Polycarbonate resin, method for producing the same, and optical lens

By optimizing the structural unit composition and melt polycondensation process of polycarbonate resin, the problem of high refractive index, low Abbe number and moisture and heat resistance in the existing technology is solved, and a high-performance polycarbonate resin is achieved, which is suitable for modern applications. Electronic equipment and optical lenses.

CN113603878BActive Publication Date: 2024-10-29MITSUBISHI GAS CHEM CO INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202110966461.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2017-07-19
Publication Date
2024-10-29
Estimated Expiration
2037-07-19

AI Technical Summary

Technical Problem

It is difficult for existing polycarbonate resins to achieve high refractive index, low Abbe number and high moisture and heat resistance at the same time, and the optical properties decline after PCT testing, making it unable to meet the water resistance and heat resistance requirements of modern electronic equipment.

Method used

Polycarbonate resin composed of specific structural units, including structural units of general formula (1), general formula (2) and general formula (3), is manufactured through a melt polycondensation process to optimize the molar ratio and polymerization structure of the resin to improve refraction efficiency and heat and humidity resistance.

Benefits of technology

It achieves high refractive index, low Abbe number and high moisture and heat resistance. The resin's total light transmittance remains above 60% after PCT testing, making it suitable for high-performance optical lenses and other optical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113603878B_ABST
    Figure CN113603878B_ABST
Patent Text Reader

Abstract

The present invention provides a polycarbonate resin having a high refractive index, a low Abbe number and high resistance to moisture and heat. The above-mentioned problems can be solved by a polycarbonate resin containing a structural unit represented by the following general formula (1) in one embodiment. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the patent application with the same name with application number 201780044148.7 filed on July 19, 2017. Technical Field

[0002] The present invention relates to a polycarbonate resin and a method for producing the same. The present invention also relates to an optical lens containing the polycarbonate resin. Background Art

[0003] Optical glass or optical resin is used as the material of optical lenses used in the optical systems of various cameras such as cameras, film-integrated cameras, and video cameras. Although optical glass has excellent heat resistance, transparency, dimensional stability, and chemical resistance, it has the problems of high material cost, poor molding processability, and low production efficiency.

[0004] On the other hand, optical lenses made of optical resins have the advantage of being able to be mass-produced by injection molding. For example, polycarbonate resins are used in camera lenses. However, in recent years, due to the trend toward thinner and lighter products, it is necessary to develop resins with high refractive indexes. Generally speaking, when the refractive index of an optical material is high, a surface with a smaller curvature can be used to realize a lens element with the same refractive index, thereby reducing the amount of aberration generated on the surface. As a result, it is possible to reduce the number of lenses, reduce the sensitivity of the lens to decentering, or reduce the thickness of the lens to achieve lightweighting.

[0005] In addition, in general, in the optical system of a camera, aberration correction is performed by combining multiple concave lenses and convex lenses. That is, for the chromatic aberration caused by the convex lens, a concave lens having a chromatic aberration with a sign opposite to that of the convex lens is combined to cancel the chromatic aberration in a synthetic manner. In this case, the concave lens needs to have a high dispersion (i.e., a low Abbe number).

[0006] Therefore, resins with high refractive index and low Abbe number for optical lenses have been developed. For example, Patent Document 1 discloses that the refractive index of a copolymer of a bisphenol A type polycarbonate structural unit and a structural unit represented by the following formula (E) is improved. In the examples of Patent Document 1, it is recorded that the refractive index reaches 1.62 to 1.64 and the Abbe number reaches 23 to 26. The improvement in the refractive index can be considered to be caused by the structural unit represented by formula (E).

[0007]

[0008] Patent Document 2 discloses a copolymer of a polycarbonate resin containing a structural unit having a fluorene structure and bisphenol A. The examples in this document describe that the refractive index reaches 1.616 to 1.636. However, the structural unit disclosed in this document is different from that of formula (E).

[0009] As described above, a polycarbonate resin and an optical lens having a high refractive index and a low Abbe number have not yet been provided.

[0010] Moreover, in recent years, various electronic devices require water resistance and heat resistance. As an environmental test for evaluating the water resistance and heat resistance of such electronic devices, the "PCT test" (pressure cooker test) is implemented. This test is a moisture and heat resistance test, which accelerates the intrusion of moisture into the inside of the sample in time for evaluation. Therefore, the optical lens composed of optical resin used in electronic devices not only needs to have a high refractive index and a low Abbe number, but also needs to be able to maintain optical properties after the PCT test.

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: International Publication No. 2007 / 142149

[0014] Patent Document 2: Japanese Patent Application Laid-Open No. 6-25398 Summary of the invention

[0015] Problems to be solved by the invention

[0016] The problem to be solved by the present invention is to provide a polycarbonate resin having a high refractive index, a low Abbe number and high resistance to moisture and heat. Another object of the present invention is to provide an excellent optical lens by using the resin.

[0017] Methods for solving problems

[0018] The inventors of the present invention have conducted intensive studies to solve the above-mentioned problems and, as a result, have found that the above-mentioned problems can be solved by the following polycarbonate resin and optical lens, thereby completing the present invention.

[0019] The present invention is described as follows, for example.

[0020] [1] A polycarbonate resin comprising a structural unit represented by the following general formula (1).

[0021]

[0022] (In the general formula (1), X represents an alkylene group having 1 to 4 carbon atoms, and a and b each independently represent an integer of 1 to 10.)

[0023] [2] The polycarbonate resin according to [1], wherein

[0024] It also contains structural units represented by the following general formula (2) and / or the following general formula (3).

[0025]

[0026] (In the general formula (2), Y represents an alkylene group having 1 to 4 carbon atoms, and c and d each independently represent an integer of 1 to 10.)

[0027]

[0028] (In general formula (3),

[0029] Z represents an alkylene group having 1 to 4 carbon atoms,

[0030] R1 to R6 each independently represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a cycloalkyl group having 5 to 20 carbon atoms, a cycloalkoxy group having 5 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aryloxy group having 6 to 20 carbon atoms,

[0031] e and f each independently represent an integer of 0 to 5.)

[0032] [3] The polycarbonate resin according to [2], comprising structural units represented by general formulas (1) to (3), wherein:

[0033] The ratio of the structural unit represented by the general formula (1) is 10 to 80 mol%.

[0034] The ratio of the structural unit represented by the general formula (2) is 10 to 60 mol%.

[0035] The ratio of the structural unit represented by the general formula (3) is 5 to 80 mol%.

[0036] [4] The polycarbonate resin according to [2], comprising structural units represented by general formulas (1) to (3), wherein:

[0037] The ratio of the structural unit represented by the general formula (1) is 20 to 80 mol%.

[0038] The ratio of the structural unit represented by the general formula (2) is 10 to 60 mol%.

[0039] The ratio of the structural unit represented by the general formula (3) is 5 to 70 mol%.

[0040] [5] The polycarbonate resin according to [2], comprising structural units represented by the general formulae (1) and (2), wherein:

[0041] The ratio of the structural unit represented by the general formula (1) is 10 to 80 mol%.

[0042] The proportion of the structural unit represented by the general formula (2) is 20 to 90 mol%.

[0043] [6] The polycarbonate resin according to [2], comprising structural units represented by the general formulae (1) and (2), wherein:

[0044] The ratio of the structural unit represented by the general formula (1) is 30 to 60 mol%.

[0045] The ratio of the structural unit represented by the general formula (2) is 40 to 70 mol%.

[0046] [7] An optical lens comprising the polycarbonate resin according to any one of [1] to [6].

[0047] [8] A method for producing a polycarbonate resin according to any one of [1] to [6], comprising the step of melt-polycondensing a dihydroxy compound including a dihydroxy compound represented by the following general formula (4) with a carbonic acid diester.

[0048]

[0049] (In the general formula (4), X represents an alkylene group having 1 to 4 carbon atoms, and a and b each independently represent an integer of 1 to 10.)

[0050] Effects of the Invention

[0051] The polycarbonate resin of the present invention exhibits a high refractive index, a low Abbe number, and high resistance to moisture and heat. In addition, by using the resin, an excellent optical lens can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 is the H of the resin obtained in Example 1 1 -NMR spectrum.

[0053] Figure 2 is the H of the resin obtained in Example 2 1 -NMR spectrum.

[0054] Figure 3 is the H of the resin obtained in Example 14 1 -NMR spectrum. DETAILED DESCRIPTION

[0055] Hereinafter, the present invention will be described in detail.

[0056] (1) Polycarbonate resin

[0057] The polycarbonate resin of the present invention is a polycarbonate resin having a structural unit represented by the general formula (1) (hereinafter also referred to as “structural unit (1)”).

[0058]

[0059] (In the general formula (1), X represents an alkylene group having 1 to 4 carbon atoms, and a and b each independently represent an integer of 1 to 10.)

[0060] The polycarbonate resin of the present invention may contain one or more other structural units in addition to the structural unit (1). As the other structural unit, a fluorene derivative unit and / or a binaphthol derivative unit are preferred.

[0061] Specifically, the polycarbonate resin of the present invention preferably further contains a binaphthol derivative unit represented by the following general formula (2) and / or a fluorene derivative unit represented by the following general formula (3).

[0062]

[0063] (In the general formula (2), Y represents an alkylene group having 1 to 4 carbon atoms, and c and d each independently represent an integer of 1 to 10.)

