Anti-glare film, polarizing plate and display device
By using a combination of inorganic and organic particles with specific particle sizes in the anti-glare film to form a hard coating with an irregular structure, the deficiencies in the anti-glare effect and physical properties of the existing anti-glare films are solved and excellent anti-glare properties are achieved. Performance and durability.
Patent Information
- Application Number
- CN202080021332.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-23
- Filing Date
- 2020-11-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-11-24
AI Technical Summary
Existing anti-glare films are ineffective at preventing flash defects caused by external light, rainbow phenomena, image formation and light expansion of lamps, and are insufficient in scratch resistance and stain resistance.
An anti-glare film including a light-transmitting substrate and a hard coating layer is used. The hard coating layer contains a first inorganic particle aggregate with an average particle diameter of 1 μm to 2 μm, a second inorganic particle aggregate of 3 μm to 5 μm, and a display layer of 1 μm to 10 μm. A combination of organic particles in the form of primary particles, achieving excellent anti-glare properties and physical properties through the irregular structure of these particles.
Significantly improves the anti-glare effect of the anti-glare film, preventing flash defects, rainbows, lamp image formation and light expansion, while improving scratch resistance and stain resistance.
Smart Images

Figure GDA0003262877570000181
Abstract
Description
Technical Field
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2019-0153705 filed on November 26, 2019 and Korean Patent Application No. 10-2020-0157960 filed on November 23, 2020, the entire contents of which are incorporated herein by reference.
[0003] The present disclosure relates to an anti-glare film, a polarizing plate including the same, and a display device. Background Art
[0004] As flat panel display technology develops toward large-area and high-resolution displays, application products are shifting from home and office applications such as TVs, monitors, and mobile devices to large displays such as outdoor billboards and electronic signs. If a flat panel display such as LCD, PDP, OLED, rear-projection TV is exposed to external light such as sunlight, the user feels his / her eyestrain or headache due to the light reflected from the surface, and thinks that the image produced in the display is unclear.
[0005] In order to solve this disadvantage, an anti-glare film is applied to scatter external light from the surface by forming irregularities on the surface of the display, or to cause internal scattering by utilizing the refractive index between the resin forming the coating film and the particles. Conventional anti-glare films applied to the surface of a display device or the like for this purpose have a problem that an image of external light (e.g., a lamp) is formed on the film or light spreading is caused by the external light. For this reason, an anti-glare film that not only has an anti-glare effect but also prevents the formation of an image on the display device or light spreading caused by the external light is required. Summary of the invention
[0006] Technical issues
[0007] According to the present disclosure, there is provided an excellent anti-glare film capable of preventing glitter defects, the occurrence of rainbows, image formation of lamps, and light spreading while having excellent anti-glare properties and excellent physical properties such as scratch resistance and stain resistance.
[0008] In addition, a polarizing plate and a display device are provided, which are capable of preventing glitter defects, the occurrence of rainbows, image formation of lamps, and light spreading while having excellent anti-glare characteristics and excellent physical properties such as scratch resistance and stain resistance.
[0009] Technical Solution
[0010] In the present disclosure, an anti-glare film is provided, which includes a light-transmitting substrate; and a hard coating layer comprising a binder resin and particles dispersed in the binder resin, wherein the particles include first inorganic particle aggregates with an average particle size of 1 μm to 2 μm; second inorganic particle aggregates with an average particle size of 3 μm to 5 μm; and organic particles in the form of primary particles with an average particle size of 1 μm to 10 μm.
[0011] Furthermore, a polarizing plate including the above anti-glare film is provided.
[0012] In the present disclosure, a display device including the above anti-glare film is also provided.
[0013] Hereinafter, an anti-glare film, a polarizing plate and a display device including the same according to specific embodiments of the present disclosure will be described in more detail.
[0014] In the present disclosure, the terms “first”, “second” and the like are used to describe a plurality of components, and these terms are used only to distinguish a certain component from other components.
[0015] Furthermore, (meth)acrylate includes both acrylate and methacrylate.
[0016] In addition, the photocurable resin generally refers to a polymer resin that is polymerized by light irradiation, for example, by visible light irradiation or ultraviolet light irradiation.
[0017] Furthermore, (co)polymers include both copolymers and homopolymers.
[0018] Furthermore, the inorganic particle aggregate refers to a secondary or tertiary particle in which two or more inorganic particles in the form of primary particles are aggregated.
[0019] According to the present disclosure, an anti-glare film can be provided, which includes a light-transmitting substrate; and a hard coating layer comprising a binder resin and particles dispersed in the binder resin, wherein the particles include first inorganic particle aggregates with an average particle size of 1 μm to 2 μm; second inorganic particle aggregates with an average particle size of 3 μm to 5 μm; and organic particles in the form of primary particles with an average particle size of 1 μm to 10 μm.
[0020] The inventors have determined that when a hard coating layer includes first inorganic particle aggregates having an average particle diameter of 1 to 2 μm, second inorganic particle aggregates having an average particle diameter of 3 to 5 μm, and organic particles in the form of primary particles having an average particle diameter of 1 to 10 μm, an anti-glare film including a light-transmitting substrate and a hard coating layer has excellent anti-glare properties while preventing flash defects, the appearance of rainbows, image formation of lamps, and light expansion, thereby exhibiting remarkably excellent visibility. And, the inventors have completed the present invention.
[0021] Specifically, in addition to the anti-glare property, the anti-glare film should also have excellent visibility even when external light is scattered. When the anti-glare film according to the present embodiment is illuminated by external light, such as a lamp, no lamp image is formed, so that the lamp image is not clearly recognized. In addition, light expansion hardly occurs, so that the eye does not easily recognize the afterimage of the lamp.
[0022] The hard coating layer included in the anti-glare film contains a binder resin and particles dispersed in the binder resin. In addition, the particles contained in the hard coating layer can be three or more types of particles, specifically, first inorganic particle aggregates with an average particle size of 1 μm to 2 μm, second inorganic particle aggregates with an average particle size of 3 μm to 5 μm, and organic particles in the form of primary particles with an average particle size of 1 μm to 10 μm.
