Wiring substrate, electronic device, and electronic module

By using a combined structure of AlN insulating substrate, Cu conductor and Ni film on the wiring substrate, combined with Ti oxide recess and interlayer technology, the corrosion and ion migration problems caused by Ni film peeling are solved and the reliability of electronic devices is improved.

CN113614904BActive Publication Date: 2024-10-25KYOCERA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080023216.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-25
Filing Date
2020-03-25
Publication Date
2024-10-25
Estimated Expiration
2040-03-25

AI Technical Summary

Technical Problem

Existing wiring substrates can easily cause conductor corrosion and ion migration when the Ni film is peeled off, affecting the reliability of electronic devices.

Method used

Using a combined structure of AlN insulating substrate, Cu conductor and Ni film, multiple recesses are formed by spreading Ti oxide on the insulating substrate to increase the contact area of ​​the Ni film, and an intermediate layer is formed through sintering and plating processes during the manufacturing process , enhance the bonding strength between the Ni film and the insulating substrate.

Benefits of technology

It effectively inhibits the peeling of the Ni film, improves the bonding strength between the Ni film and the insulating substrate, reduces conductor corrosion and ion migration, and improves the reliability of electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113614904B_ABST
    Figure CN113614904B_ABST
Patent Text Reader

Abstract

Provided is a wiring substrate capable of suppressing the peeling of a Ni film. Also provided is an electronic device and an electronic module having such a wiring substrate. The device comprises: an insulating substrate including AlN, having a first surface and a second surface opposite to the first surface; a conductor including Cu, located on the first surface; and a Ni film, which is provided over the upper surface, the side surface and the first surface of the conductor. The device also comprises a plurality of Ti oxides dispersed on the first surface, and the Ni film has a portion in contact with the Ti oxides.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a wiring substrate, an electronic device, and an electronic module. Background Art

[0002] Conventionally, there is known a wiring substrate in which an Al-based wiring conductor is provided on a Si substrate via an insulating film and a titanium-based metal film (see, for example, Japanese Patent Application Laid-Open No. 5-182926). Summary of the invention

[0003] Means for solving problems

[0004] The wiring substrate of the present disclosure comprises:

[0005] An insulating substrate including AlN, having a first surface and a second surface opposite to the first surface;

[0006] A conductor including Cu, located on the first surface; and

[0007] A Ni film is provided over the upper surface, the side surface and the first surface of the conductor,

[0008] The device further includes a plurality of Ti oxides dispersed on the first surface.

[0009] The electronic device disclosed herein comprises:

[0010] The above wiring substrate; and

[0011] The electronic components are mounted on the wiring substrate.

[0012] The electronic module involved in the present disclosure has:

[0013] The electronic device mentioned above; and

[0014] The module substrate is provided with the electronic device. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1A This is a longitudinal sectional view showing a part of the wiring substrate according to the embodiment.

[0016] Figure 1B It is a top view showing a part of the wiring substrate according to the embodiment.

[0017] Figure 1C This is a plan view of the wiring substrate according to the embodiment with the Ni film removed.

[0018] Figure 2 It is a plan view showing the entire wiring substrate according to the embodiment.

[0019] Figure 3AIt is a diagram showing the concentration distribution of constituent elements in the intermediate layer between the wiring conductor and the insulating substrate.

[0020] Figure 3B : is a graph showing the concentration distribution of constituent elements in the intermediate layer under the Ni film.

[0021] Figure 4A This is a diagram showing an electron microscope image of one lower end portion of a wiring conductor in a wiring substrate according to the embodiment.

[0022] Figure 4B This is a diagram showing an electron microscope image of one lower end portion of a wiring conductor in a wiring substrate according to the embodiment.

[0023] Figure 4C This is a diagram showing an electron microscope image of one lower end portion of a wiring conductor in a wiring substrate according to the embodiment.

[0024] Figure 5 It is an explanatory diagram showing an example of a method for manufacturing a wiring substrate according to an embodiment.