[0064]

[0065] (In general formula (3),

[0066] Z represents an alkylene group having 1 to 4 carbon atoms,

[0067] R1 to R6 each independently represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a cycloalkyl group having 5 to 20 carbon atoms, a cycloalkoxy group having 5 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aryloxy group having 6 to 20 carbon atoms,

[0068] e and f each independently represent an integer of 0 to 5.)

[0069] The polycarbonate resin of the present invention preferably contains structural units represented by general formulae (1) to (3), and more preferably consists essentially of structural units represented by general formulae (1) to (3). In the present specification, "consisting essentially of" means that the polycarbonate resin of the present invention may contain other structural units within a range that does not impair the effects of the invention. For example, among the structural units of the polycarbonate resin of the present invention, preferably 90% or more, more preferably 95% or more, and further preferably 98% or more are composed of structural units represented by general formulae (1) to (3). When the polycarbonate resin of the present invention contains structural units represented by general formulae (1) to (3), preferably the proportion of the structural units represented by general formula (1) is 10 to 80 mol%, the proportion of the structural units represented by general formula (2) is 10 to 60 mol%, and the proportion of the structural units represented by general formula (3) is 5 to 80 mol%. In addition, from the viewpoint of obtaining a high refractive index, it is more preferred that the proportion of the structural unit represented by the general formula (1) is 20 to 80 mol%, the proportion of the structural unit represented by the general formula (2) is 10 to 60 mol%, and the proportion of the structural unit represented by the general formula (3) is 5 to 70 mol%. The polycarbonate resin of the present invention having a composition having a more preferred proportion has a very high refractive index of 1.670 or more, which has not been achieved so far.

[0070] The polycarbonate resin of the present invention preferably contains structural units represented by general formulae (1) and (2), and more preferably consists essentially of structural units represented by general formulae (1) and (2). For example, of the structural units of the polycarbonate resin of the present invention, preferably 90% or more, more preferably 95% or more, and even more preferably 98% or more are composed of structural units represented by general formulae (1) and (2). When the polycarbonate resin of the present invention contains structural units represented by general formulae (1) and (2), preferably the proportion of the structural units represented by general formula (1) is 10 to 80 mol%, and the proportion of the structural units represented by general formula (2) is 20 to 90 mol%. By setting such a proportion, a polycarbonate resin having a very high refractive index of 1.670 or more, which has not been achieved so far, can be obtained. In addition, from the viewpoint of being able to obtain better moldability, it is more preferable that the proportion of the structural units represented by general formula (1) is 30 to 60 mol%, and the proportion of the structural units represented by general formula (2) is 40 to 70 mol%.

[0071] When the polycarbonate resin of the present invention contains structural units represented by general formulae (1) to (3), or contains structural units represented by general formulae (1) and (2), there is no particular limitation on the form in which these structural units are contained in the resin. In one embodiment of the present invention, the polycarbonate resin may contain a copolymer containing structural units represented by general formulae (1) to (3) or structural units represented by general formulae (1) and (2), or may be a ternary resin or a binary resin containing a homopolymer composed of each structural unit. Alternatively, it may be a blend obtained by blending a copolymer containing structural units represented by general formulae (1) and (2) with a homopolymer containing structural units represented by general formulae (3), or a blend obtained by blending a copolymer containing structural units represented by general formulae (1) and (2) with a copolymer containing structural units represented by general formulae (1) and (3).

[0072] The polycarbonate resin of the present invention may include any of random, block, and alternating copolymer structures.

[0073] The polycarbonate resin of the present invention preferably has a polystyrene-equivalent weight average molecular weight (Mw) of 20,000 to 200,000.

[0074] The polystyrene-equivalent weight average molecular weight (Mw) is more preferably 25,000 to 120,000, further preferably 28,000 to 55,000, particularly preferably 30,000 to 45,000.

[0075] When Mw is less than 20,000, the molded product becomes brittle and is not preferred. When Mw is greater than 200,000, the melt viscosity increases, making it difficult to take out the resin after production, and the fluidity deteriorates, making it difficult to perform injection molding in a molten state, which is not preferred.

[0076] The refractive index (nD) of the polycarbonate resin of the present invention at 23°C and a wavelength of 589 nm is preferably 1.635 to 1.695, more preferably 1.640 to 1.690, further preferably 1.645 to 1.685, and particularly preferably 1.670 to 1.685. The polycarbonate resin of the present invention has a high refractive index (nD) and is suitable for optical lens materials. The refractive index can be measured using an Abbe refractometer according to the method of JIS-K-7142 for a film having a thickness of 0.1 mm.

[0077] The Abbe number (ν) of the polycarbonate resin of the present invention is preferably 24 or less, more preferably 22 or less, and further preferably 20 or less. The Abbe number can be calculated from the refractive index at wavelengths of 486 nm, 589 nm, and 656 nm at 23° C. using the following formula.

[0078] ν=(nD-1) / (nF-nC)

[0079] nD: refractive index at a wavelength of 589nm

[0080] nC: refractive index at a wavelength of 656nm

[0081] nF: refractive index at a wavelength of 486nm

[0082] The polycarbonate resin of the present invention may be blended with other resins for the production of a molded article. Examples of other resins include polyamide, polyacetal, polycarbonate, modified polyphenylene ether, polyethylene terephthalate, and polybutylene terephthalate.

[0083] The polycarbonate resin of the present invention may further include an antioxidant, a mold release agent, an ultraviolet absorber, a fluidity improver, a crystal nucleating agent, a reinforcing agent, a dye, an antistatic agent, or an antibacterial agent.

[0084] Examples of the molding method include, in addition to injection molding, compression molding, cast molding, roll processing, extrusion molding, stretching, and the like, but the method is not limited thereto.

[0085] When the polycarbonate resin of the present invention is used for injection molding, the glass transition temperature (Tg) is preferably 90 to 180°C, more preferably 95 to 175°C, further preferably 100 to 170°C, further preferably 130 to 170°C, and particularly preferably 135 to 150°C. When Tg is lower than 90°C, it is not preferred because the use temperature range becomes narrow. When it exceeds 180°C, the melting temperature of the resin increases, and the resin is easily decomposed or colored, which is not preferred. When the glass transition temperature of the resin is too high, the difference between the mold temperature and the glass transition temperature of the resin increases when a general mold temperature controller is used. Therefore, in applications where precise surface accuracy is required for products, it is difficult to use a resin with a too high glass transition temperature, so it is not preferred. In addition, from the viewpoint of molding fluidity and molding heat resistance, the lower limit of Tg is preferably 130°C, more preferably 135°C, and the upper limit of Tg is preferably 160°C, more preferably 150°C.

[0086] The total light transmittance of the optical molded body obtained by using the polycarbonate resin of the present invention is preferably 85% or more, more preferably 88% or more. When the total light transmittance is 85% or more, it is comparable to bisphenol A type polycarbonate resin and the like.

[0087] The polycarbonate resin of the present invention has high resistance to moisture and heat. Resistance to moisture and heat can be evaluated by performing a "PCT test" (pressure cooker test) on an optical molded body obtained using the polycarbonate resin and measuring the total light transmittance of the optical molded body after the test. The PCT test can be performed by keeping an injection molded body with a diameter of 50 mm and a thickness of 3 mm under the conditions of 120°C, 0.2 MPa, and 100% RH for 20 hours. The total light transmittance of the polycarbonate resin of the present invention after the PCT test is above 60%, preferably above 70%, more preferably above 75%, further preferably above 80%, and particularly preferably above 85%. When the total light transmittance is above 60%, it can be said that it has high resistance to moisture and heat relative to existing polycarbonate resins.

[0088] The b value of the polycarbonate resin of the present invention is preferably not more than 5. A smaller b value indicates less yellowing and better hue.

[0089] The amount of residual phenol contained in the polycarbonate resin of the present invention is preferably 500 ppm or less, more preferably 300 ppm or less, and further preferably 50 ppm or less.

[0090] The amount of residual diphenyl carbonate (DPC) contained in the polycarbonate resin of the present invention is preferably 200 ppm or less, more preferably 100 ppm or less, and further preferably 50 ppm or less.

[0091] (Vene terminal group amount)

[0092] As described later, the polycarbonate resin of the present invention is a resin obtained by using a compound represented by the following general formula (4) as a dihydroxy component and reacting it with a carbonate precursor such as a carbonic acid diester.

[0093]

[0094] (In the general formula (4), X represents an alkylene group having 1 to 4 carbon atoms, and a and b each independently represent an integer of 1 to 10.)

[0095] However, when manufacturing the resin, there are cases where a polymer having a terminal structure represented by the following formula (A) and a compound represented by the following formula (B) are produced as by-products from the compound represented by the above-mentioned general formula (4) and are included in the polycarbonate resin of the present invention; and / or a polymer having a terminal structure represented by the following formula (A) is formed after the terminal of the polymer represented by the formula (1) is obtained and modified to a vinyl group.

[0096]

[0097] [In formulas (A) and (B),

[0098] X represents an alkylene group having 1 to 4 carbon atoms,

[0099] a and b each independently represent an integer of 1 to 10,

[0100] Hm are hydrogen atoms,

[0101] * is the polymer chain. ]

[0102] According to a preferred embodiment of the present invention, regarding the total content of the polymer having the terminal structure represented by the general formula (A) and the compound represented by the general formula (B) contained in the polycarbonate resin, when measuring the H of the polycarbonate resin, 1 In the case of -NMR spectrum, the amount satisfying the following relationship (ie, "the amount of fluorene-based vinyl terminal groups 1") is preferred.

