Semiconductor structure and method of forming a semiconductor device
By injecting threshold modification impurities into the suspended nanostructure of nanosheet devices and adjusting their size, the problem of threshold voltage regulation in full-ring gate transistors is solved, simplified process and efficient threshold voltage control are achieved, and device performance is improved.
Patent Information
- Application Number
- CN202110449422.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-02-08
- Filing Date
- 2021-04-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-04-25
AI Technical Summary
In nanosheet devices, especially in full-ring gate (GAA) transistors, threshold voltage (Vt) regulation is difficult to control, especially due to smaller depletion areas and smaller channel volumes and migration caused by heavy doping The problem of lowering rates leads to complex and easy introduction of defects in traditional methods.
By forming vertically stacked suspended nanostructures on multiple fins and injecting thresholds therein modifying impurities such as germanium, adjusting the critical size and threshold voltage of the suspended nanostructures, combined with an etching and annealing process to form transistors with different threshold voltages, Simplify the manufacturing process to achieve wide range adjustment of threshold voltages.
The fine adjustment of the threshold voltage of the p-type GAA transistor is achieved, reducing process complexity and defect risks, and improving manufacturing efficiency and device performance.
Smart Images

Figure CN113571471B_ABST
Abstract
Description
Technical Field
[0001] Embodiments of the present application relate to semiconductor structures and methods of forming semiconductor devices. Background Art
[0002] The semiconductor integrated circuit (IC) industry has experienced exponential growth. Technological advances in IC materials and design have produced generations of ICs, each with smaller and more complex circuits than the previous generation. Over the course of IC evolution, functional density (i.e., the number of interconnected devices per chip area) has generally increased, while geometry size (i.e., the smallest component (or line) that can be produced using a manufacturing process) has decreased. This scaling down process generally provides benefits by increasing production efficiency and reducing associated costs. This scaling down has also increased the complexity of processing and manufacturing ICs, and similar developments in IC processing and manufacturing are needed to achieve these advances.
[0003] For example, efforts have been made to introduce multi-gate devices to improve gate control by increasing gate-channel coupling, reducing off-state current, and reducing short channel effects (SCE). One such multi-gate device is a nanosheet device, such as a gate-all-around (GAA) transistor, whose gate structure extends around its horizontal channel region that provides access to the channel region on all sides. Nanosheet transistors are compatible with conventional complementary metal oxide semiconductor (CMOS) processes, allowing them to aggressively scale down while maintaining gate control and mitigating SCE. However, conventional nanosheet devices have difficulty controlling their threshold voltage (Vt) due to issues such as smaller depletion regions and smaller channel volumes and reduced mobility caused by heavy doping. Therefore, while conventional nanosheet devices have generally been adequate for their intended purposes, they are not satisfactory in every respect. Summary of the invention
[0004] Some embodiments of the present application provide a method for forming a semiconductor device, comprising: providing a substrate having a plurality of first semiconductor layers and a plurality of second semiconductor layers arranged above the substrate, wherein the first semiconductor layers and the second semiconductor layers have different material compositions and are alternately arranged relative to each other in a vertical direction; patterning the first semiconductor layer and the second semiconductor layer to form a first fin and a second fin; removing the first semiconductor layer from the first fin and the second fin, so that a first portion of the patterned second semiconductor layer becomes a first suspended nanostructure in the first fin, and a second portion of the patterned second semiconductor layer becomes a second suspended nanostructure in the second fin; doping threshold modifying impurities into the first suspended nanostructure of the first fin; forming a first gate stack above the first fin, wherein a portion of the first gate stack wraps the first suspended nanostructure, thereby forming a first transistor having a first threshold voltage; and forming a second gate stack above the second fin, wherein a portion of the second gate stack wraps the second suspended nanostructure, thereby forming a second transistor having a second threshold voltage greater than the first threshold voltage.
[0005] Other embodiments of the present application provide a method for forming a semiconductor device, comprising: forming a plurality of first suspension layers in a first fin, and forming a plurality of second suspension layers in a second fin, wherein the first suspension layer and the second suspension layer include the same first semiconductor material; implementing a first etching process to simultaneously remove portions of the first suspension layer and the second suspension layer, thereby reducing the thickness of the first suspension layer and the second suspension layer; implementing a second etching process to remove an additional portion of the second suspension layer without etching the first suspension layer, thereby further reducing the thickness of the second suspension layer; and forming a first gate stack and a second gate stack that respectively join the first suspension layer and the second suspension layer.
[0006] Some other embodiments of the present application provide a semiconductor structure, including: a substrate; a first fin, disposed on the substrate, the first fin including a plurality of first suspended nanostructures stacked vertically with each other; a first gate stack, joining the first suspended nanostructure; a second fin, disposed on the substrate, the second fin including a plurality of second suspended nanostructures stacked vertically with each other; and a second gate stack, joining the second suspended nanostructure, wherein a concentration of germanium in a middle portion of the first suspended nanostructure is higher than a concentration of germanium in a middle portion of the second suspended nanostructure. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] When read in conjunction with the accompanying drawings, various aspects of the present invention can be best understood from the following detailed description. It should be emphasized that, in accordance with standard practice in the industry, the various components are not drawn to scale. In fact, for the sake of clarity of discussion, the size of the various components can be arbitrarily increased or reduced.
[0008] Figure 1A , Figure 1B and Figure 1C is a flow chart of a method of forming a semiconductor device according to various aspects of the present invention.
[0009] Figure 2 , Fig.13 and Fig.23 is a perspective view of a semiconductor structure provided according to various aspects of the present invention.
[0010] Figure 3 , Figure 4 , Figure 5 , Figure 6 , Figure 7 , Figure 8 , Fig. 9 , Fig.10 , Fig.11 , Fig.12 , Fig.14 , Fig.15 , Fig.16 , Fig.17 , Fig.18 , Fig.19 , Fig. 20 , Fig.21 , Fig. 22 , Fig.24 , Fig.25 , Fig.26 , Fig. 27 , Fig.28 , Fig.29 , Fig.30 , Fig.31 and Fig.32 According to some embodiments of the present invention Figures 1A to 1C sectional views of a semiconductor device at various manufacturing stages constructed by a corresponding method in FIG. DETAILED DESCRIPTION
[0011] The following disclosure provides many different embodiments or examples for implementing different features of the present invention. Specific examples of components and arrangements are described below to simplify the present invention. Of course, these are merely examples and are not intended to limit the present invention. For example, in the following description, forming a first component above or on a second component may include an embodiment in which the first component and the second component are directly in contact with each other, and may also include an embodiment in which an additional component may be formed between the first component and the second component so that the first component and the second component may not be in direct contact. In addition, the present invention may repeat reference numerals and / or characters in various examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or configurations discussed.
[0012] In addition, in the following invention, the formation of a component on, connected to and / or coupled to another component may include an embodiment in which the component is formed in the form of direct contact, and may include an embodiment in which an additional component may be interposed between the components so that the components may not be in direct contact. In addition, spatial relative terms such as "lower", "upper", "horizontal", "vertical", "above", "above", "below", "below", "upward", "downward", "top", "bottom" and their derivatives (e.g., "horizontally", "downward", "upward", etc.) are used to easily understand the relationship between one component of the present invention and another component. Spatial relative terms are intended to include different orientations of the device of the component. In addition, when "about", "approximately", etc. are used to describe a numerical value or a numerical range, the term is intended to cover a numerical value within a reasonable range including the numerical value, such as within + / -10% of the numerical value or other values understood by those skilled in the art. For example, the term "about 5nm" covers a size range from 4.5nm to 5.5nm.
[0013] The present invention relates generally to semiconductor devices and methods of forming the same. More particularly, the present invention relates to threshold voltage (Vt) tuning in nanosheet devices (eg, gate-all-around (GAA) devices).
[0014] A nanosheet device includes any device having its gate structure or portions thereof formed on four sides of a channel region (e.g., portions surrounding the channel region). It should first be understood that the channel region of a nanosheet device can be formed by channel components, such as nanosheets as well as nanowires, nanorods, and / or other suitable structures. In some embodiments, the channel region of a nanosheet device has a plurality of horizontal nanowires, nanosheets, and / or nanorods spaced vertically, such that the nanosheet device becomes a stacked horizontal nanosheet device. Channel components may also be referred to as nanostructures (or suspended nanostructures) due to their nanoscale dimensions. The nanosheet devices presented herein include p-type metal oxide semiconductor nanosheet devices or n-type metal oxide semiconductor nanosheet devices. In addition, the nanosheet device has one or more channels (e.g., nanowires) associated with a single, continuous gate structure or multiple gate structures. One of ordinary skill in the art may recognize other examples of semiconductor devices that may benefit from aspects of the present invention.
[0015] Described herein are embodiments of nanosheet devices for implementing n-type and p-type transistors having vertically stacked n-type channels and p-type channels located on two adjacent fins, which are generally referred to as complementary metal oxide semiconductor field effect transistors (MOSFETs) using complementary and symmetrical p-type and n-type transistor pairs. Complementary MOSFETs implemented by GAA devices are useful in many integrated circuits (ICs), but as device sizes shrink, some manufacturing methods encounter various problems. For example, threshold voltage adjustment for p-type transistors in complementary transistor pairs becomes difficult due to problems such as smaller depletion regions and smaller channel volumes and reduced mobility caused by heavy doping. Similarly, how to achieve different threshold voltages for p-type transistors in different regions (e.g., low Vt (LVt) regions, standard Vt (SVt) regions, and / or high Vt (HVt) regions) remains a challenge. Some methods require complex metal work function structures to adjust the threshold voltage for p-type transistors. However, such methods generally increase the difficulty of the process (e.g., it is difficult to deposit complex metal work function layers in high aspect ratio gate trenches) and lead to defects.
