the figure. In addition to the orientation shown in the figure, spatially relative terms are intended to include different orientations of the device in use or operation. The device can be oriented in other ways (rotated 90 degrees or in other orientations), and the spatially relative descriptors used herein can be interpreted accordingly. In addition, the term "made of..." may mean "including" or "consisting of...". In addition, in the following manufacturing process, there may be one or more additional operations in / between the described operations, and the order of the operations may be changed. In the present invention, the phrase "one of A, B and C" means "A, B and / or C" (A, B, C, A and B, A and C, B and C or A, B and C), and unless otherwise described, it does not mean an element from A, an element from B, and an element from C. In other embodiments, the same or similar materials, configurations, sizes, processes, and / or operations as those described using one embodiment may be used, and detailed explanations may be omitted.
[0027] The disclosed embodiments relate to semiconductor devices and methods of manufacturing the same, and in particular to source / drain regions of field effect transistors (FETs). Embodiments such as those disclosed herein are generally applicable not only to FinFETs but also to other FETs.
[0028] Figure 1 A process flow diagram is shown and Figure 2 to Figure 1 6 shows a cross-sectional view of various stages of manufacturing a semiconductor device according to an embodiment of the present invention. Figure 1 and Figure 2 to Figure 1 Additional operations may be provided before, during, and after the process shown in FIG. 6 , and some operations described below may be replaced or eliminated for additional embodiments of the method. The order of operations / processes may be interchanged.
[0029] exist Figure 1 In S101 and Figure 2 and Figure 3As shown in , one or more fin structures 20 are formed above the substrate 10. The fin structure of the FinFET can be patterned by any suitable method. For example, the fin structure can be patterned using one or more photolithography processes, including double patterning or multi-patterning. Typically, the double patterning or multi-patterning process combines photolithography and self-alignment processes, thereby allowing the formation of a pattern having, for example, a smaller pitch than that originally obtainable using a single direct photolithography process. For example, in one embodiment, a sacrificial layer is formed above the substrate and patterned using a photolithography process. A spacer is formed next to the patterned sacrificial layer using a self-alignment process. Then, the sacrificial layer is removed, and the remaining spacers or mandrels can then be used to pattern the fin structure. The multi-patterning process combining photolithography and self-alignment processes typically forms a pair of fin structures.
[0030] In some embodiments, a mask layer 15 is formed on the substrate 10 to fabricate the fin structure. The mask layer 15 is formed by, for example, a thermal oxidation process and / or a chemical vapor deposition (CVD) process. For example, the substrate 10 has a thickness between about 1×10 15 cm -3 With about 1×10 16 cm -3 In other embodiments, the substrate is a p-type silicon or germanium substrate having an impurity concentration between about 1×10 15 cm -3 With about 1×10 16 cm -3 The impurity concentration is between that of an n-type silicon or germanium substrate.
[0031] Alternatively, the substrate 10 may include another element semiconductor such as germanium; a compound semiconductor including a group IV to IV compound semiconductor such as SiC and SiGe, a group III to V compound semiconductor such as GaAs, GaP, GaN, InP, InAs, InSb, GaAsP, AlGaN, AlInAs, AlGaAs, GaInAs, GaInP, and / or GaInAsP or a combination thereof. In one embodiment, the substrate 10 is a silicon layer of an SOI (silicon on insulator) substrate. When an SOI substrate is used, the fin structure may protrude from the silicon layer of the SOI substrate or may protrude from the insulator layer of the SOI substrate. In the latter case, the silicon layer of the SOI substrate is used to form the fin structure. An amorphous substrate such as amorphous Si or amorphous SiC, or an insulating material such as silicon oxide may also be used as the substrate 10. The substrate 10 may include various regions that have been appropriately doped with impurities (e.g., p-type or n-type conductivity).
[0032] In some embodiments, the mask layer 15 includes, for example, an oxide pad (e.g., silicon oxide) layer 15A and a silicon nitride mask layer 15B. The oxide pad layer 15A may be formed by using a thermal oxidation or CVD process. The silicon nitride mask layer 15B may be formed by physical vapor deposition (PVD), such as sputtering, CVD, plasma enhanced chemical vapor deposition (PECVD), atmospheric pressure chemical vapor deposition (APCVD), low pressure CVD (LPCVD), high density plasma CVD (HDPCVD), atomic layer deposition (ALD) and / or other processes.
[0033] In some embodiments, the thickness of the oxide pad layer 15A is between about 2 nm and about 15 nm, and the thickness of the silicon nitride mask layer 15B is between about 2 nm and about 50 nm. A mask pattern is further formed on the mask layer. The mask pattern is, for example, an etch-resistant pattern formed by a photolithography operation.
[0034] By using the mask pattern as an etching mask, a hard mask pattern 15 of an oxide pad layer and a silicon nitride mask layer is formed, as shown in FIG. Figure 2 as shown in .
[0035] Then, if Figure 3 As shown in , the substrate 10 is patterned into the fin structure 20 by trench etching using a dry etching method and / or a wet etching method by using the hard mask pattern 15 as an etching mask.
[0036] exist Figure 3 In the embodiment of the present invention, a fin structure is provided above the substrate 10. However, the number of fin structures is not limited to three. The number may be as small as one or greater than three. In some embodiments, the number of fin structures is between 5 and 1000, connected by source / drain epitaxial layers formed in subsequent operations. In other embodiments, the number of fin structures is between 5 and 100, connected by source / drain epitaxial layers formed in subsequent operations. In certain embodiments, the number of fin structures is between 5 and 20, connected by source / drain epitaxial layers formed in subsequent operations. In addition, one or more dummy fin structures may be provided adjacent to both sides of the fin structure 20 to improve pattern fidelity in the patterning process.
[0037] The fin structure 20 may be made of the same material as the substrate 10 and may extend continuously from the substrate 10. In this embodiment, the fin structure is made of Si. The silicon layer of the fin structure 20 may be intrinsic or appropriately doped with n-type impurities or p-type impurities.
[0038] In some embodiments, the width W1 of the fin structure 20 is between about 3 nm and about 40 nm, and in other embodiments, between about 7 nm and about 12 nm. In some embodiments, the spacing S1 between two fin structures is between about 10 nm and about 50 nm. In some embodiments, the height (along the Z direction) of the fin structure 20 is between about 100 nm and about 300 nm, and in other embodiments, between about 50 nm and about 100 nm.
[0039] The lower portion of the fin structure 20 under the gate structure 40 (see Fig. 6A ) may be referred to as a well region, and the upper portion of the fin structure 20 may be referred to as a channel region. Under the gate structure 40, the well region is embedded in the isolation insulating layer 30 (see Fig. 6A ), and the channel region protrudes from the isolation insulating layer 30. The lower portion of the channel region may also be embedded in the isolation insulating layer 30 to a depth of about 1 nm to about 5 nm.
[0040] In some embodiments, the height of the well region is between about 60 nm and 100 nm, and the height of the channel region is between about 40 nm and 60 nm, and in other embodiments between about 38 nm and about 55 nm.
[0041] After forming the fin structure 20, in some embodiments, the substrate 10 is further etched to form a mesa shape 10M, such as Figure 4 In other embodiments, the mesa shape 10M is formed first and then the fin structure 20 is formed. In some embodiments, the mesa shape is not formed.
