Chip packaging method
By using a ceramic substrate and cover plate with a 3D structure in the chip package, instead of traditional wire bonding, higher density and more effective heat dissipation are achieved, and the problems of low chip packaging density and poor heat dissipation efficiency in the prior art are solved.
Patent Information
- Application Number
- CN202110793872.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-14
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-07-14
AI Technical Summary
The existing chip packaging technology has poor heat dissipation efficiency, low density and high parasitic parameters. This is mainly due to the limitations of wire bonding and single-sided heat dissipation technology, which leads to the packaging design being limited by the planar structure of the copper clad substrate, making it difficult to effectively improve the chip packaging density.
Using a 3D structure ceramic substrate and ceramic cover plate, metal surface layer and pattern layer are prepared by etching or multi-layer welding, instead of traditional wire bonding, vacuum active brazing or direct bonding is used to achieve the connection of metal surface layer, and through Laser fine engraving or etching to prepare the graphic layer of the ceramic cover plate, welding and fixing the chip to form a high-density packaging structure.
The chip package density is significantly improved and the traditional wire bonding is replaced by the line layer on the ceramic cover plate, providing more efficient heat dissipation and interconnect reliability, improving the overall performance of the package.
Smart Images

Figure CN113571476B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, in particular to a chip packaging method. Background Art
[0002] Ceramic substrates have the characteristics of high thermal conductivity, good heat resistance, low thermal expansion coefficient, high mechanical strength, good insulation, corrosion resistance, and radiation resistance. They are widely used in electronic device packaging. According to different preparation principles and processes, the current mainstream products can be divided into thick film printing ceramic substrates (Thick Printing Ceramic Substrate, TPC), direct bonded copper ceramic substrates (Direct Bonded Copper Ceramic Substrate, DBC), active metal brazing ceramic substrates (Active Metal Brazing Ceramic Substrate, AMB), etc. Miniaturized high-voltage and high-power modules are one of the important development directions of semiconductor devices. In the design of semiconductor devices, as the size decreases, the chip power density increases sharply, which puts forward new requirements for the reliability of module heat dissipation packaging.
[0003] The biggest defects of existing chip packages are poor heat dissipation efficiency, low chip packaging density, and excessively high parasitic parameters, which are related to the wire bonding (ultrasonic aluminum wire bonding) and unilateral heat dissipation technology they use.
[0004] In order to solve the above problems, various methods are adopted in the prior art, including 1) direct wire bonding structure: using solder to directly connect copper wires to the chip surface. Compared with wire bonding technology, the copper wires used in this technology can effectively reduce parasitic inductance. At the same time, due to the large interconnection area between the copper wires and the chip surface, the interconnection reliability can also be improved; 2) 2.5D module structure: different power chips are welded on the same substrate, and the interconnection between the chips is realized by adding a layer of metal wires in the adapter plate. The adapter plate and the power chip are very close, and high-temperature resistant materials need to be used. Low-temperature co-fired ceramic (LTCC) adapter plates are often used in this structure; 3) 3D module structure: two power chips or power chips and driving circuits are vertically interconnected through metal through holes or bumps. The 3D module packaging is realized by the pressing process (Press-Pack). This pressing process uses direct contact instead of wire bonding or welding to realize the interconnection between metal and chip. The structure includes 3 layers of conductive and heat-conductive flat plates, and the power chip is placed between the flat plates. The size of the flat plates is determined by the size of the interconnected chips and the layout structure of the chip surface that needs to be interconnected. In addition, a typical chip embedded packaging structure and method are provided in the related patent documents CN210668333U and CN110797318A, in which the chip is located in a through hole of a substrate, and a wiring layer is made on the back side.
[0005] As mentioned above, the chip packaging depends on the structure of the packaging component, that is, the structure of the packaging component restricts the chip packaging design. The existing technology uses wire bonding to replace lead bonding, which is effective but poor. The method of improving chip packaging density relies on additional wiring layers or multi-layer board structures, but no significant improvement is made to the copper-clad substrate. The existing technology is limited by the planar structure of the copper-clad substrate, so the effect is limited. Summary of the invention
[0006] In view of the problems existing in the prior art, the present invention provides a chip packaging method to solve at least one of the above technical problems.