[0023] In particular, the hard coat layer may include two types of inorganic particle aggregates having different average particle sizes, specifically, a first inorganic particle aggregate having an average particle size of 1 μm to 2 μm and a second inorganic particle aggregate having an average particle size of 3 μm to 5 μm. Due to the first inorganic particle aggregate and the second inorganic particle aggregate, fine irregularities may be formed on the surface of the hard coat layer. Specifically, fine irregularities may be formed on the surface of the hard coat layer facing the interface between the hard coat layer and the light-transmitting substrate, i.e., on the surface of the hard coat layer that is not in contact with the light-transmitting substrate.
[0024] Generally, a single organic particle or inorganic particle in the form of a primary particle protrudes from the surface of the hard coat layer to form irregularities. However, the first inorganic particle aggregate and the second inorganic particle aggregate contained in the hard coat layer are in the form of secondary particles formed by respectively aggregating a plurality of the first inorganic particles and the second inorganic particles in the form of primary particles. In particular, the first inorganic particle and the second inorganic particle are gathered in a plane in a horizontal or vertical direction relative to the hard coat layer to form the first inorganic particle aggregate and the second inorganic particle aggregate respectively. Therefore, the first inorganic particle aggregate and the second inorganic particle aggregate become convex portions on the surface of the hard coat layer, thereby forming fine irregularities on the surface of the hard coat layer. Due to the formation of the above-mentioned fine irregularities on the surface of the hard coat layer, it is possible to prevent flash defects, image formation of lamps and light expansion while showing excellent anti-glare properties.
[0025] In addition, the anti-glare film includes a hard coating layer, the hard coating layer includes two types of inorganic particle aggregates having different average particle sizes, specifically, a first inorganic particle aggregate having an average particle size of 1 μm to 2 μm and a second inorganic particle aggregate having an average particle size of 3 μm to 5 μm, thereby achieving excellent anti-glare visibility. When the hard coating layer includes only the first inorganic particle aggregate having a relatively small average particle size, a lamp image may be formed to cause glare. When the hard coating layer includes only the second inorganic particle aggregate having a relatively large average particle size, a lamp image is not formed, but the degree of light expansion is large, so that the lamp may be vaguely visible, and the visibility of the screen may be poor.
[0026] The first inorganic particle aggregates may have an average particle size of 1 to 2 μm, 1.1 to 1.9 μm, or 1.2 to 1.8 μm. In addition, the second inorganic particle aggregates may have an average particle size of 3 to 5 μm, 3.1 to 4.8 μm, or 3.2 to 4.5 μm.
[0027] The average particle diameter ratio of the second inorganic particle aggregate to the first inorganic particle aggregate can be 1.5 to 4 times, 2 to 3.5 times, or 2 to 3 times. When the ratio is less than 1.5 times, the size of the surface irregularity is reduced, and a lamp image is formed on the screen, causing glare. When the ratio exceeds 4 times, the degree of light expansion is large, so that the lamp is vaguely visible, the visibility of the screen may be poor, and flashing may occur.
[0028] As described above, the first inorganic particle aggregate is a form of secondary particles formed by aggregating a plurality of first inorganic particles in the form of primary particles. Specifically, 5 or more, 10 or more, 30 or more, or 30 to 50 first inorganic particles can be aggregated to form the first inorganic particle aggregate, and the first inorganic particles can be aggregated into a grape cluster, etc. In addition, the average particle size of the first inorganic particles in the form of primary particles can be 50nm or less, 5nm to 45nm, or 10nm to 40nm.
[0029] In addition, the second inorganic particle aggregate is a form of secondary particles formed by aggregating a plurality of second inorganic particles in the form of primary particles. Specifically, 5 or more, 10 or more, 30 or more, or 30 to 50 second inorganic particles can be aggregated to form a second inorganic particle aggregate, and the second inorganic particles can be aggregated into a grape cluster, etc. In addition, the average particle size of the second inorganic particles in the form of primary particles can be 50nm or less, 5nm to 45nm, or 10nm to 40nm.
[0030] The weight ratio of the first inorganic particle aggregate to the second inorganic particle aggregate can be 1: 0.1 to 5, 1: 0.15 to 4, or 1: 0.2 to 3. When the content of the second inorganic particle aggregate is too low compared to the first inorganic particle aggregate, the size of the surface irregularity is small, resulting in a lamp image, which may cause glare. When the content of the second inorganic particle aggregate is too high compared to the first inorganic particle aggregate, the degree of light expansion is high, and the lamp may be vaguely visible, resulting in poor visibility.
[0031] Specific types of the first inorganic particle aggregates and the second inorganic particle aggregates may be at least one selected from silicon oxide, titanium dioxide, indium oxide, tin oxide, zirconium oxide, zinc oxide, and polysilsesquioxane particles (specifically, silsesquioxane particles having a cage structure), but the present disclosure is not limited thereto.
[0032] The hard coating layer may include organic particles in the form of primary particles having an average particle size of 1 μm to 10 μm. The refractive index of the organic particles in the form of primary particles at a wavelength of 500 nm to 600 nm may be 1.480 to 1.620, 1.490 to 1.610, or 1.500 to 1.600. Since the hard coating layer includes organic particles having a high refractive index as described above, it is possible to prevent flash defects and unevenness (mura) occurring inside the panel while exhibiting excellent anti-glare properties.
[0033] The average particle size of the organic particles in the form of primary particles may be 1 μm to 10 μm, 1.5 μm to 8 μm, or 2 μm to 6 μm. When the average particle size of the organic particles in the form of primary particles is too large, there may be a problem that the flash defect becomes serious due to the refraction of light caused by the particles. When the average particle size of the organic particles in the form of primary particles is too small, the dispersibility of the particles may deteriorate, resulting in a problem of appearance defects due to particle aggregation.
[0034] Organic particles in the form of primary particles can achieve the haze of the anti-glare film within a specific range by utilizing the refractive index difference with the binder resin in the hard coat layer, thereby preventing flash defects, the appearance of rainbows, the image formation of lamps and light expansion while having excellent visibility. Specifically, the refractive index difference between the organic particles in the form of primary particles and the binder resin can be 0.05 to 0.1, 0.06 to 0.09 or 0.07 to 0.08. When the refractive index difference between the organic particles and the binder resin is too small, a large amount of particles must be included to achieve appropriate haze, so the problem of poor image clarity may occur. When the refractive index difference between the organic particles and the binder resin is too large, white turbidity may become serious. The refractive index can be measured at a wavelength of 500nm to 600nm.