[0042] After forming the fin structure 20 and the mesa shape 10M, Figure 1In S102, an isolation insulating layer 30 is formed in the space between the fin structures and / or in the space between one fin structure and another element formed above the substrate 10. The isolation insulating layer 30 may also be referred to as a "shallow trench isolation (STI)" layer. The insulating material of the isolation insulating layer 30 may include one or more silicon oxide, silicon nitride, silicon oxynitride (SiON), SiOCN, fluorine-doped silicate glass (FSG) or low-k dielectric material layers. The isolation insulating layer is formed by LPCVD (low pressure chemical vapor deposition), plasma CVD or flowable CVD. In flowable CVD, a flowable dielectric material may be deposited instead of silicon oxide. The flowable dielectric material, as indicated by its name, can "flow" during deposition to fill a gap or interval with a high aspect ratio. Typically, various chemical components are added to the silicon-containing precursor to allow the deposited film to flow. In some embodiments, hydrogenated nitrogen bonds are added. Examples of flowable dielectric precursors, particularly flowable silicon oxide precursors, include silicates, siloxanes, methyl silsesquioxane (MSQ), hydrogen silsesquioxane (HSQ), MSQ / HSQ, perhydropolysilazane (TCPS), perhydropoly-polysilazane (PSZ), tetraethyl orthosilicate (TEOS) or silane amines, such as trimethylsilyl (TSA). These flowable silicon oxide materials are formed in a multi-operation process. After the flowable film is deposited, it is solidified and annealed to remove undesirable elements to form silicon oxide. When the undesirable elements are removed, the flowable film densifies and shrinks. In some embodiments, multiple annealing processes are performed. The flowable film is solidified and annealed more than once. The flowable film can be doped with boron and / or phosphorus.
[0043] First, an insulating layer 30 is formed in the thick layer so that the fin structure is embedded in the thick layer and the thick layer is recessed to expose the upper portion of the fin structure 20, as shown in FIG. Figure 5 . In some embodiments, the height H11 of the fin structure from the upper surface of the isolation insulating layer 30 is between about 20 nm and about 100 nm, and in other embodiments is between about 30 nm and about 50 nm. After or before recessing the isolation insulating layer 30, a thermal process, for example, an annealing process, may be performed to improve the quality of the isolation insulating layer 30. In some embodiments, the thermal process is performed by using a rapid thermal annealing (RTA) at a temperature between about 900° C. and about 1050° C. for about 1.5 seconds to about 10 seconds in an inert gas environment such as an N2, Ar, or He environment.
[0044] After forming the insulating layer 30, Figure 1 In S103, a sacrificial gate structure 40 is formed above the fin structure 20, such as FIG. 6A to FIG. 6C shown. Fig. 6A is an illustrative perspective view, Figure 6B It is along Fig. 6A and Figure 6C An exemplary cross-sectional view of line aa of Figure 6C It is along Fig. 6A An exemplary cross-sectional view along line bb in FIG. Figure 7 , Fig. 8A , Fig. 10A and Fig.11A , Fig. 12A , Fig.13A Also along Fig. 6A Cross-sectional view along line bb. Figure 8B and Fig. 10B It is along Fig. 6A Cross-sectional view along line cc.
[0045] like Fig. 6A As shown in , the sacrificial gate structure 40 extends in the X direction, while the fin structure 20 extends in the Y direction. In order to make the sacrificial gate structure 40, a dielectric layer and a polysilicon layer are formed over the isolation insulating layer 30 and the exposed fin structure 20, and then a patterning operation is performed to obtain a sacrificial gate structure, the sacrificial gate structure including a sacrificial gate pattern 44 made of polysilicon and a sacrificial dielectric layer 42. In some embodiments, the polysilicon layer is patterned by using a hard mask and the hard mask remains on the gate pattern 44 as a hard mask layer 46. The hard mask layer 46 includes one or more insulating material layers. In some embodiments, the hard mask layer 46 includes a silicon dioxide layer 46-2 formed over a silicon nitride layer 46-1. In other embodiments, the hard mask layer 46 includes a silicon nitride layer formed over a silicon dioxide layer. The insulating material of the hard mask layer 46 can be formed by CVD, PVD, ALD, electron beam evaporation or other suitable processes. In some embodiments, the sacrificial dielectric layer 42 may include one or more silicon oxide, silicon nitride, silicon oxynitride, or high-k dielectric layers. In some embodiments, the thickness of the dielectric layer 42 is between about 2 nm and about 20 nm, and in other embodiments, between about 2 nm and about 10 nm. In some embodiments, the height H12 of the sacrificial gate structure is between about 50 nm and about 400 nm, and in other embodiments, between about 100 nm and 200 nm.
[0046] In addition, Figure 1At S104, gate sidewall spacers 48 are formed on both sides of the sidewalls of the sacrificial gate pattern. The sidewall spacers 48 include one or more insulating material layers, such as SiO2, SiN, SiON, SiOCN or SiCN, which are formed by CVD, PVD, ALD, electron beam evaporation or other suitable processes. Low-k dielectric materials may be used as sidewall spacers. The sidewall spacers 48 are formed by forming a capping layer of insulating material followed by post-anisotropic etching. In an embodiment, the sidewall spacer layer 48 is made of a silicon nitride-based material, such as SiN, SiON, SiOCN or SiCN. In some embodiments, the sidewall spacers 48 are also formed on the exposed sidewalls of the fin structure 20, such as Figure 6C as shown in .
[0047] In some embodiments, Figure 1 At S105 , one or more ion implantation operations are performed to implant ions into the source / drain region of the fin structure before and / or after the gate sidewall spacers 48 to form a lightly doped drain (LDD) structure.
[0048] Then, if Figure 7 As shown in Figure 1 At S106, a fin mask layer 50 (fin sidewall) is formed over the fin structure 20. The fin mask layer 50 is made of a dielectric material, including a silicon nitride-based material, such as SiN, SiON, SiOCN, or SiCN. In one embodiment, SiN is used as the fin mask layer 50. The fin mask layer 50 is formed by CVD, PVD, ALD, electron beam evaporation, or other suitable processes. In some embodiments, the thickness of the fin mask layer 50 is between about 3 nm and about 30 nm.
[0049] After forming the fin mask layer 50, Figure 1 At S107, the upper portion of the fin structure 20 is recessed, and a portion of the fin mask layer 50 and the sidewall spacer 48 is removed by dry etching and / or wet etching. The upper portion of the fin structure 20 is recessed (etched) to a plane equal to or lower than the upper surface of the fin mask layer 50 on the upper surface isolation insulating layer 30, as shown in FIG. Fig. 8A as shown in .
[0050] In some embodiments, recess 22 is formed separately for n-type FET and p-type FET. In some embodiments, recess 22 (and subsequent epitaxial layer) for n-type FET is formed first, and the region for p-type FET is covered by capping layer 49 (e.g., silicon nitride) (see Fig. 9B ), and then the recess 22 of the p-type FET is formed (and the subsequent epitaxial layer), while the region of the n-type FET is covered by the capping layer (see Figure 1 at S113 and S114).