[0025] Figure 6 2 is a cross-sectional view showing an electronic device and an electronic module according to an embodiment of the present disclosure. DETAILED DESCRIPTION

[0026] Hereinafter, each embodiment of the present disclosure will be described in detail with reference to the drawings.

[0027] Figures 1A to 1C is a diagram showing a portion of a wiring substrate according to an embodiment, Figure 1A is a longitudinal section view, Figure 1B It is a top view. Figure 1C This is a top view with the Ni (nickel) film removed. Figure 2 1 is a top view showing the entire wiring substrate of the embodiment. In this specification, the direction from the second surface 12 toward the first surface 11 of the insulating substrate 10 is described as the upper direction. However, the directions described in this specification may be different from the directions when the wiring substrate 1 is installed or used.

[0028] The wiring substrate 1 of the present embodiment is a base interposed between the electronic component and the mounting destination in order to mount the electronic component on a module substrate or a package, for example. The wiring substrate 1 includes: an insulating substrate 10 made of a ceramic material including AlN (aluminum nitride), a wiring conductor 20 formed on the insulating substrate 10, and a Ni film 30 covering the upper surface and side surfaces of the wiring conductor 20. The wiring conductor 20 is equivalent to an example of a conductor involved in the present disclosure.

[0029] The insulating substrate 10 is a ceramic material containing AlN as a constituent element. The insulating substrate 10 has a first surface (first main surface) 11 and a second surface (second main surface) 12 on the opposite side thereof, and a wiring conductor 20 is formed on the first surface 11 side. In addition, in the insulating substrate 10, the wiring conductor 20 can also be formed on both the first surface 11 side and the second surface 12 side. When the wiring conductor 20 on the second surface 12 is regarded as the conductor involved in the present disclosure, the second surface 12 is equivalent to the first surface involved in the present disclosure, and the first surface 11 is equivalent to the second surface involved in the present disclosure.

[0030] like Figure 1A to Figure 1C As shown in FIG. 1 , a plurality of Ti oxides 13 are dispersed on the first surface 11 of the insulating substrate 10. That is, the Ti oxides 13 are dispersed in the surface direction of the first surface 11. The Ti oxides 13 may be, for example, TiO 2 (Titanium oxide) The Ti oxide 13 may be located in a recess 11D of the first surface 11 described later.

[0031] The insulating substrate 10 has a plurality of fine recesses 11D on the first surface 11. The recesses 11D may have a maximum width of 1 μm to 20 μm at the opening, for example. The first surface 11 may have a plurality of recesses 11D at an area ratio of 10% to 60%. The recesses 11D are formed on the entire first surface 11, but may be formed only at a portion in contact with the Ni film 30. In the following, the recesses 11D are described as portions where the Ti oxide 13 is dispersed on the first surface 11.

[0032] The plurality of recesses 11D include a composite recess 11DW (see Figure 1C ), the composite recess 11DW has a shape in which two or more recesses overlap when the planar shape of each recess 11D is regarded as a granular shape.

[0033] The wiring conductor 20 is a conductor with Cu (copper) as the main component, and is formed on the insulating substrate 10 with a layer of Ti oxide 13 interposed therebetween. The Ti oxide 13 is gathered in the recess 11D by a sintering process described later, and the interface between the insulating substrate 10 and the wiring conductor 20 may include a portion where the layer of Ti oxide 13 remains and a portion where the layer of Ti oxide 13 disappears. The portion where Ti oxide 13 is gathered in the recess 11D under the wiring conductor 20 forms an intermediate layer 16a ( Figure 1A Furthermore, in the concave portion 11D where the Ni film 30 is in contact, the same intermediate layer 16b may be retained ( Figure 1A ).

