High air stability inorganic sulfide solid electrolytes, their preparation methods and applications
By replacing the phosphorus element with antimony element in the inorganic sulfide electrolyte, a solid solution phase structure is formed, which solves the instability problem of the electrolyte under air conditions, achieves high air stability and high lithium ion conductivity, and is suitable for all-solid-state applications. Lithium battery.
Patent Information
- Application Number
- CN201980093980.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-04-30
- Filing Date
- 2019-12-06
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2039-12-06
AI Technical Summary
Existing inorganic sulfide electrolytes are unstable under air conditions, resulting in structural changes and reduced ionic conductivity, limiting their application in all-solid-state lithium batteries.
By partially or completely replacing the phosphorus element with antimony element in the sulfide electrolyte, an inorganic sulfide electrolyte material with a solid solution phase structure is formed, thereby improving its air stability and lithium ion conductivity.
The obtained material has higher stability and ionic conductivity in the air, simplifies the production process of all-solid-state lithium batteries, reduces production costs, and maintains good performance in dry environments.
Smart Images

Figure CN113614971B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application No. 201910358953.8, filed on April 30, 2019, entitled “High air stability inorganic sulfide solid electrolyte and its preparation method and application”, which is incorporated into the present disclosure in its entirety by reference. Technical Field
[0003] The present disclosure belongs to the technical field of lithium-ion batteries, and particularly relates to a method for improving the air stability of an inorganic sulfide solid electrolyte, the obtained material, and its application in all-solid-state lithium secondary batteries. Background Art
[0004] Since its commercialization in the early 1990s, lithium-ion secondary batteries have developed rapidly due to their advantages such as high energy density and long service life. However, the lithium-ion batteries commonly used at present are liquid-phase batteries, which contain flammable organic electrolytes and therefore pose serious safety hazards. In recent years, the frequent occurrence of safety accidents in liquid-phase lithium-ion power batteries has greatly restricted the further use of this system. The use of non-flammable inorganic solid materials as electrolytes for lithium-ion batteries can not only eliminate the safety hazards caused by leakage of organic electrolytes and thermal runaway inside the battery during the use of the battery, but also can be used under extreme conditions such as high and low temperatures. Further enhance the value of lithium secondary batteries and expand their application areas. Therefore, the research and development of inorganic solid electrolytes with high stability and high lithium ion conductivity is a key content in the development of lithium secondary batteries with high safety.
[0005] According to the type of negative ions in inorganic solid electrolyte materials, oxide solid electrolytes and sulfide solid electrolytes are currently the most studied and have the greatest application potential (Kerman K, Luntz A, Viswanathan V, et al. Practical challenges hindering the development of solid state Li ion batteries [J]. Journal of The Electrochemical Society, 2017, 164 (7): A1731-A1744.). Oxide solid electrolytes are mainly based on Li2O-LaO-ZrO2, Li2O-B2O3, Li2O-LiCl and other systems (Thangadurai V, Narayanan S, Pinzaru D. Garnet-type solid-state fast Li ion conductors for Li batteries: critical review [J]. Chemical Society Reviews, 2014, 43 (13): 4714-4727), but generally have low ion conductivity. Compared with oxide electrolytes, the electronegativity of sulfur ions in sulfide electrolytes is smaller, so the binding force on cations is lower; at the same time, the radius of sulfur ions is larger, which is conducive to the migration of lithium ions. Therefore, the ion conductivity of sulfide electrolytes is higher than that of oxides. For example, the Li 10 GeP2S 12 Materials (room temperature ion conductivity up to 12 mS cm -1 ,Kamaya N,Homma K,Yamakawa Y,et al.A lithium superionic conductor[J].Nature materials,2011,10(9):682) and the Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 (Room temperature ion conductivity up to 25 mS cm -1, Kato Y, Hori S, Saito T et al. High-power all-solid-state batteries using sulfide superionic conductors [J]. Nature Energy, 2016, 1 (4): 16030) materials, whose lithium ion conductivity is higher than that of organic electrolytes. At present, the research on inorganic sulfide electrolytes mainly focuses on Li2S-P2S5, Li2S-MS x -P2S5 and Li2S-P2S5-LiX systems (Sun C, Liu J, GongY, et al. Recent advances in all-solid-state rechargeable lithium batteries[J]. Nano Energy, 2017, 33: 363-386).
