Method for producing resin composition and resin composition

A novel resin composition production method using water washing and coagulation techniques addresses the issues of residual emulsifiers and solvents in epoxy resin compositions, achieving high dispersibility and reduced impurities for improved resin quality and environmental sustainability.

CN113646382BActive Publication Date: 2024-12-03KANEKA CORP
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
CN202080025049.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-28
Filing Date
2020-03-30
Publication Date
2024-12-03
Estimated Expiration
2040-03-30

AI Technical Summary

Technical Problem

Existing methods for producing epoxy resin compositions face issues with residual emulsifiers and organic solvents, leading to high environmental impact and impurity content, particularly when dispersing polymer particles smaller than 1 μm in thermosetting resins.

Method used

A method involving washing resin compositions containing polymer microparticles and a resin with water at specific viscosities and weight ratios, followed by coagulation and aggregation, to reduce impurities and environmental load, using techniques like shearing, freezing, and coagulation, and using specific additives to ensure thorough mixing, results in a uniformly dispersed resin composition.

Benefits of technology

The method effectively reduces impurities and environmental impact, enhancing the dispersibility and quality of the resin composition, suitable for electronic materials, with improved cleaning efficiency and reduced manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003281721980000581
    Figure BDA0003281721980000581
  • Figure BDA0003281721980000591
    Figure BDA0003281721980000591
Patent Text Reader

Abstract

A resin composition is produced by a method including a washing step, wherein the washing step is to wash the resin composition with water, wherein the resin composition contains polymer particles (A) and a resin (B) having a predetermined viscosity, wherein the polymer particles (A) have a graft portion, the graft portion being composed of a polymer containing a constituent unit derived from one or more monomers selected from an aromatic vinyl monomer, a vinyl cyanide monomer, and a (meth)acrylate monomer, and when the total of the polymer particles (A) and the resin (B) is 100% by weight, the polymer particles (A) are 1 to 70% by weight, and the resin (B) is 30 to 99% by weight.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a resin composition and the resin composition. Background Art

[0002] Thermosetting resins are used in various fields because they have various excellent properties such as high heat resistance and mechanical strength. Among thermosetting resins, epoxy resins are used in a wide range of applications, for example, as a matrix resin for electronic circuit sealants, coatings, adhesives, and fiber-reinforced materials. Epoxy resins have excellent heat resistance, chemical resistance, insulation, etc., but have the problem of insufficient impact resistance, which is a characteristic of thermosetting resins. In order to improve the impact resistance of thermosetting resins, the method of adding elastomers to thermosetting resins is widely used.

[0003] As the above-mentioned elastomer, polymer particles (such as cross-linked polymer particles) can be cited. It is relatively easy to simply mix polymer particles and thermosetting resins (such as epoxy resins). As a mixing method, for example, a method of mechanically mixing the powder and the thermosetting resin after a small amount of polymer particles having a particle size smaller than 1 μm are collected to make a powder of polymer particles having a particle size of 1 μm or more can be cited. In addition, the powder of polymer particles prepared by collecting a certain number of such polymer particles is called secondary particles, and the polymer particles having a particle size smaller than 1 μm before becoming a powder are called primary particles. The above-mentioned mixing method can also be used to disperse the secondary particles of polymer particles in the thermosetting resin. However, it is very difficult to disperse the primary particles of polymer particles having a particle size smaller than 1 μm in the thermosetting resin at the industrial production level.

[0004] As a countermeasure to this dispersibility, for example, Patent Document 1 reports a method for producing an epoxy resin composition in which epoxy resin is mixed in latex and devolatilized, and the epoxy resin composition is uniformly dispersed directly in fine particle epoxy resin of core / shell type particle crosslinking copolymer (Examples, etc.). In addition, Patent Document 2 discloses that an aqueous latex of rubbery polymer particles is brought into contact with an organic medium partially soluble in water, and then further brought into contact with an organic medium having a lower partial solubility in water than the organic medium to substantially separate water, and then the rubbery polymer particles are taken out as a dispersion dispersed in the organic medium, and then mixed with an epoxy resin, and the volatile components are distilled off, thereby obtaining an epoxy resin composition in which the rubbery polymer particles are well dispersed in the epoxy resin and the inclusions are small.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent document 1: Japanese Patent Publication No. 8-183836

[0008] Patent document 2: International Publication No. WO2004 / 108825. Summary of the invention

[0009] However, in the technology of Patent Document 1, the following problem is found: the emulsifier used in the polymerization of the core / shell type particle-shaped cross-linked copolymer all remains in the epoxy resin. In addition, in the technology of Patent Document 2, the following problem is found: impurities from the polymerization of the rubbery polymer particles are removed, and the organic medium (solvent) remains in the resin.

[0010] One embodiment of the present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a novel resin composition having a small environmental load and a small amount of impurities.

[0011] The present inventors have conducted intensive studies to solve the above problems and have found a new finding that water-soluble impurities can be efficiently washed out by washing aggregates containing polymer microparticles and a resin of a specific viscosity at a predetermined weight ratio with water, thereby completing the present invention.

[0012] That is, one embodiment of the present invention includes the following configurations.

[0013] A method for producing a resin composition, comprising a washing step of washing the following resin composition with water,

[0014] The resin composition comprises polymer particles (A) and a resin (B),

[0015] The polymer microparticles (A) have a graft portion, the graft portion is composed of a polymer containing a constituent unit derived from one or more monomers selected from an aromatic vinyl monomer, a vinyl cyanide monomer and a (meth)acrylate monomer, and the resin (B) is a liquid, a semisolid or a solid having a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25° C., and when the total of the polymer microparticles (A) and the resin (B) is 100 weight %, the polymer microparticles (A) are 1 to 70 weight % and the resin (B) are 30 to 99 weight %.

[0016] A resin composition comprising polymer microparticles (A) and a resin (B), wherein the polymer microparticles (A) have a graft portion, the graft portion being composed of a polymer containing constituent units derived from one or more monomers selected from an aromatic vinyl monomer, a vinyl cyanide monomer and a (meth)acrylate monomer, and the resin (B) is a liquid, semisolid or solid having a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25° C., and when the total of the polymer microparticles (A) and the resin (B) is taken as 100% by weight, the polymer microparticles (A) account for 30 to 70% by weight, and the resin (B) account for 30 to 70% by weight.

[0017] According to one embodiment of the present invention, a resin composition having a small environmental load and a small amount of impurities can be provided. DETAILED DESCRIPTION

[0018] An embodiment of the present invention is described below, but the present invention is not limited thereto. The present invention is not limited to the various configurations described below, and various changes can be made within the scope indicated by the claims. In addition, embodiments or embodiments obtained by appropriately combining the technical means respectively disclosed in different embodiments or examples are included in the technical scope of the present invention. Moreover, by combining the technical means respectively disclosed in each embodiment, new technical features can be formed. In addition, all academic literature and patent literature described in this specification are cited as references in this specification. In addition, in this specification, unless otherwise specified, "A to B" indicating a numerical range means "Above A (including A and larger than A) and below B (including B and smaller than B)".

[0019] [1. Method for producing resin composition]

[0020] A method for producing a resin composition according to one embodiment of the present invention comprises a washing step of washing the resin composition with water, wherein the resin composition comprises polymer microparticles (A) and a resin (B), wherein the polymer microparticles (A) have a graft portion, the graft portion being composed of a polymer comprising a constituent unit derived from one or more monomers selected from an aromatic vinyl monomer, a vinyl cyanide monomer, and a (meth)acrylate monomer, and the resin (B) has a viscosity of 1,000,000 mPa·s or less at 25° C., and when the total of the polymer microparticles (A) and the resin (B) is 100% by weight, the polymer microparticles (A) are 1 to 70% by weight, and the resin (B) are 30 to 99% by weight. Hereinafter, the method for producing a resin composition according to one embodiment of the present invention may be simply referred to as the present production method.

[0021] The present inventors have found that the cleaning efficiency of the polymer particles in the technology of the above-mentioned Patent Document 1 is poor, and a large amount of impurities are contained in the epoxy resin. In order to solve the above-mentioned problems, the present inventors have repeatedly conducted in-depth studies and found that by cleaning the resin composition, which is an aggregate containing polymer particles (A) and a resin (B) of a specific viscosity at a specific weight ratio, the impurities contained in the resin composition can be effectively reduced. In particular, it was found that when the resin composition containing polymer particles (A) and resin (B) is not in the form of powder or granules, but in the form of liquid, paste (a viscous rubber-like substance), or crumb (also called a star candy shape), an excellent cleaning effect is achieved.