[0035] Based on 100 parts by weight of the total weight of the first inorganic particle aggregate and the second inorganic particle aggregate, the content of the organic particles in the form of primary particles can be 30 parts by weight to 90 parts by weight, 40 parts by weight to 85 parts by weight, or 40 parts by weight to 80 parts by weight. When the content of the organic particles is too small, it is difficult to achieve sufficient internal haze at an appropriate thickness, and when the content of the organic particles is too large, the internal haze increases at an appropriate thickness, resulting in a problem that blackness and contrast may be reduced.
[0036] Specific types of organic particles in the form of primary particles may be copolymers of any one or two or more selected from the group consisting of polystyrene, polymethyl methacrylate, polymethyl acrylate, polyacrylate, polyacrylate-co-styrene, polymethyl acrylate-co-styrene, polymethyl methacrylate-co-styrene, polycarbonate, polyvinyl chloride, polybutylene terephthalate, polyethylene terephthalate, polyamide, polyimide, polysulfone, polyphenylene ether, polyacetal, epoxy resin, phenol resin, silicone resin, melamine resin, benzoguanamine, polydivinylbenzene, polydivinylbenzene-co-styrene, polydivinylbenzene-co-acrylate, polydiallyl phthalate, and triallyl isocyanate, but the present disclosure is not limited thereto.
[0037] The first inorganic particle aggregate, the second inorganic particle aggregate and the organic particles in the form of primary particles may have a particle shape such as spherical, elliptical, rod-like or amorphous. In the case of rod-like or amorphous shapes, the length of the maximum dimension may satisfy the above particle size range, etc.
[0038] In addition, the average particle size of the first inorganic particle aggregates, the second inorganic particle aggregates and the organic particles in the form of primary particles can be measured by, for example, dynamic light scattering, laser diffraction, centrifugal sedimentation, FFF (Field Flow Fractionation) method, pore resistance method, etc.
[0039] The anti-glare film may have a reflection intensity ratio (R) calculated by the following Equation 1 of 0.6% to 1%, 0.6% to 0.9%, or 0.62% to 0.8%.
[0040] [Equation 1]
[0041] Reflection intensity ratio (R) = (R1 / R2) × 100%
[0042] In equation 1,
[0043] R1 is a reflection intensity value measured at 45° corresponding to regular reflection of the incident angle after irradiating light to the hard coating layer at an incident angle of 45°, and
[0044] R2 is a reflection intensity value measured at 45° corresponding to specular reflection of the incident angle after irradiating light to the light-transmitting substrate at an incident angle of 45°.
[0045] The reflection intensity ratio of Equation 1 is calculated as a percentage of the reflection intensity value measured for the hard coating layer (R1) to the reflection intensity value measured for the light-transmitting substrate (R2).
[0046] When visible light is irradiated to the hard coating or light-transmitting substrate to be measured at an angle of 45° to the normal of the surface, some light is diffused at 45° corresponding to the specular reflection of the incident angle. Depending on the object to be measured, the intensity of the light measured at 45° in the specular reflection direction of the incident angle is defined as the R1 reflection intensity and the R2 reflection intensity, respectively. In addition, in order to suppress the reflection of the back surface and meet the conditions in actual use, a non-transmissive substrate is attached to the back surface of the object.
[0047] The non-transmissive substrate is a substrate that does not transmit light such as visible light and has a transmittance of about 0%, and may be, for example, a black acrylic plate, a black cardboard, or a film coated with a black pressure-sensitive adhesive. The film applied with a black pressure-sensitive adhesive may be, for example, a polyethylene terephthalate film applied with a black pressure-sensitive adhesive.
[0048] More specifically, in order to measure the reflection intensity (R1), a non-transmissive substrate having no irregularities or warpage may be attached to one surface of the light-transmitting substrate to face the hard coating layer. Thereafter, light is irradiated to the hard coating layer at an angle of 45° to the normal line of the surface, and the reflection intensity (R1) may be measured at 45° corresponding to the specular reflection of the incident angle.
[0049] In addition, in order to measure the reflection intensity (R2), only a light-transmitting substrate on which a hard coating layer is not formed is prepared, and a non-transmitting substrate is attached to one surface of the light-transmitting substrate. Thereafter, light is irradiated at an angle of 45° to the normal line of the surface to one surface of the light-transmitting substrate on which the non-transmitting substrate is not attached, and the reflection intensity (R2) can be measured at 45° of the specular reflection corresponding to the incident angle. Thereafter, the measured reflection intensities R1 and R2 are substituted into Equation 1 to calculate the reflection intensity ratio (R).
[0050] If the reflection intensity ratio (R) is less than 0.6%, no lamp image is formed when the lamp is illuminated, but the degree of light expansion is large, so that the lamp may be vaguely visible, and the visibility of the screen may be poor. If the reflection intensity ratio (R) exceeds 1.0%, a lamp image may be formed, causing glare.
[0051] The reflection intensity ratio (R) of the anti-glare film can be determined by the following: the average particle size of each of the two types of inorganic particle aggregates with different average particle sizes contained in the hard coating layer and the organic particles in the form of primary particles, the average particle size difference between them, the volume fraction of the inorganic / organic particles in the hard coating layer, the refractive index difference between the organic particles contained in the hard coating layer and the binder resin, the average height of irregularities formed on the hard coating layer, the height deviation of irregularities formed on the hard coating layer, etc.
[0052] In addition, the reflection intensity (R1) may be 300 to 700. In addition, the reflection intensity (R2) may be 50,000 to 70,000.
[0053] In addition, when a flat non-transmissive substrate without irregularities or warping is attached to one surface of a light-transmitting substrate to face the hard coating layer, and light is irradiated to the hard coating layer at an angle of 45° to the normal of the surface, diffuse light in which the incident light is reflected can be emitted at an angle other than 45° corresponding to the specular reflection of the incident angle.