[0016] The present invention solves the above problems by providing an improved method for forming a nanosheet transistor on multiple fins. According to some embodiments, after forming a suspended nanostructure of a first fin for an n-type GAA transistor and a suspended nanostructure of a second fin for a p-type GAA transistor, the method injects a threshold modification impurity into the suspended nanostructure of the p-type GAA transistor. In some embodiments, the threshold modification impurity is germanium (Ge). The injection of the threshold modification impurity forms a unique distribution in the p-type channel. In addition, the critical dimension (CD) of the suspended nanostructure for the p-type GAA transistor can be trimmed to adjust the threshold voltage. CD trimming and threshold modification impurity doping can be combined to achieve a wider threshold voltage adjustment range. Various methods in the embodiments of the present invention can be applied to each p-type FET region in the IC to achieve the same threshold voltage adjustment, or applied to a specific p-type FET region to achieve multiple threshold voltages in different regions (such as forming an LVt region, an SVt region, and / or an HVt region). Therefore, a simplified manufacturing process can be used to achieve threshold voltage adjustment in a p-type GAA transistor.
[0017] Figure 1A 1 is a flow chart of a method 100 of forming a semiconductor device 200 (also referred to as device 200) according to various aspects of the present invention. Method 100 is merely an example and is not intended to limit the present invention beyond the scope expressly recited in the claims. Additional operations may be provided before, during, and after method 100, and some of the operations described may be replaced, eliminated, or moved for additional embodiments of the method. Figures 2 to 12 Some embodiments of method 100 are described. Figure 2 is a perspective view of the device 200 . Figures 3 to 12 is the edge of the device 200 Figure 2 The cross-sectional views shown are along the AA cut line and the BB cut line (arranged side by side), which pass through the corresponding channel region along the longitudinal direction of the transistor (in the YZ plane). Fig.12 A cross-sectional view through the channel region along the longitudinal direction of an additional p-type GAA transistor of the device 200 is also depicted.
[0018] In operation 102, method 100 ( Figure 1A ) provides a device 200 including a first device structure 206a and a second device structure 206b, such as Figure 2As shown. Each of the device structures 206a and 206b includes a substrate 208, an isolation structure 210, a fin 212a or 212b including vertically stacked alternating semiconductor layers 220 and 222 (also referred to as stacked fins 212a or 212b), and a dummy gate structure 216 that joins the stacked fins 212a and 212b. As explained in more detail below, an exemplary n-type GAA transistor will be formed from the first device structure 206a, and an exemplary p-type GAA transistor will be formed from the second device structure 206b. Device 200 is provided for illustrative purposes and does not necessarily limit embodiments of the invention to any number of devices, any number of regions, or any configuration of structures or regions. In addition, device 200 is an intermediate device manufactured during processing of an IC or a portion thereof and may include: static random access memory (SRAM) and / or logic circuits; passive components such as resistors, capacitors, and inductors; and active components such as p-type field effect transistors (PFETs), n-type FETs (NFETs), multi-gate FETs (such as FinFETs), metal oxide semiconductor field effect transistors (MOSFETs), complementary metal oxide semiconductor (CMOS) transistors, bipolar transistors, high voltage transistors, high frequency transistors, other memory cells, and combinations thereof.
[0019] In some embodiments, the substrate 208 includes silicon. Alternatively or additionally, the substrate 208 includes: another element semiconductor, such as germanium; a compound semiconductor, such as silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide and / or indium antimonide; an alloy semiconductor, such as silicon germanium (SiGe), GaAsP, AlInAs, AlGaAs, GaInAs, GaInP and / or GaInAsP; or a combination thereof. In some embodiments, the substrate 208 includes one or more III-V group materials, one or more II-IV group materials, or a combination thereof. In some embodiments, the substrate 208 is a semiconductor-on-insulator substrate, such as a silicon-on-insulator (SOI) substrate, a silicon-germanium-on-insulator (SGOI) substrate, or a germanium-on-insulator (GOI) substrate. The semiconductor-on-insulator substrate can be manufactured using isolation by implantation of oxygen (SIMOX), wafer bonding, and / or other suitable methods. The substrate 208 may include various doped regions configured according to the design requirements of the semiconductor device 200. The p-type doped region may include a p-type dopant, such as boron, indium, other p-type dopants, or a combination thereof. The N-type doped region may include an n-type dopant, such as phosphorus, arsenic, other n-type dopants, or a combination thereof. In some embodiments, the substrate 208 includes a doped region formed using a combination of a p-type dopant and an n-type dopant. Each doped region may be formed directly on and / or in the substrate 208, for example, a p-well structure, an n-well structure, a double-well structure, a raised structure, or a combination thereof. An ion implantation process, a diffusion process, and / or other suitable doping processes may be implemented to form each doped region. In some embodiments, a p-type GAA device and a p-type FinFET device are formed above the n-type well, and an n-type GAA device and an n-type FinFET device are formed above the p-type well. Each of the device structures 206a and 206b may be an n-type or p-type device, respectively.
[0020] The isolation structure 210 may include silicon oxide, silicon nitride, silicon oxynitride, fluorine-doped silicate glass (FSG), low-k dielectric material, and / or other suitable insulating materials. The isolation structure 210 may be a shallow trench isolation (STI) component. Other isolation structures such as field oxide, local oxidation of silicon (LOCOS), and / or other suitable structures are also possible. The isolation structure 210 may include, for example, a multilayer structure having one or more thermal oxide liner layers.
[0021] Each of the stacked fins 212a and 212b has a stack of semiconductor layers 220 and 222 in a staggered or alternating manner (e.g., semiconductor layer 220 is disposed above semiconductor layer 222, then another semiconductor layer 222 is disposed above semiconductor layer 220, and so on). In some embodiments, semiconductor layers 220 and 222 are alternately disposed in a vertical direction to form a semiconductor stack. In various embodiments, the stack includes any number of alternately disposed semiconductor layers 220 and 222. In some embodiments, semiconductor layers 220 and 222 have different thicknesses. In addition, semiconductor layer 220 may have different thicknesses from one layer to another, and semiconductor layer 222 may have different thicknesses from one layer to another. In some embodiments, the thickness of each of semiconductor layers 220 and 222 is in the range of several nanometers to tens of nanometers. In an embodiment, each semiconductor layer 220 has a thickness in the range of about 5 nm to about 10 nm, and each semiconductor layer 222 has a thickness in the range of about 5 nm to about 10 nm.
[0022] The two types of semiconductor layers 220 and 222 have different compositions. In various embodiments, the semiconductor layer 222 has a composition that provides a different oxidation rate and / or a different etching selectivity than the semiconductor layer 220. In an embodiment, the semiconductor layer 222 includes silicon germanium (Si 1-x Ge x ), and the semiconductor layer 220 includes silicon (Si). In an embodiment, each semiconductor layer 220 is undoped silicon or substantially free of dopants (ie, having about 0 cm -3 About 1×10 17 cm -3 The concentration of non-intrinsic dopants is determined by the semiconductor layer 220 (e.g., silicon), wherein no intentional doping is performed when forming the semiconductor layer 220 (e.g., silicon). Optionally, each semiconductor layer 220 is intentionally doped. In an example, the semiconductor layer 220 is made of silicon doped with a p-type dopant (such as boron (B), aluminum (Al), indium (In), and gallium (Ga)) or an n-type dopant (such as phosphorus (P), arsenic (As), antimony (Sb)). In some embodiments, each semiconductor layer 222 is Si including Ge in a molar ratio of less than 50% (x < 0.5). 1-x Ge x For example, Ge includes Si in a molar ratio of 1-x Ge x The semiconductor layer 220 may include about 15% to about 35% of the semiconductor layer 222. In addition, the semiconductor layers 222 may include different compositions therebetween, and the semiconductor layers 220 may include different compositions therebetween.
[0023] In various embodiments, any of the semiconductor layers 220 and 222 includes other materials, such as compound semiconductors (e.g., silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide, and / or indium antimonide) or alloy semiconductors (e.g., GaAsP, AlInAs, AlGaAs, InGaAs, GaInP, and / or GaInAsP), or combinations thereof. The materials of the semiconductor layers 220 and 222 may be selected based on providing different oxidation rates and / or etching selectivities. The semiconductor layers 220 and 222 may be doped or undoped, as discussed above.
[0024] In some embodiments, semiconductor layers 220 and 222 are epitaxially grown layer by layer from the top surface of substrate 208. In an example, each of semiconductor layers 220 and 222 is grown by a molecular beam epitaxy (MBE) process, a chemical vapor deposition (CVD) process (such as a metal organic CVD (MOCVD) process), and / or other suitable epitaxial growth processes. During epitaxial growth, the crystal structure of substrate 208 is extended upward, resulting in semiconductor layers 220 and 222 having the same crystal orientation as substrate 208.