[0034] The Ni film 30 is a film mainly composed of Ni, and covers a portion of the first surface 11 of the insulating substrate 10 from the upper surface 21 of the wiring conductor 20 through the side surface 22. The Ni film 30 has a protrusion 31 protruding to the side opposite to the wiring conductor 20 at the lower part of the first surface 11 of the insulating substrate 10. Furthermore, when viewed from a direction perpendicular to the first surface 11 of the insulating substrate 10, the outer edge of the protrusion 31 has a plurality of peaks h1 to h4 and a plurality of valleys c1 to c3 ( Figure 1B ).

[0035] The Ni film 30 is in contact with any one of the plurality of recesses 11D on the first surface 11 of the insulating substrate 10 via the Ti oxide 13. Hereinafter, the contact between the Ni film 30 and the recess 11D via the Ti oxide 13 is also referred to as the contact between the Ni film 30 and the recess 11D. Hereinafter, the recess in contact with the Ni film 30 among the plurality of recesses 11D is also plotted as a contact recess 11Da. The plurality of contact recesses 11Da may also include a composite recess 11DW.

[0036] like Figure 1C As shown in FIG. 1 , a plurality of contact recesses 11Da are arranged along the side surface 22 of the wiring conductor 20 (specifically, the lower side 22e of the side surface 22). Figure 2 As shown in FIG. 1 , the protrusion 31 of the Ni film 30 in contact with the insulating substrate 10 exists all around the wiring conductor 20, and the contact recess 11Da exists all around the wiring conductor 20. Figure 1C Therefore, the plurality of contact recesses 11Da surround the wiring conductor 20 and exist in at least four directions around the wiring conductor 20. Among the plurality of contact recesses 11Da, there are contact recesses that are partially not covered by the Ni film 30 and are exposed, and contact recesses that are not exposed and are completely covered by the Ni film 30. The fact that the entire contact recess 11Da is covered by the Ni film 30 means that the protrusion 31 protrudes beyond the position of the contact recess 11Da.

[0037] The wiring substrate 1 may include a portion where two or more contact recesses 11Da exist under the Ni film 30 in any cross section perpendicular to the first surface 11 and the side surface 22 of the wiring conductor 20. By including the protrusion 31 of the Ni film 30, the contact area between the Ni film 30 and the insulating substrate 10 is increased, and the Ni film 30 can contact more recesses 11D.

[0038] Figure 3A It is a diagram showing the concentration distribution of constituent elements in the intermediate layer between the wiring conductor and the insulating substrate. Figure 3B: is a diagram showing the concentration distribution of constituent elements in the intermediate layer under the Ni film. The constituent elements and concentration distribution of the intermediate layers 16a and 16b shown below show the measurement results of electron energy loss spectroscopy (TEM-EELS: Electron Energy-Loss Spectroscopy). The concentration is expressed in at% (atomic percentage).

[0039] The intermediate layer 16a existing at the interface between the wiring conductor 20 and the recessed portion 11D has a thickness of 20 nm to 80 nm. Figure 3A As shown, the intermediate layer 16a includes Al (aluminum), N (nitrogen), Cu (copper), Ti (titanium), and O (oxygen). Furthermore, the intermediate layer 16a has a concentration gradient in which the concentrations of Al, N, and Cu gradually change. The concentration gradients of Al and N are gradients in which the concentrations decrease as they approach the wiring conductor 20, and the concentration gradient of Cu is gradients in which the concentrations increase as they approach the wiring conductor 20. These concentration gradients may also exist from the wiring conductor 20 side of the intermediate layer 16a to the insulating substrate 10 side.

[0040] The intermediate layer 16b existing at the interface between the Ni film 30 and the contact recess 11Da has a thickness of 20 nm to 80 nm. Figure 3B As shown, in addition to containing Al, N, Cu, Ti, and O, there is also a concentration gradient in which the concentrations of Al, N, and Cu gradually change. The concentration gradients of Al and N are gradients in which the concentrations are lower as they are closer to the Ni film 30, and the concentration gradient of Cu is gradients in which the concentrations are higher as they are closer to the Ni film 30. These concentration gradients can also be formed from the Ni film 30 side of the intermediate layer 16b to the insulating base PA216263D

[0041] The plate 10 side exists.