[0054] Herein, the angle of the diffuse light at which 1 / 10 times the reflection intensity R1 is measured may be 30° to 35° and 55° to 60°. Specifically, after irradiating the hard coating with light at an incident angle of 45°, the reflection intensity value measured in the diffuse light at 30° to 35° and 55° to 60° may be 1 / 10 times the reflection intensity R1. If 1 / 10 times the reflection intensity R1 does not appear within the above-mentioned angle range of the diffuse light, the degree of light expansion is large, so that the lamp may be vaguely visible when the lamp is illuminated, resulting in poor visibility of the screen, or a lamp image may be formed, causing glare.
[0055] In addition, the angle of the diffuse light at which 1 / 100 times the reflection intensity R1 is measured can be 20° to 25° and 65° to 70°. Specifically, after irradiating the hard coating with light at an incident angle of 45°, the reflection intensity value measured in the diffuse light at 20° to 25° and 65° to 70° can be 1 / 100 times the reflection intensity R1. If 1 / 100 times the reflection intensity R1 does not appear within the above-mentioned angle range of the diffuse light, the degree of light expansion is large, so that the lamp may be vaguely visible when the lamp is illuminated, resulting in poor visibility of the screen, or a lamp image may be formed, causing glare.
[0056] Generally, the higher the haze value, the greater the degree of diffusion of external light, making the anti-glare effect excellent. However, there is a problem of reduced contrast due to image distortion caused by surface scattering and whitening phenomenon caused by internal scattering. On the other hand, the anti-glare film has a total haze of 20% to 40%, 23% to 35%, or 25% to 30%; an internal haze of 10% to 20%, 12% to 19%, or 13% to 18%; and an external haze of 10% to 30%, 12% to 25%, or 14% to 20%. Therefore, it is possible to prevent flash defects, rainbow appearance, image formation of lamps, and light expansion while showing excellent visibility.
[0057] In addition, the ratio of the external haze to the internal haze of the anti-glare film may be 0.6 to 2.0, 0.8 to 1.9, or 1.0 to 1.8. The ratio of the external haze to the internal haze of the anti-glare film may be determined by the average particle size of each of the two types of inorganic particle aggregates having different average particle sizes contained in the hard coating layer and the organic particles in the form of primary particles, the average particle size difference therebetween, the volume fraction of the inorganic / organic particles in the hard coating layer, the refractive index difference between the organic particles contained in the hard coating layer and the binder resin, etc.
[0058] If the ratio of the external haze to the internal haze is less than 0.6, the anti-glare effect is reduced due to insufficient anti-glare visibility, and when the anti-glare film is located under the cover glass, the ANR (Anti-Newton) effect caused by external irregularities formed on the hard coating layer is reduced, causing interference fringes, which may deteriorate optical characteristics. If the ratio exceeds 2.0, the external haze increases, so that the flare caused by the external irregularities may become serious and the image clarity may be reduced.
[0059] The ratio of the external haze to the reflection intensity ratio (R) of the anti-glare film may be 15 to 30, 20 to 29, or 21 to 28. The ratio of the external haze to the reflection intensity ratio (R) may be determined by the average particle size of each of the two types of inorganic particle aggregates having different average particle sizes contained in the hard coating layer and the organic particles in the form of primary particles, the average particle size difference therebetween, the volume fraction of the inorganic / organic particles in the hard coating layer, the refractive index difference between the organic particles contained in the hard coating layer and the binder resin, and the like.
[0060] If the ratio of the external haze to the reflection intensity ratio (R) is less than 15, the anti-glare effect is reduced due to severe light reflection, and when the anti-glare film is located under the cover glass, the ANR (anti-Newton) effect caused by external irregularities formed on the hard coating layer is reduced, causing interference fringes, which may deteriorate the optical characteristics. If the ratio exceeds 30, the light expansion caused by external light becomes severe, resulting in poor visibility of the screen. In addition, the flare caused by external irregularities becomes severe, and the image clarity may be reduced.
[0061] The binder resin of the hard coat layer included in the anti-glare film may include a (co)polymer of a vinyl-based monomer or a (meth)acrylate-based monomer.
[0062] The vinyl-based monomer or the (meth)acrylate-based monomer may include a monomer or an oligomer including one or more, two or more, or three or more (meth)acrylate or vinyl groups.
[0063] Specific examples of monomers or oligomers containing (meth)acrylates may include pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, toluene diisocyanate, xylene diisocyanate, hexamethylene diisocyanate, trimethylolpropane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, trimethylolpropane trimethacrylate, ethylene glycol dimethacrylate, butanediol dimethacrylate, hexaethyl methacrylate, butyl methacrylate, and mixtures of two or more thereof; and urethane-modified acrylate oligomers, epoxide acrylate oligomers, ether acrylate oligomers, dendritic acrylate oligomers, and mixtures of two or more thereof. In this article, the weight average molecular weight of the oligomer may be 1,000 to 10,000.
[0064] Specific examples of the monomer or oligomer including a vinyl group may include divinylbenzene, styrene, and p-methylstyrene.
[0065] In addition, the polymer or copolymer contained in the binder resin may also contain a portion derived from at least one monomer selected from the following: a reactive acrylate oligomer group consisting of urethane acrylate oligomers, epoxy acrylate oligomers, polyester acrylates and polyether acrylates; a multifunctional acrylate monomer group consisting of dipentaerythritol hexaacrylate, dipentaerythritol hydroxypentaacrylate, pentaerythritol tetraacrylate, pentaerythritol triacrylate, trimethylenepropyl triacrylate, propoxylated glycerol triacrylate, trimethylpropane ethoxy triacrylate, 1,6-hexanediol diacrylate, propoxylated glycerol triacrylate, tripropylene glycol diacrylate and ethylene glycol diacrylate.
[0066] Based on 100 parts by weight of the binder resin, the hard coat layer may include 2 to 10 parts by weight, 3 to 8 parts by weight, or 4 to 7 parts by weight of organic particles in the form of primary particles. If less than 2 parts by weight of organic particles are included based on 100 parts by weight of the binder resin, the haze caused by internal scattering may not be fully achieved, and if more than 10 parts by weight are included, the haze caused by internal scattering may become too high, resulting in reduced contrast.
[0067] The thickness of the hard coating layer may be 1 to 10 μm, or 2 to 8 μm. If the thickness of the hard coating layer is less than 1 μm, it is difficult to obtain the desired hardness, and if the thickness of the hard coating layer exceeds 10 μm, the hard coating layer may be bent during the curing of the resin when forming the hard coating layer.