[0007] In order to achieve the above object, the present invention provides a chip packaging method, characterized in that it includes the following steps:
[0008] Step 1: Etching or multi-layer welding a metal surface layer of a 3D structure on a ceramic substrate;
[0009] When the metal surface layer is prepared by etching, after the groove is etched normally, screen printing ink is used for masking and etching step by step;
[0010] When the metal surface layer is prepared by multi-layer welding, the metal layer in contact with the ceramic sheet is vacuum active brazing or direct bonding, and the remaining metal layers are diffusion welded;
[0011] Step 2: applying a cover plate metal layer on the ceramic cover plate, and preparing a graphic layer on the cover plate metal layer by laser engraving or etching;
[0012] Step 3, soldering the chip to the chip mounting position on the metal surface layer;
[0013] Step 4: After assembling the ceramic cover plate and the ceramic base plate up and down, fix them by welding.
[0014] Further preferably, the graphic layer in step 2 includes a circuit layer;
[0015] In step 4, the chip terminals on the chip are connected to the circuit layer.
[0016] The circuit layer replaces the original bonding wires or conductors that connect the chips.
[0017] Furthermore, in step 2, the graphic layer further comprises a clamping structure clamped with the ceramic metal surface layer;
[0018] A separation gap is provided between the clamping structure and the circuit layer.
[0019] Further preferably, the metal surface layer includes an isolated chip mounting portion; the metal surface layer also includes a cover mounting portion; the height of the chip mounting portion is lower than the height of the cover mounting portion;
[0020] The chip mounting portion is located at the center of the ceramic substrate;
[0021] The cover plate mounting portion is provided on the edge of at least one side of the ceramic substrate, and the cover plate mounting portion is clamped with the clamping structure.
[0022] Further preferably, the metal surface layer further comprises an isolated metal wiring welding area, and the metal wiring welding area is located between the chip mounting portion and the cover mounting portion;
[0023] When the ceramic cover plate and the ceramic substrate are assembled together, the chip terminals on the chip are electrically connected to the metal wiring pads through the circuit layer.
[0024] Further preferably, the metal surface layer includes a first metal layer, a second metal layer and a third metal layer arranged in sequence from top to bottom;
[0025] The second metal layer is provided with a bayonet recess;
[0026] The snap-fit structure is a snap-fit protrusion that matches the snap-fit recess.
[0027] Further preferably, after step 4, silica gel is injected between the ceramic cover plate and the ceramic substrate.
[0028] Further preferably, in step 2, holes are opened on the ceramic cover plate to lead out terminals on the circuit layer.
[0029] Further preferably, the third metal layer includes a second metal layer covering area whose orthographic projection area matches the second metal layer and a chip covering area located in the center, and the chip mounting position is fixed in the chip covering area;
[0030] A groove exists between the chip covering area and the second metal layer covering area;
[0031] The second metal layer is located above the second metal layer coverage area;
[0032] The second metal layer comprises a first metal layer covering area whose orthographic projection area matches the first metal layer and a connection area for engaging with the bayonet protrusion;
[0033] The connection area is located on at least one side of the periphery of the chip coverage area;
[0034] The first metal layer covers the first metal layer covering area.
[0035] Beneficial effects: 1) The 3D structured ceramic substrate can significantly improve the chip packaging density; 2) The circuit layer is etched on the ceramic cover plate, and the ceramic cover plate is welded to the ceramic substrate and the chip to replace the traditional wire bonding or conductor bonding, providing a new method to replace wire bonding. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is an exploded view of the present invention;
[0037] Figure 2 It is an exploded view from another perspective of the present invention;
[0038] Figure 3 Another structural schematic diagram of the present invention;
[0039] Figure 4 It is a structural schematic diagram of the ceramic substrate and the ceramic cover plate of the present invention in a spliced state.
[0040] Among them: 1 is a ceramic substrate, 11 is a chip mounting portion, 12 is a cover mounting portion, 13 is a metal wiring welding area, 2 is a ceramic cover, 22 is a circuit layer, and 23 is a clamping structure. DETAILED DESCRIPTION
[0041] The present invention will be further described below in conjunction with the accompanying drawings.
[0042] Specific embodiment 1, see Figures 1 to 4 , a chip packaging method, comprising the following steps:
[0043] Step 1: Etch or weld multiple layers of a 3D metal surface layer on the ceramic substrate 1.
[0044] When the metal surface layer is prepared by etching, after the groove is etched normally, screen printing ink is used for masking and etching step by step;
[0045] When multi-layer welding is used to prepare the metal surface layer, the metal layer in contact with the ceramic sheet is vacuum-active brazing or directly bonded, and the remaining metal layers are diffusion-welded. Among them, the temperature of vacuum-active brazing is controlled at 700℃-940℃, the vacuum degree is less than 0.01Pa, and the sintering time is 60min-540min. The process parameters of diffusion welding: the diffusion welding sintering temperature is 500℃-900℃, the vacuum degree is less than 0.1Pa, and the sintering time is 10min-540min. Take the metal surface layer including the first metal layer, the second metal layer and the third metal layer arranged from top to bottom as an example. The third metal layer is vacuum-active brazed or directly bonded to the ceramic sheet. The first metal layer and the second metal layer are diffusion-welded.