[0025] The stacked fins 212a and 212b can be formed by epitaxially growing semiconductor layers 220 and 222 over substrate 208, and then patterned by any suitable method to form separate stacked fins 212a and 212b. For example, one or more lithography processes including double patterning or multiple patterning processes can be used to pattern the stacked fins 212a and 212b. Typically, the double patterning or multiple patterning process combines lithography and self-alignment processes, thereby allowing the creation of patterns with, for example, a pitch smaller than that obtainable using a single, direct lithography process. For example, in one embodiment, a sacrificial layer is formed over a substrate and patterned using a lithography process. Spacers are formed next to the patterned sacrificial layer using a self-alignment process. The sacrificial layer is then removed, and the remaining spacers or mandrels can then be used to pattern the stacked fins 212a and 212b by etching the initial semiconductor layers 220, 222 and substrate 208. The etching process may include dry etching, wet etching, reactive ion etching (RIE), and / or other suitable processes. In the illustrated embodiment, the stacked fins 212a and 212b extend longitudinally in the same direction (with longitudinal axes parallel).
[0026] The dummy gate structure 216 reserves an area for the metal gate stack and includes a dummy interface layer 231, a dummy gate electrode 232, a first gate hard mask layer 234, and a second gate hard mask layer 236. The dummy interface layer 231 is formed over the top surface and sidewall surface of each of the stacked fins 212a and 212b and over the top surface of the isolation structure 210. The dummy interface layer 231 may include a dielectric material such as an oxide layer (e.g., SiO2) or an oxynitride layer (e.g., SiON), and may be deposited by chemical oxidation, thermal oxidation, atomic layer deposition (ALD), chemical vapor deposition (CVD), and / or other suitable methods.
[0027] The pseudo gate electrode 232 may include polycrystalline silicon (poly-Si) and may be formed by a suitable deposition process such as low pressure chemical vapor deposition (LPCVD) and plasma enhanced CVD (PECVD). Each of the gate hard mask layers 234 and 236 may include one or more layers of dielectric materials such as silicon oxide and / or silicon nitride and may be formed by CVD or other suitable methods. For example, the first gate hard mask layer 234 may include a silicon oxide layer adjacent to the pseudo gate electrode 232, and the second gate hard mask layer 236 may include a silicon nitride layer. The individual layers 231, 232, 234, and 236 may be patterned by photolithography and etching processes.
[0028] In operation 104, method 100 ( Figure 1A ) A gate spacer 238 is formed on the sidewall of the dummy gate structure 216, such as Figure 3 As shown. Gate spacer 238 may include a dielectric material such as silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, other dielectric materials, or combinations thereof, and may include one or more layers of material. Gate spacer 238 may be formed by depositing a spacer material as a blanket layer over device 200. The spacer material is then etched by an anisotropic etching process. The portion of the spacer material on the sidewall of dummy gate structure 216 becomes gate spacer 238.
[0029] In operation 106, method 100 ( Figure 1A) The stacked fins 212a and 212b are recessed at the S / D regions using one or more photolithography and etching operations, thereby forming S / D trenches. In some embodiments, the substrate 208 is also partially etched. At this stage, the ends (also referred to as lateral ends) of the stacked semiconductor layers 220 and 222 are exposed in the S / D trenches. The method 100 also etches the semiconductor layer 222 laterally in the Y direction through the S / D trenches in operation 106, thereby forming a cavity. In some embodiments, the amount of etching the first semiconductor layer 222 is in the range of about 2nm to about 5nm. When the semiconductor layer 222 is Ge or SiGe and the semiconductor layer 220 is Si, the semiconductor layer 222 can be selectively etched by using a wet etchant such as, but not limited to, ammonium hydroxide (NH4OH), tetramethylammonium hydroxide (TMAH), ethylenediamine catechol (EDP), or potassium hydroxide (KOH) solution. Lateral etching of the semiconductor layer 222 can also remove a small portion of the semiconductor layer 220. Therefore, the thickness T1 of the lateral end of the semiconductor layer 220 is smaller than the thickness T0 of other portions of the semiconductor layer 220 below the sacrificial gate structure, such as Figure 4 As shown. An internal spacer 224 is then formed in the cavity adjacent to the lateral end of the semiconductor layer 222. In some embodiments, the internal spacer 224 includes a dielectric material (such as SiN, SiOC, SiOCN, SiCN, SiO2) and / or other suitable materials (such as a low-k dielectric material having a dielectric constant of less than about 3.9).
[0030] Operation 106 also forms S / D features 240 in the S / D region, such as Figure 4As shown. For example, operation 106 may epitaxially grow semiconductor material in the S / D trenches. The semiconductor material may protrude above the top surface of the corresponding stacked fins. Operation 106 may form S / D features 240 for n-type and p-type devices, respectively. For example, operation 106 may form the S / D features 240 using n-type doped silicon for n-type devices and using p-type doped silicon germanium for p-type devices. Operation 106 may further form a contact etch stop (CESL) layer 242 over the S / D features 240, and an interlayer dielectric (ILD) layer 244 over the CESL layer 242. The CESL layer 242 may include silicon nitride, silicon oxynitride, silicon nitride with oxygen (O) or carbon (C) elements, and / or other materials; and may be formed by CVD, PVD (physical vapor deposition), ALD, or other suitable methods. The ILD layer 244 may include tetraethyl orthosilicate (TEOS) oxide, undoped silicate glass or doped silicon oxide (such as borophosphosilicate glass (BPSG), fused silica glass (FSG), phosphosilicate glass (PSG), boron-doped silica glass (BSG)) and / or other suitable dielectric materials. The ILD layer 244 may be formed by PECVD or FCVD (flowable CVD) or other suitable methods. A CMP process may be performed after operation 104 to remove excess dielectric material. In some embodiments, the CMP process also removes gate hard masks 234 and 236 and exposes the dummy gate electrode 232.
[0031] In operation 108, method 100 ( Figure 1A ) removes the dummy gate stack 216 to form a gate trench 246, such as Figure 5 As shown. Channel regions such as the n-type channel region 230a of the first device structure 206a and the p-type channel region 230b of the second device structure 206b are exposed in the gate trench 246. Operation 108 may include one or more etching processes that are selective to the material in the dummy gate structure 216. By selecting an etchant that resists etching the gate spacer 238 and the ILD layer 244, portions of the gate spacer 238 and the ILD layer 244 adjacent to the dummy gate structure 216 are exposed in the gate trench 246 without substantially etching losses. The etching process may include any suitable etching technique, such as wet etching, dry etching, RIE, ashing, and / or other etching methods. In an example, the etching process is a dry etching process using a fluorine-based etchant (e.g., CF4, CHF3, CH2F2, etc.).
[0032] In operation 110, method 100 ( Figure 1A ) releases the suspended nanostructure (eg, nanowire or nanosheet) in the exposed channel region. Forming the suspended nanostructure includes a selective etching process to selectively remove the semiconductor layer 222 from the corresponding channel region of the FET. Figure 6 In an example, the semiconductor layer 222 (eg, Si) is removed from the channel region of the stacked fins 212a and 212b. 1-x Ge x ), while the semiconductor layer 220 (e.g., Si) is substantially retained as a channel layer. In other words, in the channel regions 230a and 230b, the semiconductor layer 220 is removed. Therefore, the portions of the semiconductor layer 220 in the channel regions 230a and 230b are suspended in the corresponding openings. Therefore, after operation 110, the semiconductor layer 220 is also referred to as a suspended nanostructure 220.
[0033] In an embodiment, the semiconductor layer to be removed is etched by a selective wet etching process, while other semiconductor layers having different compositions remain substantially unchanged. In some embodiments, the selective wet etching process includes hydrogen fluoride (HF) or NH4OH etchants. In an embodiment where semiconductor layer 222 includes SiGe and semiconductor layer 220 includes Si, selective removal of SiGe layer 222 includes a SiGe oxidation process followed by a SiGeO x In an example, the SiGe oxidation process includes forming and patterning various masking layers so as to control the oxidation to the SiGe layer 222. In other embodiments, the SiGe oxidation process is a selective oxidation due to the different compositions of the semiconductor layers 220 and 222. In some examples, the SiGe oxidation process is performed by exposing the device 200 to a wet oxidation process, a dry oxidation process, or a combination thereof. Thereafter, the SiGeO is removed by an etchant such as NH4OH or diluted HF. x The semiconductor layer 222 may be oxidized by the selective dry etching process, while other semiconductor layers having different compositions remain substantially unchanged. In some embodiments, the selective dry etching process includes hydrogen fluoride (HF), fluoride (F2), carbon fluoride (CF x ), hydrogen (H2) based etchants.
[0034] The threshold voltage of the n-type FET can be set by the metal work function layer. In order to achieve the appropriate threshold voltage p-type FET, the method 100 then continues to fine-tune the channel region 230b of the second device structure 206b to fine-tune the threshold voltage of the p-type FET to be formed. The fine-tuning in the channel region 230b includes various processes and operations, such as operations 112 and 114 described next.
[0035] In operation 112, method 100 ( Figure 1A ) forms a patterned mask on the top surface of the device 200. Figure 7As shown, the patterned mask covers the first device structure 206a and includes an opening exposing the second device structure 206b. In one embodiment, the patterned mask includes a hard mask 252 (rather than a soft mask, such as a patterned resist layer) disposed on the first device structure 206a. In some instances, the hard mask 252 includes silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, silicon carbonitride, silicon carbonitride, other semiconductor materials and / or other dielectric materials. In an embodiment, the hard mask 252 has a thickness in the range of about 1nm to about 40nm. The hard mask 252 is formed by thermal oxidation, chemical vapor deposition (CVD), atomic layer deposition (ALD), or any other suitable method. The hard mask 252 is patterned using any suitable method such as a photolithography process, which may include: forming a resist layer on the hard mask 252; exposing the resist by a photolithography exposure process; performing a post-exposure bake process; developing the photoresist layer to form a patterned photoresist layer exposing a portion of the hard mask 252; patterning the hard mask 252; and finally removing the patterned resist layer. The photolithography process may optionally be replaced by other suitable techniques, such as electron beam writing, ion beam writing, maskless patterning, or molecular printing.