[0068] The thickness of the hard coat layer can be obtained by observing the cross section of the anti-glare film using a scanning electron microscope (SEM) and measuring the thickness of the binder portion of the hard coat layer. On the other hand, since the thickness obtained by the method of deducting the arithmetic mean roughness Ra of the hard coat layer from the thickness of the entire hard coat layer containing inorganic particles (measured by using a thickness measuring instrument (manufactured by TESA Co., Ltd.)) is almost consistent with the thickness of the binder portion measured by SEM observation, such a method can be used.
[0069] As a light-transmitting substrate, a plastic film with transparency can be used. For example, triacetyl cellulose (TAC), polyester (TPEE), polyethylene terephthalate (PET), polyimide (PI), polyamide (PA), aromatic polyamide, polyethylene (PE), polyacrylate (PAR), polyether sulfone, polysulfone, diacetyl cellulose, polypropylene (PP), polyvinyl chloride, acrylic resin (PMMA), polycarbonate (PC), epoxy resin, urea resin, urethane resin, melamine resin, etc. can be used. In particular, conventional anti-glare films usually use triacetyl cellulose as a substrate, but the triacetyl cellulose film is easily affected by moisture, so it has the disadvantage of poor durability when used for outdoor displays. Therefore, a polyethylene terephthalate film with excellent moisture permeability is used as a substrate, but there is a problem that the rainbow defect caused by the birefringence of polyethylene terephthalate must be solved.
[0070] However, according to the anti-glare film of the present embodiment, the in-plane delay (Re) measured at a wavelength of 400nm to 800nm by the light-transmitting substrate included in the anti-glare film can be 500mm or less, or 5000nm or more. Specifically, the in-plane delay (Re) measured at a wavelength of 400nm to 800nm by the light-transmitting substrate can be 500mm or less, 450nm or less, or 10nm to 400nm, or 5000nm or more, 5100nm or more, or 5200nm to 8000nm. More specifically, the light-transmitting substrate can be a polyethylene terephthalate film that satisfies the above-mentioned in-plane delay. Using this film as a light-transmitting substrate can prevent the rainbow phenomenon caused by the interference of visible light.
[0071] In-plane retardation (Re) can be defined by the following equation, where d is the thickness of the transparent substrate, n x is the refractive index in the slow axis direction in the plane, and n y is the refractive index along the in-plane fast axis.
[0072] Re=(n x -n y )*d
[0073] Furthermore, the delay value may be an absolute value and may be defined as a positive number.
[0074] Considering productivity, the thickness of the light-transmitting substrate may be 10 μm to 300 μm, 30 μm to 250 μm, or 40 μm to 200 μm, but is not limited thereto.
[0075] According to another embodiment of the present disclosure, a composition for forming a hard coating layer of an anti-glare film is provided, which comprises a binder resin and particles dispersed in the binder resin, wherein the particles include first inorganic particle aggregates with an average particle size of 1 μm to 2 μm; second inorganic particle aggregates with an average particle size of 3 μm to 5 μm; and organic particles in the form of primary particles with an average particle size of 1 μm to 10 μm.
[0076] The binder resin and particles contained in the composition for forming the hard coat layer are as described in the antiglare film.
[0077] The composition for forming a hard coat layer may be coated on a light-transmitting substrate, dried and cured to form a hard coat layer of an anti-glare film.
[0078] In addition, the first inorganic particle aggregates, the second inorganic particle aggregates, and the organic particles in the form of primary particles contained in the composition for forming the hard coating layer do not aggregate further during drying or curing, so that the first inorganic particle aggregates, the second inorganic particle aggregates, and the organic particles in the form of primary particles themselves can be present in the final hard coating layer.
[0079] In addition, the composition for forming a hard coating layer may further include a photopolymerization initiator. Therefore, the photopolymerization initiator may remain in the hard coating layer prepared from the composition for forming a hard coating layer.
[0080] As the photopolymerization initiator, any compound known to be used in a composition for forming a hard coating layer can be used without limitation, specifically, a benzophenone-based compound, an acetophenone-based compound, a biimidazole-based compound, a triazine-based compound, an oxime-based compound, or a mixture of two or more thereof can be used.
[0081] The photopolymerization initiator may be used in an amount of 1 to 10 parts by weight, 2 to 9 parts by weight, or 3 to 8 parts by weight based on 100 parts by weight of the binder resin. If the amount of the photopolymerization initiator is too small, uncured material may be generated in the photocuring step of the composition for forming the hard coat. If the amount of the photopolymerization initiator is too large, the unreacted initiator may remain as an impurity or the crosslinking density may be reduced, thereby deteriorating the mechanical properties of the film to be prepared.
[0082] In addition, the composition for forming the hard coating layer may further include an organic solvent. Non-limiting examples of the organic solvent include ketones, alcohols, acetates, ethers, benzene derivatives, and mixtures of two or more thereof.
[0083] Specific examples of the organic solvent include ketones such as methyl ethyl ketone, methyl isobutyl ketone, acetylacetone or isobutyl ketone; alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol or tert-butanol; acetates such as ethyl acetate, isopropyl acetate or polyethylene glycol monomethyl ether acetate; ethers such as tetrahydrofuran or propylene glycol monomethyl ether; and mixtures of two or more thereof.
[0084] The organic solvent can be included in the composition for forming the hard coat by: adding the organic solvent when mixing the components included in the composition for forming the hard coat, or adding the organic solvent by dispersing the components in the organic solvent or mixing with the organic solvent. If the amount of the organic solvent in the composition for forming the hard coat is too little, the fluidity of the composition for forming the hard coat is reduced, so defects such as stripes may occur in the final film. In addition, when an excessive amount of organic solvent is added, the solid content is reduced, so that coating and film formation may not be fully performed. Therefore, the physical properties or surface characteristics of the film may deteriorate, and defects may occur during drying and curing. Therefore, the composition for forming the hard coat may include an organic solvent so that the total solid concentration of the components included therein is 1% by weight to 50% by weight or 2% by weight to 20% by weight.
