Method for electrolytic deposition of chromium oxide layers

By depositing a chromium oxide layer on the black steel plate and using an iridium oxide or tantalum oxide catalytic layer, the problem of insufficient adhesion during the plating process of trivalent chromium compound electrolyte solution is solved, and an efficient plating process that complies with the REACH standard is achieved. For non-food applications.

CN113597481BActive Publication Date: 2024-11-15TATA STEEL IJMUIDEN BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080021693.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-18
Filing Date
2020-02-25
Publication Date
2024-11-15
Estimated Expiration
2040-02-25

AI Technical Summary

Technical Problem

In the prior art, it is difficult to improve the adhesion between the black steel plate and the organic coating during the plating process, and the hexavalent chromium compounds used in traditional electrolytic chromium plating steel are prohibited by REACH, so it is necessary to develop REACH-compliant. Substitute.

Method used

Using a water-soluble chromium (III) salt electrolyte solution without halide ions, the pH value of the electrolyte is controlled by depositing a chromium oxide layer on the black steel plate, and using a mixed metal oxide of iridium oxide or iridium oxide and tantalum oxide as the anode catalytic layer. and temperature, avoid the use of complexing agents to prevent the deposition of chromium metal, forming a closed chromium oxide layer to improve adhesion.

Benefits of technology

The adhesion between the chromium oxide layer and the organic coating on black steel plates is significantly improved, providing a REACH compliant alternative, suitable for non-food applications, and an efficient plating process on industrial production lines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113597481B_ABST
    Figure CN113597481B_ABST
Patent Text Reader

Abstract

The present invention relates to a process for the electrolytic deposition of a chromium oxide layer onto i) black steel sheets or onto ii) black steel sheets coated with a chromium electrodeposited coating produced by electroplating based on chromium (III) technology, and to the coated products obtained thereby.
Need to check novelty before this filing date? Find Prior Art

Description

Field of the Invention

[0001] The present invention relates to a method for electroplating steel strip with a coating and improvements thereto. Background of the Invention

[0003] Tin mill products traditionally include electrolytic tin plated steel, electrolytic chrome plated steel (also known as tin free steel or TFS) and black steel. Although not limited thereto, most applications of tin mill products are used by the container industry in the manufacture of cans, end caps and closures for the food and beverage industry.

[0004] In continuous steel strip plating, a cold rolled steel strip is provided, which is usually annealed after cold rolling to soften the steel by recrystallization annealing or recovery annealing. After annealing and before plating, the steel strip is first cleaned for removing oil and other surface contaminants. After the cleaning step, the steel strip is pickled in a sulfuric acid or hydrochloric acid solution for removing the oxide film. Between the different treatment steps, the steel strip is rinsed to prevent contamination by the solution used for the next treatment step. During the rinsing and transportation of the steel strip to the plating section, a new thin oxide layer is immediately formed on the exposed steel surface. It is necessary to protect the exposed steel surface from further oxidation by depositing a coating layer onto the steel.

[0005] This protection is provided by a process called electrodeposition used in electroplating. The part to be plated (steel strip) is the cathode of the circuit. The anode of the circuit can be made of the metal to be plated on the part (dissolving anodes, such as those used in conventional tinning) or dimensionally stable anodes (which do not dissolve during the plating process). The anode and cathode are immersed in an electrolyte solution containing ions of the metal to be deposited on the black steel plate substrate.

[0006] Black steel plate is a tin rolled product that has not (yet) received any metallic coating during the production process. It is the base material for the production of other tin rolled products. Black steel plate can be single-thinned or double-thinned. For single-thinned black steel plate, the hot-rolled strip is thinned to the desired thickness in a cold rolling mill and then recrystallized or recovery annealed in a continuous or batch annealing process and optionally temper rolled. For double-thinned black steel plate, the single-rolled substrate is subjected to a second rolling thinning of greater than 5%. Single-thinned black steel plate that is temper rolled is generally not considered to be double-thinned black steel plate, because the temper rolling thinning is less than 5%.

[0007] SR or DR black steel plates are usually supplied in the form of coiled strip.

[0008] (Trivalent chromium coating technology) is a REACH compliant alternative to electrolytically chromed steel (ECCS). ECCS is a SR or DR black steel sheet coated by electrolytic deposition, which has metallic chromium covered with a chromium oxide film. This type of coated steel is always produced based on a technology using harmful Cr(VI) compounds. REACH (EU Chemicals Regulation) prohibits the use of these hexavalent chromium compounds. Therefore, alternatives have been developed over time based on harmless compounds. Developed by Tata Steel based on harmless Cr(III) technology. WO2014202316-A1 discloses a Cr(III) electrolyte using 120 g / l (=385 mM) basic chromium(III) sulfate, although this substrate already has better performance compared to other alternatives and has comparable performance to ECCS, but the adhesion between TCCT-substrate and organic coating needs further improvement.