[0006] However, the inorganic sulfide electrolytes containing P elements reported so far are unstable under air conditions. This type of sulfide electrolyte undergoes irreversible chemical reactions with oxygen, water vapor, carbon dioxide, etc. in the air atmosphere, resulting in structural changes and a decrease in ionic conductivity, which seriously restricts its application in all-solid-state lithium batteries. In response to this problem, a large amount of research has focused on improving it by introducing additives and surface protective layers. For example, a composite solid electrolyte material has an inner layer of a sulfide electrolyte material and an outer shell of a protective layer such as lithium borate (Yang Rong et al., Chinese Patent CN106887638A). In addition, doping a small amount of low-valent metal elements or a small amount of oxide LMO (M = Si, P, Ge, B, Al, Ga, In) into the sulfide electrolyte system can improve the thermal / air stability of the material (Xu Xiaoxiong, Qiu Zhijun, Huang Zhen, Chen Wanchao, Chen Xiaotian, Chinese Patent, CN10353184A; Bachman JC, Muy S, Grimaud A, et al. Inorganic solid-state electrolytes for lithium batteries: mechanisms and properties governing ion conduction [J]. Chemical reviews, 2015, 116 (1): 140-162.). From a theoretical analysis, by adjusting the lithium ion migration channel in the sulfide electrolyte material and the binding force of sulfur ions on cations through the structure of the solid solution phase, the ionic conductivity of the material can be controlled, thereby obtaining an inorganic sulfide electrolyte material with higher ionic conductivity. Furthermore, the structure of the solid solution phase can also change its electronic structure to improve its chemical properties, thereby achieving better stability in the air and enabling large-scale use in air environments / dry rooms. Summary of the Invention
[0007] The present invention aims to provide a method for improving the air stability of inorganic sulfide electrolytes and the application of the resulting material in all-solid-state lithium secondary batteries. This method is simple and effective, and the resulting material is easy to prepare and has low production costs. It also exhibits good air stability and high lithium ion conductivity, potentially addressing the practical application of inorganic sulfide electrolytes as electrolytes for high-performance all-solid-state lithium secondary batteries.
[0008] This study reveals that replacing some or all of the phosphorus in a sulfide electrolyte with Sb can form an inorganic sulfide solid electrolyte material with a solid-solution phase structure, resulting in higher air stability and higher ion mobility. In particular, increasing the amount of Sb substitution in the inorganic sulfide solid electrolyte increases the resulting material's air stability, making it suitable for use in all-solid-state lithium secondary batteries.
[0009] Specifically, the present disclosure provides an inorganic sulfide electrolyte material as shown in the following formula (I): Li 10 M(P 1- a Sb a )2S 12 , (I);
[0010] Wherein, M is one or more of Ge, Si, and Sn, 0.01≤a≤1; preferably, 0.01≤a≤0.2. For example, a can be selected from 0.01, 0.025, 0.05, 0.075, 0.1, 0.125, 0.15, 0.2, 0.3, 0.4, or 1.
[0011] Specifically, the inorganic sulfide electrolyte material represented by formula (I) is Li 10 Ge(P 0.99 Sb 0.01 )2S 12 、Li 10 Ge(P 0.975 Sb 0.025 )2S 12 、Li 10 Ge(P 0.925 Sb 0.075 )2S 12 、Li 10 Ge(P 0.9 Sb 0.1 )2S 12 、Li 10 Ge(P 0.875 Sb 0.125 )2S 12 、Li 10 Sn(P 0.95 Sb 0.05 )2S 12 or Li 10 Si(P 0.95 Sb 0.05 )2S 12 .
[0012] The present disclosure also provides an inorganic sulfide electrolyte material represented by the following formula (II):
[0013] Li6(P 1-a Sb a )S5X, (II);
[0014] wherein X is one or more of F, Cl, Br, and I, and 0.01≤a≤1; preferably, 0.025≤a≤0.2. For example, a can be selected from 0.025, 0.05, 0.075, 0.1, 0.15, 0.2, 0.5, or 1.
[0015] Specifically, the inorganic sulfide electrolyte material represented by formula (II) is Li6(P 0.975 Sb 0.025 )S5Cl or Li6(P 0.95 Sb 0.05 )S5Cl.
[0016] The present disclosure also provides an inorganic sulfide electrolyte material represented by the following formula (III):
[0017] Li3(P 1-a Sb a )S4, (III);
[0018] wherein 0.01≤a≤1; preferably, 0.05≤a≤0.3; further preferably, a is selected from 0.05, 0.1, 0.2 or 0.3.
[0019] The inorganic sulfide electrolyte materials disclosed herein can be prepared according to conventional techniques in the art.
[0020] For example, the required raw materials can be mixed according to a specific ratio, ground, and then heat-treated to obtain the sulfide electrolyte material represented by the above formulas (I), (II), and (III). The grinding time is preferably greater than 3 hours; and / or the heat treatment temperature is preferably greater than 300°C and less than 600°C; and / or the heat treatment temperature is preferably greater than 230°C and less than 600°C. The present disclosure relates to a solid solution phase sulfide solid electrolyte material.
[0021] Further research has revealed that increasing the amount of Sb in the solid solution phase of any of the aforementioned sulfide solid electrolyte materials improves air stability. Furthermore, by adjusting the ratio of P and Sb in the solid solution, the lithium ion conductivity of the material can be further adjusted, exceeding the conductivity of other existing solid electrolytes and organic liquid electrolytes.