[0036] In operation 114, method 100 ( Figure 1A ) doping threshold modification impurities into the channel region 230b to adjust the threshold voltage of the second device structure 206b. In some embodiments, the threshold modification impurities include germanium. In one example, in the case of forming the suspended nanostructure 220 in the silicon material, the germanium dopant can form a dipole with the silicon material. The dipole formation can be used to adjust the threshold voltage of a FET transistor formed using the suspended nanostructure 220 as a channel layer. In one example, the threshold voltage of the FET transistor can be changed by controlling the dose of the germanium concentration in the suspended nanostructure 220, wherein the magnitude of the threshold voltage change can be proportional to the dose. For example, when the FET transistor to be formed is a p-type FET, the germanium dopant implantation can reduce the threshold voltage of the field effect transistor, so that a higher dose results in a greater reduction in the threshold voltage.
[0037] In one embodiment of operation 114, doping the threshold modification impurity includes a germanium implantation process 254, such as Figure 8 The implantation process may be performed at an energy between about 0.5 keV and about 30 keV. In an embodiment, the implantation process is a substantially vertical implantation (e.g., perpendicular to the top surface of the substrate). In an embodiment, the implantation process is an inclined implantation. The inclination angle may be between about 0 degrees and about 30 degrees. The dose of the implanted germanium is about 1x10 15 / cm 2 and about 5x10 15 / cm 2, and the threshold voltage of the p-type FET can be proportionally reduced by about 10 mV to about 120 mV. The germanium implantation can be performed at an elevated temperature (e.g., greater than 400° C.) to prevent amorphization of the suspended nanostructure 220 during the implantation. For example, the environment in which the germanium implantation occurs can be heated to a temperature greater than about 450° C., and the device 200 itself (e.g., including the substrate 208) can be heated to a temperature greater than about 400° C. during the germanium implantation. In another embodiment, doping the germanium includes a low temperature plasma doping process that drives germanium ions into the suspended nanostructure 220. In one example, a plasma doping process is performed that has an RF source of less than about 1000 W at about 2 MHz and a pulsed DC bias of less than about 10 KV at about 0.5-10 KHz, and the plasma doping process is performed at a pressure of about 6 mTorr to about 200 mTorr and at a temperature of less than about 100° C.
[0038] In yet another embodiment of operation 114, the method 200 forms a semiconductor layer 258 around each of the suspended nanostructures 220 located in the second device structure 206b (but not in the first device structure 206a), such as Fig. 9 As shown. The semiconductor layer 258 contains threshold modification impurities and has a different composition than the suspended nanostructures 220. In an embodiment, the semiconductor layer 258 includes silicon germanium (Si 1-x Ge x ), and the suspended nanostructure 220 includes silicon (Si). For example, each layer 258 is Si including Ge in a molar ratio of about 10% to about 100% (0.1≤x≤1). 1-x Ge x In another embodiment, the semiconductor layer 258 includes germanium tin (Ge x Sn 1-x ), and the suspended nanostructure 220 includes silicon (Si). For example, each layer 258 is Ge including Ge in a molar ratio of about 10% to about 100% (0.1≤x≤1). x Sn 1-x A sufficient amount of Ge in each layer 258 helps reduce the threshold voltage of the channel region 230b in the second device structure 206b. For example, Ge may include a molar ratio of Si 1-x Ge x Or Ge x Sn 1-x The Ge range is about 60% to about 80% of the layer 258. Such a Ge range (in conjunction with subsequent processing steps) effectively reduces the threshold voltage of the channel region 230b of the second device structure 206b. In addition, the semiconductor layers 258 can include other different compositions therebetween.
[0039] Still reference Fig. 9 In some embodiments, semiconductor layer 258 is epitaxially grown from the surface of semiconductor layer 220. For example, each semiconductor layer 258 is grown by an MBE process, a CVD process such as an MOCVD process, and / or other suitable epitaxial growth process. The epitaxial growth method allows the materials in semiconductor layer 258 to form a lattice consistent with those of semiconductor layer 220. In some embodiments, each semiconductor layer 258 is a conformal layer with a substantially uniform thickness. In one example, each semiconductor layer 258 has a thickness of about 1 nm to about 4 nm. In some embodiments, the thickness ratio between semiconductor layer 258 and its surrounding semiconductor layer 220 is about 1:4 to about 1:2. In other words, semiconductor layer 258 is thinner than its corresponding semiconductor layer 220. Such a thickness ratio provides a suitable amount of germanium required for threshold adjustment.
[0040] like Fig. 9 As shown, each semiconductor layer 220 includes a middle portion exposed in the gate trench 246 and two end portions under the gate spacer 238. The middle portion is suspended in the space (and wrapped by the metal gate stack in a subsequent step), and the end portions are joined (e.g., surrounded or wrapped) by the inner spacer 224 and the gate spacer 238. In an embodiment, because only the middle portion is exposed, the semiconductor layer 258 is epitaxially grown only in the middle portion and not in the end portions of the suspended nanostructure 220. In other words, the semiconductor layer 258 is formed only at the gate contact area and stops at the gate spacer 238 and the inner spacer 224.
[0041] refer to Fig.10 , the method 100 further removes the patterned mask (e.g., hard mask 252) from the device 200 in operation 114, and optionally performs an annealing process to drive the germanium contained in the semiconductor layer 258 into their corresponding semiconductor layer 220. The device 200 is exposed to a gas containing nitrogen (N), phosphorus, or other suitable elements. In order to avoid oxidizing the semiconductor layer 252 (e.g., silicon germanium or germanium tin), in some embodiments, the gas does not contain oxygen. The conditions of the annealing process are adjusted to control the profile and characteristics of the resulting channel. In an example, the annealing process is performed at a temperature between about 700° C. and about 1200° C. The annealing process can be performed for a relatively long period of time, such as 10 seconds to 100 seconds (referred to as "soaking"), or a relatively short period of time, such as hundreds of milliseconds to a few seconds (e.g., 200 milliseconds to 2 seconds) (referred to as "spike").
[0042] The annealing process causes germanium atoms (and possibly silicon or tin atoms) contained in the semiconductor layer 258 to diffuse or migrate into the corresponding semiconductor layer 220. On the other hand, silicon atoms contained in the semiconductor layer 220 can also diffuse or migrate into the corresponding semiconductor layer 258. Due to the migration of atoms, the germanium content of the semiconductor layer 258 decreases, and the germanium content of the semiconductor layer 220 increases. In an embodiment, after the annealing process, each of the semiconductor layers 258 is Si including Ge with a molar ratio greater than 0% but equal to or less than about 70% (0.1 < x ≤ 0.7). 1-x Ge x or Ge x Sn 1-x . Such a Ge range is due to diluting the initial concentration of Ge in the semiconductor layer 258 (e.g., about 60% to about 80%, as described above) and effectively reducing the threshold voltage in the channel region 230b. As the material compositions of the semiconductor layers 258 and 220 become the same or similar (e.g., when germanium is uniformly distributed throughout the semiconductor layers 258 and 220), each semiconductor layer 258 and its corresponding semiconductor layer 220 can be effectively combined to form a new suspended nanostructure (for simplicity, still denoted by the reference numeral 220).
[0043] Still referring to Fig.10 , since the suspended nanostructure 220 in the second device structure 206b is formed as a combination of two semiconductor layers, the suspended nanostructure 220 in the second device structure 206b can be thicker (wider in the X direction) in the Z direction than the suspended nanostructure 220 in the first device structure 206a. Method 100 can optionally perform a trimming operation in operation 114 to reduce the thickness of the suspended nanostructure 220 in the second device structure 206b. The trimming operation uses any suitable etching process, such as dry etching, wet etching, and / or RIE. In an embodiment, the suspended nanostructure 220 in the second device structure 206b is trimmed to have approximately the same dimensions (thickness and / or width) as the suspended nanostructure 220 in the first device structure 206a. In a particular instance, method 100 includes, in operation 114, a cyclic process of repeating the epitaxial growth of the germanium-containing semiconductor layer 258, annealing to drive in germanium atoms, and trimming the suspended nanostructure as a way to further increase the germanium content to more than 80% in the suspended nanostructure 220, such as about 95% or approaching 100%.