[0085] Any method and apparatus commonly used for coating a composition for forming a hard coating layer may be used without particular limitation. For example, a rod coating method such as a Meyer rod method, a gravure coating method, a double roll reverse coating method, a vacuum slot die coating method, a double roll coating method, etc. may be used.
[0086] In the step of photocuring the composition for forming a hard coat layer, ultraviolet light or visible light having a wavelength of 200 nm to 400 nm may be irradiated, and the exposure amount during irradiation is preferably 100 mJ / cm 2 Up to 4,000mJ / cm 2 The exposure time is not particularly limited and may be appropriately changed depending on the exposure device used, the wavelength of the irradiated light, or the exposure amount. In addition, in the step of photocuring the composition for forming the hard coat layer, nitrogen purging may be performed to apply a nitrogen atmosphere condition.
[0087] According to another embodiment of the present disclosure, a polarizing plate including an anti-glare film may be provided. The polarizing plate may include a polarizing film and an anti-glare film formed on at least one surface of the polarizing film.
[0088] The material and preparation method of the polarizing film are not particularly limited, and conventional materials and preparation methods known in the art may be used. For example, the polarizing film may be a polyvinyl alcohol-based polarizing film.
[0089] A protective film may be provided between the polarizing film and the anti-glare film. The protective film may be at least one selected from the following: a cycloolefin polymer (COP)-based film, an acrylic film, a triacetyl cellulose (TAC)-based film, a cycloolefin copolymer (COC)-based film, a polynorbornene (PNB)-based film, and a polyethylene terephthalate (PET)-based film, and the present disclosure is not limited thereto.
[0090] The protective film may use a substrate for forming a single coating layer in the preparation of the anti-glare film. The polarizing film and the anti-glare film may be laminated by an adhesive such as an aqueous adhesive or a non-aqueous adhesive.
[0091] According to another embodiment of the present disclosure, a display device including an anti-glare film may be provided.
[0092] Specific examples of the display device may include devices such as a liquid crystal display, a plasma display, or an organic light emitting diode, but the present disclosure is not limited thereto.
[0093] For example, the display device may be a liquid crystal display including a pair of polarizing plates facing each other; a thin film transistor, a color filter, and a liquid crystal unit sequentially stacked between the pair of polarizing plates; and a backlight unit. In a display device including an anti-glare film, the anti-glare film may be positioned on one surface of a polarizing plate relatively far from the backlight unit in the pair of polarizing plates.
[0094] In the display device, the anti-glare film may be disposed on the outermost surface on the observer side or the backlight side of the display panel. More specifically, the display device may be a device for a notebook computer display, a TV display, or a large-area advertising display, and the anti-glare film may be located on the outermost surface of the device for a notebook computer display, a TV display, or a large-area advertising display.
[0095] Beneficial Effects
[0096] According to the present disclosure, an excellent anti-glare film capable of preventing glitter defects, the occurrence of rainbows, lamp image formation, and light spreading while having excellent anti-glare properties and excellent physical properties such as scratch resistance and stain resistance, and a polarizing plate and a display device including the same are provided. DETAILED DESCRIPTION
[0097] The present invention will be described in more detail in the following examples. However, these examples are only for illustrating the present invention, and the scope of the present invention is not limited thereto.
[0098] <Examples and Comparative Examples: Preparation of Anti-glare Film>
[0099] (1) Preparation of composition for forming hard coating layer
[0100] (1-1) Preparation Example 1
[0101] As binder resins, 50 parts by weight of EB-1290 (photocurable aliphatic urethane hexaacrylate, manufactured by SK Entis, having a weight average molecular weight of 1000) and 50 parts by weight of trimethylolpropane triacrylate were prepared. Based on 100 parts by weight of the binder resin, 5 parts by weight of IRG184 (Irgacure 184, hydroxycyclohexyl phenyl ketone, manufactured by Ciba Specialty Chemicals, Switzerland) as an initiator, 50 parts by weight of toluene as a solvent, 50 parts by weight of methyl ethyl ketone as a solvent, 5.5 parts by weight of SS-50F (surface-treated hydrophobic silica with an average particle size of 1 μm to 2 μm, manufactured by Tosoh Silica Co., Ltd.) as a first inorganic particle aggregate, 2.3 parts by weight of Acematt 3600 (silica aggregate with an average particle size of 3 μm to 4 μm, manufactured by Evonik Tego) as a second inorganic particle aggregate, and 4.0 parts by weight of PS spherical particles a (polystyrene spherical particles with an average particle size of 2 μm and a refractive index of 1.595) as organic particles in the form of primary particles were prepared and mixed to prepare a composition for forming a hard coating layer of Preparation Example 1.
[0102] In addition, the average particle size of each of the inorganic particle aggregates and the organic particles can be determined by a known method. For example, it can be calculated and obtained by measuring the radius of each particle determined in an electron micrograph (SEM, TEM, etc.), or can be calculated by an X-ray scattering experiment.
[0103] (1-2) Preparation Example 2
[0104] As binder resins, 50 parts by weight of EB-1290 (photocurable aliphatic urethane hexaacrylate, manufactured by SK Entis, weight average molecular weight 1000) and 50 parts by weight of pentaerythritol triacrylate (manufactured by SK Entis) were prepared. Based on 100 parts by weight of the binder resin, 5 parts by weight of IRG184 (Irgacure 184, hydroxycyclohexyl phenyl ketone, manufactured by Ciba Specialty Chemicals, Switzerland) as an initiator, 50 parts by weight of toluene as a solvent, 50 parts by weight of methyl ethyl ketone as a solvent, 7.5 parts by weight of SS-50 (surface-treated hydrophobic silica aggregates with an average particle size of 1 μm to 2 μm, manufactured by Tosoh Silica Co., Ltd.) as a first inorganic particle aggregate, 1.5 parts by weight of Acematt 3600 as a second inorganic particle aggregate, and 5.3 parts by weight of PS spherical particles b (polystyrene spherical particles with an average particle size of 1.3 μm and a refractive index of 1.595) as organic particles in the form of primary particles were prepared and mixed to prepare a composition for forming a hard coating layer of Preparation Example 2.