[0009] Purpose of the Invention

[0010] The object of the present invention is to deposit a chromium oxide layer on a metal strip from an electrolyte solution comprising a trivalent chromium compound.

[0011] It is also an object of the present invention to provide a REACH compliant alternative to Cr(VI) based treatments that improves the adhesion of paints to Cr coated black steel sheets.

[0012] Description of the invention

[0013] One or more objects are achieved by the following method, which is based on a method for electrolytically depositing a chromium oxide layer onto a black steel sheet or onto a black steel sheet coated with a chromium electrodeposition coating produced based on chromium (III) technology. The deposition of the chromium oxide layer is carried out from an aqueous electrolyte solution containing a halide ion and comprising a trivalent chromium compound provided by a water-soluble chromium (III) salt in a continuous high-speed plating line, the continuous high-speed plating line operating at a line speed of at least 50 m / min. The black steel sheet or the coated black steel sheet serves as a cathode. An anode is provided, which comprises i) iridium oxide or ii) a catalytic coating of a mixed metal oxide, the mixed metal oxide comprising iridium oxide and tantalum oxide, for reducing or eliminating Cr 3+ - ions oxidized to Cr 6+ -ions, and wherein the electrolyte solution contains at least 50 mM and at most 1000 mM Cr 3+ ions, a total of 25-2800 mM sodium sulfate or potassium sulfate, a pH measured at 25°C between 2.50 and 3.6, and wherein the plating temperature is between 40 and 70°C and wherein no other compounds are added to the electrolyte, except for optional sulfuric acid or sodium or potassium hydroxide to adjust the pH to the desired value. In addition, only unavoidable impurities may be present in the electrolyte.

[0014] For the sake of clarity, note that 1 mM means 1 millimole / l. It should also be noted that there are two potential sources of sodium sulfate in the electrolyte. First, if basic chromium sulfate is used as the water-soluble chromium (III) salt, its chemical formula is (CrOHSO4)2×Na2SO4, then 0.5 mM of Na2SO4 is also added to the electrolyte for each mM of Cr. However, Na2SO4 can also be added as a salt, for example as a salt that enhances conductivity, or to increase the dynamic viscosity of the electrolyte. The total amount of Na2SO4 is the sum of the addition of Na2SO4 and the amount together with the basic chromium (III) sulfate. If basic chromium sulfate is not used as the water-soluble chromium (III), and for example chromium (III) sulfate or chromium (III) nitrate is used, any Na2SO4 present in the electrolyte is added as sodium sulfate. The above Cr (III) salts, including basic chromium (III) sulfate, can be provided alone or in combination.

[0015] A steel substrate in the sense of the present invention is intended to mean a steel substrate including a metallic layer, if present, which has been deposited on the steel substrate before the chromium oxide layer is deposited according to the invention.

[0016] The absence of complexing agents in the electrolyte means that there are no necessary components for the deposition of Cr-metal. Complexing agents are required for the very stable [Cr(H2O)6] 3+ The complex is unstable. The inventors unexpectedly discovered that by avoiding the use of complexing agents (such as NaCOOH), the deposition of chromium metal is prevented but a closed chromium oxide layer is deposited instead. In addition, the absence of a carbon-containing complexing agent also prevents the co-deposition of chromium carbide in the oxide layer. If present in the oxide layer in a detectable amount, any residual amount of chromium carbide is therefore the result of a small and unavoidable amount of residual other compounds present in the base material that produces the electrolyte. The presence of sulfate in the electrolyte causes the presence of sulfate in the chromium oxide coating layer under the plating conditions according to the present invention. The maximum amount of sulfate detected at the surface is about 10%. The minimum amount of sulfate at the surface is 0.5%, and in most cases at least 2%. These values ​​are obtained from the XPS depth distribution within the first 3nm starting from the outer surface.

[0017] Due to the closed chromium oxide layer on the substrate, the adhesion between the substrate on which the closed chromium oxide layer is deposited and the organic coating layer is greatly improved.

[0018] If the pH of the electrolyte solution becomes too high or too low, sulfuric acid or sodium hydroxide may be added to adjust the pH to a value within the desired range. Likewise, different acids or bases may be used, but sulfuric acid and sodium hydroxide are preferred in view of simplifying the bath chemistry.

[0019] Sodium sulfate or potassium sulfate also acts as a salt that enhances conductivity. In order to keep the electrolyte as simple as possible, and to prevent the formation of chlorine or bromine, the salt that enhances conductivity is a sulfate. The cation is preferably sodium or potassium. In order for the electrolyte not to become too viscous, a maximum amount of 2800mM of sodium sulfate or potassium sulfate is still permissible. For reasons of simplicity, the cation is preferably sodium. A pH exceeding 4 leads to a colloidal reaction in the electrolyte, making it unusable for electroplating. A pH below 2.50 is undesirable because the increase in surface pH at the cathode required for the deposition of chromium oxide (CrOx) cannot be obtained in the electrolyte at these low pH values. High pH also enables the use of lower current densities during deposition, resulting in less hydrogen evolution. Excessive hydrogen evolution is believed to cause a streaky appearance of the surface at lower pH (below 2.50). A relatively high electrolyte temperature electrolyte of at least 40°C also allows the use of lower current densities, which also helps to reduce hydrogen evolution.