[0044] According to the above-disclosed embodiments of operation 114, the driven-in germanium atoms are distributed in the suspended nanostructure 220 in various ways, which can be customized by controlling the implantation energy, implantation species, implantation dose, annealing conditions, etc. As discussed above and as Figure 8 and Fig. 9As shown, during the germanium implantation or epitaxial growth of the germanium-containing semiconductor layer, the middle portion of the suspended nanostructure 220 of the second device structure 206b is affected by the process. Therefore, during doping, germanium atoms can be mainly driven into the middle portion (rather than the end portion) of the corresponding suspended nanostructure 220. Fig.10 An exemplary concentration profile of germanium in the suspended nanostructure 220 along its longitudinal direction (Y direction) is also depicted. Fig.10 As shown, the concentration of germanium in the middle portion of the suspended nanostructure 220 is higher than the concentration of germanium in the end portions. Any suitable method for determining the concentration may be used (e.g., by determining an average concentration or a median concentration). In an embodiment, the concentration of germanium in the middle portion of each suspended nanostructure 220 is substantially uniform, while the concentration of germanium in the end portions is gradient distributed (e.g., gradually decreasing from a high concentration in the middle portion until the concentration becomes zero). It should be noted that due to the diffusion characteristics of germanium migration, the concentration of germanium may vary. Fig.10 Points C and C' shown begin to decrease, which may be a few nanometers from the interface between the middle portion and the end portion (i.e., a few nanometers from a position flush with the sidewall of the gate spacer 238). In some embodiments (e.g., when the annealing process has a short duration and / or a low temperature), the germanium does not reach a far enough distance under the gate spacer 238 to reach the source region and the drain region. Instead, the concentration of germanium drops to zero at points D and D'. Therefore, at least a portion of the two end portions (which are in direct contact with the gate spacer 238, the inner spacer 224, and the source / drain feature 240) is substantially free of germanium. In an embodiment, the entire end portion of the suspended nanostructure 220 is substantially free of germanium. Similarly, for the XZ plane cross-sectional tangent between points C and C', the concentration of germanium in the core portion of each suspended nanostructure 220 can be equal to or lower than the concentration of germanium in the edge (outer) portion of the suspended nanostructure 220. In one example, a uniform concentration of germanium of about 34% to 38% is achieved in the core and edge portions of the suspended nanostructure 220. In yet another example, a germanium concentration of about 45% to 50% is achieved in the edge portion of the suspended nanostructure 220, while the core portion of the suspended nanostructure 220 is substantially free of germanium atoms. Such a gradient profile may be caused by the relatively short duration of the annealing process (e.g., the germanium does not have enough time to migrate all the way to the core). In some embodiments, the edge portion of the suspended nanostructure 220 includes a thin tin-containing outer layer as a substrate containing Ge. x Sn 1-x Remnants of the semiconductor layer 258.
[0045] In operation 116, method 100 ( Figure 1A) Continue to form gate stacks 260a and 260b over the channel regions 230a and 230b of the first device structure 206a and the second device structure 206b, respectively. The gate stack 260a engages the n-type channel region 230a, thereby forming an n-type GAA transistor on the first device structure 206a. The gate stack 260b engages the p-type channel region 230b, thereby forming a p-type GAA transistor on the second device structure 206b. Fig.11 In an example of the present invention, gate stacks 230a and 230b fill the openings in the channel region and wrap around each of the suspended nanostructures 220. Gate stacks 260a and 260b have similar structures, but in some embodiments, different metals and / or different layer thicknesses are used. In the present embodiment, gate stacks 260a and 260b include a gate dielectric layer 262, which may include one or more layers of dielectric material on the inner surface of the opening and directly wrap around each of the suspended nanostructures 220. The gate dielectric layer 262 includes a dielectric material such as silicon oxide or silicon oxynitride, and is formed by chemical oxidation, thermal oxidation, ALD, CVD, and / or other suitable methods. In some embodiments, the gate dielectric layer 262 also includes a high-k dielectric layer, such as hafnium oxide, zirconium oxide, lanthanum oxide, titanium oxide, yttrium oxide, strontium titanate, other suitable metal oxides, or combinations thereof; and is formed by ALD and / or other suitable methods. The gate stacks 260a and 260b also include a gate metal layer 264, which may include one or more metal work function layers above the gate dielectric layer 262 and a metal fill layer above the metal work function layer. In some embodiments, the metal work function layer is an n-type metal work function layer or a p-type metal work function layer. The n-type metal work function layer includes a metal selected from the group of but not limited to titanium, aluminum, tantalum carbide, tantalum carbonitride, tantalum silicon nitride, or a combination thereof. The p-type metal work function layer includes a metal selected from the group of but not limited to titanium nitride, tantalum nitride, ruthenium, molybdenum, tungsten, platinum, or a combination thereof. In some embodiments, the p-type or n-type metal work function layer includes a plurality of layers deposited by CVD, PVD, and / or other suitable processes. By doping the channel layer of the p-type FET with threshold modification impurities, the threshold voltage can be finely adjusted without the need for a complex metal work function structure in the p-type FET. The metal fill layer includes aluminum, tungsten, cobalt, copper, and / or other suitable materials, and is formed by CVD, PVD, plating, and / or other suitable processes. In some embodiments, the gate stacks 260a and 260b wrap the vertically stacked horizontally oriented channel semiconductor layers. Therefore, the device 200 is a stacked horizontal gate-all-around (S-HGAA) device. In an embodiment, after the gate stacks are deposited, a CMP process is performed to planarize the top surface of the device 200.
[0046] In various embodiments, the method 100 may optionally skip the trimming process in operation 114 without reducing the thickness and / or width of the suspended nanostructure 220 in the p-type channel of the second device structure 206 b. Therefore, the cross-sectional area of the suspended nanostructure 220 in the p-type GAA transistor may be larger than the cross-sectional area of the suspended nanostructure 220 in the n-type GAA transistor. Because the p-type channel relies on holes for conduction (which have a slower mobility than electrons in the n-type channel), the larger cross-sectional area in the p-type channel helps increase the effective channel width, and thus has a higher current and better transistor performance.
[0047] In the above discussion, method 100 ( Figure 1A ) In operation 114, a threshold modification impurity (e.g., germanium) may be globally doped into all p-type regions in the device 200. Optionally, the method 100 may dope the threshold modification impurity into the selective p-type region in operation 114 to produce a threshold voltage difference between the p-type FETs. The device 200 may have two or more regions with different threshold voltages, such as at least a standard threshold voltage (SVt) region and a low threshold voltage (LVt) region. Fig.12 In the example of , the first device structure 206a for forming an n-type FET and the second device structure 206b for forming a first p-type FET are located in the SVt region. Fig.12 A third device structure 206c for forming a second p-type FET in the LVt region is also depicted. The transistor in the LVt region has a lower threshold voltage and operates faster than the transistor in the SVt region. Therefore, the transistor in the LVt region may be suitable for high-speed applications. Method 100( Figure 1A ) A hard mask 252 covering the first device structure 206a and the second device structure 206b having an opening exposing the third device structure 206c may be formed accordingly in operation 112. Therefore, the doping process (e.g., germanium implantation, low temperature plasma doping, or epitaxial layer growth and annealing drive-in containing germanium) is limited to the channel region 230c of the third device structure 206c. Therefore, the threshold voltage of the first p-type FET formed on the second device structure 206b is not adjusted, and the threshold voltage of the second p-type FET formed on the third device structure 206c has a lower threshold voltage than the first p-type FET formed on the second device structure 206b.
[0048] Still reference Fig.12 In yet another embodiment, the method 100( Figure 1A) may include two impurity doping processes in operation 114. The hard mask 252 may first cover the first device 206a having an opening exposing the channel region 230b of the second device structure 206b and the channel region 230c of the third device structure 206c. The method 100 performs a first impurity doping process in operation 114 to dope a portion of the total dose into the channel regions 230b and 230c. Subsequently, a new hard mask is formed to cover the first device 206a and the second device 206b having an opening exposing the third device structure 206c. Then, the method 100 performs a second impurity doping process in operation 114 to dope the remaining portion of the total dose into the channel region 230c. For example, if the total dose to be delivered is 2×10 15 / cm 2 , the first impurity doping process can be used to convert 1x10 15 / cm 2 The germanium dose is delivered to all p-type FET regions on the device 200, and the second impurity doping process can be used to deliver only 1x10 15 / cm 2 In this way, all p-type FETs formed will have a reduced threshold voltage, while the p-type FETs in the LVt region have a lower Vt due to the higher received dose.
[0049] Attention now turns to method 300 . Figure 1B A flow chart of method 300 according to various aspects of the present invention is shown. Throughout the present invention, like reference numerals represent like parts in terms of composition and formation. Some details of the operations in method 300 may be simplified or omitted if similar details have been described in conjunction with method 100. Method 300 is merely an example and is not intended to limit the present invention beyond the scope expressly recited in the claims. Additional operations may be provided before, during, and after method 300, and some of the operations described may be replaced, eliminated, or moved around for additional embodiments of the method. Figures 13 to 22 Some embodiments of method 300 are described. Fig.13 is a perspective view of the device 200 . Figures 14 to 22 is the edge of the device 200 Fig.13 The cross-sectional views shown are those taken along the BB cut line and the CC cut line (arranged side by side), which pass through the corresponding channel regions along the longitudinal direction (in the YZ plane) of the p-type transistor. Fig. 22 A cross-sectional view through the channel region along the longitudinal direction of an additional p-type transistor of the device 200 is also depicted.
[0050] In operation 302, method 300 ( Figure 1B) provides a device 200 including two or more regions of different threshold voltages, such as at least a standard threshold voltage (SVt) region and a low threshold voltage (LVt) region. Fig.13 In the example of , the first device structure 206a for forming an n-type FET and the second device structure 206b for forming a first p-type FET are located in the SVt region. Fig.13 Also depicted is a third device structure 206c for forming a second p-type FET in the LVt region. Fig.13 As shown, each of the device structures 206a-206c includes a substrate 208, an isolation structure 210, fins 212a-212c each including vertically stacked alternating semiconductor layers 220 and 222 (also referred to as stacked fins 212a-212c), and a dummy gate structure 216 that joins the stacked fins 212a-212c. Since the substrate 202, the isolation structure 210, the semiconductor layers 220 and 222, and the dummy gate structure 216 have been described above, their detailed descriptions are omitted here.