[0042] The intermediate layers 16 a and 16 b may contain 10 at % or less of C (carbon). The concentration of C in the intermediate layers 16 a and 16 b (10 at % or less) may be substantially the same as the concentration of C in the wiring conductor 20 .

[0043] Figure 4A to Figure 4C The electron microscope images of the lower end portions of the wiring conductors in the wiring substrates of the embodiments are shown respectively. Figure 4A to Figure 4CAs shown in FIG. 1 , in fact, a shape (bite) that is concave inward is generated at the lower corners E1 to E3 of the wiring conductor 20, and the Ni film 30 extends along the side surface of the wiring conductor 20 to the lower corners E1 to E3 of the wiring conductor 20. Furthermore, a part of the Ni film 30 is formed to protrude from the lower corners E1 to E3 of the wiring conductor 20 along the first surface 11 of the insulating substrate 10 in the direction opposite to the wiring conductor 20, and this part constitutes a protrusion 31. The boundary between the Ni film 30 and the insulating substrate 10 including the protrusion 31 includes a contact recess 11Da. If the interface in the contact recess 11Da is measured by energy dispersive X-ray spectroscopy (EDS) or electron energy loss spectroscopy, Ti and O can be observed.

[0044] <Manufacturing method>

[0045] Figure 5 It is an explanatory diagram showing a method for manufacturing a wiring substrate according to an embodiment.

[0046] The method for manufacturing the wiring board 1 of the present embodiment includes, in chronological order, a pretreatment step J1, a Ti film forming step J2, an electroless plating and sintering step J3, a resist processing step J4, an electrolytic plating step J5, a resist removal and etching step J6, and a plating step J7.

[0047] In the pre-treatment process J1, the ceramic before sintering, that is, the ceramic green sheet 70 is formed into a substrate shape by punching or die processing. The ceramic green sheet 70 may also be provided with a through hole v for conducting inside the substrate. The insulating substrate 10 is formed by sintering the ceramic green sheet 70. In the pre-treatment process J1, the ceramic green sheet 70 before or after sintering may be anisotropically etched using a reagent or reactive ions. By the above-mentioned anisotropic etching, the size and density of the recessed portions 11D on the first surface 11 and the second surface 12 of the insulating substrate 10 can be controlled.

[0048] The Ti film forming step J2 is a step of applying an organic Ti liquid to the ceramic green sheet 70 before or after sintering and sintering. The sintering can be performed, for example, at a temperature of 400° C. or above and for 30 minutes or more. By sintering, the organic Ti liquid 71 changes into a solidified titanium oxide layer 71A. The sintering of the titanium oxide layer 71A and the sintering of the ceramic green sheet 70 can also be performed simultaneously and in parallel.

[0049] In the electroless plating and sintering process J3, after electroless Cu plating is performed on the insulating substrate 10 having the titanium oxide layer 71A, a sintering treatment is performed to diffuse the elements of the interface. The conditions for the sintering treatment can be above 300°C and for more than 30 minutes in an inert gas atmosphere. The Cu plating layer 74 is formed by electroless Cu plating. The above-mentioned intermediate layers 16a and 16b are formed by sintering. The sintered titanium oxide layer 71A and the Cu plating layer 74 function as seed layers. In this way, since the seed layer is formed by a wet process, it is possible to seek to reduce manufacturing costs.

[0050] In the resist processing step J4, for example, a wiring conductor 20 is formed on the Cu plating layer 74 by using a DFR (Dry Film Resist) 81 (see Figure 2 In the electrolytic Cu plating step J5, electrolytic Cu plating is performed on the Cu plating layer 74 according to the pattern of the DFR 81 to form a Cu conductor 75 of a given thickness. When a through hole v is formed in the insulating substrate 10, the Cu conductor 75 is filled in the through hole v in the electrolytic Cu plating step J5.