[0046] Step 2: applying a cover plate metal layer on the ceramic cover plate 2, and preparing a graphic layer on the cover plate metal layer by laser engraving or etching;
[0047] Step 3, soldering the chip to the chip mounting position on the metal surface layer;
[0048] Step 4: After the ceramic cover plate 2 and the ceramic base plate 1 are assembled up and down, they are fixed by welding.
[0049] The graphic layer in step 2 includes a circuit layer 22. In step 4, the chip terminals on the chip are connected to the circuit layer 22. The circuit layer 22 replaces the bonding wires or wires originally connected to the chip.
[0050] In step 2, the graphic layer further includes a clamping structure 23 clamped with the ceramic metal surface layer; a separation gap is provided between the clamping structure 23 and the circuit layer 22 .
[0051] See also Figure 1 The metal surface layer includes an isolated chip mounting portion 11 and a cover mounting portion 12; the height of the chip mounting portion 11 is lower than the height of the cover mounting portion 12; the chip mounting portion 11 is located in the center of the ceramic substrate 1; the edge of at least one side of the ceramic substrate 1 is provided with a cover mounting portion 12, and the cover mounting portion 12 is clamped with the clamping structure 23. In step 1, a groove between the chip mounting portion 11 and the cover mounting portion 12 is formed by normal etching.
[0052] Of course, other metal surface structures can also be used, see Figure 3 , the metal surface layer includes an isolated chip mounting portion 11 and a cover mounting portion 12; the height of the chip mounting portion 11 is lower than the height of the cover mounting portion 12; the chip mounting portion 11 is located in the center of the ceramic substrate 1; the edge of at least one side of the ceramic substrate 1 is provided with a cover mounting portion 12, and the cover mounting portion 12 is clamped with the clamping structure 23. In step one, normal etching is performed to form a groove between the chip mounting portion 11 and the cover mounting portion 12. The metal surface layer also includes an isolated metal wiring pad 13, and the metal wiring pad 13 is located between the chip mounting portion 11 and the cover mounting portion 12; when the ceramic cover 2 and the ceramic substrate 1 are assembled up and down, the chip terminals on the chip are electrically connected to the metal wiring pad through the circuit layer 22. In step one, normal etching is performed to form a groove between the chip mounting portion 11, the cover mounting portion 12, and the metal wiring pad 13. The metal wiring pad 13 is higher than the chip mounting portion.
[0053] The metal surface layer includes a first metal layer, a second metal layer and a third metal layer which are arranged in sequence from top to bottom; a bayonet recess is arranged on the second metal layer; and the clamping structure 23 is a bayonet protrusion which matches the bayonet recess.
[0054] In step 1, when etching is used to prepare the metal surface layer, the groove of the third metal layer can be formed by normal etching. Screen printing ink is used for blocking, and after etching once, the first metal layer is formed, screen printing ink is used for blocking, etching is performed for the second time to form the second metal layer, screen printing ink is used for blocking, etching is performed for the third time to form the third metal layer, and then a metal surface layer with a three-layer structure is formed. For the structure with a bayonet recess on the second metal layer, the bayonet recess is etched between the first etching and the second etching.
[0055] In step 1, a metal surface layer is prepared by multi-layer welding, and the first metal layer, the second metal layer, the third metal layer, the solder and the ceramic sheet can be stacked in sequence and then welded. Alternatively, after the first metal layer, the second metal layer and the third metal layer are diffusely welded to form the metal surface layer, the metal surface layer and the ceramic sheet are vacuum-activated brazing or directly bonded.
[0056] After step 4, silica gel is injected between the ceramic cover plate 2 and the ceramic substrate 1. The chip is encapsulated in the silica gel.
[0057] In step 2, holes are opened on the ceramic cover plate 2 to lead out the terminals on the circuit layer 22. The thickness of the metal surface layer is 0.127 mm-1.2 mm.
[0058] The first metal layer includes a second metal layer covering area whose orthographic projection area matches the second metal layer and a chip covering area located in the center, and the chip mounting position is fixed in the chip covering area; there is a groove between the chip covering area and the second metal layer covering area; the second metal layer is located above the second metal layer covering area; the second metal layer includes a first metal layer covering area whose orthographic projection area matches the first metal layer and a connection area for snapping the protrusion of the snap-in; the connection area is located on at least one side of the four sides of the chip covering area; the first metal layer covers the first metal layer covering area. The connection area is provided with a step, and the connection area includes an upper part and a lower part arranged up and down, and the upper part is provided with a snap-in recess, and the upper surface of the upper part is used to resist the area of the ceramic cover plate where the cover plate metal layer is not provided. The lower part is used to resist the snap-in structure of the cover plate metal layer. The second metal layer also includes a wiring area, and there is a gap between the connection area and the first metal layer covering area.