[0051] In operation 304, method 300 ( Figure 1B ) A gate spacer 238 is formed on the sidewall of the dummy gate structure 216, such as Fig.14 As shown (for simplicity, the AA cut line for forming the first device structure 206a of the n-type FET is omitted here). Since operation 304 is similar to operation 104 described above, their detailed description is omitted for brevity.
[0052] In operation 306, method 300 ( Figure 1B ) to form an internal spacer 224 and an S / D component 240, such as Fig.15 As shown. Due to the lateral etching process in forming the cavity to deposit the internal spacer 224 therein, the lateral etching may also remove a small portion of the semiconductor layer 220. Therefore, the thickness T1 of the end portion of the semiconductor layer 220 is smaller than the thickness T0 of the other portion of the semiconductor layer 220 under the sacrificial gate structure. Because operation 306 is similar to operation 106 described above, their detailed description is omitted for brevity.
[0053] In operation 308, method 300 ( Figure 1B ) removes the dummy gate stack 216 to form a gate trench 246, such as Fig.16 Because operation 308 is similar to operation 108 described above, their detailed description is omitted for brevity.
[0054] In operation 310, method 300 ( Figure 1B ) releases the suspended nanostructures 220 in the exposed channel region, such as Fig.17Because operation 310 is similar to operation 110 described above, their detailed descriptions are omitted for brevity.
[0055] In operation 312, method 300 ( Figure 1B ) A trimming process 270 is performed to reduce the thickness of the suspended nanostructure 202 in the channel regions 230b and 230c (but not in the channel region 230a for the N-type FET), such as Fig.18 As shown. After the trimming process 270, the suspended nanostructures 220 in the channel regions 212b and 212c have substantially the same size (thickness and / or width). The trimming operation uses any suitable etching process, such as dry etching, wet etching and / or RIE. During the trimming process 270, the gate spacer 238 protects the suspended nanostructure 202 below it from etching. The trimming process 270 selectively removes the portion of the suspended nanostructure 202 that is vertically aligned with the gate trench 246, while leaving the two end portions of the suspended nanostructure 202 substantially unetched. The trimmed thickness of the middle portion of the suspended nanostructure 202 is represented as T2. In the illustrated embodiment, a small portion of the suspended nanostructure 202 directly below the gate spacer 238 but not sandwiched by the internal spacer 224 can still maintain the original thickness T0, which is greater than the thickness T1 of the two end portions and the trimmed thickness T2 of the middle portion, such as about 1nm to about 3nm. In various embodiments, the trimmed thickness T2 can be less than or greater than the thickness T1 of the two end portions. In one embodiment, the trimmed thickness T2 is substantially equal to the thickness T1. The reduced thickness of the suspended nanostructure 220 increases the threshold voltage in the corresponding channel region, such that a smaller trimmed thickness T2 of the suspended nanostructure results in a larger increase in the threshold voltage. In some embodiments, an increase in the range of about 20 mV to about 100 mV can be achieved by trimming the middle portion of the suspended nanostructure by about 1 nm to about 3 nm (T0-T2) in proportion.
[0056] In operation 314, method 300 ( Figure 1B ) forms a patterned mask on the top surface of the device 200, such as the hard mask 252 described above, as Fig.19 The patterned mask covers the third device structure 206c and has an opening exposing the second device structure 206b. Since operation 314 is similar to operation 112 described above, their detailed descriptions are omitted for brevity.
[0057] In operation 316, method 300 ( Figure 1B ) A second trimming process 272 is performed to further reduce the thickness of the suspended nanostructure 202 in the channel region 230b of the second device structure 206b, such as Fig. 20As shown. The trimming operation uses any suitable etching process, such as dry etching, wet etching and / or RIE. During the trimming process 272, the hard mask 252 protects the suspended nanostructure 202 in the third device structure 206c from etching. The trimming process 272 selectively removes additional portions of the suspended nanostructure 202 in the second device structure 206b that are vertically aligned with the gate trench 246, while leaving the two end portions of the suspended nanostructure 202 substantially unetched. Due to the trimming process 272, the trimmed thickness of the middle portion of the suspended nanostructure 202 in the channel region 230b is further reduced, represented as T3. In the illustrated embodiment, a small portion of the suspended nanostructure 202 directly below the gate spacer 238 but not sandwiched by the internal spacer 224 can still maintain the original thickness T0, which is greater than the thickness T1 of the two end portions and the trimmed thickness T3 of the middle portion, such as about 1nm to about 4nm. The trimmed thickness T3 in the channel region 230b is about 1 nm to about 3 nm less than the trimmed thickness T2 in the channel region 230c. In various embodiments, the trimmed thickness T3 may be less than or greater than the thickness T1 of the two end portions. In one embodiment, the trimmed thickness T3 is substantially equal to the thickness T1. In a specific example, the trimmed thickness T3 of the middle portion in the channel region 230b is less than the thickness T1 of the end portion, while the trimmed thickness T2 of the middle portion in the channel region 230c is greater than the thickness T1 of the end portion. Because the reduced thickness of the suspended nanostructure further increases the threshold voltage in the corresponding channel region, the p-type FET formed in the SVt region on the second device structure 230b has a greater threshold voltage than the p-type FET formed in the LVt region on the third device structure 230c. After operation 316, the hard mask 252 is removed in a suitable etching process.
[0058] In operation 318, method 300 ( Figure 1B ) continues to form a gate stack above the corresponding channel region, such as Fig.21 As shown. Because operation 318 is similar to operation 116 described above, their detailed description is omitted for brevity. It should be noted that due to the removal of the additional portion of the suspended nanostructure 220 of the second device structure 206b, the gate metal layer 264 in the gate stack 260b has a larger volume than the gate metal layer 264 in the gate stack 230c. By trimming the channel layer of the P-type FET, the threshold voltage can be finely adjusted without the need for a complex metal work function structure in the gate stack of the P-type FET.
[0059] refer to Fig. 22Optionally, the device 200 may further include a high threshold voltage (HVt) region in addition to the SVt region and the LVt region and a fourth device structure 206d for forming a third P-type FET in the HVt region. Because the reduced thickness of the suspended nanostructure further increases the threshold voltage of the corresponding field effect transistor, the method 300 may perform a first trimming process 270 on all three device structures 206b-206d, then perform a second trimming process 272 on the device structures 206b and 206d (by covering the device structure 206c with a patterned mask), and then perform a third trimming process 274 on the fourth device structure 206d only in the HVt region (by forming another patterned mask to cover the device structures 206b-206c). Therefore, the fourth device structure 206d receives three trimming processes and has the smallest thickness, denoted as T4. The thicknesses T0, T2, T3, and T4 have a relationship T0>T2>T3>T4. In this manner, all p-type FETs in the three regions will have an increased Vt due to receiving at least one trimming process, while the p-type FETs in the SVt region have a higher threshold voltage than the p-type FETs in the LVt region due to receiving an additional trimming process and a correspondingly smaller channel layer thickness, and the p-type FETs in the HVt region have the highest threshold voltage due to receiving two additional trimming processes and a correspondingly smallest channel layer thickness. In one embodiment, T1 is greater than T3 and T4, but less than T2.
[0060] Attention now turns to method 500 . Figure 1C A flow chart of method 500 according to various aspects of the present invention is shown. Throughout the present invention, similar reference numerals represent the same parts in terms of composition and formation. Some details of the operations in method 500 may be simplified or omitted if similar details have been described in conjunction with methods 100 and 300. Method 500 is merely an example and is not intended to limit the present invention beyond the scope expressly recited in the claims. Additional operations may be provided before, during, and after method 500, and some of the operations described may be replaced, eliminated, or moved around for additional embodiments of the method. Figures 23 to 32 Some embodiments of method 500 are described. Fig.23 is a perspective view of the device 200 . Figures 24 to 32 is the edge of the device 200 Fig.23 The cross-sectional views shown are those along the BB cut line, the CC cut line, and the DD cut line (arranged side by side), which pass through the corresponding channel regions along the longitudinal direction (in the YZ plane) of the p-type transistor.
[0061] In operation 502, method 500 ( Figure 1C) provides a device 200 including three different threshold voltage regions, namely, a standard threshold voltage (SVt) region, a low threshold voltage (LVt) region, and a high threshold voltage (HVt) region. Fig.23 In the example of FIG. 2 , a first device structure 206a for forming an n-type FET and a second device structure 206b for forming a first p-type FET are located in the SVt region. A third device structure 206c for forming a second p-type FET is located in the LVt region. A fourth device structure 206d for forming a third p-type FET is located in the HVt region. Fig.23 As shown, each of the device structures 206a-206d includes a substrate 208, an isolation structure 210, fins 212a-212d each including vertically stacked alternating semiconductor layers 220 and 222 (also referred to as stacked fins 212a-212d), and a dummy gate structure 216 that joins the stacked fins 212a-212d. Since the substrate 202, the isolation structure 210, the semiconductor layers 220 and 222, and the dummy gate structure 216 have been described above, their detailed descriptions are omitted here.
[0062] In operation 504, method 500 ( Figure 1C ) A gate spacer 238 is formed on the sidewall of the dummy gate structure 216, such as Fig.24 As shown (for simplicity, the AA cut line for forming the first device structure 206a of the n-type FET is omitted here). Since operation 504 is similar to operation 104 described above, their detailed description is omitted for brevity.
[0063] In operation 506, method 500 ( Figure 1C ) to form an internal spacer 224 and an S / D component 240, such as Fig.25 As shown. Due to the lateral etching process in forming the groove to deposit the internal spacer 224 therein, the lateral etching may also remove a small portion of the semiconductor layer 220. Therefore, the thickness T1 of the lateral end of the semiconductor layer 220 is smaller than the thickness T0 of the other portion of the semiconductor layer 220 under the sacrificial gate structure. Because operation 506 is similar to operation 104 described above, their detailed description is omitted for brevity.