[0022] Furthermore, any of the above-mentioned sulfide solid electrolyte materials is crystalline, amorphous, or a crystalline-amorphous composite type.
[0023] Furthermore, the operating temperature of any of the above sulfide solid electrolyte materials is between -100 and 300°C.
[0024] The present disclosure also provides a use of any of the above-mentioned sulfide solid electrolyte materials in preparing an all-solid-state lithium secondary battery.
[0025] Specifically, the present disclosure provides an all-solid-state lithium secondary battery, comprising a positive electrode, an electrolyte material and a negative electrode, wherein the electrolyte material is the sulfide electrolyte material described in the above scheme or the sulfide electrolyte material prepared by the above scheme.
[0026] The present disclosure uses Sb to replace part or all of the P element in the sulfide electrolyte to form an inorganic sulfide solid electrolyte material with a solid solution phase structure, thereby obtaining a material with higher air stability and higher ion mobility. Compared with the prior art, the present disclosure provides a new method for improving the air stability of sulfides based on element substitution. The method is simple and effective, and the obtained sulfide electrolyte can be stably stored under air conditions without any coating layer or additive protection. This type of material is simple to prepare and has low production costs. At the same time, the obtained inorganic sulfide solid electrolyte material has controllable ion conductivity and has excellent performance when used as an inorganic electrolyte and electrode material additive in all-solid-state lithium batteries.
[0027] The present disclosure has the following advantages:
[0028] 1) By adjusting the ratio of P and Sb in the inorganic sulfide solid electrolyte material, various types of sulfide solid electrolytes with solid solution phase structures are obtained. Increasing the amount of Sb substitution improves the air stability of the resulting inorganic sulfide solid electrolyte material, further enabling the use of the sulfide solid electrolyte material in dry rooms, simplifying the solid-state battery production process and reducing production costs.
[0029] 2) In sulfide solid electrolytes with a solid solution phase structure, the partial substitution of Sb for P can adjust the chemical properties of the material, thereby achieving high chemical stability and compatibility with electrode materials. This reduces the reactivity between the electrolyte and lithium metal and common lithium-ion positive and negative electrode materials.
[0030] 3) By adjusting the ratio of P and Sb in the inorganic sulfide solid electrolyte material, the material's crystal structure and electronic structure can be easily adjusted, further improving the material's electrical conductivity. In some proportions of this type of solid solution phase inorganic sulfide solid electrolyte material, the conductivity reaches or even exceeds that of existing sulfide solid electrolytes.
[0031] 4) The proposal and acquisition of sulfide solid electrolytes with solid solution phase structure will help further understand the chemical stability of electrolytes and the migration of lithium ions in solid electrolytes in theoretical research, and further guide the development and research of high-conductivity sulfide electrolytes; in practical applications, many different types of high-conductivity and high-air-stability electrolyte materials can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is the X-ray diffraction pattern obtained when a=0.01 in Example 1;
[0033] Figure 2 is a partial X-ray diffraction pattern obtained for the system in Example 1;
[0034] Figure 3 The electrochemical impedance spectroscopy diagram and ionic conductivity diagram at different temperatures obtained when a=0.01 in Example 1 are shown;
[0035] Figure 4 is a graph showing the relationship between the ionic conductivity of the material obtained in Example 1 and the a value;
[0036] Figure 5 is the X-ray diffraction pattern obtained when a=0.025 in Example 2;
[0037] Figure 6 is a partial X-ray diffraction pattern obtained for the system in Example 2;
[0038] Figure 7 The electrochemical impedance spectroscopy diagram and ionic conductivity diagram at different temperatures obtained when a=0.025 in Example 2 are shown;
[0039] Figure 8 is a graph showing the relationship between the ionic conductivity of the material obtained in Example 2 and the a value;
[0040] Figure 9 is the X-ray diffraction pattern obtained when a=0.05 in Example 3;
[0041] Figure 10 The electrochemical impedance spectroscopy diagram and ionic conductivity diagram at different temperatures obtained when a=0.05 in Example 3 are shown;