[0022] The present inventors have established the following relationship with respect to the weight ratio of polymer particles (A) and resin (B) in a resin composition and their shapes: when the total of polymer particles (A) and resin (B) is taken as 100 wt %, (i) when the polymer particles (A) exceed 0 wt % and are less than 30 wt %, the composition is in a liquid state; (ii) when the polymer particles (A) are 30 wt % to less than 50 wt %, the composition is in a paste state; (iii) when the polymer particles (A) are 50 wt % to 70 wt %, the composition is in a crumb state; and (iv) when the polymer particles (A) exceed 70 wt %, the composition tends to be in a powdery state.

[0023] The shapes of the resin composition are mainly in accordance with the above-mentioned definitions, but other definitions include the following: after the resin composition is pulverized by a mill, when the total of the polymer fine particles (A) and the resin (B) is taken as 100% by weight, (v) when the polymer fine particles (A) exceed 0% by weight and less than 50% by weight, and 20% or more of the polymer fine particles pass through the metal mesh after being placed on a metal mesh of 8 mesh at 25°C for 10 minutes, it is a liquid state; (vi) when the polymer fine particles (A) exceed 0% by weight and less than 50% by weight, and 20% or more of the polymer fine particles do not pass through the metal mesh after being placed on a metal mesh of 8 mesh at 25°C for 10 minutes, it is a paste state; (vii) when the polymer fine particles (A) exceed 50% by weight and less than 100% by weight, and 20% or more of the polymer fine particles do not pass through the metal mesh after being placed on a metal mesh of 8 mesh at 25°C for 10 minutes, it is a crumb state; (viii) when the polymer fine particles (A) exceed 50% by weight and less than 100% by weight, and 20% or more of the polymer fine particles pass through the metal mesh after being placed on a metal mesh of 8 mesh at 25°C for 10 minutes, it is a powder state.

[0024] In addition, by mixing polymer particles (A) and a resin (B) having a specific viscosity, a resin composition in which polymer particles (A) are uniformly dispersed in the resin (B) is obtained. In the case where the resin composition in which the polymer particles (A) are uniformly dispersed in the resin (B) is in the form of a liquid, paste or crumbs, impurities can be effectively reduced by cleaning. In addition, since the cleaning efficiency is high, the cleaning water can be reduced and the manufacturing equipment can be reduced. Due to the increased productivity, the drainage is also reduced, thereby reducing the environmental load. It should be noted that the reduced cleaning efficiency in the case of a powdery granular body means that impurities located on the surface of the powdery granular body as an agglomerate can be removed, and it is speculated that this is because the impurities located inside the powdery granular body cannot be removed. In this manufacturing method, a resin composition in a shape other than the above-mentioned powdery granular body, that is, a liquid, paste or crumb-like resin composition is used as an object.

[0025] In this specification, "powder and granule" includes both powder and granule, and refers to an aggregate of powder, granule, etc. In addition, in the case of special distinction, "powder" refers to a powder with a volume average particle size of 0.01mm to 0.1mm, and "granule" refers to a volume average particle size of 0.1mm to 10mm. Among them, powders with a coarse particle size of 10mm or more can be included in the powder and granule. In addition, the "volume average particle size" in the range of less than 10μm can be measured using a dynamic light scattering (DLS) particle size distribution measuring device Nanotrac WaveII-EX150 (manufactured by Micro Track Bell Co., Ltd.), and the "volume average particle size" in the range of more than 10μm can be measured using a laser diffraction particle size distribution measuring device Micro Track MT3000II (manufactured by Micro Track Bell Co., Ltd.).

[0026] In addition, according to the present manufacturing method, a low-inclusion aggregate can be obtained. In addition, since no organic solvent is used, the environmental load is small and the negative impact on the human body is also small. In addition, since there are few impurities (water-soluble compounds) from emulsifiers, coagulants (inorganic salts) and metal soaps, the quality of the resin composition (cured product) such as coloring and storage stability is improved. In addition, it is suitable for use in electronic materials and the like.

[0027] Hereinafter, each step of the present production method will be described in detail, and then the polymer fine particles (A), the resin (B), etc. will be described.

[0028] (1-1. Cleaning process)

[0029] The present production method may include a washing step of washing the resin composition with water. By washing the resin composition as an aggregate, a resin composition having a small content of inclusions etc. is obtained. The washing step is more preferably washing with ion exchange water or pure water.

[0030] The washing step may be a step of washing the resin composition with water, and the specific method is not particularly limited. For example, the resin composition and water are mixed and sheared by a stirrer, a homogenizer, a high shear emulsifier, etc., a method of kneading the resin composition and water using a kneader, a method of mixing using a rotation and revolution mixer, and the like. As the kneader, various batch kneaders, continuous kneaders, extruders, etc. can be used.

[0031] This cleaning process can be carried out in various embodiments without particular limitation. For example, there can be mentioned: (i) an emulsifier is provided in a container into which the resin composition is put, and the process is carried out in a batch process, (ii) the resin composition is circulated through an emulsifier and the like and the process is carried out multiple times, (iii) an emulsifier is provided on the flow path of the resin composition, and the cleaning process is continuously carried out, (iv) the process is carried out multiple times through an emulsifier in the process (iii), (v) the resin composition passed through an emulsifier in the process (iii) or (iv) is separated into aggregates and water, and the process (iii) or (iv) is cleaned multiple times, etc.

[0032] The washing time is not particularly limited, and may be, for example, 1 second to 60 seconds, preferably 1 second to 45 minutes, and more preferably 1 second to 30 minutes.

[0033] The number of times of washing is not particularly limited, and for example, it is 1 to 10 times, preferably 1 to 6 times, and more preferably 1 to 4 times.

[0034] The amount of washing water is not particularly limited, and for example, 0.5 to 1000 parts by weight, preferably 1 to 500 parts by weight, and more preferably 5 to 200 parts by weight can be cited relative to 1 part by weight of the resin composition. In addition, when washing is performed by kneading using a kneader, the amount of washing water can be reduced, which is more preferred.

[0035] The temperature of the washing water is not limited, and for example, room temperature or heated water can be used appropriately. Examples of the temperature of the warm water include 10°C to 100°C, preferably 15°C to 90°C, more preferably 20°C to 85°C, and particularly preferably 25°C to 60°C. Since warm water has a good washing effect, heated washing water is used. In addition, when the resin composition is thermally degraded, a low washing temperature is preferred, and a short washing time is preferred.

[0036] It is particularly preferred that the temperature of the water in the washing process is below 60°C. When the washing temperature is below 60°C, the viscosity of the resin composition becomes a viscosity that is not easy to wash away impurities by washing, which can improve the washing efficiency. When the viscosity of the object to be washed is low, the washing efficiency is usually high. In other words, it can be said that the viscosity of the object to be washed usually becomes lower and the washing efficiency is improved at high temperatures. However, as a result of the inventor's in-depth research, it was surprisingly found that in the washing process of the present manufacturing method, when the temperature during washing is below the specified temperature, the viscosity is higher than at high temperatures, and on the other hand, the washing efficiency is improved.

[0037] When the temperature during the above-mentioned cleaning is below the specified temperature, the object to be cleaned becomes a so-called viscous region, and it is inferred that impurities can be cleaned efficiently. Cleaning in a viscous region can be in other words a process of cleaning with a loss tangent tan (δ) ln of more than 1. The mechanism by which cleaning can be efficiently performed in a viscous region can be inferred as follows. The resin composition comprising polymer particles (A) and resin (B) of the present manufacturing method has a tendency to decrease in viscosity with temperature rise, and tan δ decreases. Thus, the present inventors, in the case of a viscosity-dominated domain based on the above-mentioned resin composition tan δ being more than 1, the distribution and mixing of polymer particles (A) in the resin composition is improved, and on the other hand, it is inferred that the dispersion and mixing of polymer particles (A) is reduced in an elastic-dominated domain of less than 1. That is, if elastic dominance is achieved, the polymer particles (A) in the resin composition form clusters with each other, and the resin (B) obtained inside it floats to the surface, and the cleaning efficiency is further deteriorated. In particular, when the concentration of polymer particles (A) is low, it is inferred that the clusters become larger and the cleaning efficiency is further deteriorated. Therefore, it is presumed that by setting the temperature during washing to a predetermined value or less and performing washing in a viscosity-dominated region with high viscosity, impurities present between particles of the polymer microparticles (A) can be efficiently discharged.