[0064] In operation 508, method 500 ( Figure 1C ) removes the dummy gate stack 216 to form a gate trench 246, such as Fig.26 Because operation 508 is similar to operation 108 described above, their detailed description is omitted for brevity.
[0065] In operation 510, method 500 ( Figure 1C ) releases the suspended nanostructure 220 in the exposed channel region, such as Fig. 27Since operation 510 is similar to operation 108 described above, their detailed description is omitted for brevity.
[0066] In operation 512, method 500 ( Figure 1C ) A trimming process 270 is performed to reduce the thickness of the suspended nanostructure 220 in all three channel regions 230b-230d (but not in the channel region 230a for the n-type FET), as shown in FIG. Fig.28 As shown. After the trimming process 270, the suspended nanostructures 220 in the channel regions 212b-212d have substantially the same size (thickness and / or width). The trimming operation uses any suitable etching process, such as dry etching, wet etching and / or RIE. During the trimming process 270, the gate spacer 238 protects the suspended nanostructure 202 below it from etching. The trimming process 270 selectively removes the portion of the suspended nanostructure 202 that is vertically aligned with the gate trench 246, while leaving the two end portions of the suspended nanostructure 202 substantially unetched. The trimmed thickness of the middle portion of the suspended nanostructure 202 is represented as T2. In the illustrated embodiment, a small portion of the suspended nanostructure 202 directly below the gate spacer 238 but not sandwiched by the internal spacer 224 can still maintain the original thickness T0, which is greater than the thickness T1 of the two end portions and the trimmed thickness T2 of the middle portion, such as about 1nm to about 3nm. In various embodiments, the trimmed thickness T2 can be less than or greater than the thickness T1 of the two end portions. In one embodiment, the trimmed thickness T2 is substantially equal to the thickness T1. The reduced thickness of the suspended nanostructure can increase the threshold voltage of the field effect transistor, such that a smaller thickness of the suspended nanostructure results in a larger increase in the threshold voltage. In some embodiments, an increase in the range of about 20 mV to about 100 mV can be achieved by trimming the middle portion of the suspended nanostructure by about 1 nm to about 3 nm (T0-T2) in proportion.
[0067] In operation 514, method 500 ( Figure 1C ) forms a patterned mask, such as a hard mask 252, on the top surface of the device 200. Fig.29 The patterned mask covers the second device structure 206b and the fourth device structure 206d, and has an opening exposing the third device structure 206c. Since operation 514 is similar to operation 112 described above, their detailed descriptions are omitted for brevity.
[0068] In operation 516, method 500 ( Figure 1C ) doping a threshold modification impurity into the channel region 230c to adjust the threshold voltage of the third device structure 206c, such as Fig.30As shown. Doping threshold modification impurities (e.g., germanium implantation, low temperature plasma doping, or germanium-containing epitaxial layer growth and annealing drive-in) is limited to the channel region 230c of the third device structure 206c. Therefore, the threshold voltages of the first p-type FET formed on the second device structure 206b in the SVt region and the third p-type FET formed on the fourth device structure 206d in the HVt region are no longer further adjusted, and the second p-type FET formed on the third device structure 206c in the LVt region now has the lowest threshold voltage. Because operation 516 is similar to operation 114 described above, their detailed descriptions are omitted for brevity. As discussed above in conjunction with operation 114, the middle portion of the suspended nanostructure doped with the threshold modification impurity can be grown in thickness. The thickness of the middle portion of the suspended nanostructure in the channel region 230c (denoted as T2') can be correspondingly greater than the thickness T2 in the other channel regions 230b and 230d. The method 500 may also optionally perform a trimming operation at operation 516 to reduce the thickness T2 ′ to T2 so that the suspended nanostructures 220 in all three regions have substantially the same size.
[0069] In operation 518, method 500 ( Figure 1C ) A second trimming process 272 is performed to further reduce the thickness of the suspended nanostructure 220 in the channel region 230d in the HVt region, as shown in FIG. Fig.31 As shown. In operation 518, method 500 first forms a patterned mask to cover the second device structure 206b and the third device structure 206c having an opening to expose the fourth device structure 206d. Then, in operation 518, method 500 implements a suitable etching process, such as dry etching, wet etching and / or RIE, to remove an additional portion from the middle portion of the suspended nanostructure 220 in the channel region 230d. Because operation 518 is similar to operation 316 described above, their detailed description is omitted for brevity. Due to the trimming process 272, the trimmed thickness of the middle portion of the suspended nanostructure 202 is further reduced, represented as T3. T3 is less than T2 and T2'. Combined with method 300 ( Figure 1B ) receives three finishing processes Fig. 22 Compared with the thickness T4 in the HVt transistor, Fig.31 The thickness T3 in the HVt transistor in the fourth device structure 230d is due to receiving two trimming processes, T3 is greater than T4 and has a stronger mechanical strength for the suspended nanostructure. Because the reduced thickness of the suspended nanostructure further increases the threshold voltage in the corresponding channel region, the p-type transistor in the HVt region formed on the fourth device structure 230d therefore has a larger threshold voltage than the p-type transistor on the second device structure 230b formed in the SVt region and the p-type transistor on the third device structure 230c formed in the LVt region.
[0070] In operation 520, method 500 ( Figure 1C ) continues to form a gate stack above the corresponding channel region, such as Fig.32 As shown. Because operation 520 is similar to operation 116 described above, their detailed description is omitted for brevity. It should be noted that due to the removal of the additional portion of the suspended nanostructure 220 of the fourth device structure 206d, the gate metal layer 264 in the gate stack 260d has a larger volume than the gate metal layer 264 in the gate stack 230b and the gate metal layer 264 in the gate stack 230c. Compared with the second device structure 206b and the fourth device structure 206d, the channel layer of the third device structure 206c also further includes threshold modification impurities. By doping threshold modification impurities and trimming the corresponding channel layer, the threshold voltage can be finely adjusted without the need for a complex metal work function structure in the gate stack of the P-type FET.
[0071] In method 100, 300, or method 500, further processes may be performed to complete manufacturing device 200. For example, the method may continue to form contact openings, contact metals, and various contacts, vias, wirings, and multi-layer interconnect features (e.g., metal layers and interlayer dielectrics) over the GAA transistor configured to connect various components to form functional circuits that may include one or more multi-gate devices.
[0072] Although not intended to be limiting, one or more embodiments of the present invention provide many benefits to semiconductor devices and processes for forming the same. According to some embodiments, the threshold voltage of a p-type GAA FET is achieved using a simplified manufacturing process. In some embodiments, based on device performance considerations, the various threshold voltages of the P-type GAA FET can be fine-tuned in different regions to form SVt, LVt, and / or HVt FETs. In addition, embodiments of the present invention can be integrated into existing CMOS manufacturing processes to provide an improved process window.
[0073] In one exemplary aspect, the present invention provides a method for forming a semiconductor device. The method includes: providing a substrate having a plurality of first semiconductor layers and a plurality of second semiconductor layers disposed above the substrate, wherein the first semiconductor layers and the second semiconductor layers have different material compositions and are alternately disposed relative to each other in a vertical direction; patterning the first semiconductor layers and the second semiconductor layers to form a first fin and a second fin; removing the first semiconductor layer from the first fin and the second fin, so that a first portion of the patterned second semiconductor layer becomes a first suspended nanostructure in the first fin, and a second portion of the patterned second semiconductor layer becomes a second suspended nanostructure in the second fin; doping a threshold modification impurity into the first suspended nanostructure of the first fin; forming a first gate stack above the first fin, wherein a portion of the first gate stack wraps the first suspended nanostructure, thereby forming a first transistor having a first threshold voltage; and forming a second gate stack above the second fin, wherein a portion of the second gate stack wraps the second suspended nanostructure, thereby forming a second transistor having a second threshold voltage greater than the first threshold voltage. In some embodiments, the threshold modification impurity is Ge. In some embodiments, doping the threshold modification impurity includes: forming a plurality of third semiconductor layers on the first suspended nanostructure of the first fin; and performing an annealing process to drive the threshold modification impurities contained in the third semiconductor layer into the first suspended nanostructure in the first fin. In some embodiments, forming the third semiconductor layer includes epitaxially growing each of the third semiconductor layers to surround the corresponding first suspended nanostructure in the first fin, and wherein the third semiconductor layer has a different material composition than the second semiconductor layer. In some embodiments, the third semiconductor layer includes one of SiGe and GeSn. In some embodiments, doping the threshold modification impurity includes applying a low temperature plasma enhanced doping process. In some embodiments, the method further includes: doping the threshold modification impurity into the second suspended nanostructure of the second fin, wherein the threshold modification impurity has a higher concentration in the first suspended nanostructure in the first fin than in the second suspended nanostructure in the second fin. In some embodiments, doping the threshold modification impurity into the first suspended nanostructure in the first fin includes: doping the threshold modification impurity into the first suspended nanostructure of the first fin and the second suspended nanostructure of the second fin at the same time; and doping the threshold modification impurity into the first suspended nanostructure in the first fin secondly, but not into the second suspended nanostructure in the second fin. In some embodiments, the method further comprises: before doping the threshold modification impurity into the first suspended nanostructure, trimming the first suspended nanostructure and the second suspended nanostructure to reduce their thickness. In some embodiments, the method further comprises: after doping the threshold modification impurity into the first suspended nanostructure, trimming the second suspended nanostructure to further reduce their thickness.