[0042] Figure 11 is the X-ray diffraction pattern obtained when a=0.05 in Example 4;
[0043] Figure 12 The electrochemical impedance spectroscopy diagram and ionic conductivity diagram at different temperatures obtained when a=0.05 in Example 4 are shown;
[0044] Figure 13 The electrochemical impedance spectroscopy diagram and ionic conductivity diagram at different temperatures obtained when a=0.1 in Example 5 are shown;
[0045] Figure 14 It is Li6(P in Application Example 1 0.975 Sb 0.025 ) XRD comparison of S5Cl material before and after exposure to air;
[0046] Figure 15It is Li6(P in Application Example 1 0.9 Sb 0.1 ) XRD comparison of S5Cl material before and after exposure to air;
[0047] Figure 16 It is Li6(P in Application Example 1 0.975 Sb 0.025 ) Electrochemical impedance spectroscopy of S5Cl material before and after exposure to air and the calculated ionic conductivity comparison diagram;
[0048] Figure 17 It is Li6(P in Application Example 1 0.9 Sb 0.1 ) Electrochemical impedance spectroscopy of S5Cl material before and after exposure to air and the calculated ionic conductivity comparison diagram;
[0049] Figure 18 It is Li6(P in Application Example 1 0.975 Sb 0.025 )S5Cl and Li6(P 0.9 Sb 0.1 ) Temperature-dependent ionic conductivity of S5Cl material and current-time relationship at a constant external voltage of 0.3 V;
[0050] Figure 19 Li in Application Example 2 10 Ge(P 0.875 Sb 0.125 )2S 12 XRD comparison of the material before and after exposure to air;
[0051] Figure 20 Li in Application Example 2 10 Ge(P 0.975 Sb 0.025 )2S 12 、Li 10 Ge(P 0.925 Sb 0.075 )2S 12 、Li 10 Ge(P 0.9 Sb 0.1 )2S 12 He Li 10 Ge(P 0.875 Sb 0.125 )2S 12 Comparison of changes in ionic conductivity of solid electrolyte materials before and after exposure to air;
[0052] Figure 21 The solid solution phase Li is obtained in Example 3. 10 Ge(P 0.99 Sb 0.01 )2S12 Charge and discharge curves of solid electrolyte materials used in all-solid-state Li-LiCoO2 secondary batteries. DETAILED DESCRIPTION
[0053] The following examples are provided to illustrate the present disclosure but are not intended to limit the scope of the present disclosure. Where specific techniques or conditions are not specified in the examples, the experiments were performed according to those described in literature in the art or according to the product instructions. Reagents or instruments used, where the manufacturer is not specified, are conventional products available through regular channels.
[0054] Example 1 Preparation of Li 10 Ge(P 1-a Sb a )2S 12 Solid electrolyte material (0.01≤a≤1)
[0055] Grind and mix 15 mmol of Li2S (0.69 g), 3 mmol of GeS2 (0.411 g), (3-3a) mmol of P2S5, and 3a mmol of Sb2S5 powder in a mortar, where 0.01 ≤ a ≤ 1. For a = 0.01, the raw material ratios are as follows: Li2S: 0.69 g, GeS2: 0.411 g, P2S5: 0.66 g, and Sb2S5: 0.012 g. For a = 0.1, the raw material ratios are as follows: Li2S: 0.69 g, GeS2: 0.411 g, P2S5: 0.599 g, and Sb2S5: 0.121 g. And so on. After grinding and mixing, place the mixture in a 50 ml zirconia ball mill and mill at 400 rpm for 12 hours. The ball-milled sample was pressed into discs using a powder press at 100 MPa, and then sealed in a vacuum quartz tube for calcination. The calcination temperature was controlled by programmed temperature rise, from room temperature to 550 degrees Celsius over 4 hours, and maintained at this temperature for 4 hours, and then cooled to 50 degrees Celsius over 4 hours to obtain Li 10 Ge(P 1-a Sb a )2S 12 Solid electrolyte material (0.01≤a≤1).
[0056] Figure 1 When a=0.01, the system material (i.e. Li 10 Ge(P 0.99 Sb 0.01 )2S 12 solid electrolyte materials) and Li 10 GeP2S 12 X-ray diffraction pattern of the standard card (JPCDF:04-020-5216); Figure 2These are the X-ray diffraction patterns obtained for different a values in this system, where a is 0.01, 0.025, 0.05, 0.075, 0.1, 0.125, 0.15, 0.2, 0.3, 0.4 and 1 from top to bottom. Figure 3 When a=0.01, the system material (i.e. Li 10 Ge(P 0.99 Sb 0.01 )2S 12 Solid electrolyte material) electrochemical impedance diagram at different temperatures and ion conductivity curve with temperature. Figure 3 It can be obtained that the ionic conductivity of the material is 11.4 millisiemens per centimeter at 25 degrees Celsius and the activation energy is 11.0 kilojoules per mole. Figure 4 The graph is the relationship between the ion conductivity and a value of the solid solution phase sulfide electrolyte material obtained under this system. Figure 4 It was found that when the value of a is 0.075 (i.e. Li 10 Ge(P 0.925 Sb 0.075 )2S 12 Solid electrolyte material), the system material has the highest room temperature ion conductivity, which is 17.5 millisiemens per centimeter, which is higher than the Li 10 GeP2S 12 The material's room-temperature ion conductivity is even higher (12 millisiemens per centimeter).