[0038] In addition, the higher the concentration of the polymer microparticles (A) in the resin composition, the higher the viscosity of the resin composition tends to be. In the cleaning step of the present production method, the cleaning efficiency may be improved when the concentration of the polymer microparticles (A) is high, that is, when the viscosity of the resin composition is high. As described above, it is generally believed that the object to be cleaned is easier to clean when the viscosity is low, so it can be said that there is specificity in the cleaning step of the present production method.

[0039] The method for removing the washing water is not limited, and examples thereof include extraction of the washing water, reduced pressure filtration, oil-water separation, and squeeze dehydration.

[0040] The objects to be cleaned refer to all impurities contained in the resin composition without particular limitation, and include, in addition to inclusions from emulsifiers (e.g., phosphorus-based emulsifiers, sulfonic acid-based emulsifiers), inclusions from coagulants when the coagulant described later is used, etc.

[0041] Examples of the emulsifier include (a) anionic emulsifiers such as the acids exemplified below, alkali metal salts of the acids, or ammonium salts of the acids, (b) nonionic emulsifiers such as alkyl or aryl substituted polyethylene glycol, and (c) polyvinyl alcohol, alkyl substituted cellulose, polyvinyl pyrrolidone, polyacrylic acid derivatives, etc. Examples of the above-mentioned acids include (a1) alkyl or aryl sulfonic acids or alkyl or aryl ether sulfonic acids represented by dioctyl sulfosuccinic acid and dodecylbenzenesulfonic acid, (a2) alkyl or aryl sulfuric acids or alkyl or aryl ether sulfuric acids represented by dodecyl sulfuric acid, (a3) ​​alkyl or aryl substituted phosphoric acids or alkyl or aryl ether substituted phosphoric acids, (a4) N-alkyl or aryl sarcosine represented by dodecyl sarcosine, and (a5) alkyl or aryl carboxylic acids or alkyl or aryl ether carboxylic acids represented by oleic acid and stearic acid. Here, anionic emulsifiers formed from the acids described in (a1) and (a2) are referred to as sulfur-based emulsifiers, anionic emulsifiers formed from the acids described in (a3) ​​are referred to as phosphorus-based emulsifiers, anionic emulsifiers formed from the acids described in (a4) are referred to as sarcosine-based emulsifiers, and anionic emulsifiers formed from the acids described in (a5) are referred to as carboxylic acid-based emulsifiers. These emulsifiers may be used alone or in combination of two or more.

[0042] (1-2. Aggregation process)

[0043] Furthermore, the present production method preferably comprises a coagulation step of obtaining the above-mentioned resin composition from latex as an aggregate containing polymer microparticles (A) and resin (B) by using at least one method selected from the group consisting of a coagulant, shearing, and freezing. In this coagulation step, the resin composition can be recovered from the latex as an aggregate, and the coagulant, shearing, and freezing can be implemented separately or in combination. In addition, this coagulation step is preferably implemented before the cleaning step.

[0044] (Coagulant)

[0045] As the coagulant, an aqueous solution of an inorganic acid (salt) and / or an organic acid (salt) having the property of coagulating and solidifying the emulsion polymer latex, or a high molecular weight coagulant may be used. For example, preferably, inorganic salts such as sodium chloride, potassium chloride, lithium chloride, sodium bromide, potassium bromide, lithium bromide, potassium iodide, sodium iodide, potassium sulfate, sodium sulfate, ammonium sulfate, ammonium chloride, sodium nitrate, potassium nitrate, calcium chloride, ferrous sulfate, magnesium sulfate, zinc sulfate, copper sulfate, barium chloride, ferric chloride, ferrous chloride, magnesium chloride, ferrous sulfate, aluminum sulfate, potassium alum, and iron alum are used. Aqueous solution; aqueous solution of inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid; organic acids such as acetic acid and formic acid and their aqueous solutions, aqueous solutions of organic acid salts such as sodium acetate, calcium acetate, sodium formate, and calcium formate, as a polymer coagulant, it can be a polymer compound having a hydrophilic group and a hydrophobic group, without special limitation, and can also be any polymer coagulant in anionic, cationic, and nonionic systems. From the viewpoint of further improving the effect of one embodiment of the present invention, a cationic polymer coagulant is preferably used. As a cationic polymer coagulant, a polymer coagulant having a cationic group in the molecule, that is, a polymer coagulant showing cationicity when dissolved in water, such as polyamines, polydicyanamides, cationized starch, cationic poly (meth) acrylic acid amide, water-soluble aniline resin, polythiourea, polyethyleneimine, quaternary ammonium salts, polyvinyl pyridines, chitosan, etc. can be mixed and used, and two or more can be used alone or in combination. Among these, aqueous solutions of monovalent or divalent inorganic salts or inorganic acids such as sodium chloride, potassium chloride, sodium sulfate, ammonium chloride, calcium chloride, magnesium chloride, magnesium sulfate, barium chloride, hydrochloric acid, and sulfuric acid can be preferably used.

[0046] There is no particular limitation on the method for adding the coagulant, and the coagulant may be added all at once, added in batches, or added continuously. The coagulant may be added to the latex containing the polymer microparticles (A), and then the resin (B) may be mixed in the latex, or the coagulant may be added to the resin (B), and then the latex containing the polymer microparticles (A) and the resin (B) may be mixed. Alternatively, the coagulant may be added to the latex containing the polymer microparticles (A) and the resin (B).

[0047] The amount of the coagulant added may be 1 to 50 parts by weight, preferably 2 to 30 parts by weight, more preferably 3 to 20 parts by weight, relative to 100 parts by weight of the resin composition. The amount of the coagulant added may be appropriately changed depending on the type of latex.

[0048] The concentration of the polymer fine particles (A) in the latex is preferably 20% to 70%, more preferably 25% to 65%, further preferably 30% to 60%, further preferably 35% to 55%. Within this range, the efficiency of obtaining aggregates is improved.

[0049] When the resin (B) to which a coagulant has been previously added is mixed with the latex containing the polymer fine particles (A), or when the coagulant is added to the latex containing the polymer fine particles (A) and the resin (B), the granulation step is not required and the process can be simplified.

[0050] (shear)

[0051] This is a method for recovering aggregates, i.e., a resin composition, from latex by weakening emulsification through shearing. For example, there can be mentioned a step of mixing a resin (B) with a latex containing polymer microparticles (A); a shearing step of imparting shear stress to the latex obtained by the above step; and a step of separating an aggregate, i.e., a resin composition, containing polymer microparticles (A) and resin (B) and a water component from the latex after the above shearing step.

[0052] The method of applying shear stress to the latex is not particularly limited, and examples thereof include methods using a homomixer, a high shear emulsifier, and the like.

[0053] In addition, in this process, as a pre-stage of mixing polymer particles (A) and resin (B), a method of pre-applying shear stress to the latex containing polymer particles (A) before mixing resin (B). In addition, a method of pre-applying shear stress to resin (B) is also included. Moreover, it can also be a method of applying shear stress to both the latex containing polymer particles (A) and the resin (B) before the step of mixing polymer particles (A) and resin (B). These methods are preferred from the viewpoint of weakening the emulsifying power of the latex and efficiently obtaining an agglomerate.

[0054] (freeze)

[0055] As an example of a method for obtaining an agglomerate by freezing, there can be cited a method comprising the following steps: a step of rapidly freezing a latex containing polymer particles (A); a step of thawing the frozen latex by the above step; a step of mixing a resin (B) with the latex after the above step; and a separation step of separating an agglomerate containing polymer particles (A) and resin (B), i.e., a resin composition and a water component from the latex after the above thawing step and the resin mixing step.