[0051] In the resist removal and etching step J6, the DFR 81 is first removed. When the DFR is removed, the seed layer (Cu plating layer 74 and titanium oxide layer 71A) is exposed. Then, the exposed seed layer is etched by etching using a reagent. At this time, the etching amount is controlled to a degree that the components of the titanium oxide layer 71A remain in the concave portion 11D of the insulating substrate 10. In steps J6 and J7, although Figure 5 Although the drawing is simplified in FIG. 1 , the titanium oxide layer 71A is not in a layered form but is in a form dispersed in the recessed portion 11D.

[0052] In the plating step J7, electroless plating of Ni is performed on the surface where the Cu conductor 75 is formed. At this time, the Ni film 30 covers the Cu conductor 75 and the surroundings of the residual body 74a of the Cu plating layer 74 below the Cu conductor 75. Furthermore, by leaving the components of the titanium oxide layer 71A in the plurality of recesses 11D on the insulating substrate 10, the Ni film 30 is slightly extended on the insulating substrate 10 and formed so as to contact the recesses 11D near the Cu conductor 75 and the residual body 74a. In the plating step J7, in addition to forming the Ni film 30, other metals (such as Pd (palladium) and Au (gold)) can be plated again on the Ni film 30.

[0053] The wiring board 1 according to the present embodiment can be manufactured by the manufacturing method as described above.

[0054] <Electronic Devices and Electronic Modules>

[0055] Figure 6 2 is a cross-sectional view showing an electronic device and an electronic module according to an embodiment of the present disclosure.

[0056] The electronic device 60 involved in this embodiment is constituted by mounting an electronic component 50 on a wiring substrate 1. The electronic component 50 may be bonded to the wiring conductor 20 and the Ni film 30 via a bonding material. The electrodes of the electronic component 50 may be connected to the wiring conductor 20 and the Ni film 30 via bonding wires. Other metal films such as a Pd film and an Au film may also be formed on the Ni film 30. The electronic device 60 may also be a structure having a package that accommodates the wiring substrate 1 and the electronic component 50.

[0057] As the electronic component 50, various electronic components can be applied, such as optical elements such as LD (Laser Diode), PD (Photo Diode), LED (Light Emitting Diode), imaging elements such as CCD (Charge Coupled Device) type and CMOS (Complementary Metal Oxide Semiconductor) type, piezoelectric resonators such as quartz resonators, surface acoustic wave elements, semiconductor elements such as semiconductor integrated circuit elements (IC: Integrated Circuit), capacitor elements, inductor elements or resistors.

[0058] The electronic module 100 involved in this embodiment is configured by mounting an electronic device 60 on a module substrate 110. In addition to the electronic device 60, other electronic devices, electronic components, and electrical components may be mounted on the module substrate 110. Electrode pads 111 are provided on the module substrate 110, and the electronic device 60 may be bonded to the electrode pads 111 via a bonding material 113 such as solder. In addition, a wiring conductor 20 and a Ni film 30 may be provided at a portion of the electronic device 60 bonded to the bonding material 113. In addition, when the electronic device 60 has a package, the wiring conductor of the package may be bonded to the electrode pads 111 of the module substrate 110.

[0059] As described above, according to the wiring substrate 1 of the present embodiment, the Ni film 30 covers the upper surface and the side surface of the wiring conductor 20 having Cu as a constituent element. Furthermore, the lower edge portion of the Ni film 30 reaches the insulating substrate 10 and contacts the Ti oxide 13. Therefore, the lower edge portion of the Ni film 30 is bonded to the insulating substrate 10 with high strength via the Ti oxide 13, and it is possible to suppress the Ni film 30 from peeling off from the lower edge portion. Therefore, it is possible to suppress the unfavorable situation that a part of the wiring conductor 20 is exposed due to the peeling of the Ni film 30 and corrosion occurs in the exposed portion, or ion migration occurs from the exposed portion to the insulating substrate 10.