[0051] In some embodiments, the top of the recessed fin structure 20 (the bottom of the groove 22) is located on the upper surface of the isolation insulating layer 30. Fig. 8A In other embodiments, the top of the recessed fin structure 20 (the bottom of the groove 22 ) is located at the same plane as the upper surface of the isolation insulating layer 30 or is lower than the upper surface of the isolation insulating layer 30 .
[0052] In some embodiments, depending on the spacing between two adjacent fin structures and the spacing between two adjacent fin structures and another fin structure, the etching of the fin mask layer 50 and the sidewall spacer 48 is symmetrical about the fin structure, such as Figure 8B as shown in . Figure 8B Also shown is the fin structure before recessing (or under the sacrificial gate structure). In some embodiments, the remaining fin mask layer 50 and sidewall spacers 48 of one of the two adjacent fin structures have a lower height on the side facing the other fin structure than the remaining fin mask layer 50 and sidewall spacers 48 of one of the two adjacent fin structures on the other side. In other embodiments, the height relationship is relative.
[0053] In some embodiments, the upper surface of the recessed fin structure 20 has a U-shape, a W-shape, or a wavy shape.
[0054] exist Figure 1 At S109, an epitaxial source / drain structure of an n-type FET is formed above the recessed fin structure 20. The epitaxial source / drain structure is made of one or more semiconductor material layers having a different lattice constant from the fin structure 20 (channel region). FIG. 9A to FIG. 13B and FIG. 16A to FIG. 16B In FIG. 1 , “A” shows a cross-sectional view along the X direction (the direction in which the gate extends), and “B” shows a cross-sectional view along the Y direction (the direction in which the material extends).
[0055] In some embodiments, Fig. 9A and Fig. 9B As shown in FIG. 1 , a first epitaxial layer 62 is formed over the recessed fin structure 20. In some embodiments, the first epitaxial layer 62 includes SiAs and / or SiGeAs, which can inhibit phosphorus (P) from diffusing from a subsequently formed second epitaxial layer into the channel region of the fin structure. In some embodiments, the As concentration in the first epitaxial layer 62 is between about 5×10 19 Atom / cm 3 With about 5×10 21 Atom / cm 3 and in other embodiments between about 1×10 20 Atom / cm 3 With about 2×1021 Atom / cm 3 If the As concentration is too low, the diffusion barrier effect against P is insufficient. It is difficult to include As greater than the upper limit of the range, and a high As concentration will weaken the stress applied to the channel and increase resistance. In other embodiments, SiGe doped with P is used as the first epitaxial layer 62.
[0056] In some embodiments, the thickness T0 of the first epitaxial layer 62 is between about 3 nm and about 20 nm, and in other embodiments between about 10 nm and about 15 nm. If the thickness T0 is too small, the diffusion barrier effect against P is insufficient; and if the thickness is too large, it will weaken the stress applied to the channel and increase the resistance. In some embodiments, the first epitaxial layer 62 is deposited until it is equal to or slightly below (less than 2 nm) the plane of the bottom of the gate sidewall spacer 48.
[0057] In some embodiments, the epitaxial growth of the first epitaxial layer 62 includes one or more deposition stages and one or more etching stages to control the shape of the epitaxial layer. The deposition and etching stages can be performed alternately. In some embodiments, the substrate 10 is a (100) Si substrate. The SiAs first epitaxial layer grows faster along the (100) plane than the (110) and (111) planes. However, the post-etching SiAs first epitaxial layer 62 forms a small facet of (111) at the top, and is etched faster along the (110) and (111) directions than along the (100) direction. Therefore, in some embodiments, there is a thickness difference between the bottom and the side of the first epitaxial layer. In some embodiments, the bottom thickness is greater than the side thickness, and the thickness difference between the bottom (along the vertical or Z direction) and along the channel side (along the Y direction) is between about 5nm and about 10nm.
[0058] After forming the first epitaxial layer 62, the second epitaxial layer 64 includes a lower layer 64-1 and an upper layer 64-2 formed on the first epitaxial layer. Fig. 10A , Fig. 10B , Fig.11A and Fig. 11B In some embodiments, the second epitaxial layer 64 includes SiP or SiCP.
[0059] In some embodiments, the phosphorus (P) concentration in the second epitaxial layer 64 is between about 2×10 20 Atom / cm 3 With about 1×10 22 Atom / cm 3 and in other embodiments between about 5×10 20 Atom / cm 3 With about 5 × 10 21 Atom / cm 3If the P concentration is too low, the resistance of the second epitaxial layer increases; and if the P concentration is too high, the stress applied to the channel is weakened.
[0060] like Fig. 10A and Fig. 10B As shown, the lower layer 64-1 grows substantially symmetrically about the corresponding fin structure. In some embodiments, the epitaxial growth of the lower epitaxial layer 64-1 includes one or more deposition stages and one or more etching stages that can be performed alternately to control the shape of the epitaxial layer. After the last etching stage, in some embodiments, a (110) facet is formed on the top of the lower layer 64-1. Fig. 10A As shown in FIG. 1 , the lower layer 64 - 1 of the second epitaxial layer does not merge with the lower layer 64 - 1 above the adjacent fin structure.
[0061] Then, if Fig.11A and Fig. 11B As shown, the upper layer 64-2 is formed so that the second epitaxial layers of adjacent fin structures merge with each other through the upper layer 64-2. Fig.11A As shown in , the merging point is located at a plane relatively high from the surface of the isolation insulating layer 30. In some embodiments, when the fin height (under the sacrificial gate structure) from the upper surface of the isolation insulating layer is H1, the height H2 of the bottom of the merging point is between about 0.5H1 and about 0.8H1, and in other embodiments, between about 0.65H1 and 0.75H1. In some embodiments, the thickness H3 of the upper layer 64-2 at the merging point is between about 7nm and about 30nm. Fig. 10A As shown in FIG. 6 , a gap 65 is formed below the merging point. After forming the upper layer 64 - 2 , the upper surface of the second epitaxial layer 64 has a wavy shape having a non-uniformity (peak to valley) between about 2 nm and about 10 nm in the Z direction in some embodiments.
[0062] In some embodiments, the P concentration in the lower layer 64-1 is the same as or different from the P concentration in the upper layer 64-2. In some embodiments, the upper layer 64-2 is formed after performing the etching phase of the lower layer 64-1. During the formation of the upper layer 64-2, no etching phase is included. In some embodiments, the thickness of the second epitaxial layer along the Z direction is between about 10nm and about 50nm. In some embodiments, the second epitaxial layer 64 is deposited until it is equal to or slightly below (less than 2nm) the plane of the bottom of the gate sidewall spacer 48. In other embodiments, the second epitaxial layer 64 is deposited to be slightly higher than (less than 2nm) the top of the fin structure 20 under the sacrificial gate structure. In some embodiments, the thickness ratio of the upper layer 64-2 to the lower layer 64-1 along the vertical direction above the fin structure is between about 0.1 and about 0.3.
[0063] Then, if Fig. 12A and Fig. 12B As shown, a third epitaxial layer 66 is formed on the second epitaxial layer 64. In some embodiments, the third epitaxial layer 66 includes SiP or SiCP. In some embodiments, the third epitaxial layer 66 further includes Ge to reduce the contact resistance of the source / drain contacts formed subsequently.