[0105] (1-3) Preparation Example 3
[0106] The composition for forming a hard coating layer of Preparation Example 3 was prepared in the same manner as in Preparation Example 1, except that 7.5 parts by weight of PS-PMMA spherical particles a (polystyrene-polymethyl methacrylate copolymerized spherical particles, with an average particle size of 5 μm and a refractive index of 1.555) and 5.8 parts by weight of PS-PMMA spherical particles (polystyrene-polymethyl methacrylate copolymerized spherical particles, with an average particle size of 3.5 μm and a refractive index of 1.515) were used instead of 5.5 parts by weight of SS-50F as the first inorganic particle aggregate, 2.3 parts by weight of Acematt 3600 as the second inorganic particle aggregate, and 4.0 parts by weight of PS spherical particles a as organic particles in the form of primary particles.
[0107] (1-4) Preparation Example 4
[0108] The composition for forming a hard coating layer of Preparation Example 4 was prepared in the same manner as in Preparation Example 1, except that 9.5 parts by weight of SS-50 as the first inorganic particle aggregate and 5.0 parts by weight of PS spherical particles a as organic particles in the form of primary particles were used instead of 5.5 parts by weight of SS-50F as the first inorganic particle aggregate, 2.3 parts by weight of Acematt 3600 as the second inorganic particle aggregate, and 4.0 parts by weight of PS spherical particles a as organic particles in the form of primary particles.
[0109] (1-5) Preparation Example 5
[0110] 50 parts by weight of pentaerythritol triacrylate (manufactured by SK Entis) and 50 parts by weight of trimethylolpropane triacrylate were prepared as a binder resin. Based on 100 parts by weight of the binder resin, 5 parts by weight of IRG184 (Irgacure 184, hydroxycyclohexyl phenyl ketone, manufactured by Ciba Specialty Chemicals, Switzerland) as an initiator, 50 parts by weight of toluene as a solvent, 50 parts by weight of methyl ethyl ketone as a solvent, 10 parts by weight of Acematt 3600 as a second inorganic particle aggregate, and 4.5 parts by weight of PS spherical particles a as organic particles in the form of primary particles were prepared and mixed to prepare a composition for forming a hard coating layer of Preparation Example 5.
[0111] (1-6) Preparation Example 6
[0112] A composition for forming a hard coating layer of Preparation Example 6 was prepared in the same manner as in Preparation Example 5, except that 4.5 parts by weight of T145A (POSS (silsesquioxane), with an average particle size of 5 μm, a refractive index of 1.42, manufactured by Toshiba) as inorganic particles in the form of primary particles and 7 parts by weight of PS-PMMA spherical particles b were used instead of 10 parts by weight of Acematt 3600 as a second inorganic particle aggregate and PS spherical particles a as organic particles in the form of primary particles.
[0113] (1-7) Preparation Example 7
[0114] A composition for forming a hard coating layer of Preparation Example 7 was prepared in the same manner as in Preparation Example 1, except that 4.5 parts by weight of SS-50 (surface-treated hydrophobic silica aggregates having an average particle size of 1 μm to 2 μm, manufactured by Tosoh Silica Co., Ltd.) was used instead of 2.3 parts by weight of Acematt 3600 as the second inorganic particle aggregate.
[0115] (2) Preparation of anti-glare film
[0116] As shown in Table 1 below, the composition for forming a hard coating layer prepared in one of Preparation Examples 1 to 7 was coated on triacetyl cellulose (TAC, 60 μm thick) as a light-transmitting substrate using a #10 meyer rod and dried at 90° C. for 1 minute. The dried material was heated with 150 mJ / cm 2 The hard coating layer was formed by ultraviolet irradiation and an anti-glare film was prepared. At this time, the thickness of the hard coating layer is shown in Table 1 below.
[0117] [Table 1]
[0118] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Composition for forming a hard coating Preparation Example 1 Preparation Example 2 Preparation Example 3 Preparation Example 4 Preparation Example 5 Preparation Example 6 Preparation Example 7 Hard coating thickness (μm) 5 5 4 4 6 7 5
[0119] <Experimental example>
[0120] 1. Transmittance and haze
[0121] A 4 cm × 4 cm sample was prepared from the anti-glare film obtained in one of the embodiments and the comparative examples, and the haze was measured three times using a haze meter (HM-150, light source A, manufactured by Murakami). Thereafter, the average value thereof was calculated as the total haze. Herein, the transmittance and the total haze were measured simultaneously. Specifically, the transmittance was measured according to the JIS K 7361 standard, and the haze was measured according to the JIS K 7136 standard.
[0122] In the measurement of internal haze, an adhesive film having a total haze of 0 is attached to the coated surface of the optical film to be measured to make the uneven surface flat, and then the internal haze is measured in the same manner as the above total haze. The external haze is calculated as the average value of the difference between the total haze and the internal haze, and the transmittance, internal haze, and external haze are shown in Table 2 below.
[0123] 2. Reflection intensity ratio
[0124] The sample was prepared by attaching a flat polyethylene terephthalate film coated with a black pressure-sensitive adhesive without irregularities or warpage on one surface of a light-transmitting substrate to face the hard coating layer of the anti-glare film obtained in one of the embodiments and comparative examples. Thereafter, the sample was mounted on a goniometer (GC5000L, manufactured by Nippon Denshoku Industries), and the hard coating layer of the sample was irradiated with light at an angle of 45° to the normal line of the surface. After irradiating the surface of the hard coating layer with light, the reflection intensity (R1) was measured at 45° of the specular reflection corresponding to the incident angle.
[0125] In addition, a light-transmitting substrate on which a hard coating layer was not formed by the Examples and Comparative Examples was prepared, specifically, a light-transmitting substrate described in the above Table 1. A specimen was prepared by attaching a flat polyethylene terephthalate film coated with a black pressure-sensitive adhesive without irregularities or warpage on one surface of the light-transmitting substrate, and the reflection intensity (R2) was measured in the same manner as in the reflection intensity (R1).
[0126] The measured reflection intensities R1 and R2 were substituted into the following Equation 1 to calculate the reflection intensity ratio (R), and the results are shown in Table 2 below.
[0127] [Equation 1]
[0128] Reflection intensity ratio (R) = (R1 / R2) × 100%
[0129] Furthermore, the ranges in which the diffuse light of 1 / 10 times the reflection intensity R1 and 1 / 100 times the reflection intensity R1 were measured were determined, and the results are shown in Table 2 below.