[0057] Example 2 Preparation of Li6(P 1-a Sb a )S5Cl solid electrolyte material (0.01≤a≤1)
[0058] 20 mmol of Li2S (0.92 g), 8 mmol of LiCl (0.336 g), (4-4a) mmol of P2S5, and 4a mmol of Sb2S5 powders were ground and mixed in a mortar, where 0.01 ≤ a ≤ 1. For a = 0.025, the raw material ratios were as follows: Li2S: 0.92 g, LiCl: 0.336 g, P2S5: 0.866 g, and Sb2S5: 0.03 g. For a = 0.1, the raw material ratios were as follows: Li2S: 0.92 g, LiCl: 0.336 g, P2S5: 0.799 g, and Sb2S5: 0.121 g. And so on. After grinding and mixing, the mixture was placed in a 50 ml zirconia ball mill and ball milled at 400 rpm for 12 hours. The ball-milled sample was pressed into discs using a powder press at 100 MPa, and then sealed in a vacuum quartz tube for calcination. The calcination temperature was controlled by programmed temperature rise, from room temperature to 550 degrees Celsius over 4 hours, and maintained at this temperature for 5 hours, and then naturally cooled to 50 degrees Celsius to obtain Li6(P1-a Sb a )S5Cl solid electrolyte material (0.01≤a≤1).
[0059] Figure 5 When a=0.025, the system material (i.e. Li6(P 0.975 Sb 0.025 )S5Cl solid electrolyte material) and Li6PS5Cl standard card (JPCDF: 04-018-1429); Figure 6 These are the X-ray diffraction patterns obtained for different a values in this system, where a is 0.025, 0.05, 0.075, 0.1, 0.15, 0.2, 0.5 and 1 from top to bottom. Figure 7 When a=0.025, the system material (i.e. Li6(P 0.975 Sb 0.025 )S5Cl solid electrolyte material) electrochemical impedance spectroscopy at different temperatures and ion conductivity curves with temperature. Figure 7 It can be obtained that the ionic conductivity of the material is 2.5 millisiemens per centimeter at 25 degrees Celsius and the activation energy is 18.4 kilojoules per mole. Figure 8 The graph is the relationship between the ion conductivity and a value of the solid solution phase sulfide electrolyte material obtained under this system. Figure 8 It was found that when the a value is 0.05 (i.e. Li6(P 0.95 Sb 0.05 )S5Cl solid electrolyte material), this system material has the highest room temperature ion conductivity of 2.9 millisiemens per centimeter, which is higher than the room temperature ion conductivity (1.3 millisiemens per centimeter) of the non-solid solution phase Li6PS5Cl material obtained under the same conditions.
[0060] Example 3 Preparation of Li 10 Sn(P 0.95 Sb 0.05 )2S 12 Solid electrolyte materials
[0061] 15 mmoles of Li2S (0.69 g), 3 mmoles of SnS2 (0.549 g), 2.85 mmoles of P2S5 (0.633 g), and 0.15 mmoles of Sb2S5 (0.061 g) powders were ground and mixed in a mortar. After grinding and mixing, they were placed in a 50 ml zirconia ball mill for ball milling at a speed of 400 rpm for 12 hours. The ball-milled sample was pressed into discs using a powder tablet press at 100 MPa, and then sealed in a vacuum quartz tube for calcination. The calcination temperature was controlled by programmed temperature rise, rising from room temperature to 550 degrees Celsius over 4 hours, and maintained at this temperature for 4 hours, and then cooled to 50 degrees Celsius over 4 hours to obtain Li10 Sn(P 0.95 Sb 0.05 )2S 12 Solid electrolyte materials.
[0062] Figure 9 For Li 10 Sn(P 0.95 Sb 0.05 )2S 12 X-ray diffraction patterns of solid electrolyte materials; Figure 10 The electrochemical impedance spectroscopy diagram of the solid electrolyte material at different temperatures and the ion conductivity curve with temperature are shown in Figure 2. Figure 10 It can be obtained that the ion conductivity of the material is 5.6 millisiemens per centimeter at 25 degrees Celsius and the activation energy is 11.6 kilojoules per mole. Figure 10 It was found that the Li 10 Sn(P 0.95 Sb 0.05 )2S 12 Solid electrolyte materials have high room temperature ion conductivity, which is consistent with the reported Li 10 SnP2S 12 The material's room-temperature ion conductivity (6.3 millisiemens per centimeter) is relatively low.