[0064] In some embodiments, the phosphorus (P) concentration in the third epitaxial layer 66 is equal to or less than the phosphorus (P) concentration in the second epitaxial layer 64 and is between about 2×10 20 Atom / cm 3 With about 1×10 22 Atom / cm 3 In other embodiments, the range is between about 5×10 20 Atom / cm 3 With about 5×10 21 Atom / cm 3 If the P concentration is too low, the resistance of the second epitaxial layer increases, and if the P concentration is too high, the stress applied to the channel will be weakened. In some embodiments, the Ge concentration in the third epitaxial layer 66 is between about 0.2 atomic % and about 10 atomic %, and in other embodiments between about 0.5 atomic % and about 5 atomic %. A small amount of Ge promotes TiSi formation and reduces contact resistance, while this effect cannot be obtained when the amount is too small. When the Ge concentration is too high, Ge sintering is induced during TiSi formation and increases contact resistance and defects, and also weakens the stress in the epitaxial layer. In some embodiments, epitaxially growing the third epitaxial layer 66 includes one or more deposition stages and one or more etching stages that can be alternately performed to control the shape of the epitaxial layer. In some embodiments, the thickness of the third epitaxial layer along the Z direction is between about 5nm and about 10nm. If the thickness is too small, the desired epitaxial layer shape cannot be obtained. If the thickness is too large, it will induce merging with nearby NFET or PFET devices and also weaken the wavy shape. In some embodiments, the third epitaxial layer 66 completely covers the surface of the second epitaxial layer 64 except the gap 65 and contacts the first epitaxial layer. In some embodiments, the first and third epitaxial layers sandwiching the second epitaxial layer inhibit phosphorus from diffusing outward from the second epitaxial layer to the channel region or the metal gate electrode. Fig.13A and Fig. 13B As shown, a fourth epitaxial layer 68 is formed as a protective layer on the third epitaxial layer 66. In some embodiments, the fourth epitaxial layer 68 includes SiP or SiCP. In some embodiments, Ge is not included in the fourth epitaxial layer.
[0065] In some embodiments, the phosphorus (P) concentration in the fourth epitaxial layer 68 is equal to or different from the phosphorus (P) concentration in the third epitaxial layer 66 and is between about 2×1020 Atom / cm 3 With about 1×10 22 Atom / cm 3 In other embodiments, the range is between about 5×10 20 Atom / cm 3 With about 5×10 21 Atom / cm 3 In some embodiments, the thickness of the fourth epitaxial layer 68 along the Z direction is between about 5 nm and about 10 nm. The fourth epitaxial layer 68 grows mainly in the (100) direction, which maintains the (100) shape on the fin structure and the (110) shape between the fin structures. Fig.13A As shown in , the first to fourth epitaxial layers are collectively referred to as source / drain epitaxial layer (structure) 60 .
[0066] Fig.14 A line drawing of a TEM image of the source / drain structure 60 is shown. Due to the light-transmitting nature of the TEM, the fin structure under the sacrificial gate can also be seen. Fig.14 , dimension T1 corresponds to the thickness of the first epitaxial layer 62 and is between about 5 nm and about 20 nm in some embodiments. In some embodiments, the top of the first epitaxial layer 62 is located at about 80% to about 100% of the height of the fin mask layer 50 and / or the sidewall spacer 48 on the fin structure from the upper surface of the isolation insulating layer 30.
[0067] Dimension T2 is the height of the bottom of the merge point from the upper surface of the isolation insulating layer 30, and in some embodiments is between about 20 nm and about 50 nm. In some embodiments, the merge point is located at or above 75% of the height T6 of the top of the fin structure under the sacrificial gate structure from the upper surface of the isolation insulating layer. The high merge point of the second epitaxial layer can improve the short channel effect.
[0068] Dimension T3 is the distance between the top of the first epitaxial layer and the bottom of the merge point. Dimension T4 is the thickness of the merge point. The merge point is defined at a central position adjacent to the fin structure. In some embodiments, thickness T4 is between about 5 nm and about 20 nm, depending on process and / or design requirements. If thickness T4 is too small, then the margin for the source / drain contacts may be insufficient, and if thickness T4 is too thick, then the top surface of the source / drain epitaxial layer may be flatter, which will increase the contact resistance of the source / drain contacts. Dimension T5 is the thickness of the source / drain epitaxial layer on the top of the fin structure, and in some embodiments is between about 2 nm and about 10 nm. If thickness T5 is too small, then the margin for the source / drain contacts may be insufficient, and if thickness T5 is too thick, then the top surface of the source / drain epitaxial layer may be flatter, which will increase the contact resistance of the source / drain contacts.
[0069] Dimension T6 is the material (channel) height from the bottom of the first epitaxial layer (or the upper surface of the isolation insulating layer) to the top of the fin structure, and is between about 40nm and about 80nm, depending on the process and / or design requirements. Dimension T7 is the total height from the bottom of the first epitaxial layer (or the upper surface of the isolation insulating layer) to the top of the source / drain epitaxial layer, and is between about 50nm and about 90nm, depending on the process and / or design requirements. In some embodiments, the ratio T4 / T7 is between about 0.1 and about 0.3, and in other embodiments is between about 0.15 and about 0.25. Dimension W is the total (maximum) width of the combined source / drain epitaxial layer 60, and is between about 40nm and about 80nm, depending on the process and / or design requirements.
[0070] Fig.15 FIG. 2 shows a process flow for forming a source / drain epitaxial layer 60 of an n-type FET according to an embodiment of the present invention. After recessing the source / drain region of the fin structure to form the source / drain spacer 22, a pre-cleaning operation is performed, such as Fig.15 In some embodiments, the pre-cleaning operation includes a plasma treatment using Ar and / or NH3 plasma. In some embodiments, the process temperature is between about 300°C and about 600°C. Next, a pre-etching operation is performed to control the shape of the subsequently formed epitaxial layer, such as Fig.15 In some embodiments, the pre-etching operation is performed in a H2 and HCl gas environment. The process temperature is higher than the process temperature of the pre-cleaning operation, and in some embodiments is between about 550°C and about 750°C.
[0071] Next, a first epitaxial layer 62 ( ) is formed by using a gas containing Si, such as SiH 4 , Si 2 H 6 , or SiCl 2 H 2 , and a dopant gas, such as AsH 3 or organic As with H 2 as a carrier gas. Fig.15 1). The process temperature for forming the first epitaxial layer 62 is equal to or higher than the process temperature of the pre-etching operation, and in some embodiments is between about 650°C and about 750°C. After forming the first epitaxial layer 62, an etching operation is performed to control the shape of the epitaxial layer. In some embodiments, the etching operation includes a plasma or dry treatment using N2 and HCl gases. The process temperature is higher than the growth temperature of the first epitaxial layer and in some embodiments is between about 700°C and about 800°C.
[0072] After forming and etching the first epitaxial layer 62, the second epitaxial layer 64 (64-1 and 64-2) is formed. Fig.15The process temperature for forming the second epitaxial layer 64 is lower than the process temperature of the L1 etching operation and the process temperature for forming the first epitaxial layer 62, and in some embodiments is between about 600° C. and about 700° C. The second epitaxial layer 64 is formed by using a Si-containing gas, such as SiH4, Si2H6, or SiCl2H2, and a dopant gas, such as PH3 or organic As with H2 or N2 as a carrier gas.