[0056] The rapid freezing process is a process of rapidly freezing the latex containing polymer particles (A). In this specification, "rapid freezing" means that the latex is preferably thawed in 1 second to less than 20 minutes, and the latex is frozen in 10 seconds to 10 minutes. There is no particular limitation on the specific method of rapid freezing, and various techniques related to flash freezing and rapid freezing can be used. For example, preferably exemplified are a method of contacting the latex with a metal surface cooled to -80°C to -10°C; a method of spraying the latex into cold air using a spray cooler to instantly cool and solidify it; a method of adding latex to liquid nitrogen; a method of contacting dry ice with latex, etc.

[0057] It should be noted that the step of mixing the resin (B) can be performed at any stage before or after the thawing step. For example, when it is performed before the thawing step, the resin (B) can be added to the frozen latex, and then the latex can be thawed to mix the latex and the resin (B). Alternatively, when it is performed after the thawing step, the resin (B) can be added to the thawed latex and mixed.

[0058] In addition, as another example of a method for performing freeze coagulation, there can be cited a method comprising the following steps: a step of mixing a resin (B) into a latex containing polymer particles (A); a freezing step of freezing the latex in which the resin (B) obtained by the above step is dispersed; a step of thawing the latex frozen by the above step; and a separation step of separating an aggregate containing polymer particles (A) and resin (B), i.e., a resin composition and a water component, from the latex after the above step.

[0059] The "freezing" of the method of the other examples mentioned above includes a process of rapid freezing and a process of slow freezing. The method of rapid freezing is the same as the above. In addition, "slow freezing" preferably freezes the latex in 20 minutes to 24 hours, and freezes the latex in 30 minutes to 12 hours. For example, as an example of a method with a slow freezing speed, a method of directly placing the latex in a freezer can be cited, and as an example of a method with a fast freezing speed, a method of leaving the latex on a metal surface when placing it in a freezer can be cited.

[0060] (1-3. Intermediate cleaning process)

[0061] In the present manufacturing method, the above-mentioned coagulation step preferably includes the following steps: a first coagulation step of obtaining agglomerates containing polymer particles (A) from a latex containing polymer particles (A); an intermediate washing step of washing the agglomerates obtained in the above-mentioned first coagulation step with water; and a second coagulation step of mixing the agglomerates after the above-mentioned intermediate washing step with a resin (B) to obtain agglomerates containing polymer particles (A) and resin (B).

[0062] This method is a method in which an aggregate containing polymer microparticles (A) is first obtained and then washed at once, and then a resin (B) is mixed, and finally an aggregate containing polymer microparticles (A) and resin (B), i.e., a resin composition, is recovered. The above-mentioned washing step can be subsequently performed to wash in multiple stages, and a resin composition with less impurities can be obtained.

[0063] In the first and second coagulation steps, as a method of obtaining an aggregate, shearing or freezing of the coagulant can be mentioned.

[0064] In addition, for this intermediate washing step, the same method as the above-mentioned washing step can be used. Here, this intermediate washing step preferably includes washing the agglomerates obtained in the above-mentioned first coagulation step with water having a temperature lower than the glass transition temperature (Tg) of the above-mentioned polymer particles (A). In addition, the Tg of the polymer particles (A) refers to the Tg of the grafted part described later. In addition, this intermediate washing step more preferably includes a step of washing the agglomerates obtained in the above-mentioned first coagulation step with water below 40°C, and further preferably below 30°C. This is because the agglomerates containing the polymer particles (A) obtained in the above-mentioned first coagulation step are washed in this temperature range, so that the agglomerates can be slowly obtained, and then it is easy to disperse evenly when mixed with the resin (B), which has such an advantage.

[0065] (1-4. Polymer microparticles (A))

[0066] The polymer microparticles (A) may be microparticles obtained by polymerization, and are not particularly limited. As the polymer microparticles (A), for example, as constituent units, it is preferred that the polymer microparticles (A) have a graft portion composed of a polymer containing constituent units of one or more monomers selected from aromatic vinyl monomers, vinyl cyanide monomers, and (meth)acrylate monomers. The polymer microparticles (A) may be referred to as graft copolymers.

[0067] (Grafting)

[0068] In this specification, a polymer to which any polymer is graft-bonded is referred to as a graft portion. The graft portion is composed of a polymer comprising constituent units derived from one or more monomers selected from aromatic vinyl monomers, vinyl cyanide monomers, and (meth)acrylate monomers. The graft portion has the above-mentioned structure and can play various roles. "Various roles" include, for example, (a) improving the compatibility of polymer particles (A) and thermosetting resins, (b) improving the dispersibility of polymer particles (A) of the matrix resin, i.e., thermosetting resin, which is the mixing object, and (c) dispersing polymer particles (A) in the form of primary particles in a resin composition or its cured product.

[0069] Specific examples of the aromatic vinyl monomer include styrene, α-methylstyrene, p-methylstyrene, and divinylbenzene.

[0070] Specific examples of the vinyl cyanide monomer include acrylonitrile and methacrylonitrile.

[0071] Specific examples of the (meth)acrylate monomer include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hydroxyethyl (meth)acrylate, and hydroxybutyl (meth)acrylate. In the present specification, (meth)acrylate refers to acrylate and / or methacrylate.

[0072] The one or more monomers selected from the group consisting of aromatic vinyl monomers, vinyl cyanide monomers and (meth)acrylate monomers may be used alone or in combination of two or more.

[0073] The grafted portion preferably comprises a constituent unit derived from a monomer containing a reactive group. The reactive group-containing monomer preferably comprises a monomer selected from epoxy, oxetane, hydroxyl, amino, imide, carboxylic acid, carboxylic anhydride, cyclic ether, cyclic amide, benzoic acid, The present invention is a monomer containing one or more reactive groups selected from the group consisting of an oxazine group and a cyanate group, and more preferably a monomer containing one or more reactive groups selected from the group consisting of an epoxy group, a hydroxyl group and a carboxylic acid group. If the above-mentioned structure is adopted, the grafted portion of the polymer microparticles (A) can be chemically bonded to the thermosetting resin in the resin composition. Thus, the polymer microparticles (A) can be maintained in a good dispersion state in the resin composition or in its cured product without agglomerating the polymer microparticles (A).

[0074] Specific examples of the monomer having an epoxy group include glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, and allyl glycidyl ether.

[0075] Specific examples of monomers having a hydroxyl group include, for example, hydroxyl straight-chain alkyl (meth)acrylates (particularly hydroxyl straight-chain C1-6 alkyl (meth)acrylates) such as ethyl 2-hydroxy(meth)acrylate, hydroxypropyl (meth)acrylate, and butyl 4-hydroxy(meth)acrylate; caprolactone-modified hydroxy(meth)acrylates; hydroxyl straight-chain alkyl (meth)acrylates such as methyl α-(hydroxymethyl)acrylate and ethyl α-(hydroxymethyl)acrylate; hydroxyl-containing (meth)acrylates such as mono(meth)acrylates of polyester diols (particularly saturated polyester diols) obtained from dicarboxylic acids (phthalic acid, etc.) and diols (propylene glycol, etc.); and the like.

[0076] Specific examples of the monomer having a carboxylic acid group include monocarboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid, and dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid. As the monomer having a carboxylic acid group, the above monocarboxylic acids can be preferably used.

[0077] The above-mentioned reactive group-containing monomers may be used alone or in combination of two or more.

[0078] The grafted portion preferably contains 0.5 to 90% by weight of the constituent unit derived from the monomer containing a reactive group in 100% by weight of the grafted portion, more preferably 1 to 50% by weight, further preferably 2 to 35% by weight, and particularly preferably 3 to 20% by weight. The grafted portion has the following advantages: in the case where the constituent unit (a) derived from the monomer containing a reactive group contains 0.5% by weight or more in 100% by weight of the grafted portion, the obtained resin composition can provide a cured product having sufficient impact resistance, and in the case where the constituent unit (b) contains 90% by weight or less, the obtained resin composition can provide a cured product having sufficient impact resistance, and the storage stability of the resin composition is good.

[0079] The constituent unit derived from the reactive group-containing monomer is preferably contained in the graft portion, and more preferably contained only in the graft portion.