[0103]

[0104] The fluorene vinyl terminal group content 1 calculated by formula (I) is more preferably 0.001 to 0.8, particularly preferably 0.01 to 0.5. When the fluorene vinyl terminal group content 1 calculated by formula (I) is within the above range, the polycarbonate resin is preferred because of excellent fluidity and strength, such as flexural strength and tensile strength.

[0105] Formula (I) corresponds to the following formula.

[0106]

[0107] In the above formula, "Ha in the repeating unit of the compound of formula (4)" refers to all hydrogen atoms contained in X of formula (4). For example, when X is ethylene, the position of Ha is as follows. In the case where the compound represented by general formula (5) and / or (6) is further used as a dihydroxy component, the integral value of "Hb in the repeating unit of the compound of formula (5)" and "Hc in the repeating unit of the compound of formula (6)" is added to the denominator of the above formula, which will be described later.

[0108]

[0109] Here, "proton peak integral value" and "peak integral value" are the values ​​of the proton peak measured by NMR (nuclear magnetic resonance) spectroscopy. 1 The NMR spectrum of H 1 H-NMR spectrum) is the area value of the signal of the NMR spectrum, that is, the integral value. Generally speaking, NMR spectroscopy is a measurement method that focuses on the atomic nuclei of substances and can quantitatively measure the atomic nuclei themselves that constitute each molecule. That is, 1 In the case of H-NMR, the integral value of the observed signal represents the 1 The existence ratio of H. In the present invention, by1 Estimation of chemical shift values ​​from H-NMR spectra 1 The attribution of H was obtained for each chemical shift value. 1 The integrated value of the H signal.

[0110] The polycarbonate resin of the present invention is preferably a resin obtained by using, in addition to the compound represented by the above general formula (4), a compound represented by the following general formula (5) and / or (6) as a dihydroxy component and reacting it with a carbonate precursor such as a carbonic acid diester.

[0111]

[0112] (In the general formula (5), Y represents an alkylene group having 1 to 4 carbon atoms, and c and d each independently represent an integer of 1 to 10.)

[0113]

[0114] (In general formula (6),

[0115] Z represents an alkylene group having 1 to 4 carbon atoms,

[0116] R1 to R6 each independently represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a cycloalkyl group having 5 to 20 carbon atoms, a cycloalkoxy group having 5 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aryloxy group having 6 to 20 carbon atoms, and e and f each independently represent an integer of 0 to 5.)

[0117] However, when such a resin is produced, there is a case where a polymer having a terminal structure represented by the following formula (C) and / or (E) and a compound represented by the following formula (D) and / or (F) are produced as by-products from the compound represented by the above-mentioned general formula (5) and / or (6) and are contained in the polycarbonate resin of the present invention, and / or the terminal of the obtained polymer is modified to a vinyl group to form a polymer having a terminal structure represented by the following formula (C) and / or (E).

[0118]

[0119] [In formulas (C) to (F),

[0120] Y and Z each independently represent an alkylene group having 1 to 4 carbon atoms,

[0121] R1 to R6 each independently represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a cycloalkyl group having 5 to 20 carbon atoms, a cycloalkoxy group having 5 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aryloxy group having 6 to 20 carbon atoms,

[0122] c and d each independently represent an integer of 1 to 10,

[0123] e represents an integer from 1 to 5,

[0124] f represents an integer from 0 to 5, and f-1 is greater than 0,

[0125] Hn and Hо are hydrogen atoms respectively;

[0126] * is the polymer chain. ]

[0127] According to a preferred embodiment of the present invention, regarding the total content of the polymer having a terminal structure represented by the general formula (C) and the compound represented by the general formula (D) contained in the polycarbonate resin, when measuring the H of the polycarbonate resin, 1 In the case of -NMR spectrum, the amount satisfying the following relationship (ie, "the amount of binaphthol-based vinyl terminal groups") is preferred.

[0128]

[0129] The amount of binaphthol-based vinyl terminal groups calculated by formula (II) is more preferably 0.05 to 0.8, particularly preferably 0.1 to 0.6. When the amount of binaphthol-based vinyl terminal groups calculated by formula (II) is within the above range, the polycarbonate resin is preferred because of excellent fluidity and strength.

[0130] Formula (II) corresponds to the following formula.

[0131]

[0132] In the above formula, "Hb in the repeating unit of the compound of formula (5)" and "Hc in the repeating unit of the compound of formula (6)" refer to all hydrogen atoms contained in Y and Z of formulas (5) and (6), respectively. For example, when Y and Z are ethylene, the positions of Hb and Hc are as follows.

[0133]

[0134] According to a preferred embodiment of the present invention, regarding the total content of the polymer having a terminal structure represented by the general formula (E) and the compound represented by the general formula (F) contained in the polycarbonate resin, when measuring the H of the polycarbonate resin, 1 In the case of -NMR spectrum, the amount that satisfies any of the following relationships (ie, "the amount of fluorene-based vinyl terminal groups 2" and "the amount of fluorene-based vinyl terminal groups 3").

[0135]

[0136]

[0137] Here, when R1 to R4 in formula (5′), (E) and (F) are not aromatic groups with 6 to 20 carbon atoms or aromatic oxy groups with 6 to 20 carbon atoms, the above mathematical formula (III) applies; when at least one of R1 to R4 in formula (5′), (E) and (F) is an aromatic group with 6 to 20 carbon atoms or an aromatic oxy group with 6 to 20 carbon atoms, the above mathematical formula (IV) applies.

[0138] The fluorene vinyl terminal group amount 2 calculated by formula (III) is more preferably 0.001 to 0.8, particularly preferably 0.01 to 0.5. When the fluorene vinyl terminal group amount 2 calculated by formula (III) is within the above range, the polycarbonate resin is preferred because of excellent fluidity and strength.

[0139] The fluorene vinyl terminal group content 3 calculated by formula (IV) is more preferably 0.001 to 0.8, particularly preferably 0.01 to 0.5. When the fluorene vinyl terminal group content 3 calculated by formula (IV) is within the above range, the polycarbonate resin is preferred because of excellent fluidity and strength.

[0140] Formulae (III) and (IV) correspond to the following formulae.

[0141]

[0142] (2) Method for producing polycarbonate resin

[0143] The polycarbonate resin having the structural unit represented by the general formula (1) of the present invention can be produced by using a compound represented by the following general formula (4) as a dihydroxy component and reacting it with a carbonate precursor such as a carbonic acid diester.

[0144]

[0145] (In the general formula (4), X represents an alkylene group having 1 to 4 carbon atoms, and a and b each independently represent an integer of 1 to 10.)

[0146] Specifically, it can be produced by reacting a compound represented by the general formula (4) and a carbonate precursor such as a carbonic acid diester by a melt polycondensation method in the presence of a basic compound catalyst, an ester exchange catalyst or a mixed catalyst consisting of both, or in the absence of a catalyst.

[0147] Examples of the compound of the general formula (4) include 9,9-bis(hydroxy(poly)alkoxynaphthyl)fluorenes. For example, examples of the compound of the general formula (4) include 9,9-bis[6-(1-hydroxymethoxy)naphth-2-yl]fluorene, 9,9-bis[6-(2-hydroxyethoxy)naphth-2-yl]fluorene, 9,9-bis[6-(3-hydroxypropoxy)naphth-2-yl]fluorene, and 9,9-bis[6-(4-hydroxybutoxy)naphth-2-yl]fluorene. Among them, 9,9-bis[6-(2-hydroxyethoxy)naphth-2-yl]fluorene is preferred. These may be used alone or in combination of two or more.

[0148] When manufacturing the compound of the general formula (4), as an impurity, a compound in which either a or b is 0 is sometimes produced as a by-product as an impurity. Regarding the content of such impurities, in the monomer with the compound of the general formula (4) as the main component, the total amount is preferably less than 1000 ppm, more preferably less than 500 ppm, further preferably less than 200 ppm, and particularly preferably less than 100 ppm. In addition to such impurities, fluorenone, which is one of the raw materials, is sometimes contained as an impurity. Regarding the content of fluorenone, in the monomer with the compound of the general formula (4) as the main component, it is preferably less than 1000 ppm, more preferably less than 100 ppm, further preferably less than 50 ppm, and particularly preferably less than 10 ppm. The fluorenone contained in the monomer with the compound of the general formula (4) as the main component sometimes remains in the resin after polymerization. The lower the content of fluorenone, the better the hue of the resin, so it is preferred. Furthermore, although the compounds in which a and b in the general formula (4) are different (i.e., a≠b) are not impurities, their total content in the monomer containing the compound of the general formula (4) as the main component is preferably 50 ppm or less, more preferably 20 ppm or less.

[0149] The compound of the general formula (4) can be produced by various synthesis methods. For example, it can be produced by the following method: as described in Japanese Patent No. 5442800, 9,9-bis(hydroxynaphthyl)fluorene is obtained by (a) reacting fluorenones with hydroxynaphthalenes in the presence of hydrogen chloride gas and mercaptocarboxylic acid, (b) reacting 9-fluorenone with hydroxynaphthalenes in the presence of an acid catalyst (and alkyl mercaptan), (c) reacting fluorenones with hydroxynaphthalenes in the presence of hydrochloric acid and mercaptans (such as mercaptocarboxylic acid), (d) reacting fluorenones with hydroxynaphthalenes in the presence of sulfuric acid and mercaptans (such as mercaptocarboxylic acid) and precipitating crystals using a crystallization solvent composed of hydrocarbons and polar solvents to produce binaphthol fluorene. For example, 9,9-bis[6-(2-hydroxyethoxy)naphthyl]fluorene can be obtained by reacting 9,9-bis[6-hydroxynaphthyl]fluorene with 2-chloroethanol under alkaline conditions.