[0073] In some embodiments, after forming the second epitaxial layer 64, a cleaning operation is optionally performed. The cleaning operation includes chemical dry cleaning (etching) using SiH4 and / or GeH4 and HCl gas. The process temperature of the cleaning operation is lower than the process temperature of forming the first epitaxial layer 62 and higher than the process temperature of forming the second epitaxial layer 64, and in some embodiments is between about 650° C. and about 750° C.
[0074] After the cleaning operation, a third epitaxial layer 66 ( Fig.15 Indicated as L3 in FIG. 1 ). The process temperature for forming the third epitaxial layer 66 is higher than the process temperature for forming the first and second epitaxial layers, and in some embodiments is between about 650° C. and about 750° C. The third epitaxial layer 66 is formed by using a gas containing Si, such as SiH4, Si2H6, or SiCl2H2, a gas containing Ge, such as GeH4 or Ge2H6, and a dopant gas, such as PH3 or organic As with H2 or N2 as a carrier gas. After forming the third epitaxial layer 66, an etching operation is performed to control the shape of the epitaxial layer. In some embodiments, the etching operation includes a plasma or dry treatment using GeH4, H2, and HCl gases. The process temperature is higher than the growth temperature of the third epitaxial layer, and in some embodiments is between about 750° C. and about 800° C. The L3 etch creates a V shape between the fin structures.
[0075] Next, a fourth epitaxial layer 68 ( ) is formed by using a gas containing Si, such as SiH4, Si2H6 or SiCl2H2, and a dopant gas, such as PH3 or organic As with H2 or N2 as a carrier gas. Fig.15 The process temperature for forming the fourth epitaxial layer 68 is lower than the process temperature of the L3 etching operation and the L3 deposition, and is between about 650° C. and about 750° C. in some embodiments.
[0076] In some embodiments, Figure 1 At S110 of the embodiment, after forming the epitaxial layer 60 of the n-type FET, the fin mask layer and the sidewall are removed. In other embodiments, the fin mask layer and the sidewall spacer are removed. In some embodiments, Figure 1At S110, the capping layer covering the p-type region is removed, and then Figure 1 Cleaning operation at S111.
[0077] Then, similar to Figure 1 The operation of S106 at S112 forms a fin mask layer (fin sidewall) of the p-type FET, and then Figure 1 At S113, a recess is formed in the source / drain region of the fin structure of the p-type FET. The process for making the recess of the p-type FET is the same or similar to the process for making the recess 22 of the n-type FET. Figure 1 At S114 , a cleaning operation similar to that of S108 is performed.
[0078] Then, in Figure 1 At S115, an epitaxial source / drain structure of a p-type FET is formed above the recessed fin structure 20. The epitaxial source / drain structure is made of one or more semiconductor material layers having a lattice constant different from that of the fin structure 20 (channel region). When the fin structure is made of Si, the epitaxial source / drain structure contains SiGe or Ge for p-channel FinFET. The epitaxial source / drain structure is formed epitaxially on the upper part of the recessed fin structure. The source / drain epitaxial layer can be grown at a temperature of about 600° C. to 800° C. and a pressure of about 80 Torr to 150 Torr by using a gas containing Si, such as SiH4, Si2H6, or SiCl2H2; and a gas containing Ge, such as GeH4, Ge2H6, or GeCl2H2. In some embodiments, the source / drain epitaxial layer further contains boron.
[0079] Then, in Figure 1 At S117, Fig.16A , 16B As shown in Fig. 16C, an insulating layer used as a contact etch stop layer is formed over the metal gate structure and the source / drain structure 60, and then an interlayer dielectric (ILD) layer 90 is formed. The ILD layer 90 is one or more insulating material layers. In one embodiment, the etch stop layer is made of silicon nitride formed by CVD. The material used for the ILD layer 90 includes a compound, The compound includes Si, O, C and / or H, such as silicon oxide, SiCOH and SiOC. Organic materials, such as polymers, can be used for the ILD layer 90.
[0080] Then, in Figure 1At S118 of the embodiment, a metal gate structure is formed by using a gate replacement technique. After forming the interlayer dielectric layer 90, a CMP operation is performed to expose the dummy gate electrode 44. The dummy gate structure (dummy gate electrode 44 and dummy gate dielectric layer 42) is then removed and replaced with a metal gate (metal gate electrode 86 and gate dielectric layer 82) structure, as shown in FIG. Fig. 16B and Fig. 16C as shown in .
[0081] The dummy gate electrode 44 and the dummy gate dielectric layer 42 are removed by appropriate etching processes to form a gate opening. The metal gate structure includes a gate dielectric layer 82 and a metal gate electrode 86 formed in the gate opening.
[0082] A gate dielectric layer 82 is formed over the interface layer (not shown), and in some embodiments the gate dielectric layer is disposed over the channel layer of the fin structure 20. In some embodiments, the interface layer may include silicon oxide or germanium oxide, having a thickness of 0.2 nm to 1.5 nm. In other embodiments, the thickness of the interface layer is between 0.5 nm and about 1.0 nm.
[0083] The gate dielectric layer 82 includes one or more dielectric material layers, such as silicon oxide, silicon nitride or high-k dielectric materials, other suitable dielectric materials and / or combinations thereof. Examples of high-k dielectric materials include HfO2, HfSiO, HfSiON, HfTaO, HfTiO, HfZrO, zirconium oxide, aluminum oxide, titanium oxide, hafnium oxide-aluminum oxide (HfO2-Al2O3) alloys, other suitable high-k dielectric materials and / or combinations thereof. The gate dielectric layer is formed by, for example, chemical vapor deposition (CVD), physical vapor deposition (PVD), atomic layer deposition (ALD), high-density plasma CVD (HDPCVD), or other suitable methods, and / or combinations thereof. In some embodiments, the thickness of the gate dielectric layer is between about 1 nm and about 10 nm, and in other embodiments between about 2 nm and about 7 nm.
[0084] A metal gate electrode 86 is formed over the gate dielectric layer. The metal gate electrode 86 includes one or more layers of any suitable metal material, such as aluminum, copper, titanium, tantalum, cobalt, molybdenum, tantalum nitride, nickel silicide, cobalt silicide, TiN, WN, TiAl, TiAlN, TaCN, TaC, TaSiN, metal alloys, other suitable materials, and / or combinations thereof.
[0085] In certain embodiments of the present invention, one or more work function regulating layers 84N, 84P are inserted between the gate dielectric layer and the metal gate electrode. The work function regulating layer is made of a conductive material, such as a single layer of TiN, TaN, TaAlC, TiC, TaC, Co, Al, TiAl, HfTi, TiSi, TaSi or TiAlC, or a multilayer of two or more of these materials. For n-channel FinFETs, one or more of TaN, TaAlC, TiN, TiC, Co, TiAl, HfTi, TiSi and TaSi are used as the work function regulating layer 84N, and for p-channel FinFETs, one or more of TiAlC, Al, TiAl, TaN, TaAlC, TiN, TiC and Co are used as the work function regulating layer 84P.
[0086] After depositing a suitable material for the metal gate structure, a planarization operation such as CMP is performed.