[0130] 3. Visibility (formation of light image)
[0131] The specimen was prepared by attaching a flat polyethylene terephthalate film coated with a black pressure-sensitive adhesive without irregularities or warpage on one surface of a light-transmitting substrate to face the hard coating layer of the anti-glare film obtained in one of the embodiments and comparative examples. Thereafter, the visibility was measured by irradiating light using a fluorescent lamp having two rows of lamps as a light source and then observing the reflected image of the fluorescent lamp in the specular reflection direction of each anti-glare film. The evaluation criteria for visibility are as follows, and the results are shown in Table 2 below.
[0132] Good: No lamp image is observed.
[0133] Poor: The lamp image is clearly visible.
[0134] 4. Optical expansion
[0135] The specimen was prepared by attaching a flat polyethylene terephthalate film coated with a black pressure-sensitive adhesive without irregularities or warpage on one surface of a light-transmitting substrate to face the hard coating layer of the anti-glare film obtained in one of the examples and comparative examples. Thereafter, when light having a lamp size of 4 mm was irradiated from a height of 20 cm, light spread was evaluated by the size of an image appearing on the specimen. Specifically, the evaluation criteria for light spread are as follows, and the results are shown in Table 2 below.
[0136] Good: No lamp image was observed, or the size of the lamp image was less than 5 cm.
[0137] Poor: The size of the lamp image exceeds 5 cm.
[0138] [Table 2]
[0139]
[0140] Referring to Table 2, it is determined that the anti-glare films of Examples 1 and 2 have a reflection intensity ratio of 0.6% to 1%, a ratio of external haze to reflection intensity ratio of 15 to 30, and a ratio of external haze to internal haze of 0.6 to 2, and no lamp image is formed and no light expansion occurs.
[0141] On the other hand, it is determined that a lamp image is formed or light expansion occurs in Comparison Example 1 in which inorganic particles are not used and the above numerical range is not satisfied; Comparison Example 2 and Comparison Example 5 in which the second inorganic particle aggregates are not used and the above numerical range is not satisfied; Comparison Example 3 in which the first inorganic particle aggregates are not used and the above numerical range is not satisfied; and Comparison Example 4 in which inorganic particle aggregates are not used and the above numerical range is not satisfied.
Claims
1. An anti-glare film comprising a light-transmitting substrate; and a hard coating layer comprising a binder resin and particles dispersed in the binder resin, The particles include first inorganic particle aggregates having an average particle diameter of 1 to 2 μm; second inorganic particle aggregates having an average particle diameter of 3 to 5 μm; and organic particles in the form of primary particles having an average particle diameter of 1 to 10 μm.
2. The anti-glare film according to claim 1, Wherein the reflection intensity ratio R calculated by the following equation 1 is 0.6% to 1%: [Equation 1] Reflection intensity ratio R = (R1 / R2) × 100% In equation 1, R1 is a reflection intensity value measured at 45° corresponding to specular reflection at an incident angle of 45° after irradiating the hard coating layer with light at the incident angle of 45°, and R2 is a reflection intensity value measured at 45° corresponding to specular reflection at an incident angle of 45° after irradiating light to the light-transmitting substrate at the incident angle of 45°.
3. The anti-glare film according to claim 2, After irradiating the hard coating layer with light at an incident angle of 45°, the reflection intensity values measured in diffuse light at 30° to 35° and 55° to 60° are 1 / 10 times the reflection intensity value R1.
4. The anti-glare film according to claim 2, After irradiating the hard coating layer with light at an incident angle of 45°, the reflection intensity values measured in diffuse light at 20° to 25° and 65° to 70° are 1 / 100 times the reflection intensity value R1.
5. The anti-glare film according to claim 1, wherein the first inorganic particle aggregate is in the form of a secondary particle in which five or more first inorganic particles in the form of primary particles are aggregated, and The first inorganic particles in the form of primary particles have an average particle diameter of 50 nm or less.
6. The anti-glare film according to claim 1, wherein the second inorganic particle aggregate is in the form of a secondary particle in which five or more second inorganic particles in the form of primary particles are aggregated, and The average particle diameter of the second inorganic particles in the form of primary particles is 50 nm or less.
7. The anti-glare film according to claim 1, The absolute value of the difference in refractive index between the organic particles in the form of primary particles having an average particle diameter of 1 μm to 10 μm and the binder resin is 0.05 to 0.
1.
8. The anti-glare film according to claim 1, The average particle size ratio of the second inorganic particle aggregates to the first inorganic particle aggregates is 1.5 to 4 times.
9. The anti-glare film according to claim 1, The weight ratio of the first inorganic particle aggregates to the second inorganic particle aggregates is 1:0.1 to 5.
10. The anti-glare film according to claim 1, The content of the organic particles in the form of primary particles is 30 parts by weight to 90 parts by weight based on 100 parts by weight of the total weight of the first inorganic particle aggregate and the second inorganic particle aggregate.
11. The anti-glare film according to claim 2, The ratio of the external haze of the anti-glare film to the reflection intensity ratio R is 15 to 30.
12. The anti-glare film according to claim 1, The ratio of the external haze to the internal haze of the anti-glare film is 0.6 to 2.
13. The anti-glare film according to claim 1, The binder resin includes a copolymer or a homopolymer of a vinyl-based monomer or a (meth)acrylate-based monomer.
14. The anti-glare film according to claim 1, The hard coating layer includes 2 parts by weight to 10 parts by weight of the organic particles in the form of primary particles based on 100 parts by weight of the binder resin.
15. The anti-glare film according to claim 1, The light-transmitting substrate has an in-plane retardation (Re) of 500 nm or less, or 5000 nm or more, measured at a wavelength of 400 nm to 800 nm.
16. A composition for forming a hard coating layer of an anti-glare film, comprising a binder resin and particles dispersed in the binder resin, The particles include first inorganic particle aggregates having an average particle diameter of 1 to 2 μm; second inorganic particle aggregates having an average particle diameter of 3 to 5 μm; and organic particles in the form of primary particles having an average particle diameter of 1 to 10 μm. 17 . A polarizing plate comprising the anti-glare film according to claim 1 .
18. A display device comprising the anti-glare film according to claim 1.