[0150] In the polycarbonate resin having the structural unit represented by the general formula (1) of the present invention, an aromatic dihydroxy compound or an aliphatic dihydroxy compound (for example, a dihydroxy compound having a fluorene skeleton or binaphthols) may be used in combination as a dihydroxy component in addition to the compound represented by the general formula (4).

[0151] The polycarbonate resin of the present invention is preferably produced using, in addition to the compound represented by the above general formula (4), a compound represented by the following general formula (5) and / or a compound represented by the following general formula (6) as a dihydroxy component.

[0152]

[0153] (In the general formula (5), Y represents an alkylene group having 1 to 4 carbon atoms, and c and d each independently represent an integer of 1 to 10.)

[0154]

[0155] (In general formula (6),

[0156] Z represents an alkylene group having 1 to 4 carbon atoms,

[0157] R1 to R6 each independently represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, a cycloalkyl group having 5 to 20 carbon atoms, a cycloalkoxy group having 5 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aryloxy group having 6 to 20 carbon atoms,

[0158] e and f each independently represent an integer of 0 to 5.)

[0159] Examples of the dihydroxy compound represented by formula (5) include 2,2′-bis(1-hydroxymethoxy)-1,1′-binaphthyl, 2,2′-bis(2-hydroxyethoxy)-1,1′-binaphthyl, 2,2′-bis(3-hydroxypropoxy)-1,1′-binaphthyl, and 2,2′-bis(4-hydroxybutoxy)-1,1′-binaphthyl. Among them, 2,2′-bis(2-hydroxyethoxy)-1,1′-binaphthyl (hereinafter sometimes abbreviated as “BHEBN”) is preferred. These may be used alone or in combination of two or more.

[0160] When manufacturing the compound of the general formula (5), a compound in which either c or d is 0 is sometimes produced as a by-product as an impurity. The content of such impurities is preferably 1000 ppm or less in total in the monomer with the compound of the general formula (5) as the main component, more preferably 500 ppm or less, further preferably 200 ppm or less, and particularly preferably 100 ppm or less. In addition, although the compound in which c and d in the general formula (5) are different (i.e., c≠d) is not an impurity, it is preferably 50 ppm or less in total in the monomer with the compound of the general formula (5) as the main component, and more preferably 20 ppm or less.

[0161] Examples of the dihydroxy compound represented by the general formula (6) include 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-methylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-tert-butylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-isopropylphenyl]fluorene, 9,9-bis[4-(2-hydroxyethoxy)-3-cyclohexylphenyl]fluorene, and 9,9-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]fluorene (hereinafter sometimes abbreviated as "BPPEF"). Among them, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene and 9,9-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]fluorene are preferred. These may be used alone or in combination of two or more.

[0162] When producing the compound of the general formula (6), a compound in which either e or f is 0 is sometimes produced as a by-product as an impurity. The content of such impurities is preferably 1000 ppm or less in total in the monomer having the compound of the general formula (6) as the main component, more preferably 500 ppm or less, further preferably 200 ppm or less, and particularly preferably 100 ppm or less. In addition, although the compound in which e and f in the general formula (6) are different (i.e., e≠f) is not an impurity, it is preferably 50 ppm or less in total in the monomer having the compound of the general formula (6) as the main component, and more preferably 20 ppm or less.

[0163] Examples of aromatic dihydroxy compounds other than those mentioned above that can be used in combination include bisphenol A, bisphenol AP, bisphenol AF, bisphenol B, bisphenol BP, bisphenol C, bisphenol E, bisphenol F, bisphenol G, bisphenol M, bisphenol S, bisphenol P, bisphenol PH, bisphenol TMC, and bisphenol Z.

[0164] As the carbonic acid diester used in the present invention, diphenyl carbonate, ditolyl carbonate, bis(chlorophenyl) carbonate, m-cresyl carbonate, dimethyl carbonate, diethyl carbonate, dibutyl carbonate, dicyclohexyl carbonate, etc. can be cited. Among these, diphenyl carbonate is particularly preferred. The usage ratio of diphenyl carbonate is preferably 0.97 to 1.20 moles, more preferably 0.98 to 1.10 moles relative to 1 mole of the total of the dihydroxy compounds.

[0165] Among the transesterification catalysts, examples of the basic compound catalyst include alkali metal compounds, alkaline earth metal compounds, and nitrogen-containing compounds.

[0166] As the alkali metal compound used in the present invention, for example, organic acid salts, inorganic salts, oxides, hydroxides, hydrides or alkoxides of alkali metals can be mentioned. Specifically, sodium hydroxide, potassium hydroxide, cesium hydroxide, lithium hydroxide, sodium hydrogen carbonate, sodium carbonate, potassium carbonate, cesium carbonate, lithium carbonate, sodium acetate, potassium acetate, cesium acetate, lithium acetate, sodium stearate, potassium stearate, cesium stearate, lithium stearate, sodium borohydride, sodium phenylborate, sodium benzoate, potassium benzoate, cesium benzoate, lithium benzoate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, dilithium hydrogen phosphate, disodium phenylphosphate, disodium salt of bisphenol A, dipotassium salt of bisphenol A, dicesium salt of bisphenol A or dilithium salt of bisphenol A, sodium salt of phenol, potassium salt of phenol, cesium salt of phenol or lithium salt of phenol can be used.

[0167] As the alkaline earth metal compound, for example, organic acid salts, inorganic salts, oxides, hydroxides, hydrides or alkoxides of alkaline earth metal compounds can be mentioned. Specifically, magnesium hydroxide, calcium hydroxide, strontium hydroxide, barium hydroxide, magnesium hydrogen carbonate, calcium hydrogen carbonate, strontium hydrogen carbonate, barium hydrogen carbonate, magnesium carbonate, calcium carbonate, strontium carbonate, barium carbonate, magnesium acetate, calcium acetate, strontium acetate, barium acetate, magnesium stearate, calcium stearate, calcium benzoate, magnesium phenylphosphate and the like can be used.

[0168] Examples of nitrogen-containing compounds include quaternary ammonium hydroxides and salts thereof, amines, etc. Specifically, quaternary ammonium hydroxides having alkyl groups, aryl groups, etc., such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, trimethylbenzylammonium hydroxide, etc.; tertiary amines such as triethylamine, dimethylbenzylamine, triphenylamine, etc.; secondary amines such as diethylamine, dibutylamine, etc.; primary amines such as propylamine, butylamine, etc.; imidazoles such as 2-methylimidazole, 2-phenylimidazole, benzimidazole, etc.; or bases or basic salts such as ammonia, tetramethylammonium borohydride, tetrabutylammonium borohydride, tetrabutylammonium tetraphenylborate, tetraphenylammonium tetraphenylborate, etc. can be used.

[0169] As the transesterification catalyst, salts of zinc, tin, zirconium, lead or the like are preferably used, and these can be used alone or in combination.

[0170] Specific examples of the transesterification catalyst that can be used include zinc acetate, zinc benzoate, zinc 2-ethylhexanoate, tin (II) chloride, tin (IV) chloride, tin (II) acetate, tin (IV) acetate, dibutyltin dilaurate, dibutyltin oxide, dibutyldimethoxytin, zirconium acetylacetonate, zirconium oxyacetate, tetrabutoxyzirconium, lead (II) acetate, and lead (IV) acetate.

[0171] The ratio of these catalysts to 1 mol of the total dihydroxy compound is 1×10 -9 ~1×10 -3 mole, preferably 1×10 -7 ~1×10 -4 Moore.

[0172] The melt polycondensation method uses the above-mentioned raw materials and catalysts, and carries out melt polycondensation under heating and at normal pressure or reduced pressure while removing by-products by transesterification reaction.

[0173] The melt polycondensation of this composition system preferably melts the compound shown in the general formula (4) and the carbonic acid diester in a reaction vessel, and then reacts in a state where the monohydroxy compound as a by-product is retained. In order to retain it, the reaction device can be closed, or pressure control such as decompression or pressurization can be performed. The reaction time of this process is more than 20 minutes and less than 240 minutes, preferably more than 40 minutes and less than 180 minutes, and particularly preferably more than 60 minutes and less than 150 minutes. At this time, when the monohydroxy compound as a by-product is immediately distilled and removed after being generated, the content of high molecular weight in the polycarbonate resin finally obtained is small. However, when the monohydroxy compound as a by-product is retained in the reaction vessel for a certain period of time, the polycarbonate resin finally obtained can obtain a product with a high content of high molecular weight.

[0174] The melt polycondensation reaction can be carried out in a continuous manner or in a batch manner. The reaction unit used during the reaction can be a vertical reaction unit equipped with an anchor-type stirring paddle, a MAXBLEND stirring paddle, a ribbon-type stirring paddle, etc., or a horizontal reaction unit equipped with a paddle blade, a lattice blade, a glasses-type blade, etc., or an extruder-type reaction unit equipped with a screw. In addition, considering the viscosity of the polymer, it is preferred to use a reaction unit that appropriately combines these reaction units to implement.