[0087] After the metal gate structure is formed, one or more interlayer dielectric layers are formed on the metal gate structure and the interlayer dielectric layer 90. The interlayer dielectric layers are collectively referred to as interlayer dielectric layers 95. Fig.17 FIG. 17 shows a line drawing of a TEM image of the source / drain structure 60 and the source / drain contacts.
[0088] exist Figure 1 At S119, a contact hole is formed in the interlayer dielectric layer 95 by using a patterning operation including photolithography to expose the epitaxial source and drain structure 60. Next, the contact hole is filled with a conductive material to form a contact plug 100, such as Fig.17 The contact plug 100 may include any suitable metal, for example, a single layer or multiple layers of Co, W, Ti, Ta, Cu, Al and / or Ni and / or nitrides thereof.
[0089] After forming the contact plugs, further CMOS processes are performed to form various features, such as additional interlayer dielectric layers, contacts / vias, interconnect metal layers, and passivation layers.
[0090] In some embodiments, Figure 1 At S106, in some embodiments, after forming the epitaxial source / drain structure 60, a silicide layer 70 is formed above the epitaxial source / drain structure 60 (see Fig.17). A metal material such as Ni, Ti, Ta and / or W is formed over the epitaxial source / drain structure 60 and an annealing operation is performed to form a silicide layer 70. In other embodiments, a silicide material such as NiSi, TiSi, TaSi and / or WSi is formed over the epitaxial source / drain structure 60 and an annealing operation is performed. The annealing operation is performed at a temperature of about 250° C. to about 850° C. The metal material or silicide material is formed by CVD or ALD. In some embodiments, the thickness of the silicide layer 70 is between about 4 nm and about 10 nm. Before or after the annealing operation, the metal material or silicide material formed over the isolation insulating layer 30 is selectively removed.
[0091] In other embodiments, the silicide layer 70 is formed after the contact hole is opened. In this case, after the epitaxial source / drain structure 60 is formed, the metal gate structure, the contact etch stop layer and the interlayer dielectric layer 95 are formed without forming the silicide layer. Then, a contact hole is formed in the interlayer dielectric layer 95 to expose the upper surface of the epitaxial source / drain structure 60, and then a silicide layer is formed on the upper surface of the epitaxial source / drain structure 60. After the silicide layer is formed, a conductive material is formed in the contact hole to form a contact plug.
[0092] Fig.18 After forming the source / drain epitaxial layer 60, Fig. 13B Element analysis in the depth direction Z shown in . Fig.18 As shown in FIG. 1 , the arsenic in the first epitaxial layer 62 ( L1 ) can effectively inhibit the diffusion of P from the second epitaxial layer 64 ( L2 ) into the fin structure.
[0093] Although the foregoing embodiments describe FinFETs, the techniques disclosed in the present invention are also applicable to other types of FETs, such as planar FETs and gate-all-around (GAA) FETs using nanowire or nanosheet semiconductors.
[0094] In the embodiment of the present invention, by forming the SiAs layer as the first epitaxial layer, it is possible to suppress the diffusion of P from the second epitaxial layer into the channel region. In addition, by setting the merging point of the merged epitaxial layers to a relatively high position, it is possible to improve the short channel effect.
[0095] It will be understood that not all advantages are necessarily discussed herein, that all embodiments or examples do not require a particular advantage, and that other embodiments or examples may provide different advantages.
[0096] According to one aspect of the present invention, a method for manufacturing a semiconductor device includes: forming a first fin structure and a second fin structure above a substrate; forming an isolation insulating layer above the substrate so that the lower portions of the first and second fin structures are embedded in the isolation insulating layer and the upper portions of the first and second fin structures are exposed outside the isolation insulating layer; forming a gate structure above the channel regions of the first and second fin structures; recessing the source / drain regions of the first and second fin structures; and forming an epitaxial source / drain structure above the recessed first and second fin structures. The epitaxial source / drain structure is a merged structure having a merge point, and the height of the bottom of the merge point from the upper surface of the isolation insulating layer is 50% or more of the height of the channel regions of the first and second fin structures from the upper surface of the isolation insulating layer. In one or more of the foregoing and following embodiments, the height of the bottom of the merge point from the upper surface of the isolation insulating layer is 75% or more of the height of the channel regions of the first and second fin structures from the upper surface of the isolation insulating layer. In one or more of the foregoing and following embodiments, the epitaxial source / drain structure includes a first, second, third and fourth epitaxial layers formed in this order above the recessed first and second fin structures. In one or more of the foregoing and following embodiments, the first epitaxial layer above the recessed first fin structure does not merge with the first epitaxial layer of the recessed second fin structure, and the second epitaxial layer produces a merging point. In one or more of the foregoing and following embodiments, the first epitaxial layer includes SiAs and the second epitaxial layer includes SiP. In one or more of the foregoing and following embodiments, the third epitaxial layer includes SiP doped with Ge, and the fourth epitaxial layer includes SiP. In one or more of the foregoing and following embodiments, the P concentration of the second epitaxial layer is the highest among the first to fourth epitaxial layers. In one or more of the foregoing and following embodiments, the third epitaxial layer is in contact with the first epitaxial layer.
[0097] According to another aspect of the present invention, a method for manufacturing a semiconductor device includes: forming a first fin structure and a second fin structure above a substrate; forming an isolation insulating layer above the substrate so that the lower portions of the first and second fin structures are embedded in the isolation insulating layer and the upper portions of the first and second fin structures are exposed outside the isolation insulating layer; forming fin sidewalls on opposite sides of the source / drain regions of the first and second fin structures; recessing the source / drain regions of the first and second fin structures; forming a first epitaxial layer above the recessed first and second fin structures, respectively; forming a second epitaxial layer having a composition different from that of the first epitaxial layer, respectively, above the first epitaxial layer to form a merged second epitaxial layer having a merge point. The height of the bottom of the merge point from the upper surface of the isolation insulating layer is 50% or more of the height of the channel regions of the first and second fin structures from the upper surface of the isolation insulating layer. In one or more of the foregoing and following embodiments, forming the second epitaxial layer includes one or more deposition stages and one or more etching stages that are performed alternately. In one or more of the foregoing and following embodiments, forming the second epitaxial layer includes forming a lower layer above the first epitaxial layer without forming the merged second epitaxial layer, and forming an upper layer above the lower layer forming the second epitaxial layer, and forming the upper layer does not include an etching stage. In one or more of the foregoing and following embodiments, the upper layer is formed after the etching stage of the lower layer. In one or more of the foregoing and following embodiments, the first epitaxial layer includes SiAs having a thickness between 1×10 20 Atom / cm 3 With 2×10 21 Atom / cm 3 In one or more of the foregoing and following embodiments, the second epitaxial layer comprises SiP having a concentration between 5×10 20 Atom / cm 3 With 5×10 21 Atom / cm 3 In one or more of the foregoing and following embodiments, the first epitaxial layer is formed to not exceed the top of the fin sidewall. In one or more of the foregoing and following embodiments, the fin sidewall includes a plurality of layers.