[0020] It is preferred to use only sodium sulfate in the electrolyte, since it keeps the composition of the electrolyte as simple as possible.

[0021] Halides such as chloride or bromide may be absent in the electrolyte. This absence is required to prevent the formation of, for example, chlorine or bromine at the anode. The electrolyte also does not contain a depolarizing agent. In many similar baths, potassium bromide is used as a depolarizing agent. The absence of this compound mitigates any risk of bromine formation at the anode. Likewise, buffers such as the commonly used boric acid (H3BO3) are absent in the electrolyte.

[0022] It is essential in the method according to the invention that the anode comprises i) a catalytic coating of iridium oxide or ii) a mixed metal oxide comprising iridium oxide and tantalum oxide. The catalytic coating is usually deposited onto a titanium anode, wherein the titanium covering is such that the titanium is not exposed to the electrolyte. It is found that the use of any other practical anode such as platinum, platinum-plated titanium or nickel-chromium leads to Cr(VI) compounds which are to be avoided due to their toxic and carcinogenic properties. 6+ - Formation of ions. Carbon as anode material breaks down over time due to the high current densities used in industrial high-speed plating lines and should also not be used.

[0023] In the method according to the invention, the steel substrate is a black steel sheet or a black steel sheet coated with a chromium electrodeposition coating produced based on chromium (III) technology, such as TCCT (see Figure 3 ).

[0024] The steel used for the black steel plate may be any steel grade suitable for producing packaging steel. By way of example, but not intended to be limiting, reference is made to steel grades used for packaging applications in EN 10202:2001 and ASTM 623-08:2008.

[0025] Black steel sheets are usually provided in the form of low carbon (LC), extra low carbon (ELC) or ultra low carbon (ULC) strips, wherein the carbon content, expressed as a weight percentage, is between 0.05 and 0.15 (LC), between 0.02 and 0.05 (ELC) or less than 0.02 (ULC), respectively. Alloying elements such as manganese, aluminum, nitrogen, but sometimes also elements such as boron are added to improve the mechanical properties (see EN 10202, 10205 and 10239). Black steel sheets may consist of interstitial-free low carbon steels, extra low carbon steels or ultra low carbon steels, such as titanium stabilized, niobium stabilized or titanium-niobium stabilized interstitial-free steels.

[0026] Single-reduced (SR) black steel sheets (as defined in international standards) fall within the range of 0.15mm to 0.49mm; double-reduced (DR) black steel sheets 0.13mm-0.29mm, with a typical range of DR being 0.14-0.24mm. For special applications, lower specifications down to 0.08mm are now available in single or double-reduced base materials.

[0027] TCCT is based on the deposition of a chromium-based layer, which is composed of chromium oxide and chromium metal, as well as some chromium carbide and some chromium sulfate. This layer is deposited in a one-step process, and therefore optimized conditions are used to deposit Cr-metal (Cr) and Cr-oxide (CrOx) simultaneously. In such a deposited layer, the oxide is distributed in the layer, not just at the top of the layer. There is no closed oxide layer, that is, an oxide layer covering the entire surface of the substrate at the surface. Although the advantage of the one-step process according to WO2014202316-A1 is simplicity, the inventors have found that by applying a Cr-CrOx layer according to WO2014202316-A1, a chromium oxide layer is deposited from a separate electrolyte according to the present invention onto Cr-CrOx (and optionally also containing chromium sulfate and / or chromium carbide), allowing better control of the oxide layer, allowing deposition of a closed oxide layer, and allowing improvement of the performance of the oxide layer in terms of improving adhesion to an organic coating. The absence of a complexing agent means no co-deposition or co-deposition of only a very small amount of metallic chromium.

[0028] The method according to the invention also allows the deposition of a closed chromium oxide layer directly on top of the black steel sheet. Although the corrosion protection of this layer is limited, the adhesion of the organic coating to the black steel sheet is greatly improved, and this will allow the application of paint or polymer films to the black steel sheet. Such a material will be suitable for applications that do not require extreme corrosion resistance, for example for some non-food applications.

[0029] Therefore, although the substrates may be different, the effect of the closed chromium oxide layer deposited on the substrate in each case leads to an improvement in the adhesion between the substrate and the organic coating.

[0030] Preferred embodiments are provided in the dependent claims.

[0031] As water-soluble chromium(III) salts, one or more salts are selected from the group consisting of basic chromium(III) sulfate, chromium(III) sulfate and chromium(III) nitrate. From the point of view of keeping the bath chemistry as simple as possible, it is preferred to use only basic chromium(III) sulfate.