[0080] The grafted portion may include a constituent unit derived from a multifunctional monomer. When the grafted portion includes a constituent unit derived from a multifunctional monomer, the following advantages are achieved: (a) swelling of the polymer microparticles (A) can be prevented in the resin composition, (b) the resin composition has good workability due to the low viscosity of the resin composition, and (c) the dispersibility of the polymer microparticles (A) of the thermosetting resin is improved.

[0081] When the graft portion does not include a structural unit derived from a polyfunctional monomer, the obtained resin composition can provide a cured product having excellent toughness and impact resistance, compared with a case where the graft portion includes a structural unit derived from a polyfunctional monomer.

[0082] A multifunctional monomer may also be referred to as a monomer having two or more free radical polymerizable reaction groups in the same molecule. The free radical polymerizable reaction group is preferably a carbon-carbon double bond. As a multifunctional monomer, examples include (meth)acrylates that do not contain butadiene and have ethylenically unsaturated double bonds such as allyl (meth)acrylate. As monomers having two (meth)acrylate groups, examples include ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, and polyethylene glycol di(meth)acrylates. As the polyethylene glycol di(meth)acrylates, examples include triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol (600) di(meth)acrylate, and the like. In addition, as a monomer having three (meth)acrylate groups, alkoxy ester trimethylolpropane tri(meth)acrylate, glycerol propoxy tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, etc. can be exemplified. As alkoxy acidic ester trimethylolpropane tri(meth)acrylates, trimethylolpropane tri(meth)acrylate, trimethylolpropane triethoxy tri(meth)acrylate, etc. can be exemplified. And as a monomer having four (meth)acrylate groups, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, etc. can be exemplified. And, as a monomer having five (meth)acrylate groups, dipentaerythritol penta(meth)acrylate, etc. can be exemplified. And, as a monomer having six (meth)acrylate groups, ditrimethylolpropane hexa(meth)acrylate, etc. can be exemplified.

[0083] Among the above-mentioned multifunctional monomers, examples of the multifunctional monomers that can be used in the polymerization of the graft portion include allyl methacrylate, ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, and polyethylene glycol di(meth)acrylates. These multifunctional monomers may be used alone or in combination of two or more.

[0084] The graft portion preferably contains 1 to 20% by weight, more preferably 5 to 15% by weight, of the structural unit derived from the polyfunctional monomer based on 100% by weight of the graft portion.

[0085] The graft portion may include a structural unit derived from another monomer in addition to the structural unit derived from the above-mentioned monomer.

[0086] In addition, the graft portion is preferably a polymer graft-bonded to an elastomer described later.

[0087] (Glass transition temperature of grafted portion)

[0088] The glass transition temperature of the grafted portion is preferably 190°C or less, more preferably 160°C or less, more preferably 140°C or less, more preferably 120°C or less, preferably 80°C or less, more preferably 70°C or less, more preferably 60°C or less, more preferably 50°C or less, more preferably 40°C or less, more preferably 30°C or less, more preferably 20°C or less, more preferably 10°C or less, more preferably 0°C or less, more preferably -20°C or less, more preferably -40°C or less, more preferably -45°C or less, more preferably - The temperature of the present invention is preferably below -50°C, more preferably below -55°C, more preferably below -60°C, more preferably below -65°C, more preferably below -70°C, more preferably below -75°C, more preferably below -80°C, more preferably below -85°C, more preferably below -90°C, more preferably below -95°C, more preferably below -100°C, more preferably below -105°C, more preferably below -110°C, more preferably below -115°C, further preferably below -120°C, and particularly preferably below -125°C.

[0089] The glass transition temperature of the grafted portion is preferably 0°C or higher, more preferably 30°C or higher, more preferably 50°C or higher, more preferably 70°C or higher, further preferably 90°C or higher, and particularly preferably 110°C or lower.

[0090] The Tg of the grafted portion can be determined by the composition of the structural units contained in the grafted portion, etc. In other words, the Tg of the obtained grafted portion can be adjusted by changing the composition of the monomers used when producing (polymerizing) the grafted portion.

[0091] The Tg of the grafted portion can be obtained by measuring the viscoelasticity using a flat plate composed of polymer particles. Specifically, the Tg can be measured as follows: (1) For a flat plate composed of polymer particles, a dynamic viscoelasticity measuring device (e.g., DVA-200 manufactured by IT Instrumentation and Control Co., Ltd.) is used to measure the dynamic viscoelasticity under stretching conditions to obtain a tanδ coordinate graph; (2) For the obtained tanδ coordinate graph, the peak temperature of tanδ is used as the glass transition temperature. Here, when multiple peaks are obtained in the tanδ coordinate graph, the highest peak temperature is used as the glass transition temperature of the grafted portion.

[0092] (Grafting rate of grafted part)

[0093] In one embodiment of the present invention, the polymer microparticles (A) are polymers having the same structure as the grafted portion, and may have a polymer that is not graft-bonded to the elastomer described later. In this specification, a polymer having the same structure as the grafted portion and a polymer that is not graft-bonded to the elastomer described later is referred to as a non-grafted polymer. The non-grafted polymer constitutes a part of the polymer microparticles (A) involved in one embodiment of the present invention. It can be said that the non-grafted polymer is a polymer that is not graft-bonded to the elastomer described later in the polymer produced in the polymerization of the grafted portion.

[0094] In this specification, the proportion of the polymer grafted to the elastomer described later, i.e., the graft portion, in the polymer produced by polymerization of the graft portion is referred to as the graft ratio. The graft ratio can be expressed as a value represented by (weight of the graft portion) / {(weight of the graft portion)+(weight of the grafted polymer)}×100.

[0095] The grafting rate of the grafted portion is preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more. When the grafting rate is 70% or more, there is an advantage that the viscosity of the resin composition does not become too high.

[0096] In this specification, the method for calculating the grafting rate is as follows. First, an aqueous latex containing polymer particles (A) is obtained, and then a powder of the polymer particles (A) is obtained from the aqueous latex. As a method for obtaining a powder of polymer particles (A) from an aqueous latex, specifically, there can be cited a method of (i) coagulating the polymer particles (A) in the above-mentioned aqueous latex, (ii) dehydrating the obtained coagulant, and (iii) further drying the coagulant to obtain a powder of polymer particles (A). Next, 2 g of the powder of the polymer particles (A) is dissolved in 50 mL of methyl ethyl ketone (hereinafter, also referred to as MEK). Thereafter, the obtained MEK solute is separated into a component soluble in MEK (MEK soluble component) and a component insoluble in MEK (MEK insoluble component). Specifically, a centrifuge (manufactured by Hitachi Koki Co., Ltd., CP60E) was used to centrifuge the obtained MEK dissolved product at a rotation speed of 30,000 rpm for 1 hour to separate the dissolved product into a MEK soluble component and a MEK insoluble component. Here, a total of 3 sets of centrifugal separation operations were performed. The weights of the obtained MEK soluble component and the MEK insoluble component were measured, and the grafting rate was calculated using the following formula.

[0097] Grafting rate (%) = {(weight of methyl ethyl ketone insoluble component) - (weight of polymer other than grafted portion)} / (weight of polymer other than grafted portion) × 100

[0098] In addition, the weight of the polymer outside the graft portion is the amount of monomers added to form the polymer outside the graft portion. The polymer outside the graft portion is, for example, an elastomer. In addition, when the polymer particles (A) are surface crosslinked polymers described later, the polymer outside the graft portion includes both elastomers and surface crosslinked polymers. In addition, in the calculation of the grafting rate, the method for coagulating the polymer particles (A) is not particularly limited, and a method using a solvent, a method using a coagulant, a method of spraying an aqueous latex, etc. can be used.

[0099] (Glass transition temperature of grafted portion)

[0100] The glass transition temperature (hereinafter, sometimes simply referred to as "Tg") of the grafted portion is preferably 190°C or lower, more preferably 160°C or lower, further preferably 140°C or lower, particularly preferably 120°C or lower.

[0101] The Tg of the grafted portion can be determined by the composition of the structural units contained in the grafted portion, etc. In other words, the Tg of the obtained grafted portion can be adjusted by changing the composition of the monomers used when producing (polymerizing) the grafted portion.