[0059] In step 1, when the metal surface layer is prepared by multi-layer welding, the independently arranged different areas, the chip mounting part 11, the cover mounting part 12, and the metal wiring welding area 13 are all stacked up and down with different metal sheets. The metal sheets at the same height constitute the same metal layer.
[0060] The surface flatness / warpage of the first metal layer, the second metal layer and the third metal layer is 0.01mm-0.2mm. The thickness of the first metal layer is 0.3-0.5 of the total thickness of the metal surface layer. The thickness of the second metal layer is 0.1-0.3 of the total thickness of the metal surface layer. The thickness of the third metal layer is 0.2-0.4 of the total thickness of the metal surface layer.
[0061] The metal surface layer is one of a copper layer or an aluminum layer. The cover plate metal layer is one of a copper layer or an aluminum layer.
[0062] Beneficial effects: 1) The 3D structured ceramic substrate can significantly improve the chip packaging density; 2) The circuit layer 22 is etched on the ceramic cover plate 2, and the ceramic cover plate 2 is welded to the ceramic substrate and the chip to replace the traditional wire bonding or conductor bonding, providing a new method to replace wire bonding.
[0063] The above are only preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A chip packaging method, characterized in that: The steps include: Step 1: Etching or multi-layer welding a metal surface layer of a 3D structure on a ceramic substrate; When the metal surface layer is prepared by etching, after the groove is etched normally, screen printing ink is used for masking and etching step by step; When the metal surface layer is prepared by multi-layer welding, the metal layer in contact with the ceramic sheet is vacuum active brazing or direct bonding, and the remaining metal layers are diffusion welded; Step 2: applying a cover plate metal layer on the ceramic cover plate, and preparing a graphic layer on the cover plate metal layer by laser engraving or etching; Step 3, soldering the chip to the chip mounting position on the metal surface layer; Step 4: After the ceramic cover plate and the ceramic base plate are assembled up and down, they are welded and fixed; The graphic layer in step 2 includes a circuit layer; in step 2, the graphic layer also includes a clamping structure clamped with the ceramic metal surface layer; A separation gap is provided between the clamping structure and the circuit layer; In step 4, the chip terminals on the chip are connected to the circuit layer.
2. A chip packaging method according to claim 1, characterized in that: The metal surface layer includes an isolated chip mounting portion, and the metal surface layer also includes a cover mounting portion; the height of the chip mounting portion is lower than the height of the cover mounting portion; The chip mounting portion is located at the center of the ceramic substrate; The cover plate mounting portion is provided on the edge of at least one side of the ceramic substrate, and the cover plate mounting portion is clamped with the clamping structure.
3. A chip packaging method according to claim 2, characterized in that: The metal surface layer further comprises an isolated metal wiring pad, the metal wiring pad being located between the chip mounting portion and the cover mounting portion; When the ceramic cover plate and the ceramic substrate are assembled together, the chip terminals on the chip are electrically connected to the metal wiring pads through the circuit layer.
4. A chip packaging method according to claim 2, characterized in that: The metal surface layer includes a first metal layer, a second metal layer and a third metal layer arranged in sequence from top to bottom; The second metal layer is provided with a bayonet recess; The snap-fit structure is a snap-fit protrusion that matches the snap-fit recess.
5. A chip packaging method according to claim 2, characterized in that: After step 4, silicone is injected between the ceramic cover plate and the ceramic substrate.
6. A chip packaging method according to claim 2, characterized in that: In step 2, holes are opened on the ceramic cover plate to lead out the terminals on the circuit layer.
7. A chip packaging method according to claim 4, characterized in that: The thickness of the metal surface layer is 0.127mm-1.2mm.
8. A chip packaging method according to claim 4, characterized in that: The third metal layer includes a second metal layer covering area whose orthographic projection area matches the second metal layer and a chip covering area located in the center, and the chip mounting position is fixed in the chip covering area; A groove exists between the chip covering area and the second metal layer covering area; The second metal layer is located above the second metal layer coverage area; The second metal layer comprises a first metal layer covering area whose orthographic projection area matches the first metal layer and a connection area for engaging with the bayonet protrusion; The connection area is located on at least one side of the periphery of the chip coverage area; The first metal layer covers the first metal layer covering area.