[0032] In embodiments, the electrolyte solution contains up to 500 mM Cr 3+ -ions, preferably up to 350 mM, more preferably up to 250 mM or even up to 225 mM Cr 3+ - ions. The electrolyte solution preferably contains at least 100 mM Cr 3+ -ions, preferably at least 125 mM Cr 3+ -ions. These preferred ranges provide good results.

[0033] In a preferred embodiment, the pH of the electrolyte is measured at 25°C between 2.50 and 3.25. Preferably the plating temperature is between 40 and 65°C. In an embodiment, the pH of the electrolyte solution is at most 3.30, preferably at most 3.00. In an embodiment, the pH is at least 2.60 or even at least 2.70. The pH range between 2.55 and 3.25 provides excellent results in terms of coating quality. Likewise, at values ​​greater than 3.25, there is no risk of colloidal reactions in the electrolyte making it unusable for electroplating in the method according to the invention. In the pH range between 3.25 and 4, the risk increases from acceptable just above 3.25 to unacceptable if the pH is greater than 4. Less than 2.55, the process becomes less economical because the effort required to increase the surface pH at the cathode at lower pH is greater.

[0034] The plating time, i.e. the duration of applying current to the cathode (which is significantly shorter than the immersion time), is preferably as short as possible to allow the method to be used in an industrial production line. At low production line speeds and / or long anode lengths, the plating time is at most 3 seconds. A maximum plating time of at most 1000ms is still permissible, preferably at most 900ms. At very high production line speeds, it may be necessary to increase the current density and / or total anode length to keep the production line at a practical minimum. Although it is preferred that there is no complexing agent at all in the electrolyte in the method according to the present invention, it may still occur that, despite all appropriate care and the use of an intermediate rinse bath, a small amount is inevitably present as an inevitable impurity in the electrolyte due to the introduction of the previous upstream electrolyte bath in the plating production line. The maximum permissible value is 10mM of a complexing agent such as NaCOOH, preferably at most 5mM, preferably at most 2mM. It was found that these amounts did not result in any significant chromium metal deposition and the deposited oxide layer adhesion quality appeared unaffected. Nevertheless, it is preferred that there is no such complexing agent in the electrolyte according to the method of the present invention.

[0035] In embodiments, the electrolyte solution contains at least 210 mM and / or at most 845 mM sodium sulfate.

[0036] In a preferred embodiment the plating temperature is at least 50°C, preferably at least 55°C.

[0037] In embodiments the line speed of the continuous plating line is at least 100 m / min, more preferably at least 200 m / min.

[0038] In a preferred embodiment, the aqueous electrolyte consists only of basic chromium (III) sulfate, sodium sulfate and optionally sulfuric acid or sodium hydroxide in an amount sufficient to adjust the pH of the electrolyte to the desired value, and unavoidable impurities. The pH is preferably adjusted to a value of 2.55 or greater, and preferably to a value of 3.25 or less.

[0039] In a preferred embodiment, the black steel sheet is pre-coated on one or both sides with a metallic coating layer before being provided with an oxide layer according to the method of the invention, the coating layer(s) comprising chromium metal and chromium oxide and optionally also one or more of chromium carbide and chromium sulfate, and wherein the metallic coating layer is deposited from an electrolyte solution comprising a water-soluble chromium (III) salt, wherein the electrolyte solution is free of chloride ions and boric acid buffer, the conductive substrate serves as the cathode and the anode comprises a catalytic coating of iridium oxide or a mixed metal oxide, for example a mixed metal oxide comprising iridium oxide and tantalum oxide, for reducing or eliminating Cr 3+ - ions oxidized to Cr 6+ -ions, wherein the electrolyte solution contains at least 50 mM and at most 1000 mM Cr 3+ions (=52g / lCr(III)), complexing agent

[0040]

[0041] The molar ratio is at least 1:1, preferably at least 1.5:1 and more preferably at least 2:1, and wherein the formate / Cr 3+ The molar ratio is up to 2.5:1, 1 to 2800 mM (= 398 g / l) of sodium sulfate (Na2SO4), the pH measured at 25°C is between 1.5 and 3.6, and the plating temperature is between 30 and 70°C. For Cr(III) is 40 g / l, in formate / Cr 3+ Good results are obtained for a ratio of 2.0 and a plating temperature of 45°C. Preferably the plating temperature is at least 35°C and at most 55°C, more preferably at most 50°C. Formate ions are required as complexing agents to deposit Cr metal and a ratio of at most 2.5:1 has proven to be sufficient in most cases. Preferably the electrolyte solution contains at least 50 mM and at most 750, more preferably at most 500 and most preferably at most 250 mM Cr 3+ -ion.

[0042] In the case of higher Cr (III) content, the stability of the plating process of the Cr metal layer is improved. The plating window in terms of current density is also larger at higher concentrations. Similarly, higher formate / Cr ratios increase the plating window. The plating temperature also affects the efficiency, because depositing a certain amount of Cr (in mg / m 2 The process robustness in terms of sensitivity to fluctuations becomes less at higher Cr(III) concentrations and higher formate / Cr ratios.