[0063] Example 4 Preparation of Li 10 Si(P 0.95 Sb 0.05 )2S 12 Solid electrolyte materials
[0064] 15 mmoles of Li2S (0.69 g), 3 mmoles of SiS2 (0.276 g), 2.85 mmoles of P2S5 (0.633 g), and 0.15 mmoles of Sb2S5 (0.061 g) powders were ground and mixed in a mortar. After grinding and mixing, they were placed in a 50 ml zirconia ball mill for ball milling at a speed of 400 rpm for 12 hours. The ball-milled sample was pressed into discs using a powder tablet press at 100 MPa, and then sealed in a vacuum quartz tube for calcination. The calcination temperature was controlled by programmed temperature rise, rising from room temperature to 550 degrees Celsius over 4 hours, and maintained at this temperature for 4 hours, and then cooled to 50 degrees Celsius over 4 hours to obtain Li 10 Si(P 0.95 Sb 0.05 )2S 12 Solid electrolyte materials.
[0065] Figure 11 For Li 10 Si(P 0.95 Sb 0.05 )2S 12X-ray diffraction patterns of solid electrolyte materials; Figure 12 The electrochemical impedance spectroscopy diagram of the solid electrolyte material at different temperatures and the ion conductivity curve with temperature are shown in Figure 2. Figure 12 It can be obtained that the ion conductivity of the material is 2.5 millisiemens per centimeter at 25 degrees Celsius and the activation energy is 11.6 kilojoules per mole. Figure 12 It was found that the Li 10 Si(P 0.95 Sb 0.05 )2S 12 Solid electrolyte materials have high room temperature ion conductivity, which is consistent with the reported Li 10 SiP2S 12 The material's room-temperature ion conductivity is even higher (2 millisiemens per centimeter).
[0066] Example 5 Preparation of Li3(P 1-a Sb a )S4 solid electrolyte material (0.01≤a≤1)
[0067] 9 mmol of Li2S (0.414 g), (3-3a) mmol of P2S5, and 3a mmol of Sb2S5 powders were ground and mixed in a mortar, where 0.01 ≤ a ≤ 1. For a = 0.05, the raw material ratios were as follows: 0.414 g of Li2S, 0.633 g of P2S5, and 0.061 g of Sb2S5. For a = 0.1, the raw material ratios were as follows: 0.414 g of Li2S, 0.599 g of P2S5, and 0.121 g of Sb2S5. The same formula was used for the above. After grinding and mixing, the mixture was placed in a 50 ml zirconia ball mill and ball-milled at 400 rpm for 12 hours. The milled sample was pressed into discs using a powder press at 100 MPa and then sealed in a vacuum quartz tube for calcination. The calcination temperature was controlled by programmed temperature rise, which was raised from room temperature to 260 degrees Celsius over 3 hours, maintained at this temperature for 4 hours, and then cooled to 50 degrees Celsius over 4 hours to obtain Li3(P 1-a Sb a )S4 solid electrolyte material (0.01≤a≤1).
[0068] Figure 13 When a=0.1, the system material (i.e. Li3(P 0.9 Sb 0.1 )S4 solid electrolyte material) electrochemical impedance spectroscopy at different temperatures and ion conductivity curves with temperature. Figure 13 It can be obtained that the ionic conductivity of the material is 0.06 millisiemens per centimeter at 25 degrees Celsius and the activation energy is 16.0 kilojoules per mole.
[0069] Application Example 1Li6(P1-a Sb a Air Stability Test and Application of S5Cl Solid Electrolyte Materials
[0070] The Li6(P 1-a Sb a )S5Cl solid electrolyte material was subjected to dry air stability test (a=0.025, 0.1). In the glove box, the Li6(P 0.975 Sb 0.025 )S5Cl and Li6(P 0.9 Sb 0.1 )100 mg of S5Cl solid electrolyte material was placed in a 1 ml open glass bottle, which was then placed in a reaction box with a dry air flow. It was allowed to stand at room temperature for 24 hours at a dry air flow of 100 ml per minute. After the standing period, the sample was taken out and tested for XRD, ion conductivity, and electron conductivity.
[0071] Figure 14 Li6(P 0.975 Sb 0.025 ) XRD comparison of S5Cl material before and after exposure to air; Figure 15 Li6(P 0.9 Sb 0.1 ) XRD comparison of S5Cl material before and after exposure to air; Figure 16 Li6(P 0.975 Sb 0.025 ) Electrochemical impedance spectroscopy of S5Cl material before and after exposure to air and the calculated ionic conductivity comparison diagram; Figure 17 Li6(P 0.9 Sb 0.1 ) Electrochemical impedance spectroscopy of S5Cl material before and after exposure to air and the calculated ionic conductivity comparison diagram; Figure 18 The graphs of the ion conduction of the two materials changing with temperature and the current-time relationship at a constant external voltage of 0.3V are shown in the graphs above. 0.975 Sb 0.025 ) After the S5Cl material was exposed to air, the XRD change was not significant, but the ion conductivity decreased significantly. After 24 hours of exposure to air, the ion conductivity of the material decreased from 2.5×10 -3 S cm -1 Reduced to 1.0×10 -5 S cm -1 After being exposed to air, the ion conductivity of the material is only 0.004 times that of the material without air. As the Sb content in the solid solution phase increases to 10% (a = 0.1), the obtained Li6 (P 0.9 Sb 0.1) The air stability of S5Cl solid electrolyte material is improved. Similarly, after 24 hours of exposure to air atmosphere, the XRD pattern of the material did not change much, and the ion conductivity increased from 1.9×10 -3 S cm -1 Reduced to 2.3×10 -4 S cm -1 After exposure to air, the ion conductivity of the material was 0.12 times that of the material without air. In addition, the electronic conductivity of the above two materials did not change much.