[0102] The Tg of the grafted portion was measured using a differential scanning calorimeter (DSC) (SSC-5200, manufactured by Seiko Instruments). The sample was heated to 200°C at a rate of 25°C / min, then kept for 10 minutes, and then the temperature was lowered to 50°C at a rate of 25°C / min. The sample was heated to 200°C at a rate of 10°C / min. The integral value was calculated from the DSC curve, and the Tg was calculated from the maximum point. In the case of multiple maximum points, the Tg of the grafted portion was calculated from the maximum point with the highest temperature.

[0103] (Modification of the graft portion)

[0104] In one embodiment of the present invention, the graft portion may be composed of only one type of graft portion having constituent units of the same composition. In one embodiment of the present invention, the graft portion may be composed of a plurality of types of graft portions having constituent units of different compositions.

[0105] In one embodiment of the present invention, a case where the grafted portion is composed of a plurality of grafted portions will be described. In this case, the plurality of grafted portions are respectively designated as grafted portion 1, grafted portion 2, ..., grafted portion 3, and grafted portion 4. n (n is an integer greater than or equal to 2). The graft portion may include a graft portion 1, a graft portion 2, ... and a graft portion 3, which are polymerized separately. n The grafted portion may include grafted portion 1, grafted portion 2, ... grafted portion nThe polymers obtained by sequentially polymerizing the multiple polymers (grafting parts) are referred to as multi-stage polymerization. The polymer obtained by multi-stage polymerization of multiple grafting parts is referred to as a multi-stage polymerization grafting part. The method for producing the multi-stage polymerization grafting part is described in detail below.

[0106] In the case where the grafted portion is composed of multiple grafted portions, all of these multiple grafted portions may not be graft-bonded to the elastomer. At least a part of at least one type of grafted portion may be graft-bonded to the elastomer, and other types of (other multiple types of) grafted portions may be graft-bonded to the grafted portion graft-bonded to the elastomer. In addition, in the case where the grafted portion is composed of multiple types of grafted portions, it may be a polymer having the same structure as the multiple types of grafted portions, and may have multiple polymers (multiple types of grafted polymers) that are not graft-bonded to the elastomer.

[0107] The grafted part 1, the grafted part 2, ... and the grafted part n The multi-stage polymer grafting section is described below. n Can cover the grafted part n-1 At least a portion of the grafted portion may be covered n-1 In the multi-stage polymer grafting part, the grafting part n A part of it can also enter the grafting part n-1 inside.

[0108] In a multi-stage polymer grafted portion, each of the multiple grafted portions may have a layer structure. For example, when a multi-stage polymer grafted portion is composed of a grafted portion 1, a grafted portion 2, and a grafted portion 3, the grafted portion 1 is the innermost layer of the grafted portion, a layer of the grafted portion 2 exists on the outside of the grafted portion 1, and further, a layer of the grafted portion 3 exists as the outermost layer on the outside of the layer of the grafted portion 2. In this way, a multi-stage polymer grafted portion in which each of the multiple grafted portions has a layer structure may be referred to as a multi-layer grafted portion. That is, in one embodiment of the present invention, the grafted portion may include a mixture of multiple grafted portions, a multi-stage polymer grafted portion, and / or a multi-layer grafted portion.

[0109] In the production of polymer microparticles (A), when the elastomer and the graft part are polymerized sequentially, at least a portion of the graft part can cover at least a portion of the elastomer in the obtained polymer microparticles (A). In other words, sequential polymerization of the elastomer and the graft part can be referred to as multi-stage polymerization of the elastomer and the graft part. The polymer microparticles (A) obtained by multi-stage polymerization of the elastomer and the graft part can be referred to as multi-stage polymers.

[0110] When the polymer microparticles (A) are multistage polymers, the grafted portion may cover at least a portion of the elastomer or the entire elastomer. When the polymer microparticles (A) are multistage polymers, a portion of the grafted portion may enter the inside of the elastomer.

[0111] When the polymer particles (A) are multi-stage polymers, the elastomer and the grafted portion may have a layer structure. For example, a method in which the elastomer is used as the innermost layer (also called the core layer), and the layer of the grafted portion exists as the outermost layer (also called the shell layer) on the outside of the elastomer is one method of the present invention. The structure in which the elastomer is used as the core layer and the grafted portion is used as the shell layer can be called a core-shell structure. In this way, the polymer particles (A) having a layer structure (core-shell structure) of the elastomer and the grafted portion can be called a multilayer polymer or a core-shell polymer. That is, in one embodiment of the present invention, the polymer particles (A) may be a multi-stage polymer, and / or may also be a multilayer polymer or a core-shell polymer. However, as long as there is a grafted portion, the polymer particles (A) are not limited to the above-mentioned structure.

[0112] At least a part of the grafted portion preferably covers at least a part of the elastomer. In other words, at least a part of the grafted portion preferably exists on the outermost side of the polymer microparticle (A).

[0113] (Elastomer)

[0114] The polymer particles (A) also preferably have an elastomer. That is, the polymer particles (A) are preferably a rubber-containing graft copolymer having an elastomer and a graft portion graft-bonded to the elastomer. Hereinafter, an embodiment of the present invention will be described by taking the case where the polymer particles (A) are rubber-containing graft copolymers.

[0115] The elastomer preferably includes one or more selected from diene rubber, (meth)acrylate rubber, polysiloxane, and rubber elastomer. The elastomer is also called rubber particles.

[0116] The case where the polymer fine particles (A) contain a diene rubber (case A) will be described. In case A, when the elastomer contains a diene rubber, the obtained resin composition can provide a cured product having excellent toughness and impact resistance.

[0117] The diene rubber is an elastomer containing a constituent unit derived from a diene monomer as a constituent unit. The diene monomer may also be referred to as a conjugated diene monomer. In case A, the diene rubber may contain 50 to 100% by weight of constituent units derived from a diene monomer in 100% by weight of constituent units, and 0 to 50% by weight of constituent units derived from vinyl monomers other than the diene monomers copolymerizable with the diene monomers. In case A, the diene rubber may contain constituent units of (meth)acrylate monomers in an amount less than the constituent units derived from the diene monomers.

[0118] Examples of the diene monomer include 1,3-butadiene, isoprene (2-methyl-1,3-butadiene), and 2-chloro-1,3-butadiene. These monomers may be used alone or in combination of two or more.

[0119] As the vinyl monomer other than the diene monomer copolymerizable with the diene monomer (hereinafter also referred to as vinyl monomer A), for example, vinyl aromatic hydrocarbons such as styrene, α-methylstyrene, monochlorostyrene, and dichlorostyrene; vinyl carboxylic acids such as acrylic acid and methacrylic acid; vinyl cyanides such as acrylonitrile and methacrylonitrile; chlorinated vinyls such as vinyl chloride, vinyl bromide, and chloroprene; vinyl acetate; olefins such as ethylene, propylene, butylene, and isobutylene; polyfunctional monomers such as diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene. The vinyl monomers other than the above diene monomers can be used alone or in combination of two or more. Among the vinyl monomers other than the above diene monomers, styrene is particularly preferred. In addition, in the diene rubber of case A, the constituent units derived from the vinyl monomers other than the diene monomers are arbitrary components. In case A, the diene rubber can be composed only of constituent units derived from diene monomers.

[0120] In case A, the diene rubber is preferably a butadiene rubber (also called polybutadiene rubber) composed of constituent units derived from 1,3-butadiene, or a copolymer of 1,3-butadiene and styrene, i.e., butadiene-styrene rubber (also called polystyrene-butadiene), and more preferably a butadiene rubber. If the above-mentioned composition is used, the desired effect brought about by the polymer particles (A) containing the diene rubber can be further exerted. In addition, from the viewpoint of improving the transparency of the obtained cured product by adjusting the refractive index, a butadiene-styrene rubber is more preferred.

[0121] The case where the elastomer includes a (meth)acrylate rubber (case B) will be described. In case B, a wide range of polymer designs of the elastomer can be achieved by combining a plurality of monomers.

[0122] The (meth)acrylate rubber is an elastomer containing constituent units derived from (meth)acrylate monomers. In case B, the (meth)acrylate rubber may contain 50 to 100% by weight of constituent units derived from (meth)acrylate monomers and 0 to 50% by weight of constituent units derived from vinyl monomers other than (meth)acrylate monomers copolymerizable with (meth)acrylate monomers, in 100% by weight of constituent units. In case B, the (meth)acrylate rubber may contain constituent units derived from diene monomers in a smaller amount than constituent units derived from (meth)acrylate monomers.