[0043] In a preferred embodiment, the pH of the electrolyte is between 1.5 and 3.6 measured at 25°C. In embodiments, the pH of the electrolyte solution is at most 3.30, preferably at most 3. In embodiments, the pH is at least 2.00, preferably at least 2.50, even more preferably at least 2.60 or even at least 2.70. The pH range between 2.55 and 3.25 provides excellent results in terms of coating quality. A pH of about 2.9 appears to result in an optimized plating window.

[0044] In an embodiment, the black steel plate, optionally pre-coated with the aforementioned coating layer(s) comprising chromium metal, chromium oxide, chromium carbide and chromium sulfate and provided with a chromium oxide layer applied using the method according to the present invention, is further coated on one or both sides by a film lamination step or a direct extrusion step with an organic coating consisting of a thermoplastic monolayer or a thermoplastic multilayer polymer, preferably wherein the thermoplastic polymer coating is a polymer coating system comprising one or more layers comprising thermoplastic resins such as polyesters or polyolefins, acrylic resins, polyamides, polyvinyl chlorides, fluorocarbon resins, polycarbonates, styrene-type resins, ABS resins, chlorinated polyethers, ionomers, urethane resins and functionalized polymers, and / or their copolymers, and or their blends.

[0045] Preferably the thermoplastic polymer coating is a polymer coating system comprising one or more layers of a thermoplastic resin such as a polyester or polyolefin, but may also include acrylic resins, polyamides, polyvinyl chloride, fluorocarbon resins, polycarbonates, styrenic resins, ABS resins, chlorinated polyethers, ionomers, urethane resins and functionalized polymers. To illustrate:

[0046] Polyester is a polymer composed of a dicarboxylic acid and a diol. Examples of suitable dicarboxylic acids include terephthalic acid, isophthalic acid (IPA), naphthalene dicarboxylic acid, and cyclohexane dicarboxylic acid. Examples of suitable diols include ethylene glycol, propylene glycol, butanediol, hexanediol, cyclohexane diol, cyclohexanedimethanol (CHDM), neopentyl glycol, and the like. More than two dicarboxylic acids or diols may be used together.

[0047] Polyolefins include, for example, polymers or copolymers of ethylene, propylene, 1-butene, 1-pentene, 1-hexene or 1-octene.

[0048] Acrylic resins include, for example, polymers or copolymers of acrylic acid, methacrylic acid, acrylate, methacrylate or acrylamide.

[0049] The polyamide resin includes so-called nylon 6, nylon 66, nylon 46, nylon 610, and nylon 11, for example.

[0050] Polyvinyl chloride includes homopolymers and copolymers, for example using ethylene or vinyl acetate.

[0051] Fluorocarbon resins include, for example, polyethylene tetrafluoride, polyethylene trifluoride, chloromonofluoride, ethylene-propylene hexafluoride, polyvinyl fluoride, and polyvinylidene fluoride.

[0052] • Functionalized polymers, for example by grafting with maleic anhydride, including, for example, modified polyethylene, modified polypropylene, modified ethylene acrylate copolymers and modified ethylene vinyl acetate.

[0053] Mixtures of two or more resins may be used. In addition, the resins may be mixed with antioxidants, heat stabilizers, UV absorbers, plasticizers, pigments, nucleating agents, antistatic agents, mold release agents, antiblocking agents, etc. The use of such thermoplastic polymer coating systems has been shown to provide excellent properties in can preparation and can use, such as shelf life.

[0054] Preferably the thermoplastic polymer coating is a polymer coating system comprising one or more layers comprising a thermoplastic resin such as polyester or polyolefin, acrylic resin, polyamide, polyvinyl chloride, fluorocarbon resin, polycarbonate, styrene-type resin, ABS resin, chlorinated polyether, ionomer, urethane resin and functionalized polymers, and / or copolymers thereof, and or blends thereof.

[0055] Preferably, the thermoplastic polymer coating on one or both sides of the coated black steel plate is a multi-layer coating system, the coating system comprising at least an adhesive layer for adhering to the coated black steel plate, a surface layer and a bulk layer between the adhesive layer and the surface layer, wherein the layers of the multi-layer coating system comprise or consist of polyesters, such as polyethylene terephthalate, isophthalic acid (IPA)-modified polyethylene terephthalate, cyclohexanedimethanol (CHDM)-modified polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, or copolymers or blends thereof.

[0056] The application process of the thermoplastic polymer coating is preferably carried out by laminating the polymer film to the coated black steel plate by means of extrusion coating and lamination, wherein the polymer resin is melted and formed into a hot film, which is applied to a moving substrate. The coated substrate is then usually passed between a set of counter-rotating rollers, which press the coating onto the substrate to ensure complete contact and adhesion. An alternative is film lamination, wherein a polymer film is provided and applied to a heated substrate and passed through a set of counter-rotating rollers and pressed onto the substrate between them to ensure complete contact and adhesion. Example

[0057] The materials according to Table 1 were used as substrates.