[0072] Application Example 2Li 10 Ge(P 1-a Sb a )2S 12 Air stability testing and application of solid electrolyte materials
[0073] The Li obtained in Example 1 was used 10 Ge(P 1-a Sb a )2S 12 Solid electrolyte materials were subjected to dry air stability tests (a = 0.025, 0.075, 0.1, 0.125). In the glove box, the Li 10 Ge(P 0.975 Sb 0.025 )2S 12 、Li 10 Ge(P 0.925 Sb 0.075 )2S 12 、Li 10 Ge(P 0.9 Sb 0.1 )2S 12 He Li 10 Ge(P 0.875 Sb 0.125 )2S 12 200 mg of solid electrolyte material was placed in a 1 ml open glass bottle, which was then placed in a reaction box with a dry air flow. The reaction box was left standing at room temperature for 24 hours at a dry air flow of 100 ml per minute. After the standing period, the sample was taken out and tested for XRD, ion conductivity, and electron conductivity. Figure 19 For Li 10 Ge(P 0.875 Sb 0.125 )2S 12 XRD comparison of the material before and after exposure to air; Figure 20 The comparison of the ion conduction changes of these four materials before and after exposure to air is shown in the figure above. 10 Ge(P 0.875 Sb 0.125 )2S12 After 24 hours of exposure to air, the XRD changes were not significant. Similarly, the ion conductivities of the four materials obtained above did not change much before and after air exposure. After 24 hours of air exposure, the ion conductivities of the four materials above were still able to reach 10 mS cm. -2 The above results indicate that the material has good air stability and can be used directly in a dry air atmosphere, which has great application value.
[0074] Application Example 3Li 10 Ge(P 0.99 Sb 0.01 )2S 12 Application of electrolyte materials in all-solid-state Li-LiCoO2 secondary batteries
[0075] The Li obtained in Example 1 was used 10 Ge(P 0.99 Sb 0.01 )2S 12 The electrolyte material is used in all-solid-state Li-LiCoO2 secondary batteries. The LiCoO2 cathode material is first coated with LiNbO2 on the surface through atomic layer deposition (ALD) technology. The coating layer is about 10 nanometers. 10 Ge(P 0.99 Sb 0.01 )2S 12 Electrolyte material: acetylene carbon is mixed in a ratio of 60:30:10 (mass ratio). The mixing process is carried out in a glove box. The specific process is to use a mortar to grind for 20 minutes. The ground material is used as the positive electrode powder. The metal thin indium sheet is used as the negative electrode, and the electrolyte is also the Li obtained in Example 1. 10 Ge(P 0.99 Sb 0.01 )2S 12 Electrolyte material. Take 100 mg Li 10 Ge(P 0.99 Sb 0.01 )2S 12 The electrolyte material is placed in a molded battery liner with a cross-sectional area of 0.785 square centimeters and pressed at a pressure of 200 MPa to obtain the electrolyte layer. Subsequently, 10 mg of positive electrode powder is added to one side of the electrolyte layer, spread evenly, and pressed a second time at a pressure of 350 MPa to press the positive electrode layer and the electrolyte layer together. An indium sheet is then placed on the other side as the negative electrode layer. After the entire process is completed, the liner is placed in the molded battery, pressed and tightened to seal it. After sealing, a fully solid-state Li-LiCoO2 secondary battery is obtained. The battery is charged and discharged using a current density of 32 microamperes, with a cut-off voltage of 2.0-3.6 volts. Figure 21This is the charge and discharge curve of the first two cycles of the battery. Figure 21 It can be found that the reversibility of the battery's charge and discharge process is good, and the battery capacity is maintained above 0.8 mAh. The first cycle capacity is 0.870 mAh, and the specific capacity is 145.0 mAh / g based on the mass of lithium cobalt oxide (6 mg). The first cycle discharge capacity is 0.707 mAh, and the specific capacity is 117.8 mAh / g based on the mass of lithium cobalt oxide (6 mg). The charge specific capacity and discharge specific capacity of the second cycle are 121.1 and 116.2 mAh / g, respectively. The reversibility of the battery cycle is good.