[0060] Furthermore, according to the wiring substrate 1 of the present embodiment, the Ni film 30 has the protrusion 31 protruding toward the side opposite to the wiring conductor 20 along the first surface 11 of the insulating substrate 10. Therefore, the contact area between the Ni film 30 and the insulating substrate 10 is increased by the protrusion 31, and the number of contact recesses 11Da contacted by the Ni film 30 is increased. Therefore, the bonding strength between the hem portion of the Ni film 30 and the insulating substrate 10 can be further improved, and the peeling of the Ni film 30 can be further suppressed.

[0061] Furthermore, the protrusion 31 protrudes beyond the contact recess 11Da relative to at least any one of the contact recesses 11Da. Therefore, at least in this portion, the Ni film 30 and the contact recess 11Da can be in contact via the Ti oxide 13, and high adhesion strength between the Ni film 30 and the insulating substrate 10 can be obtained.

[0062] Furthermore, according to the wiring substrate 1 of the present embodiment, the edge of the protruding side of the protruding portion 31 has a shape including a plurality of peaks h1 to h4 and valleys c1 to c3 when viewed from a direction perpendicular to the first surface 11 of the insulating substrate 10 ( Figure 1B ). Therefore, on the insulating substrate 10 where a plurality of recesses 11D are randomly arranged, the bonding strength can be improved by making contact with the plurality of recesses 11D at the peaks h1 to h4 of the protrusion 31. On the other hand, in a portion where the number of recesses 11D is small, by arranging valleys c1 to c3, the portion with low bonding strength can be shortened. In the case where the arrangement of the recesses 11D is random, such an arrangement of the peaks and valleys of the protrusion 31 can be achieved in a plurality of ranges. Through these effects, the bonding strength of the protrusion 31 to the insulating substrate 10 can be further improved, and a property that is less likely to peel off can be obtained.

[0063] Furthermore, according to the wiring substrate 1 of the present embodiment, the contact recesses 11Da in contact with the Ni film 30 are arranged along the edge of the wiring conductor 20. In addition, the contact recesses 11Da in contact with the Ni film 30 surround the wiring conductor 20. With such a structure, it is possible to suppress the peeling of the hem portion of the Ni film 30 at multiple locations around the wiring conductor 20.

[0064] Furthermore, according to the wiring substrate 1 of the present embodiment, the Ni film 30 is in contact with two or more recesses 11D in any longitudinal section perpendicular to the first surface 11 of the insulating substrate 10 and the side surface 22 of the wiring conductor 20. By contacting the two or more recesses 11D, a high bonding strength between the Ni film 30 and the insulating substrate 10 can be obtained, and the Ni film 30 can be further suppressed from peeling off from the hem portion.

[0065] Furthermore, according to the wiring substrate 1 of the present embodiment, among the plurality of recesses 11D in contact with the Ni film 30, when each recess 11D is regarded as a granular shape, a composite recess 11DW having a shape in which the plurality of recesses 11D overlap is included. The composite recess 11DW increases the contact area with the Ni film 30 via the Ti oxide 13, thereby obtaining a high bonding strength between the Ni film 30 and the insulating substrate 10, and further suppressing the Ni film 30 from peeling off from the hem portion.

[0066] Furthermore, according to the wiring substrate 1 of the present embodiment, the intermediate layer 16a having a concentration gradient of Cu, Al, and N is included at the interface between the insulating substrate 10 and the wiring conductor 20. By including the intermediate layer 16a, stress at the interface caused by thermal expansion becomes gentle, and interface damage between the insulating substrate 10 and the wiring conductor 20 caused by thermal expansion can be suppressed.