[0175] In the method for producing the polycarbonate resin used in the present invention, after the polymerization reaction is completed, the catalyst may be removed or deactivated in order to maintain thermal stability and hydrolytic stability. It is preferred to implement a method of deactivating the catalyst by adding a known acidic substance. As the acidic substance, it is specifically preferred to use esters such as butyl benzoate; aromatic sulfonic acids such as p-toluenesulfonic acid; aromatic sulfonic acid esters such as butyl p-toluenesulfonate and hexyl p-toluenesulfonate; phosphoric acids such as phosphorous acid, phosphoric acid, and phosphonic acid; phosphites such as triphenyl phosphite, monophenyl phosphite, diphenyl phosphite, diethyl phosphite, di-n-propyl phosphite, di-n-butyl phosphite, di-n-hexyl phosphite, dioctyl phosphite, monooctyl phosphite; triphenyl phosphate, diphenyl phosphate, monophenyl phosphate Phosphates such as phosphate, dibutyl phosphate, dioctyl phosphate, monooctyl phosphate, etc.; phosphonic acids such as diphenylphosphonic acid, dioctylphosphonic acid, dibutylphosphonic acid, etc.; phosphonic acid esters such as diethyl phenylphosphonate; phosphines such as triphenylphosphine, bis(diphenylphosphino)ethane, etc.; boric acids such as boric acid, phenylboric acid, etc.; aromatic sulfonates such as tetrabutylphosphonium dodecylbenzenesulfonate; organic halides such as stearoyl chloride, benzoyl chloride, p-toluenesulfonyl chloride, etc.; alkylsulfuric acid such as dimethylsulfuric acid; organic halides such as benzyl chloride, etc. These deactivators are used in an amount of 0.01 to 50 times the amount of the catalyst, preferably 0.3 to 20 times the amount of the catalyst. When the amount is less than 0.01 times the amount of the catalyst, the deactivation effect is insufficient and it is not preferred. In addition, when the amount is more than 50 times the amount of the catalyst, the heat resistance of the resin is easily reduced and the molded body is easily colored, which is not preferred.

[0176] After the catalyst is deactivated, a step of devolatilizing and removing low-boiling point compounds in the polymer at a pressure of 0.1 to 1 mmHg and a temperature of 200 to 350° C. may be provided. In this step, a horizontal device equipped with a stirring blade having excellent surface renewal ability such as a paddle blade, a lattice blade, or a spectacled blade, or a thin film evaporator is preferably used.

[0177] The polycarbonate resin of the present invention preferably has as little foreign matter content as possible, and preferably implements filtration of the molten raw material, filtration of the catalyst liquid, etc. The mesh of the filter is preferably below 5 μm, more preferably below 1 μm. In addition, it is preferred to filter the generated resin using a polymer filter. The mesh of the polymer filter is preferably below 100 μm, more preferably below 30 μm. In addition, the process of selecting the resin pellets must of course be in a low-dust environment, preferably below Class 6, more preferably below Class 5.

[0178] In the case of producing a polycarbonate resin containing structural units represented by the general formulae (1) to (3) or a polycarbonate resin containing structural units represented by the general formulae (1) and (2) in another embodiment of the present invention, a copolymer containing structural units represented by the general formulae (1) to (3) or containing structural units represented by the general formulae (1) and (2) may be produced using compounds represented by the general formulae (4) to (6), or the compounds represented by the general formulae (4) to (6) may be polymerized separately to produce a ternary resin or a binary resin containing homopolymers composed of the respective structural units. Alternatively, a copolymer containing structural units represented by the general formulae (1) and (2) and a homopolymer containing structural units represented by the general formulae (3) may be polymerized and then blended, or a copolymer containing structural units represented by the general formulae (1) and (2) and a copolymer containing structural units represented by the general formulae (1) and (3) may be polymerized and then blended.

[0179] (3) Optical molding

[0180] The polycarbonate resin of the present invention can be used to manufacture optical molded bodies. For example, it can be molded by any method such as injection molding, compression molding, extrusion molding, solution casting, etc. The polycarbonate resin of the present invention has excellent moldability and heat resistance, and is therefore particularly suitable for optical lenses that require injection molding. During molding, the polycarbonate resin of the present invention can be mixed with other polycarbonate resins or other resins such as polyester resins. In addition, additives such as antioxidants, processing stabilizers, light stabilizers, polymer metal deactivators, flame retardants, lubricants, antistatic agents, surfactants, antibacterial agents, release agents, ultraviolet absorbers, plasticizers, and compatibilizers can also be mixed.

[0181] Examples of the antioxidant include triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl) propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, The antioxidant may be butyl-4-hydroxybenzyl)benzene, N,N-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamic acid amide), 3,5-di-tert-butyl-4-hydroxy-benzylphosphonate-diethyl ester, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, and 3,9-bis{1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl}-2,4,8,10-tetraoxaspiro(5,5)undecane. The content of the antioxidant in the polycarbonate resin is preferably 0.001 to 0.3 parts by weight relative to 100 parts by weight of the polycarbonate resin.

[0182] Examples of the processing stabilizer include phosphorus-based processing heat stabilizers, sulfur-based processing heat stabilizers, etc. Examples of the phosphorus-based processing heat stabilizer include phosphorous acid, phosphoric acid, phosphonous acid, phosphonic acid, and esters thereof. Specific examples thereof include triphenyl phosphite, tris(nonylpropyl) phosphite, tris(2,4-di-tert-butylphenyl) phosphite, tris(2,6-di-tert-butylphenyl) phosphite, tridecyl phosphite, trioctyl phosphite, trioctadecyl phosphite, didecyl monophenyl phosphite, dioctyl monophenyl phosphite, diisopropyl monophenyl phosphite, monobutyl diphenyl phosphite, monodecyl diphenyl phosphite, monooctyl diphenyl phosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, bis(nonylpropyl)pentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, Bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, distearylpentaerythritol diphosphite, tributyl phosphate, triethyl phosphate, trimethyl phosphate, triphenyl phosphate, diphenyl mono-o-biphenyl phosphate, dibutyl phosphate, dioctyl phosphate, diisopropyl phosphate, dimethyl phenylphosphonate, diethyl phenylphosphonate, dipropyl phenylphosphonate, tetrakis(2,4-di-tert-butylphenyl)-4,4′-biphenylene diphosphonate, tetrakis(2,4-di-tert-butylphenyl)-4,3′-biphenylene diphosphonate, tetrakis(2,4-di-tert-butylphenyl)-3,3′-biphenylene diphosphonate, bis(2,4-di-tert-butylphenyl)-4-phenyl-phenylphosphonate and bis(2,4-di-tert-butylphenyl)-3-phenyl-phenylphosphonate, etc. The content of the phosphorus-based processing heat stabilizer in the polycarbonate resin is preferably 0.001 to 0.2 parts by weight based on 100 parts by weight of the polycarbonate resin.

[0183] Examples of the sulfur-based processing heat stabilizer include pentaerythritol tetrakis (3-lauryl thiopropionate), pentaerythritol tetrakis (3-myristyl thiopropionate), pentaerythritol tetrakis (3-stearyl thiopropionate), dilauryl-3,3′-thiodipropionate, dimyristyl-3,3′-thiodipropionate, and distearyl-3,3′-thiodipropionate. The content of the sulfur-based processing heat stabilizer in the polycarbonate resin is preferably 0.001 to 0.2 parts by weight relative to 100 parts by weight of the polycarbonate resin.

[0184] As a release agent, it is preferred that 90% by weight or more of the release agent is composed of an ester of an alcohol and a fatty acid. As the ester of an alcohol and a fatty acid, specifically, there can be mentioned an ester of a monohydric alcohol and a fatty acid, and a partial ester or full ester of a polyhydric alcohol and a fatty acid. As the ester of the monohydric alcohol and a fatty acid, an ester of a monohydric alcohol having 1 to 20 carbon atoms and a saturated fatty acid having 10 to 30 carbon atoms is preferred. In addition, as a partial ester or full ester of a polyhydric alcohol and a fatty acid, a partial ester or full ester of a polyhydric alcohol having 1 to 25 carbon atoms and a saturated fatty acid having 10 to 30 carbon atoms is preferred.

[0185] Specifically, examples of the esters of monohydric alcohols and saturated fatty acids include stearyl stearate, palmityl palmitate, butyl stearate, methyl laurate, isopropyl palmitate, etc. Examples of partial or full esters of polyhydric alcohols and saturated fatty acids include stearic acid monoglyceride, stearic acid monoglyceride, stearic acid diglyceride, stearic acid triglyceride, stearic acid monosorbitol ester, behenic acid monoglyceride, capric acid monoglyceride, lauric acid monoglyceride, pentaerythritol monostearate, pentaerythritol tetrastearate, pentaerythritol tetrapelargonate, propylene glycol monostearate, biphenyl biphenol ester, sorbitol monostearate, 2-ethylhexyl stearate, full or partial esters of dipentaerythritol such as dipentaerythritol hexastearate, etc. The content of these release agents is preferably in the range of 0.005 to 2.0 parts by weight, more preferably 0.01 to 0.6 parts by weight, and still more preferably 0.02 to 0.5 parts by weight, based on 100 parts by weight of the polycarbonate resin.

[0186] As the ultraviolet absorber, at least one ultraviolet absorber selected from the group consisting of benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, triazine ultraviolet absorbers, cyclic iminoester ultraviolet absorbers, and cyanoacrylate ultraviolet absorbers is preferred. That is, any one of the ultraviolet absorbers listed below may be used alone, or two or more may be used in combination.