[0098] According to another aspect of the present invention, a method for manufacturing a semiconductor device includes: forming a first fin structure and a second fin structure above a substrate; forming an isolation insulating layer above the substrate so that the lower portions of the first and second fin structures are embedded in the isolation insulating layer and the upper portions of the first and second fin structures are exposed outside the isolation insulating layer; forming fin sidewalls on opposite sides of the source / drain regions of the first and second fin structures; recessing the source / drain regions of the first and second fin structures; at a first temperature, forming a first epitaxial layer above the recessed first and second fin structures, respectively; at a second temperature, performing an etching operation on the first epitaxial layer; at a third temperature, forming a second epitaxial layer having a composition different from that of the first epitaxial layer, respectively, above the first epitaxial layer; at a fourth temperature, forming a third epitaxial layer having a composition different from that of the second epitaxial layer above the second epitaxial layer; at a fifth temperature, performing an etching operation on the third epitaxial layer; and at a sixth temperature, forming a fourth epitaxial layer having a composition different from that of the third epitaxial layer above the third epitaxial layer. In one or more of the foregoing and following embodiments, the second epitaxial layer forms a merged second epitaxial layer having a merge point, and the height of the bottom of the merge point from the upper surface of the isolation insulating layer is 50% or more of the height of the channel region of the first and second fin structures from the upper surface of the isolation insulating layer. In one or more of the foregoing and following embodiments, forming the second epitaxial layer includes one or more deposition stages and one or more etching stages that are performed alternately. In one or more of the foregoing and following embodiments, forming the second epitaxial layer includes forming a lower layer above the first epitaxial layer that does not form a merged second epitaxial layer, and forming an upper layer above the lower layer that forms the second epitaxial layer, and forming the upper layer does not include an etching stage. In one or more of the foregoing and following embodiments, wherein the second temperature is higher than the first temperature. In one or more of the foregoing and following embodiments, the third temperature is lower than the second temperature. In one or more of the foregoing and following embodiments, the fourth temperature is higher than the third temperature. In one or more of the foregoing and following embodiments, the fifth temperature is higher than the fourth temperature.
[0099] According to another aspect of the present invention, a semiconductor device includes: an isolation insulating layer disposed above a substrate; a first fin structure and a second fin structure disposed above the substrate; a gate structure disposed above the channel region of the first and second fin structures; and a source / drain epitaxial layer on the source / drain region of the first and second fin structures. The source / drain epitaxial layer has a merged structure, the merged structure has a merged point, and the height of the bottom of the merged point from the upper surface of the isolation insulating layer is 65% or more of the height of the channel region of the first and second fin structures from the upper surface of the isolation insulating layer. In one or more of the foregoing and following embodiments, the vertical thickness of the merged point is between 10% and 30% of the height of the source / drain epitaxial layer from the upper surface of the isolation insulating layer. In one or more of the foregoing and following embodiments, the source / drain epitaxial layer includes a first, second, third and fourth epitaxial layer formed in this order above the recessed first and second fin structures. In one or more of the foregoing and following embodiments, the first epitaxial layer includes SiAs, and the second epitaxial layer includes SiP. A fin structure is formed above the substrate.
[0100] According to one embodiment of the present application, a method for manufacturing a semiconductor device is provided, the method comprising: forming a first fin structure and a second fin structure above a substrate; forming an isolation insulating layer above the substrate so that the lower portions of the first fin structure and the second fin structure are embedded in the isolation insulating layer and the upper portions of the first fin structure and the second fin structure are exposed to the isolation insulating layer; forming a gate structure above the channel region of the first fin structure and the second fin structure; recessing the source / drain region of the first fin structure and the second fin structure; and forming an epitaxial source / drain structure above the recessed first fin structure and the second fin structure, wherein the epitaxial source / drain structure is a merged structure having a merge point, and the height of the bottom of the merge point from the upper surface of the isolation insulating layer is 50% or more of the height of the channel region of the first fin structure and the second fin structure from the upper surface of the isolation insulating layer. In some embodiments, the height of the bottom of the merge point from the upper surface of the isolation insulating layer is 75% or more of the height of the channel region of the first fin structure and the second fin structure from the upper surface of the isolation insulating layer. In some embodiments, the epitaxial source / drain structure includes a first epitaxial layer, a second epitaxial layer, a third epitaxial layer, and a fourth epitaxial layer sequentially formed above the recessed first fin structure and the second fin structure. In some embodiments, the first epitaxial layer above the recessed first fin structure and the first epitaxial layer above the recessed second fin structure do not merge, and the second epitaxial layer generates a merge point. In some embodiments, the first epitaxial layer includes As and the second epitaxial layer includes P. In some embodiments, the third epitaxial layer includes SiP doped with Ge, and the fourth epitaxial layer includes SiP. In some embodiments, the P concentration of the second epitaxial layer is the highest among the first epitaxial layer to the fourth epitaxial layer. In some embodiments, the third epitaxial layer contacts the first epitaxial layer.
[0101] According to another embodiment of the present application, a method for manufacturing a semiconductor device is provided, the method comprising: forming a first fin structure and a second fin structure above a substrate; forming an isolation insulating layer above the substrate so that the lower portions of the first fin structure and the second fin structure are embedded in the isolation insulating layer and the upper portions of the first fin structure and the second fin structure are exposed to the isolation insulating layer; forming fin sidewalls on opposite sides of the source / drain regions of the first fin structure and the second fin structure; recessing the source / drain regions of the first fin structure and the second fin structure; at a first temperature, forming a first epitaxial layer above the recessed first fin structure and the second fin structure, respectively; at a second temperature, performing an etching operation on the first epitaxial layer; at a third temperature, forming a second epitaxial layer having a composition different from that of the first epitaxial layer, respectively, above the first epitaxial layer; at a fourth temperature, forming a third epitaxial layer having a composition different from that of the second epitaxial layer above the second epitaxial layer; at a fifth temperature, performing an etching operation on the third epitaxial layer, and at a sixth temperature, forming a fourth epitaxial layer having a composition different from that of the third epitaxial layer above the third epitaxial layer. In some embodiments, wherein: the second epitaxial layer forms a merged second epitaxial layer having a merge point, and the height of the bottom of the merge point from the upper surface of the isolation insulating layer is 50% or more of the height of the channel region of the first fin structure and the second fin structure from the upper surface of the isolation insulating layer. In some embodiments, forming the second epitaxial layer includes one or more deposition stages and one or more etching stages that are performed alternately. In some embodiments, wherein: forming the second epitaxial layer includes forming a lower layer above the first epitaxial layer that does not form the merged second epitaxial layer, and forming an upper layer above the lower layer that forms the second epitaxial layer, and forming the upper layer does not include an etching stage. In some embodiments, the second temperature is higher than the first temperature. In some embodiments, the third temperature is lower than the second temperature. In some embodiments, the fourth temperature is higher than the third temperature. In some embodiments, the fifth temperature is higher than the fourth temperature.
[0102] According to another embodiment of the present application, a semiconductor device is provided, comprising: an isolation insulating layer, arranged above a substrate; a first fin structure and a second fin structure, arranged above the substrate; a gate structure, arranged above the channel region of the first fin structure and the second fin structure; and a source / drain epitaxial layer, arranged above the source / drain region of the first fin structure and the second fin structure, wherein: the source / drain epitaxial layer has a merged structure, the merged structure has a merged point, and the height of the bottom of the merged point from the upper surface of the isolation insulating layer is 65% or more of the height of the channel region of the first fin structure and the second fin structure from the upper surface of the isolation insulating layer. In some embodiments, the vertical thickness of the merged point is between 10% and 30% of the height of the source / drain epitaxial layer from the upper surface of the isolation insulating layer. In some embodiments, the source / drain epitaxial layer includes a first epitaxial layer, a second epitaxial layer, a third epitaxial layer, and a fourth epitaxial layer above the recessed first fin structure and the second fin structure. In some embodiments, the first epitaxial layer includes SiAs, and the second epitaxial layer includes SiP.