[0058] Table 1: Substrate

[0059]

[0060] Table 2: Cr(III) electrolyte composition

[0061] Components unit 1 Reference (Sample E) Cr(III) concentration <![CDATA[g l -1 ]]> 20 20 Additional Sodium Sulfate <![CDATA[g l -1 ]]> 0 42 Complexing agent <![CDATA[g l -1 ]]> 0 39(NaCOOH)

[0062] exist Figure 2 The results of the RCE experiments are presented in Figure 1. Using electrolyte 1 (20 g / l basic chromium (III) sulfate (385 mM Cr3 + ). The experiments were performed at 55°C and a pH of 2.7 on a cylindrical electrode rotating at 776 rpm. 776 rpm corresponds to a line speed of 100 m / s in an industrial coating line. For the electrodeposition experiments, a titanium anode with a catalytic mixed metal oxide coating of iridium oxide and tantalum oxide was used. The rotation speed of the RCE was kept constant at 776 RPM (Ω 0.7 =6.0s 0.7 ). The substrates are listed in Table 1 and the dimensions of the cylinders are 113.3 mm x φ73 mm. The plating time is 800 ms. Figure 2 For black steel sheets (1) and TCCT (2), the CrOx coating weight (expressed as Cr metal, mg / m 2 In the figure, the Cr coating weight is plotted as a function of current density. For sample 1, no CrOx was present on the new substrate before coating the substrate using the method according to the invention.

[0063] The amount of Cr deposited is plotted on the Y axis. The circles in the graph show the amount of Cr oxide. The amount of Cr oxide was determined by means of XRF. The XRF measurements were performed as described in the previously cited paper, which is included herein by reference. By first measuring the sample with XRF, a basic value of the total deposited chromium (i.e. metal, oxide, sulfate and (if present) carbide) was measured. After the sample was exposed to hot (90°C) concentrated (300 g l -1 ) sodium hydroxide solution for 10 minutes, which dissolves all the Cr oxides and a second XRF-measurement is performed. The difference (Δ(XRF)) is then due to the Cr oxides and this is Figure 2 The values ​​plotted in .

[0064] Table 3: Figure 6 Details of the RCE experiment drawn in

[0065] # symbol Substrate Preprocessing Color oxide layer 1 · BP Degreasing and pickling Light Gray 2 · BP Degreasing and pickling Light Gray 3 · BP Degreasing and pickling Light Gray 4 ■ TCCT Degreasing Yellow

[0066] The RCE results are comparable to those of coil tests in an industrial scale pilot line ( Figure 2 The test line has the following settings: 14 g / l Cr, T = 55 °C, line speed = 150 m / min 1 , current density = 18.75A dm -2 , plating time: 600 ms, even though the Cr(III) concentration was slightly lower. It was also found that the pretreatment of the strip had little effect on the amount of CrOx deposited onto the strip.

[0067] Similar experiments conducted at pH values ​​less than 2.50, such as those disclosed in US6099714, show unsatisfactory streaky surface quality when conducted on industrial production lines on black steel plates or steel substrates comprising a metallic coating layer on one or both sides, wherein the coating layer(s) comprise chromium metal and chromium oxide. US6099714 discloses a 3×5 inch based 2 Experiments on tinplate samples, i.e. in a laboratory setting and intended for piece-by-piece plating and on substrates other than those according to the process of the present invention. In addition to an appearance that may be perceived by consumers as aesthetically unappealing, streaking may also result in non-uniform oxide layer thickness and / or composition, which may affect the performance of the coated black steel sheet as a whole.

[0068] Table 4: Effect of pretreatment on the amount of Cr deposited as CrOx on TCCT

[0069] Preprocessing <![CDATA[Average Cr (mg m -2 )]]> none 21.3 Pickling 20.7 Pickling and degreasing 18.8

[0070] The ΔXRF results are almost identical for the various pretreatments, so that the amount of Cr as CrOx is hardly affected by the type of pretreatment of the substrate prior to depositing the chromium oxide layer according to the present invention.

[0071] Sterilization test It was carried out using black steel sheets which were pre-coated with a coating layer comprising chromium metal and chromium oxide (and optionally also one or more of chromium carbide and chromium sulfate) deposited from an electrolyte with a complexing agent (i.e. TCCT) and further provided with a chromium oxide layer applied using the method according to the invention, i.e. deposited from an electrolyte without a complexing agent. The black steel sheets were thus first provided with a Cr-CrOx layer and then with a CrOx coating. This coated black steel sheet was further coated with PET or PP on both sides, which side would become the inside of the DRD tank, by a film lamination step. The performance was compared with conventional ECCS (based on Cr(VI) technology). In all cases the black steel sheets were 0.223 mm thick, continuously annealed SR low carbon steel (TH340, 0.045 wt. % C, 0.205 wt. % Mn, 0.045 wt. % Al-solute).