[0187] Examples of the benzotriazole ultraviolet absorber include 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-3,5-dicumylphenyl)phenylbenzotriazole, 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole, 2,2′-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2N-benzotriazol-2-yl)phenol], 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, and 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole. 2-(2-hydroxy-3,5-di-tert-amylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-4-octyloxyphenyl)benzotriazole, 2,2′-methylenebis(4-cumyl-6-benzotriazolephenyl), 2,2′-p-phenylenebis(1,3-benzoxazin-4-one), 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimidomethyl)-5-methylphenyl]benzotriazole, etc.

[0188] Examples of the benzophenone-based ultraviolet absorber include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone, 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone trihydrate, 2,2′-dihydroxy-4-methoxybenzophenone, 2,2′,4,4′-tetrahydroxybenzophenone, 2,2′-dihydroxy-4,4′-dimethoxybenzophenone, 2,2′-dihydroxy-4,4′-dimethoxy-5-sodium sulfonate benzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2-hydroxy-4-n-dodecyloxybenzophenone, and 2-hydroxy-4-methoxy-2′-carboxybenzophenone.

[0189] Examples of the triazine ultraviolet absorber include 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol and 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl)-5-[(octyl)oxy]-phenol.

[0190] Examples of the cyclic imidate-based ultraviolet absorber include 2,2′-bis(3,1-benzoxazin-4-one), 2,2′-p-phenylenebis(3,1-benzoxazin-4-one), 2,2′-m-phenylenebis(3,1-benzoxazin-4-one), 2,2′-(4,4′-diphenylene)bis(3,1-benzoxazin-4-one), 2,2′-(2,6-naphthalene)bis(3,1-benzoxazin-4-one), bis(3,1-benzoxazine-4-one), 2,2′-(1,5-naphthalene)bis(3,1-benzoxazine-4-one), 2,2′-(2-methyl-p-phenylene)bis(3,1-benzoxazine-4-one), 2,2′-(2-nitro-p-phenylene)bis(3,1-benzoxazine-4-one) and 2,2′-(2-chloro-p-phenylene)bis(3,1-benzoxazine-4-one).

[0191] Examples of the cyanoacrylate-based ultraviolet absorber include 1,3-bis-[(2′-cyano-3′,3′-diphenylacryloyl)oxy]-2,2-bis[(2-cyano-3,3-diphenylacryloyl)oxy]methyl)propane and 1,3-bis-[(2-cyano-3,3-diphenylacryloyl)oxy]benzene.

[0192] The content of the ultraviolet absorber is preferably 0.01 to 3.0 parts by weight, more preferably 0.02 to 1.0 parts by weight, and further preferably 0.05 to 0.8 parts by weight relative to 100 parts by weight of the polycarbonate resin. Within this range of the amount, satisfactory weather resistance can be imparted to the polycarbonate resin depending on the application.

[0193] The polycarbonate resin of the present invention has a high refractive index and a low Abbe number. In addition to optical lenses, it can also be effectively used as an optical molded body suitable for use as a structural material or functional material for optical components such as transparent conductive substrates used in liquid crystal displays, organic EL displays, solar cells, etc., optical disks, liquid crystal panels, optical cards, sheets, films, optical fibers, adapters, vapor-deposited plastic reflectors, and displays.

[0194] The surface of the optical molded body may be provided with a coating such as an anti-reflection layer or a hard coating layer as required. The anti-reflection layer may be a single layer or a multilayer, and may be an organic substance or an inorganic substance, but is preferably an inorganic substance. Specific examples include oxides or fluorides such as silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, cerium oxide, magnesium oxide, and magnesium fluoride.

[0195] (4) Optical lens

[0196] The optical lens made by using the polycarbonate resin of the present invention can be used in the fields of telescopes, binoculars, TV projectors, etc., which are currently using expensive high-refractive-index glass lenses, because of its high refractive index, low Abbe number, and high resistance to moisture and heat, and is extremely useful. It is preferably used in the form of an aspheric lens as needed. The aspheric lens can make the spherical aberration substantially zero by using a single lens, so there is no need to eliminate the spherical aberration by combining multiple spherical lenses, and it can achieve lightweight and reduced production costs. Therefore, the aspheric lens is useful as a camera lens among optical lenses.

[0197] The optical lens can be molded by any method, such as injection molding, compression molding, injection compression molding, etc. According to the present invention, a high refractive index low birefringence aspheric lens which is technically difficult to process can be obtained more easily using a glass lens.

[0198] In order to avoid foreign matter from mixing into the optical lens as much as possible, the molding environment also needs to be a low-dust environment, preferably below level 6, and more preferably below level 5.

[0199] (5) Optical film

[0200] The optical film produced using the polycarbonate resin of the present invention is excellent in transparency and heat resistance and can be suitably used for a liquid crystal substrate film, an optical memory card, and the like.

[0201] In order to avoid foreign matter from mixing into the optical film as much as possible, the molding environment also needs to be a low-dust environment, preferably below level 6, and more preferably below level 5.

[0202] Example

[0203] The present invention is described below by way of examples, but the present invention is not limited to these examples. The measured values ​​in the examples were measured using the following methods or devices.

[0204] 1) Polystyrene-equivalent weight average molecular weight (Mw): Gel permeation chromatography (GPC) was used with tetrahydrofuran as the developing solvent and a calibration curve was prepared using standard polystyrenes of known molecular weight (molecular weight distribution = 1). Based on this calibration curve, Mw was calculated from the retention time of GPC.

[0205] 2) Refractive index (nD): The refractive index of a 0.1 mm thick film made of the polycarbonate resin obtained in the example was measured using an Abbe refractometer in accordance with the method of JIS-K-7142.

[0206] 3) Abbe number (ν): For a 0.1 mm thick film composed of the polycarbonate resin prepared in Example, the refractive index at wavelengths of 486 nm, 589 nm and 656 nm at 23° C. was measured using an Abbe refractometer, and the Abbe number was calculated using the following formula.

[0207] ν=(nD-1) / (nF-nC)

[0208] nD: refractive index at a wavelength of 589nm

[0209] nC: refractive index at a wavelength of 656nm

[0210] nF: refractive index at a wavelength of 486nm

[0211] 4) Glass transition temperature (Tg): measured using a differential scanning calorimeter (DSC).

[0212] 5) Total light transmittance: A 3 mm thick plate made of polycarbonate resin prepared for measuring the b value described below was measured using a SE2000 spectrophotometer manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with the method of JIS-K-7361-1.

[0213] 6) b value: After the obtained resin is vacuum dried at 120°C for 4 hours, it is injection molded using an injection molding machine (FANUCROBOSHOTα-S30iA) at a barrel temperature of 270°C and a mold temperature of Tg-10°C to obtain a disc-shaped test plate with a diameter of 50 mm and a thickness of 3 mm. Using this plate, the b value is measured in accordance with JIS K7105. The smaller the b value, the weaker the yellowing and the better the hue. The SE2000 spectrophotometer produced by Nippon Denshoku Industries Co., Ltd. is used for the measurement of the molded plate.

[0214] 7) Ethylene terminal group amount: 1 The H-NMR measurement was performed under the following conditions.

[0215] · 1 H-NMR measurement conditions

[0216] Device: Bruker AVANZE III HD 500MHz

[0217] Flip angle: 30 degrees

[0218] Waiting time: 1 second

[0219] Total times: 500 times

[0220] Measurement temperature: room temperature (298K)

[0221] Concentration: 5wt%

[0222] Solvent: deuterated chloroform

[0223] Internal standard substance: tetramethylsilane (TMS) 0.05wt%

[0224] 8) Residual phenol and residual diphenyl carbonate (DPC) amount: Accurately weigh 1.0 g of polycarbonate resin, dissolve it in 10 ml of dichloromethane, and slowly add it to 100 ml of methanol while stirring to reprecipitate the resin. After sufficient stirring, filter and separate the precipitate, concentrate the filtrate using an evaporator, and add 1.0 g of the accurately weighed standard substance solution to the obtained solid. Then add 1 g of chloroform, and quantify the diluted solution using GC-MS.

[0225] Standard substance solution: 200ppm, 2,4,6-trimethylphenol in chloroform

[0226] Measurement device (GC-MS): Agilent HP6890 / 5973MSD

[0227] Column: Capillary column DB-5MS, 30m×0.25mm ID, film thickness 0.5μm

[0228] Heating conditions: 50℃ (5min hold) ~ 300℃ (15min hold), 10℃ / min

[0229] Injection temperature: 300°C, injection volume: 1.0 μl (split ratio 25)

[0230] Ionization method: EI method

[0231] Carrier gas: He, 1.0ml / min

[0232] Aux temperature: 300℃

[0233] Mass scan range: 33-700

[0234] 9) Residual BHEBN amount and residual BPPEF amount:

[0235] 0.5 g of the weighed polycarbonate resin was dissolved in 50 ml of tetrahydrofuran (THF) to prepare a sample solution. A calibration curve was prepared using each pure compound as a standard, and 2 μL of the sample solution was quantified using LC-MS under the following measurement conditions. The detection limit under these measurement conditions was 0.01 ppm.