[0123] Examples of the (meth)acrylate monomers include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; aromatic ring-containing (meth)acrylates such as phenoxyethyl (meth)acrylate and benzyl (meth)acrylate; 2-hydroxyethyl (meth)acrylate, 4-hydroxyethyl (meth)acrylate, and the like; Hydroxyalkyl (meth)acrylates such as butyl (meth)acrylate; glycidyl (meth)acrylates such as glycidyl (meth)acrylate and glycidyl alkyl (meth)acrylate; alkoxyalkyl (meth)acrylates; allyl (meth)acrylate, allyl alkyl (meth)acrylates such as allyl alkyl (meth)acrylate; polyfunctional (meth)acrylates such as monoethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate. These (meth)acrylate monomers may be used alone or in combination of two or more. Among these (meth)acrylate monomers, ethyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate are particularly preferred.

[0124] As the vinyl monomers other than the (meth)acrylate monomers copolymerizable with the (meth)acrylate monomers (hereinafter also referred to as vinyl monomers other than the (meth)acrylate monomers), the monomers listed in the above-mentioned vinyl monomer A can be cited. Only one type of the vinyl monomers other than the (meth)acrylate monomers can be used, or two or more types can be used in combination. Among the vinyl monomers other than the (meth)acrylate monomers, styrene is particularly preferred. In addition, in the (meth)acrylate rubber of case B, the constituent units derived from the vinyl monomers other than the (meth)acrylate monomers are arbitrary components. In case B, the (meth)acrylate rubber can be composed only of constituent units derived from the (meth)acrylate monomers.

[0125] The case where the elastomer includes a silicone rubber-based elastomer (case C) will be described. In case C, the obtained resin composition has sufficient heat resistance and can provide a cured product having excellent impact resistance at low temperatures.

[0126] As polysiloxane rubber elastomers, for example, (a) polysiloxane polymers composed of alkyl or aryl 2-substituted cyanooxy units such as dimethylcyanooxy, diethylcyanooxy, methylphenylcyanooxy, diphenylcyanooxy, dimethylcyanooxy-diphenylcyanooxy, and (b) polysiloxane polymers composed of alkyl or aryl 1-substituted cyanooxy units such as organic hydrogen diene cyanooxy in which part of the alkyl group of the side chain is substituted with a hydrogen atom. These polysiloxane polymers can be used alone or in combination of two or more. Among these polysiloxane polymers, (a) is preferably a polymer composed of dimethylcyanooxy units, methylphenylcyanooxy units and / or dimethylcyanooxy-diphenylcyanooxy units because it can provide a cured product with excellent heat resistance of the obtained fat composition, and (b) is most preferably a polymer composed of dimethylcyanooxy units because it is easily available and economical.

[0127] In case C, the polymer fine particles (A) preferably contain 80 wt% or more, more preferably 90 wt% or more of the silicone rubber elastomer based on 100 wt% of the elastomer contained in the polymer fine particles (A). According to the above constitution, the obtained resin composition can provide a cured product having excellent heat resistance.

[0128] The elastomer may further include an elastomer other than diene rubber, (meth)acrylate rubber, and silicone rubber elastomer. Examples of the elastomer other than diene rubber, (meth)acrylate rubber, and silicone rubber elastomer include natural rubber.

[0129] (Cross-linked structure of elastomer)

[0130] From the viewpoint of ensuring the dispersion stability in the thermosetting resin of the polymer particles (A), it is preferred to introduce a cross-linked structure into an elastomer. As a method for introducing a cross-linked structure into an elastomer, a commonly used method can be adopted, for example, the following method can be cited. That is, in the manufacture of an elastomer, in the monomers that can constitute the elastomer, a cross-linked monomer such as a compound containing a multifunctional monomer and / or a thiol group is mixed, and then a method for polymerizing is carried out. In this specification, polymers such as elastomers are also referred to as polymerized polymers.

[0131] In addition, as a method for introducing a cross-linked structure into a polysiloxane rubber-based elastomer, the following methods can be cited: (a) a method of using a multifunctional alkoxysilane compound together with other materials when polymerizing a polysiloxane rubber-based elastomer, (b) a method of introducing a reactive group such as a vinyl reactive group or a mercapto group into a polysiloxane rubber-based elastomer and then adding a vinyl polymerizable monomer or an organic peroxide to carry out a free radical reaction, or (c) a method of mixing a cross-linking monomer such as a multifunctional monomer and / or a compound containing a mercapto group with other materials when polymerizing a polysiloxane rubber-based elastomer and then polymerizing the mixture.

[0132] Examples of the polyfunctional monomer include the polyfunctional monomers exemplified in the above-mentioned section (grafting part).

[0133] As the mercapto-containing compound, alkyl-substituted mercaptan, allyl-substituted mercaptan, aryl-substituted mercaptan, hydroxyl-substituted mercaptan, alkoxy-substituted mercaptan, cyano-substituted mercaptan, amino-substituted mercaptan, silyl-substituted mercaptan, acid-substituted mercaptan, halogen-substituted mercaptan and acyl-substituted mercaptan can be mentioned. As the alkyl-substituted mercaptan, an alkyl-substituted mercaptan having 1 to 20 carbon atoms is preferred, and an alkyl-substituted mercaptan having 1 to 10 carbon atoms is more preferred. As the aryl-substituted mercaptan, a phenyl-substituted mercaptan is preferred. As the alkoxy-substituted mercaptan, an alkoxy-substituted mercaptan having 1 to 20 carbon atoms is preferred, and an alkoxy-substituted mercaptan having 1 to 10 carbon atoms is more preferred. As the acid-substituted mercaptan, an alkyl-substituted mercaptan having 1 to 10 carbon atoms having a carboxyl group or an aryl-substituted mercaptan having 1 to 12 carbon atoms having a carboxyl group is preferred.

[0134] (Glass transition temperature of elastomer)

[0135] The glass transition temperature of the elastomer is preferably 80°C or less, more preferably 70°C or less, more preferably 60°C or less, more preferably 50°C or less, more preferably 40°C or less, more preferably 30°C or less, more preferably 20°C or less, more preferably 10°C or less, more preferably 0°C or less, more preferably -20°C or less, more preferably -40°C or less, more preferably -45°C or less, more preferably -50°C or less, more preferably -55°C or less, more preferably -60°C or less, more preferably -65°C or less, more preferably -70°C or less, more preferably -75°C or less, more preferably -80°C or less, more preferably -85°C or less, more preferably -90°C or less, more preferably -95°C or less, more preferably -100°C or less, more preferably -105°C or less, more preferably -110°C or less, more preferably -115°C or less, further preferably -120°C or less, and particularly preferably -125°C or less. In this specification, "glass transition temperature" may be referred to as "Tg". According to this structure, a powder or granule having a low Tg can be obtained. As a result, a resin composition containing the obtained powder or granule can provide a cured product or a molded product having excellent toughness. The Tg of the elastomer can be obtained by performing a viscoelasticity measurement using a flat plate composed of the elastomer. Specifically, the Tg can be measured as follows: (1) For a flat plate composed of an elastomer, a dynamic viscoelasticity measurement device (e.g., DVA-200 manufactured by IT Measurement and Control Co., Ltd.) is used to perform a dynamic viscoelasticity measurement under tensile conditions to obtain a coordinate graph of tan δ; (2) For the obtained coordinate graph of tan δ, the peak temperature of tan δ is set as the glass transition temperature. Here, in the coordinate graph of tan δ, when multiple peaks are obtained, the lowest peak temperature is set as the glass transition temperature of the elastomer.

[0136] On the other hand, since a cured product having sufficient elastic modulus (rigidity) can be obtained in which a decrease in the elastic modulus (rigidity) of the obtained cured product can be suppressed, the Tg of the elastomer is preferably greater than 0°C, more preferably above 20°C, further preferably above 50°C, particularly preferably above 80°C, and most preferably above 120°C.

[0137] The Tg of the elastomer can be determined by the composition of the structural units contained in the elastomer, etc. In other words, the Tg of the obtained elastomer can be adjusted by changing the composition of the monomers used when producing (polymerizing) the elastomer.