[0072] The following combinations were tested (all polymers were 3 layer systems including cling layer, bulk layer and top layer). "Inside" means the side that becomes the inside of the can:

[0073] A.PET coated Inner and outer: 20μm PET

[0074] B.PP coated Inner: 40μm PP / Outer: 20μm PET

[0075] C.PET ECCS reference: inside and outside: 20μm PET

[0076] D.PP ​​ECCS reference: Inner: 40μm PP / Outer: 20μm PET

[0077] E. Reference: Inner and outer: 20μm PET

[0078] Sample E is No TCCT variants with an additional CrOx layer deposited according to the invention. Samples C and D are conventional reference ECCS (Cr(VI) technology) samples. Samples A and B are TCCT variants with an additional CrOx layer deposited according to the invention. The amount of chromium oxide (expressed as Cr in mg / m 2 10mg / m 2 Both the TCCT coating and the oxide coating were applied on an industrial plating line. The polymer layer was laminated to the metal substrate by film lamination including high temperature post-heating and water quenching in an industrial lamination line. Standard two-piece DRD (300 ml, 65 mmφ) cans were produced from these materials.

[0079] Table 5: The test conditions are as follows:

[0080] medium condition Speak directly 2 weeks opening 3.6% NaCl with scratching 121℃60min. 5 cans - 3.6% NaCl aerated 121℃60min. 10 cans - 3.6% NaCl + 1g / l Vitamin C 121℃60min. 10 cans 10 cans 12g / l raw material + 2g / l plasma 121℃60min. 10 cans 10 cans

[0081] Table 6: The results are as follows:

[0082] T-stripping NaCl Scratching Vitamin C Broth A invention TCCT / PET 5.2 ++ 8 ++ ++ E Refer to TCCT TCCT / PET 4.5 -- 25 -- ++ C Refer to ECCS ECCS / PET 5.1 + 6 ++ ++ B invention TCCT / PP 8.1 + 7 ++ ++ D Refer to ECCS ECCS / PP 10.8 + 5 ++ ++

[0083] The peel force is measured in N and represents the adhesion of the polymer layer to the substrate. The results after two weeks are consistent with those immediately after opening, and these results show that black steel panels coated with a TCCT layer from an electrolyte with a complexing agent followed by a chromium oxide layer deposited from the same electrolyte without a complexing agent match or even outperform existing ECCS standards for PET coated substrates.

[0084] The substrates were also subjected to a painting test. Four different paints were tested under three different conditions. The test consisted of a sterilization test of the painted and cured samples (applied and cured according to the paint supplier's instructions) in NaCl, citric acid and cysteine ​​solutions at 130°C for one hour.

[0085] Table 7: Results of the paint test

[0086]

[0087] Adhesion (Gt) is tested according to the Gitterschnitt method on the flat part of the sample as described in ISO 2409: 1992, Edition 2. "0" means perfect adhesion, "5" is poor.

[0088] A 5 mm Erichsen dome was applied to each painted panel and sterilization medium / condition and adhesion on the Erichsen dome was tested by tape only without cutting.

[0089] These results clearly show that variant A (inventive example) performs much better than variant E, which is identical to A but without the chromium oxide coating according to the invention. It is also shown that variant A performs comparable to the current Cr(VI) variant (C) and even outperforms it in some combinations of lacquer and sterilization media / conditions.

[0090] BRIEF DESCRIPTION OF THE DRAWINGS

[0091] The invention will now be explained by way of the following non-limiting drawings.

[0092] Figure 1 Schematic overview of the process steps to obtain a coated product starting from a hot rolled strip.Before cold rolling, the hot rolled strip is usually pickled (not shown) to remove the hot mill scale and cleaned (not shown) to remove any contaminants from the strip.

[0093] Figure 2 : Amount of Cr-oxide as a function of current density in RCE experiments and industrial trials.

[0094] Figure 3 : Schematic diagram of a packaging steel that can be produced using a CrOx top layer deposited according to the invention:

[0095] a: Black steel plate

[0096] b.

[0097] Figure 4 : Effect of Cr(III) concentration on Cr metal deposition in metallic coatings on steel substrates. At a coating temperature of 55°C and a formate / Cr ratio of 1.5 3+ Doubling the Cr(III) concentration from 20 to 40 g / l in terms of molar ratio did not affect the onset of Cr deposition.

[0098] Figure 5 : At 2.0 formate / Cr 3+ Effect of Cr(III) concentration on Cr metal deposition in metallic coatings on steel substrates at molar ratios The onset of Cr deposition is not affected and the plating window increases with Cr concentration.

[0099] Figure 6 : The effect of reducing the plating temperature is that the efficiency of the plating process increases. Plating occurs at a lower current density.

[0100] Figure 7 : The effect of lowering the plating temperature is that the efficiency of the plating process increases. Plating occurs at lower current densities. The robustness is slightly higher for higher plating temperatures.