[0236] LC-MS assay conditions:

[0237] Measurement device (LC part): Agilent Infinity 1260LC System

[0238] Column: ZORBAX Eclipse XDB-18 and guard column

[0239] Mobile Phase:

[0240] A: 0.01 mol / L ammonium acetate aqueous solution

[0241] B: 0.01mol / L ammonium acetate methanol solution

[0242] C:THF

[0243] Gradient program of mobile phase:

[0244] Table 1

[0245]

[0246] Flow rate: 0.3ml / min

[0247] Column temperature: 45°C

[0248] Detector: UV (225nm)

[0249] Measurement device (MS part): Agilent 6120 single quad LCMS System

[0250] Ionization source: ESI

[0251] Polarity: Positive

[0252] Collision voltage: 100V

[0253] Drying gas: 10L / min, 350℃

[0254] Atomizer: 50psi

[0255] Capillary voltage: 3000V

[0256] Measured ions:

[0257] BHEBN: ion species = [M+NH 4 ]-,m / z=392.1

[0258] BPPEF: ion species = [M+NH 4 ] - , m / z = 608.3

[0259] 10) Formability: When forming is performed in the measurement of the b value, the formability is evaluated based on the following criteria.

[0260] A: There are no gaps in the molded sheet and no wavy wrinkles on the surface.

[0261] B: There are gaps in the molded sheet.

[0262] C: The surface of the molded sheet has wavy wrinkles.

[0263] D: There are gaps in the molded piece and the surface is deformed.

[0264] 11) PCT (Pressure Cooker Test): Use PC-305SIII manufactured by HIRAYAMA to keep an injection molded product with a diameter of 50 mm and a thickness of 3 mm at 120°C, 0.2 MPa, and 100% RH for 20 hours. Then take out the sample and use SE2000 spectrophotometer manufactured by Nippon Denshoku Industries Co., Ltd. to measure the color according to the method of JIS-K-7361-1.

[0265] [Manufacture of polycarbonate resin]

[0266] (Example 1)

[0267] As raw materials, 18.85 g (0.035 mol) of 9,9-bis[6-(2-hydroxyethoxy)naphth-2-yl]fluorene (hereinafter sometimes referred to as "BNEF"), 18.35 g (0.049 mol) of 2,2′-bis(2-hydroxyethoxy)-1,1′-binaphthyl (hereinafter sometimes referred to as "BHEBN"), 7.02 g (0.016 mol) of 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (hereinafter sometimes referred to as "BPEF"), 21.70 g (0.101 mol) of diphenyl carbonate (hereinafter sometimes referred to as "DPC"), and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10 -7 mole, that is, 8.0×10 -6 mol) was placed in a 300ml four-necked flask with a stirrer and a distillation apparatus and heated to 180°C under a nitrogen atmosphere of 760mmHg. After 10 minutes of heating, it was confirmed that the raw material was completely dissolved, and then stirred for 110 minutes under the same conditions. After that, the reduced pressure was adjusted to 200mmHg, and the temperature was raised to 200°C at a rate of 60°C / hr. At this time, it was confirmed that phenol generated as a by-product began to distill. After that, it was kept at 200°C for 20 minutes to allow the reaction to proceed. Further, the temperature was raised to 230°C at a rate of 75°C / hr, and 10 minutes after the temperature was raised, it was maintained at this temperature while the reduced pressure was brought to less than 1mmHg for 1 hour. After that, the temperature was raised to 245°C at a rate of 60°C / hr, and further stirred for 30 minutes. After the reaction was completed, nitrogen was introduced into the reactor to restore it to normal pressure, and the generated polycarbonate resin was taken out.

[0268] The physical properties of the obtained resin are shown in Table 2. In addition, the H 1-Ratio of NMR spectrum, (4.75 to 4.69 ppm peak integration value) / (4.85 to 2.80 ppm peak integration value) × 100 = 0.029, (4.59 to 4.55 ppm peak integration value) / (4.85 to 2.80 ppm peak integration value) × 100 = not detected, (3.62 to 3.26 ppm peak integration value) / (4.85 to 2.80 ppm peak integration value) × 100 = 0.189, (4.83 to 4.76 ppm peak integration value) / (4.85 to 2.80 ppm peak integration value) × 100 = 0.026, b value is 4.1, the amount of residual phenol in the resin is 300 ppm, and the amount of residual DPC is 50 ppm. The obtained NMR spectrum is shown in Figure 1 .

[0269] (Example 2)

[0270] As raw materials, 17.77 g (0.033 mol) of BNEF, 18.72 g (0.050 mol) of BHEBN, 10.04 g (0.017 mol) of 9,9-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]fluorene (hereinafter sometimes referred to as "BPPEF"), 21.70 g (0.101 mol) of DPC and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10 -7 mole, that is, 8.0×10 -6 The same operation as in Example 1 was carried out except for this.

[0271] The physical properties of the obtained resin are shown in Table 2. In addition, the H 1 -Ratio of NMR spectrum, (4.75 to 4.69 ppm peak integration value) / (4.85 to 2.80 ppm peak integration value) × 100 = not detected, (4.59 to 4.55 ppm peak integration value) / (4.85 to 2.80 ppm peak integration value) × 100 = 0.068, (3.62 to 3.26 ppm peak integration value) / (4.85 to 2.80 ppm peak integration value) × 100 = 0.184, (4.83 to 4.76 ppm peak integration value) / (4.85 to 2.80 ppm peak integration value) × 100 = 0.022, b value is 4.2, the amount of residual phenol in the resin is 300 ppm, and the amount of residual DPC is 50 ppm. The obtained NMR spectrum is shown in Figure 2 .

[0272] (Example 3)

[0273] As raw materials, 8.08 g (0.015 mol) of BNEF, 50.21 g (0.085 mol) of BPPEF, 21.70 g (0.101 mol) of DPC and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10 -7 mole, that is, 8.0×10 -6 The same operation as in Example 1 was performed except that the above-mentioned amount was 0.1 mol. The physical property values ​​of the obtained resin are shown in Table 2.

[0274] (Example 4)

[0275] As raw materials, 29.62 g (0.055 mol) of BNEF, 26.58 g (0.045 mol) of BPPEF, 21.70 g (0.101 mol) of DPC and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10 -7 mole, that is, 8.0×10 -6 The same operation as in Example 1 was performed except that the above-mentioned amount was 0.1 mol. The physical property values ​​of the obtained resin are shown in Table 2.

[0276] (Example 5)

[0277] As raw materials, 40.40 g (0.075 mol) of BNEF, 14.77 g (0.025 mol) of BPPEF, 21.70 g (0.101 mol) of DPC and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10 -7 mole, that is, 8.0×10 -6 The same operation as in Example 1 was performed except that the above-mentioned amount was 0.1 mol. The physical property values ​​of the obtained resin are shown in Table 2.

[0278] (Example 6)

[0279] As raw materials, 8.08 g (0.015 mol) of BNEF, 18.72 g (0.050 mol) of BHEBN, 15.35 g (0.035 mol) of BPEF, 21.70 g (0.101 mol) of DPC and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10 -7 mole, that is, 8.0×10 -6 The same operation as in Example 1 was performed except that the above-mentioned amount was 0.1 mol. The physical property values ​​of the obtained resin are shown in Table 2.

[0280] (Example 7)

[0281] As raw materials, 29.62 g (0.055 mol) of BNEF, 3.11 g (0.035 mol) of BHEBN, 4.39 g (0.010 mol) of BPEF, 21.70 g (0.101 mol) of DPC and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10 -7 mole, that is, 8.0×10 -6 The same operation as in Example 1 was performed except that the above-mentioned amount was 0.1 mol. The physical property values ​​of the obtained resin are shown in Table 2.

[0282] (Example 8)

[0283] As raw materials, 40.40 g (0.075 mol) of BNEF, 7.49 g (0.020 mol) of BHEBN, 2.19 g (0.005 mol) of BPEF, 21.70 g (0.101 mol) of DPC and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10 -7 mole, that is, 8.0×10 -6 The same operation as in Example 1 was performed except that the above-mentioned amount was 0.1 mol. The physical property values ​​of the obtained resin are shown in Table 2.

[0284] (Example 9)

[0285] As raw materials, 8.08 g (0.015 mol) of BNEF, 16.85 g (0.045 mol) of BHEBN, 23.63 g (0.040 mol) of BPPEF, 21.70 g (0.101 mol) of DPC and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10 -7 mole, that is, 8.0×10 -6 The same operation as in Example 1 was performed except that the above-mentioned amount was 0.1 mol. The physical property values ​​of the obtained resin are shown in Table 2.

[0286] (Example 10)

[0287] As raw materials, 29.62 g (0.055 mol) of BNEF, 14.98 g (0.040 mol) of BHEBN, 2.95 g (0.005 mol) of BPPEF, 21.70 g (0.101 mol) of DPC and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10-7 mole, that is, 8.0×10 -6 The same operation as in Example 1 was performed except that the above-mentioned amount was 0.1 mol. The physical property values ​​of the obtained resin are shown in Table 2.

[0288] (Example 11)

[0289] As raw materials, 40.40 g (0.075 mol) of BNEF, 7.49 g (0.020 mol) of BHEBN, 2.95 g (0.005 mol) of BPPEF, 21.70 g (0.101 mol) of DPC and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10 -7 mole, that is, 8.0×10 -6 The same operation as in Example 1 was performed except that the above-mentioned amount was 0.1 mol. The physical property values ​​of the obtained resin are shown in Table 2.

[0290] (Example 12)

[0291] The same operation as in Example 1 was carried out except that 10.77 g (0.020 mol) of BNEF and 29.95 g (0.080 mol) of BHEBN were used as raw materials, and BPEF was not used. Table 2 shows the physical property values ​​of the obtained resin.