[0074] In another exemplary aspect, the present invention provides a method. The method includes: forming a plurality of first suspension layers in a first fin, and forming a plurality of second suspension layers in a second fin, wherein the first suspension layer and the second suspension layer include the same first semiconductor material; performing a first etching process to simultaneously remove portions of the first suspension layer and the second suspension layer, thereby reducing the thickness of the first suspension layer and the second suspension layer; performing a second etching process to remove an additional portion of the second suspension layer without etching the first suspension layer, thereby further reducing the thickness of the second suspension layer; and forming a first gate stack and a second gate stack respectively joining the first suspension layer and the second suspension layer. In some embodiments, the first gate stack and the first suspension layer are located in a low threshold voltage (LVt) region, and the second gate stack and the second suspension layer are located in a standard threshold voltage (SVt) region. In some embodiments, the method further includes: doping impurities into the first suspension layer, wherein the second suspension layer is substantially free of impurities. In some embodiments, the first gate stack and the first suspension layer are located in a low threshold voltage (LVt) region, and the second gate stack and the second suspension layer are located in a high threshold voltage (HVt) region. In some embodiments, doping impurities into the first suspension layer includes: epitaxially growing a plurality of third layers on the first suspension layer, wherein the third layers include a second semiconductor material different from the first semiconductor material; and driving impurities contained in the second semiconductor material to migrate from the third layer to the first suspension layer. In some embodiments, the method further includes: forming a plurality of third suspension layers in a third fin, wherein the third suspension layers include the first semiconductor material; and performing a third etching process to remove portions of the third suspension layers without etching the first and second suspension layers, wherein the first and second etching processes also remove other portions of the third suspension layer, wherein after performing the third etching process, the first suspension layer is thicker than the second suspension layer, and the second suspension layer is thicker than the third suspension layer.
[0075] In yet another exemplary aspect, the present invention provides a semiconductor structure. The semiconductor structure includes: a substrate; a first fin disposed on the substrate, the first fin including a plurality of first suspended nanostructures stacked vertically with each other; a first gate stack joining the first suspended nanostructure; a second fin disposed on the substrate, the second fin including a plurality of second suspended nanostructures stacked vertically with each other; and a second gate stack joining the second suspended nanostructure, wherein the concentration of germanium in the middle portion of the first suspended nanostructure is higher than the concentration of germanium in the middle portion of the second suspended nanostructure. In some embodiments, the concentration of germanium in the middle portion of the first suspended nanostructure is higher than the concentration of germanium in the two end portions of the first suspended nanostructure. In some embodiments, the thickness of the middle portion of the first suspended nanostructure is greater than the thickness of the middle portion of the second suspended nanostructure. In some embodiments, the thickness of the central portion of the second suspended nanostructure is smaller than the thickness of the two end portions of the second suspended nanostructure.
[0076] The features of several embodiments are summarized above so that those of ordinary skill in the art can better understand aspects of the present invention. Those of ordinary skill in the art should understand that they can easily use the present invention as a basis to design or modify other processes and structures for implementing the same purpose and / or achieving the same advantages as the embodiments introduced herein. Those of ordinary skill in the art should also be aware that such equivalent constructions do not deviate from the spirit and scope of the present invention, and that they can make various changes, substitutions and modifications herein without departing from the spirit and scope of the present invention.
Claims
1. A method for forming a semiconductor device, comprising: Providing a substrate having a plurality of first semiconductor layers and a plurality of second semiconductor layers disposed above the substrate, wherein the first semiconductor layers and the second semiconductor layers have different material compositions and are alternately disposed relative to each other in a vertical direction; patterning the first semiconductor layer and the second semiconductor layer to form a first fin and a second fin; removing the first semiconductor layer from a first channel region of the first fin and a second channel region of the second fin, so that a first portion of the patterned second semiconductor layer becomes a first suspended nanostructure in the first channel region of the first fin, and a second portion of the patterned second semiconductor layer becomes a second suspended nanostructure in the second channel region of the second fin; doping a threshold modification impurity into the first suspended nanostructure in the first channel region; forming a first gate stack over the first fin, wherein a portion of the first gate stack wraps around the doped first suspended nanostructure in the first channel region to form a first transistor having a first threshold voltage; and A second gate stack is formed over the second fin, wherein a portion of the second gate stack wraps around the second suspended nanostructure in the second channel region to form a second transistor having a second threshold voltage greater than the first threshold voltage.
2. The method according to claim 1, wherein: The threshold modifying impurity is Ge.
3. The method according to claim 1, wherein: The threshold modification impurities doped include: forming a plurality of third semiconductor layers on the first suspended nanostructure of the first fin; and An annealing process is performed to drive the threshold modification impurities included in the third semiconductor layer into the first suspended nanostructure in the first fin.
4. The method according to claim 3, wherein: Forming the third semiconductor layers includes epitaxially growing each of the third semiconductor layers to surround a corresponding first suspended nanostructure in the first fin, and wherein the third semiconductor layers have a different material composition than the second semiconductor layer.
5. The method according to claim 3, wherein: The third semiconductor layer includes one of SiGe and GeSn.
6. The method according to claim 1, wherein: Doping the threshold modification impurities includes applying a low temperature plasma enhanced doping process.
7. The method according to claim 1, further comprising: The threshold modification impurity is doped into the second suspended nanostructure of the second fin, wherein the threshold modification impurity has a higher concentration in the first suspended nanostructure in the first fin than in the second suspended nanostructure in the second fin.
8. The method according to claim 1, wherein: Doping the threshold modification impurity into the first suspended nanostructure in the first fin includes: first doping the threshold modification impurity into the first suspended nanostructure of the first fin and the second suspended nanostructure of the second fin at the same time; and second doping the threshold modification impurity into the first suspended nanostructure in the first fin, but not doping into the second suspended nanostructure in the second fin.
9. The method according to claim 1, further comprising: Before doping the threshold modification impurity into the first suspended nanostructure, the first suspended nanostructure and the second suspended nanostructure are trimmed to reduce their thicknesses.
10. The method according to claim 9, further comprising: After doping the threshold modification impurities into the first suspended nanostructures, the second suspended nanostructures are trimmed to further reduce their thicknesses.
11. A method of forming a semiconductor device, comprising: forming a plurality of first suspension layers in a first channel region of the first fin, and forming a plurality of second suspension layers in a second channel region of the second fin, wherein the first suspension layers and the second suspension layers include the same first semiconductor material; performing a first etching process to simultaneously remove portions of the first suspension layer in the first channel region and the second suspension layer in the second channel region, thereby reducing the thickness of the first suspension layer in the first channel region and the second suspension layer in the second channel region; performing a second etching process to remove an additional portion of the second suspension layer in the second channel region without etching the first suspension layer, thereby further reducing the thickness of the second suspension layer in the second channel region; and A first gate stack and a second gate stack are formed that respectively join the first floating layer in the first channel region and the second floating layer in the second channel region.
12. The method according to claim 11, wherein: The first gate stack and the first floating layer are located in a low threshold voltage region, and the second gate stack and the second floating layer are located in a standard threshold voltage region.
13. The method according to claim 11, further comprising: Impurities are doped into the first suspension layer, wherein the second suspension layer is substantially free of impurities.
14. The method according to claim 13, wherein: The first gate stack and the first floating layer are located in a low threshold voltage region, and the second gate stack and the second floating layer are located in a high threshold voltage region.
15. The method according to claim 13, wherein: Doping impurities into the first suspension layer includes: epitaxially growing a plurality of third layers on the first suspension layer, wherein the third layers include a second semiconductor material different from the first semiconductor material; and Impurities contained in the driven-in second semiconductor material migrate from the third layer into the first suspended layer.
16. The method according to claim 11, further comprising: forming a plurality of third suspension layers in a third fin, wherein the third suspension layers include the first semiconductor material; and performing a third etching process to remove a portion of the third suspension layer without etching the first suspension layer and the second suspension layer, wherein the first etching process and the second etching process also remove other portions of the third suspension layer, Wherein, after performing the third etching process, the first suspension layer is thicker than the second suspension layer, and the second suspension layer is thicker than the third suspension layer.
17. A semiconductor structure comprising: substrate; A first fin is disposed on the substrate, wherein the first fin includes a plurality of first suspended nanostructures vertically stacked on each other; a first gate stack engaging the first suspended nanostructure in a first channel region; a gate spacer located above the first suspended nanostructure; A second fin disposed on the substrate, the second fin comprising a plurality of second suspended nanostructures vertically stacked on each other; as well as a second gate stack engaging the second suspended nanostructure in a second channel region, wherein the concentration of germanium in the middle portion of the first suspended nanostructure in the first channel region is higher than the concentration of germanium in the middle portion of the second suspended nanostructure in the second channel region, The first suspended nanostructure includes two end portions located directly below the gate spacer and a middle portion located between the two end portions, and a concentration of germanium in the middle portion of the first suspended nanostructure is higher than a concentration of germanium in the two end portions of the first suspended nanostructure.
18. The semiconductor structure according to claim 17, wherein: The first suspended nanostructure includes Si.
19. The semiconductor structure according to claim 17, wherein: The thickness of the middle portion of the first suspended nanostructure is greater than the thickness of the middle portion of the second suspended nanostructure.
20. The semiconductor structure of claim 19, wherein: A thickness of a central portion of the second suspended nanostructure is smaller than thicknesses of both end portions of the second suspended nanostructure.