[0067] Furthermore, according to the wiring substrate 1 of the present embodiment, the intermediate layer 16b having a concentration gradient of Cu, Al, and N is included at the interface between the Ni film 30 and the recessed portion 11D. Since the linear expansion coefficients of Cu and Ni are close, the stress caused by thermal expansion at the interface becomes gentle by including the intermediate layer 16b. Therefore, the interface damage between the insulating substrate 10 and the Ni film 30 caused by thermal expansion can be suppressed. Therefore, the peeling of the hem portion of the Ni film 30 can be further suppressed.

[0068] According to the electronic device 60 and the electronic module 100 of the present embodiment, by mounting the wiring substrate 1 in which the peeling of the Ni film 30 is suppressed, it is possible to improve the reliability.

[0069] The embodiments of the present disclosure have been described above. However, the present invention is not limited to the above-mentioned embodiments. For example, in the above-mentioned embodiments, an example is shown for the size and density of the recessed portion 11D on the insulating substrate 10, but it is not limited to these sizes and densities. In addition, in the above-mentioned embodiments, a structure is shown in which the Ni film 30 covers the entire area of ​​the upper surface and the side surface of the wiring conductor 20, but a part may not be covered. In addition, in the above-mentioned embodiments, a structure is shown in which the Ni film 30 has a protrusion 31, but there may not be a shape corresponding to the protrusion 31. In addition, in the above-mentioned embodiments, an example is shown for the manufacturing method of the wiring substrate 1, but the wiring substrate 1 may also be manufactured by other manufacturing methods. In addition, the details shown in the embodiments can be appropriately changed without departing from the scope of the main purpose of the invention.

[0070] Industrial Applicability

[0071] The present disclosure can be utilized in a wiring substrate, an electronic device, and an electronic module.

Claims

1. A wiring substrate comprising: An insulating substrate including AlN, having a first surface and a second surface opposite to the first surface; A conductor including Cu, located on the first surface; and A Ni film is provided over the upper surface, the side surface and the first surface of the conductor, The wiring substrate further includes a plurality of Ti oxides dispersed on the first surface. The Ni film has a portion in contact with the Ti oxide.

2. The wiring substrate according to claim 1, wherein: The Ni film has a protrusion protruding along the first surface toward a side opposite to the conductor. The protrusion is in contact with the first surface.

3. The wiring substrate according to claim 2, wherein: The protrusion protrudes beyond at least one of the Ti oxides in contact with the Ni film.

4. The wiring substrate according to claim 2 or 3, wherein: The outer edge of the protruding portion on the protruding side has a plurality of peaks and a plurality of valleys when viewed from a direction perpendicular to the first surface.

5. The wiring substrate according to any one of claims 1 to 3, wherein: The plurality of Ti oxides in contact with the Ni film are arranged along a side surface of the conductor.

6. The wiring substrate according to any one of claims 1 to 3, wherein: The plurality of Ti oxides in contact with the Ni film surround the conductor.

7. The wiring substrate according to any one of claims 1 to 3, wherein: In at least one cross section perpendicular to the first surface and the side surface, the Ni film is in contact with two or more of the Ti oxides.

8. The wiring substrate according to any one of claims 1 to 3, wherein: The first surface has a plurality of recessed portions, The plurality of recesses include recesses in which two or more grains overlap.

9. The wiring substrate according to any one of claims 1 to 3, wherein: An intermediate layer is included between the insulating substrate and the conductor, and the intermediate layer has a concentration gradient in which the concentration of Cu increases as it is closer to the conductor and the concentrations of Al and N decrease as they are closer to the conductor.

10. The wiring substrate according to any one of claims 1 to 3, wherein: An intermediate layer is included between the Ni film and the first surface, and the intermediate layer has a concentration gradient in which the concentration of Cu increases as it is closer to the Ni film and the concentrations of Al and N decrease as they are closer to the Ni film.

11. An electronic device comprising: The wiring substrate according to any one of claims 1 to 10; and The electronic components are mounted on the wiring substrate.

12. An electronic module comprising: The electronic device of claim 11; and The module substrate is equipped with the electronic device.