[0292] (Example 13)

[0293] As raw materials, 18.64 g (0.035 mol) of BNEF, 23.70 g (0.063 mol) of BHEBN, 21.30 g (0.099 mol) of DPC and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10 -7 mole, that is, 8.1×10 -6 The same operation as in Example 12 was carried out except that the above-mentioned amount was 0.1 mol. The physical property values ​​of the obtained resin are shown in Table 2.

[0294] (Example 14)

[0295] As raw materials, 29.28 g (0.054 mol) of BNEF, 16.41 g (0.044 mol) of BHEBN, 21.30 g (0.099 mol) of DPC and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10 -7 mole, that is, 8.1×10 -6The same operation as in Example 1 was performed except that the above-mentioned amount was 0.1 mol. The physical property values ​​of the obtained resin are shown in Table 2.

[0296] In addition, the H 1 -Ratio of NMR spectrum, (4.75 to 4.69 ppm peak integration value) / (4.85 to 2.80 ppm peak integration value) × 100 = not detected, (4.59 to 4.55 ppm peak integration value) / (4.85 to 2.80 ppm peak integration value) × 100 = not detected, (3.62 to 3.26 ppm peak integration value) / (4.85 to 2.80 ppm peak integration value) × 100 = 0.4925, (4.83 to 4.76 ppm peak integration value) / (4.85 to 2.80 ppm peak integration value) × 100 = 0.023. The obtained NMR spectrum is shown in Figure 3 .

[0297] (Example 15)

[0298] As raw materials, 40.00 g (0.074 mol) of BNEF, 9.12 g (0.024 mol) of BHEBN, 21.40 g (0.100 mol) of DPC and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10 -7 mole, that is, 8.1×10 -6 The same operation as in Example 1 was performed except that the above-mentioned amount was 0.1 mol. The physical property values ​​of the obtained resin are shown in Table 2.

[0299] (Example 16)

[0300] As raw materials, 8.0 kg (14.85 mol) of BNEF, 7.5 kg (20.03 mol) of BHEBN, 7.5 kg (12.70 mol) of BPPEF, 10.5 kg (49.02 mol) of DPC and 2.5×10 -2 16 ml of sodium bicarbonate aqueous solution (4.0×10 -4 mole, that is, 8.4×10 -6mol) was placed in a 50L reactor with a stirrer and a distillation device and heated to 180°C under a nitrogen atmosphere of 760mmHg. After 30 minutes from the start of heating, it was confirmed that the raw materials were completely dissolved, and then stirred for 120 minutes under the same conditions. After that, the reduced pressure was adjusted to 200mmHg, and the temperature was raised to 200°C at a rate of 60°C / hr. At this time, it was confirmed that phenol generated as a by-product began to distill. After that, it was kept at 200°C for 20 minutes to allow the reaction to proceed. Further, the temperature was raised to 230°C at a rate of 75°C / hr, and 10 minutes after the temperature was raised, it was maintained at this temperature while the reduced pressure was brought to less than 1mmHg for 2 hours. After that, the temperature was raised to 245°C at a rate of 60°C / hr, and further stirred for 40 minutes. After the reaction was completed, nitrogen was introduced into the reactor to restore it to normal pressure, and the generated polycarbonate resin was granulated and taken out. The b value of the obtained resin was 4.2, and the residual phenol content in the resin was 100 ppm, the residual DPC content was 50 ppm, the residual BHEBN content was 20 ppm, and the residual BPPEF content was 5 ppm.

[0301] (Example 17)

[0302] As raw materials, 6.9 kg (12.81 mol) of BNEF, 9.3 kg (24.84 mol) of BHEBN, 5.9 kg (9.99 mol) of BPPEF, 10.5 kg (49.02 mol) of DPC and 2.5×10 -2 16 ml of sodium bicarbonate aqueous solution (4.0×10 -4 mole, that is, 8.4×10 -6 The same operation as in Example 16 was performed except that the polycarbonate resin produced was pelletized and taken out. The b value of the obtained resin was 2.7, the residual phenol content in the resin was 200 ppm, the residual DPC content was 160 ppm, the residual BHEBN content was 15 ppm, and the residual BPPEF content was 5 ppm.

[0303] (Comparative Example 1)

[0304] As raw materials, 8.05 g (0.075 mol) of BHEBN, 10.96 g (0.025 mol) of BPEF, 21.70 g (0.101 mol) of DPC and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10 -7 mole, that is, 8.0×10 -6 The same operation as in Example 1 was carried out except for this.

[0305] The physical properties of the obtained resin are shown in Table 2. In addition, the H 1 - Ratio of NMR spectrum, (integrated value of the peak at 4.75 to 4.69 ppm) / (integrated value of the peak at 4.85 to 2.80 ppm)×100=1.013, (integrated value of the peak at 4.59 to 4.55 ppm) / (integrated value of the peak at 4.85 to 2.80 ppm)×100=not detected, (integrated value of the peak at 3.62 to 3.26 ppm) / (integrated value of the peak at 4.85 to 2.80 ppm)×100=1.615, (integrated value of the peak at 4.83 to 4.76 ppm) / (integrated value of the peak at 4.85 to 2.80 ppm)×100=not detected, b value is 5.3.

[0306] (Comparative Example 2)

[0307] As raw materials, 8.05 g (0.075 mol) of BHEBN, 14.77 g (0.025 mol) of BPPEF, 21.70 g (0.101 mol) of DPC and 2.5×10 -2 32 μl of sodium bicarbonate aqueous solution (8.0×10 -7 mole, that is, 8.0×10 -6 The same operation as in Example 1 was carried out except for this.

[0308] The physical properties of the obtained resin are shown in Table 2. In addition, the H 1 - Ratio of NMR spectrum, (integrated value of the peak at 4.75 to 4.69 ppm) / (integrated value of the peak at 4.85 to 2.80 ppm)×100=not detected, (integrated value of the peak at 4.59 to 4.55 ppm) / (integrated value of the peak at 4.85 to 2.80 ppm)×100=1.120, 0.021, (integrated value of the peak at 3.62 to 3.26 ppm) / (integrated value of the peak at 4.85 to 2.80 ppm)×100=1.570, (integrated value of the peak at 4.83 to 4.76 ppm) / (integrated value of the peak at 4.85 to 2.80 ppm)×100=not detected, b value is 6.0.

[0309] (Comparative Example 3)

[0310] As raw materials, BPEF 5.6 kg (12.81 mol), BHEBN 9.3 kg (24.84 mol), BPPEF 5.9 kg (9.99 mol), DPC 10.5 kg (49.02 mol) and 2.5×10 -2 16 ml of sodium bicarbonate aqueous solution (4.0×10 -4 mole, that is, 8.4×10-6 The same operation as in Example 16 was performed except that the polycarbonate resin produced was pelletized and taken out. The b value of the obtained resin was 4.1. The physical properties of the obtained resin are shown in Table 2.

[0311]

Table 2

[0312]

Claims

1. A method for producing a polycarbonate resin, characterized in that: The method comprises the steps of melt polycondensing a monomer composition having a compound represented by the following general formula (4) as a main component and a compound represented by the following general formula (5) with a carbonic acid diester, In the general formula (4), X represents an alkylene group having 1 to 4 carbon atoms, and a and b each independently represent an integer of 1 to 10. In the general formula (5), Y represents an alkylene group having 1 to 4 carbon atoms, c and d each independently represent an integer of 1 to 10, The compound represented by the general formula (4) is produced by reacting 9,9-bis(hydroxynaphthyl)fluorene with a halogenated alkanol. The monomer composition further contains a compound in which either a or b in the general formula (4) is 0, and the content of the compound in which either a or b in the general formula (4) is 0 is less than 1000 ppm in the monomer composition having the compound represented by the general formula (4) as a main component.

2. The manufacturing method according to claim 1, characterized in that The method comprises the step of performing melt polycondensation using an ester exchange catalyst selected from alkali metal compounds, alkaline earth metal compounds and nitrogen-containing compounds.

3. The manufacturing method according to claim 2, characterized in that: The transesterification catalyst is selected from sodium hydroxide, potassium hydroxide, cesium hydroxide, lithium hydroxide, sodium bicarbonate, sodium carbonate, potassium carbonate, cesium carbonate, lithium carbonate, sodium acetate, potassium acetate, cesium acetate, lithium acetate, sodium stearate, potassium stearate, cesium stearate, lithium stearate, sodium borohydride, sodium phenylborate, sodium benzoate, potassium benzoate, cesium benzoate, lithium benzoate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, dilithium hydrogen phosphate, disodium phenyl phosphate, disodium salt of bisphenol A, dipotassium salt of bisphenol A, dicesium salt of bisphenol A or dilithium salt of bisphenol A, sodium salt of phenol, potassium salt of phenol, cesium salt of phenol or lithium salt of phenol, and combinations thereof.

4. The manufacturing method according to claim 2 or 3, characterized in that: The ratio of the transesterification catalyst used is 1×10 -7 ~1×10 -4 Moore.

Citation Information

Patent Citations

  • Optical lens

    WO2007142149A1

  • Polycarbonate resin composition and method for producing the same

    CN101805501A

  • Optical lens comprising aromatic-aliphatic polycarbonate resin

    CN103339531A

  • Polycarbonate copolymer having high fluidity, method for producing aromatic polycarbonate resin having high molecular weight, and aromatic polycarbonate compound

    CN103619908A

  • New fluorene backbone-containing polymer