[0076] The above experimental results show that the inorganic sulfide electrolyte material provided by the present invention has good air stability, a simple preparation method, low production cost, good air stability and high lithium ion conductivity, and is expected to solve the practical application problem of inorganic sulfide electrolytes as high-performance all-solid-state lithium secondary battery electrolytes.
[0077] Although the present disclosure has been described in detail above using general descriptions and specific embodiments, it will be apparent to those skilled in the art that modifications or improvements may be made based on the present disclosure. Therefore, such modifications or improvements, which do not depart from the spirit of the present disclosure, are intended to be within the scope of protection claimed herein.
Claims
1. An inorganic sulfide electrolyte material represented by the following formula (II): Li6(P 1-a Sb a )S5X,(II); in, X is one or more of F, Cl, Br, and I, and 0.05≤a≤0.
5.
2. The inorganic sulfide electrolyte material according to claim 1, characterized in that 0.1≤a≤0.2。 3. The inorganic sulfide electrolyte material according to claim 1, characterized in that a is selected from 0.05, 0.075, 0.1, 0.15, 0.2 or 0.
5.
4. The inorganic sulfide electrolyte material according to claim 1, characterized in that The inorganic sulfide electrolyte material represented by formula (II) is Li6(P 0.975 Sb 0.025 )S5Cl or Li6(P 0.95 Sb 0.05 )S5Cl.
5. An inorganic sulfide electrolyte material represented by the following formula (III): Li3(P 1-a Sb a )S4,(III); in, 0.01≤a<1。 6. The inorganic sulfide electrolyte material according to claim 5, characterized in that 0.05≤a≤0.3。 7. The inorganic sulfide electrolyte material according to claim 5, characterized in that a is selected from 0.05, 0.1, 0.2 or 0.
3.
8. The inorganic sulfide electrolyte material according to any one of claims 1 to 7, characterized in that: It is crystalline, amorphous or a crystalline-amorphous composite; and / or, The working temperature of the inorganic sulfide electrolyte material is between -100 and 300°C.
9. The method for preparing the inorganic sulfide electrolyte material according to any one of claims 1 to 8, characterized in that: The required raw materials are mixed according to a ratio and then ground, and then heat-treated to obtain inorganic sulfide electrolyte materials represented by formula (II) and formula (III) respectively.
10. The preparation method according to claim 9, characterized in that: The grinding time is greater than 3 hours; and / or the heat treatment temperature is greater than 300°C and less than 600°C.
11. The preparation method according to claim 10, characterized in that: The grinding time is greater than 3 hours; and / or the heat treatment temperature is greater than 230°C and less than 600°C.
12. Use of the inorganic sulfide electrolyte material according to any one of claims 1 to 8 or the inorganic sulfide electrolyte material prepared by the method according to any one of claims 9 to 11 in preparing an all-solid-state lithium secondary battery.
13. An all-solid-state lithium secondary battery, characterized in that: It comprises a positive electrode, an electrolyte material and a negative electrode, wherein the electrolyte material is the inorganic sulfide electrolyte material according to any one of claims 1 to 8 or the inorganic sulfide electrolyte material prepared by the method according to any one of claims 9 to 11.
14. An all-solid-state lithium secondary battery, characterized in that: The invention comprises a positive electrode, an electrolyte material and a negative electrode, wherein the electrolyte material is an inorganic sulfide electrolyte material as shown in the following formula (I): Li 10 M(P 1-a Sp a )2S 12 ,(I); Wherein, M is one or more of Ge, Si, and Sn, and 0.01≤a<1.
15. The all-solid-state lithium secondary battery according to claim 14, characterized in that: 0.01≤a≤0.2。 16. The all-solid-state lithium secondary battery according to claim 14, characterized in that: a is selected from 0.01, 0.025, 0.05, 0.075, 0.1, 0.125, 0.15, 0.2, 0.3 or 0.
4.
17. The all-solid-state lithium secondary battery according to claim 14, characterized in that: The inorganic sulfide electrolyte material represented by formula (I) is Li 10 Ge(P 0.99 Sb 0.01 )2S 12 , Li 10 Ge(P 0.975 Sb 0.025 )2S 12 , Li 10 Ge(P 0.925 Sb 0.075 )2S 12 , Li 10 Ge(P 0.9 Sb 0.1 )2S 12 , Li 10 Ge(P 0.875 Sb 0.125 )2S 12 , Li 10 Sn(P 0.95 Sb 0.05 )2S 12 or Li 10 Si(P 0.95 Sb 0.05 )2S 12 .
18. The all-solid-state lithium secondary battery according to claim 14, characterized in that: The inorganic sulfide electrolyte material represented by formula (I) is crystalline, amorphous or crystalline-amorphous composite; and / or the working temperature of the inorganic sulfide electrolyte material is -100 to 300°C.
Citation Information
Cited By
Sulfide-based composite electrolyte with high air stability as well as preparation method and application of sulfide-based composite electrolyte
CN122224917A