Claims

1. A method for electrolytically depositing a chromium oxide layer onto black steel sheets or onto black steel sheets coated with an electrodeposited chromium coating produced on the basis of trivalent chromium technology from an aqueous electrolyte solution containing a trivalent chromium compound provided by a water-soluble trivalent chromium salt, in a continuous high-speed plating line operating at a line speed of at least 50 m / min, wherein the steel substrate serves as cathode and wherein the anode comprises i) iridium oxide or ii) a catalytic coating of a mixed metal oxide comprising iridium oxide and tantalum oxide, for reducing or eliminating Cr 3+ Ion oxidation to Cr 6+ ions, and wherein the aqueous electrolyte solution contains at least 50 mM and at most 1000 mM Cr 3+ ions, a total of 25-2800 mM sodium sulfate or potassium sulfate, a pH measured at 25°C between 2.50 and 3.6, and wherein the plating temperature is between 40 and 70°C and wherein no other compounds are added to the aqueous electrolyte solution, except optionally sulfuric acid or sodium or potassium hydroxide to adjust the pH to the desired value.

2. The process according to claim 1, wherein the pH is adjusted to a value of 2.55-3.

6.

3. The process according to claim 1, wherein the pH is adjusted to a value of 2.55-3.

25.

4. The method according to claim 1 or 2, wherein the plating time, i.e. the duration of applying the current to the cathode, is at most 1000 ms.

5. The method according to claim 1, wherein the water-soluble trivalent chromium salt is basic chromium sulfate.

6. The method according to claim 1 or 2, wherein the amount of chromium deposited as chromium oxide is at least 5 mg / m 2 .

7. The method according to claim 1 or 2, wherein the amount of chromium deposited as chromium oxide is at least 6 mg / m 2 .

8. The method according to claim 1 or 2, wherein the amount of chromium deposited as chromium oxide is at least 7 mg / m 2 .

9. The method according to claim 1 or 2, wherein the amount of chromium deposited as chromium oxide is at least 8 mg / m 2 .

10. The method according to claim 1 or 2, wherein the aqueous electrolyte solution contains up to 10 mM of sodium formate as an inevitable impurity in the electrolyte.

11. The method according to claim 1 or 2, wherein the aqueous electrolyte solution contains at least 210 mM and at most 845 mM sodium sulfate.

12. The method of claim 1 or 2, wherein the plating temperature is at least 50°C.

13. The method of claim 1 or 2, wherein the plating temperature is at least 55°C.

14. The method of claim 1 or 2, wherein the line speed of the plating line is at least 100 m / min.

15. The method according to claim 1 or 2, wherein coated with an electrodeposited chromium coating produced on the basis of trivalent chromium technology means that the steel substrate comprises on one or both sides a metallic coating layer comprising chromium metal and chromium oxide and optionally also one or more of chromium carbide and chromium sulfate, and wherein the metallic coating layer is deposited from an aqueous electrolyte solution comprising a trivalent chromium compound, wherein the aqueous electrolyte solution used for depositing the metallic coating layer is free of chloride ions and boric acid buffer, the steel substrate acts as cathode and the anode comprises a catalytic coating of iridium oxide or mixed metal oxides for reducing or eliminating Cr 3+ Ion oxidation to Cr 6+ ions, wherein the aqueous electrolyte solution contains at least 50 mM and at most 1000 mM Cr 3+ ions, formate, and 25 to 2800 mM sodium sulfate (Na2SO4), and wherein formate / Cr 3+ The molar ratio is at least 1 :1 and at most 2.5:1, the pH measured at 25°C is between 1.5 and 3.6, and wherein the plating temperature is between 30 and 70°C.

16. The method according to claim 1 or 2, wherein the steel substrate is further coated on one or both sides with an organic coating consisting of a thermoplastic monolayer or thermoplastic multilayer polymer by a film lamination step or a direct extrusion step.

17. The method of claim 16, wherein the thermoplastic polymer coating is a polymer coating system comprising one or more layers comprising a thermoplastic resin.

18. The method according to claim 17, wherein the thermoplastic resin is selected from polyester or polyolefin, acrylic resin, polyamide, polyvinyl chloride, fluorocarbon resin, polycarbonate, styrene type resin, ABS resin, chlorinated polyether, ionomer, urethane resin, and / or copolymers thereof, and / or blends thereof.

19. The method according to claim 17 or 18, wherein the thermoplastic polymer coating on one or both sides of the coated black steel sheet is a multi-layer coating system, the coating system comprising at least an adhesive layer for adhering to the coated black steel sheet, a surface layer and a bulk layer between the adhesive layer and the surface layer, wherein the layers of the multi-layer coating system comprise or consist of polyester.

20. The method according to claim 19, wherein the polyester is selected from polyethylene terephthalate, isophthalic acid-modified polyethylene terephthalate, cyclohexanedimethanol-modified polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, or copolymers or blends thereof.

21. A coated metal substrate obtainable by a process according to any one of claims 1 to 20.

22. Use of a coated metal substrate according to claim 21 in a process for producing containers for packaging purposes.