[0103] The features of several embodiments are summarized above so that those skilled in the art can better understand aspects of the present invention. Those skilled in the art should understand that they can easily use the present invention as a basis to design or modify other processes and structures for implementing the same purpose and / or achieving the same advantages as the embodiments introduced herein. Those skilled in the art should also appreciate that such equivalent constructions do not deviate from the spirit and scope of the present invention, and that they can make various changes, substitutions and modifications herein without departing from the spirit and scope of the present invention.
Claims
1. A method for manufacturing a semiconductor device, the method comprising: forming a first fin structure and a second fin structure over the substrate; forming an isolation insulating layer over the substrate, such that lower portions of the first fin structure and the second fin structure are embedded in the isolation insulating layer and upper portions of the first fin structure and the second fin structure are exposed to the isolation insulating layer; forming a gate structure above the channel regions of the first fin structure and the second fin structure; forming fin sidewalls on opposite sides of the source / drain regions of the first fin structure and the second fin structure; recessing the source / drain regions of the first and second fin structures, wherein, after recessing the source / drain regions of the first and second fin structures, a remaining fin sidewall of a first fin structure of the adjacent first and second fin structures has a lower height on a side facing the second fin structure than the fin sidewalls on other sides of the first fin structure; and forming an epitaxial source / drain structure above the recessed first fin structure and the second fin structure, Wherein, the epitaxial source / drain structure is a merged structure with a merge point, and A height of the bottom of the merging point from the upper surface of the isolation insulating layer is 50% or more of a height of the channel regions of the first fin structure and the second fin structure from the upper surface of the isolation insulating layer. The epitaxial source / drain structure includes a first epitaxial layer, a second epitaxial layer, a third epitaxial layer and a fourth epitaxial layer formed sequentially above the recessed first fin structure and the second fin structure, and the P concentration of the second epitaxial layer is the highest among the first epitaxial layer to the fourth epitaxial layer.
2. The method according to claim 1, wherein The height of the bottom of the merging point from the upper surface of the isolation insulating layer is 75% or more of the height of the channel regions of the first and second fin structures from the upper surface of the isolation insulating layer.
3. The method according to claim 1, wherein The second epitaxial layer includes SiP.
4. The method according to claim 1, wherein The first epitaxial layer over the recessed first fin structure and the first epitaxial layer over the recessed second fin structure do not merge, and the second epitaxial layer creates the merge point.
5. The method according to claim 1, wherein The first epitaxial layer contains As.
6. The method according to claim 5, wherein: The third epitaxial layer includes SiP doped with Ge, and the fourth epitaxial layer includes SiP.
7. The method according to claim 5, wherein: The first epitaxial layer includes SiAs.
8. The method according to claim 3, wherein: The third epitaxial layer contacts the first epitaxial layer.
9. A method for manufacturing a semiconductor device, the method comprising: forming a first fin structure and a second fin structure over the substrate; forming an isolation insulating layer over the substrate, such that lower portions of the first fin structure and the second fin structure are embedded in the isolation insulating layer and upper portions of the first fin structure and the second fin structure are exposed to the isolation insulating layer; forming fin sidewalls on opposite sides of the source / drain regions of the first fin structure and the second fin structure; recessing the source / drain regions of the first and second fin structures, wherein, after recessing the source / drain regions of the first and second fin structures, a remaining fin sidewall of a first fin structure of the adjacent first and second fin structures has a lower height on a side facing the second fin structure than the fin sidewalls on other sides of the first fin structure; forming a first epitaxial layer on the recessed first fin structure and the recessed second fin structure at a first temperature; performing an etching operation on the first epitaxial layer at a second temperature; forming second epitaxial layers having a different composition from the first epitaxial layers over the first epitaxial layers at a third temperature; forming a third epitaxial layer having a different composition than the second epitaxial layer over the second epitaxial layer at a fourth temperature; performing an etching operation on the third epitaxial layer at a fifth temperature, and forming a fourth epitaxial layer having a different composition than the third epitaxial layer over the third epitaxial layer at a sixth temperature, The fourth temperature is higher than the third temperature and the first temperature, and the third temperature is lower than the first temperature.
10. The method according to claim 9, wherein: The second epitaxial layer forms a merged second epitaxial layer having a merge point, and A height of a bottom of the merging point from an upper surface of the isolation insulating layer is 50% or more of a height of a channel region of the first fin structure and the second fin structure from the upper surface of the isolation insulating layer.
11. The method according to claim 9, wherein The forming of the second epitaxial layer includes alternatingly performing one or more deposition phases and one or more etching phases.
12. The method according to claim 10, wherein: The forming of the second epitaxial layer includes forming a lower layer on the first epitaxial layer where the merged second epitaxial layer is not formed, and forming an upper layer on the lower layer where the second epitaxial layer is formed, and The forming of the upper layer does not include an etching stage.
13. The method according to claim 11, wherein The second temperature is higher than the first temperature.
14. The method according to claim 13, wherein: The third temperature is lower than the second temperature.
15. The method according to claim 14, wherein The first epitaxial layer includes SiAs, and the second epitaxial layer includes SiP.
16. The method according to claim 15, wherein The fifth temperature is higher than the fourth temperature.
17. A semiconductor device comprising: an isolation insulating layer, disposed above the substrate; A first fin structure and a second fin structure are disposed above the substrate; a gate structure disposed above the channel regions of the first fin structure and the second fin structure; A source / drain epitaxial layer is disposed above the source / drain regions of the first fin structure and the second fin structure; as well as Fin sidewalls are located on opposite sides of the source / drain regions of the first fin structure and the second fin structure, wherein: The source / drain epitaxial layer has a merged structure, the merged structure has a merge point, and A height of the bottom of the merging point from the upper surface of the isolation insulating layer is 65% or more of a height of the channel regions of the first fin structure and the second fin structure from the upper surface of the isolation insulating layer. The source / drain epitaxial layer includes a first epitaxial layer, a second epitaxial layer, a third epitaxial layer, and a fourth epitaxial layer above the recessed first fin structure and the second fin structure, and the P concentration of the second epitaxial layer is the highest among the first epitaxial layer to the fourth epitaxial layer. The fin sidewall of the first fin structure of the adjacent first and second fin structures has a lower height on the side facing the second fin structure than the fin sidewalls on other sides of the first fin structure.
18. The semiconductor device according to claim 17, wherein The vertical thickness of the merging point is between 10% and 30% of the height of the source / drain epitaxial layer from the upper surface of the isolation insulating layer.
19. The semiconductor device according to claim 17, wherein The third epitaxial layer includes SiP doped with Ge, and the fourth epitaxial layer includes SiP.
20. The semiconductor device according to claim 17, wherein The first epitaxial layer includes SiAs, and the second epitaxial layer includes SiP.