[0138] Here, when a homopolymer is prepared by polymerizing only one monomer, the group of monomers that provide a homopolymer having a Tg greater than 0°C is referred to as monomer group a. In addition, when a homopolymer is prepared by polymerizing only one monomer, the group of monomers that provide a homopolymer having a Tg less than 0°C is referred to as monomer group b. An elastomer comprising 50 to 100% by weight (more preferably 65 to 99% by weight) of constituent units derived from at least one monomer selected from monomer group a and 0 to 50% by weight (more preferably 1 to 35% by weight) of constituent units derived from at least one monomer selected from monomer group b is referred to as elastomer X. The Tg of elastomer X is greater than 0°C. In addition, when the elastomer comprises elastomer X, the obtained resin composition can provide a cured product having sufficient rigidity.

[0139] When the Tg of the elastomer is higher than 0° C., it is preferred to introduce a cross-linked structure into the elastomer. Examples of the method for introducing a cross-linked structure include the above-mentioned methods.

[0140] Monomers that can be included in the above monomer group a are not limited to the following, and examples thereof include unsubstituted vinyl aromatic compounds such as styrene and 2-vinylnaphthalene; vinyl substituted aromatic compounds such as α-methylstyrene; cycloalkylated vinyl aromatic compounds such as 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 3,5-dimethylstyrene, 2,4,6-trimethylstyrene; cycloalkoxylated vinyl aromatic compounds such as 4-methoxystyrene and 4-ethoxystyrene; cyclochlorinated vinyl aromatic compounds such as 2-chlorostyrene and 3-chlorostyrene; cyclic ether substituted vinyl aromatic compounds such as 4-ethoxystyrene; Aromatic compounds; ring-hydroxylated vinyl aromatic compounds such as 4-hydroxystyrene; vinyl ethers such as vinyl benzoate and vinyl cyclohexanoate; vinyl chlorides such as vinyl chloride; aromatic monomers such as acenaphthene and indene; alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, and isopropyl methacrylate; aromatic methacrylates such as phenyl methacrylate; methacrylates such as isobornyl methacrylate and trimethylsilyl methacrylate; methacrylic monomers including methacrylic acid derivatives such as methacrylonitrile; various acrylic acid ethers such as isobornyl acrylate and tert-butyl acrylate; acrylic acid monomers including acrylic acid derivatives such as acrylonitrile, etc. As monomers that can be included in the monomer group a, there can be mentioned monomers that can provide homopolymers having a Tg of 120° C. or higher, such as acrylic acid amide, isopropyl acrylic acid amide, N-vinyl pyrrolidone, isobornyl methacrylate, dicyclopentyl methacrylate, 2-methyl-2-adamantyl methacrylate, 1-adamantyl acrylate, and 1-adamantyl methacrylate. These monomers a can be used alone or in combination of two or more.

[0141] As the above-mentioned monomer b, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, (meth) acrylate, dodecyl (meth) acrylate, 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, etc. can be mentioned. Only one of these monomers b can be used, or two or more of them can be used in combination. Among these monomers b, ethyl acrylate, butyl acrylate and 2-ethylhexyl acrylate are particularly preferred.

[0142] (Volume average particle size of elastomer)

[0143] The volume average particle size of the elastomer is preferably 0.03 μm to 50.00 μm, more preferably 0.05 μm to 10.00 μm, more preferably 0.08 μm to 2.00 μm, further preferably 0.10 μm to 1.00 μm, further preferably 0.10 μm to 0.80 μm, and particularly preferably 0.10 μm to 0.50 μm. For the volume average particle size of the elastomer, (a) when it is 0.03 μm or more, an elastomer having a desired volume average particle size can be stably obtained, and (b) when it is 50.00 μm or less, the heat resistance and impact resistance of the obtained cured product or molded product are good. The volume average particle size of the elastomer can be measured using a dynamic light scattering particle size distribution measuring device or the like, including an aqueous latex of the elastomer as a sample. The method for measuring the volume average particle size of the elastomer is described in detail in the following examples.

[0144] (Ratio of elastic body)

[0145] The ratio of the elastomer in the polymer particles (A) is preferably 40 to 97% by weight, more preferably 60 to 95% by weight, and further preferably 70 to 93% by weight, based on the total weight of the polymer particles (A) as 100% by weight. With respect to the above ratio of the elastomer, (a) when it is 40% by weight or more, the obtained resin composition can provide a cured product having excellent toughness and impact resistance, and (b) when it is 97% by weight or less, the polymer particles (A) are not easily aggregated, and thus, when the resin composition does not become highly viscous, the obtained resin composition is excellent in handling.

[0146] (Gel content of elastomer)

[0147] The elastomer is swellable in a suitable solvent, but is preferably substantially insoluble. The elastomer is preferably not essential to the thermosetting resin used.

[0148] The gel content of the elastomer is preferably 60% by weight or more, more preferably 80% by weight or more, further preferably 90% by weight or more, and particularly preferably 95% by weight or more. When the gel content of the elastomer is within the above range, the obtained resin composition can provide a cured product with excellent toughness.

[0149] In this specification, the calculation method of gel content is as follows. First, an aqueous latex containing polymer particles (A) is obtained, and then a powder of polymer particles (A) is obtained from the aqueous latex. There is no particular limitation on the method for obtaining a powder of polymer particles (A) from an aqueous latex, and examples thereof include (i) a method for obtaining a powder of polymer particles (A) by agglomerating the polymer particles (A) in the aqueous latex, (ii) dehydrating the obtained agglomerates, and (iii) further drying the agglomerates. Next, 2.0 g of the powder of polymer particles (A) is dissolved in 50 mL of methyl ethyl ketone (MEK). Thereafter, the obtained MEK solubilized material is separated into components soluble in MEK (MEK soluble components) and components insoluble in MEK (MEK insoluble components). Specifically, the obtained MEK dissolved material was centrifuged at 30000 rpm for 1 hour using a centrifuge (manufactured by Hitachi Koki Co., Ltd., CP60E) to separate the dissolved material into a MEK soluble component and a MEK insoluble component. Here, a total of 3 sets of centrifugal separation operations were performed. The weights of the obtained MEK soluble component and the MEK insoluble component were measured, and the gel content was calculated using the following formula.

[0150] Gel content (%) = (weight of methyl ethyl ketone insoluble components) / {(weight of methyl ethyl ketone insoluble components) + (weight of methyl ethyl ketone soluble components)} × 100

[0151] (Deformation example of elastic body)

[0152] In one embodiment of the present invention, the elastomer is one selected from diene rubber, (meth)acrylate rubber and polysiloxane rubber elastomer, and may be composed of one elastomer having constituent units of the same composition. In one embodiment of the present invention, the elastomer may be composed of a plurality of elastomers having constituent units of different compositions.

[0153] In one embodiment of the present invention, a case where the elastic body is composed of a plurality of elastic bodies will be described. In this case, the plurality of elastic bodies are respectively set as elastic body 1, elastic body 2, ..., and elastic body 3. n Here, n is an integer greater than or equal to 2. The elastomer may include elastomer 1, elastomer 2, ... and elastomer 3 which are polymerized separately. n The elastomer may include elastomer 1, elastomer 2, ... and elastomer nPolymers obtained by multi-stage polymerization. A polymer obtained by multi-stage polymerization of a plurality of elastomers is referred to as a multi-stage polymerized elastomer. The method for producing a multi-stage polymerized elastomer will be described in detail below.

[0154] For elastic body 1, elastic body 2, ... and elastic body n The multi-stage polymerized elastomer is described. In the multi-stage polymerized elastomer, the elastomer n Can be coated with elastomer n-1 At least a portion of the n-1 In the multi-stage polymerized elastomer, the elastomer n Sometimes part of it enters the elastomer n-1 inside.

[0155] In a multi-stage polymeric elastomer, each of the multiple elastomers may have a layer structure. For example, when the multi-stage polymeric elastomer is composed of elastomer 1, elastomer 2, and elastomer 3, elastomer 1 is the innermost layer, and a layer of elastomer 2 exists outside elastomer 1, and further, a layer of elastomer 3 exists outside the layer of elastomer 2 as the outermost layer of the elastomer, which is also one embodiment of the present invention. In this way, a multi-stage polymeric elastomer in which each of the multiple elastomers has a layer structure may also be referred to as a multi-layer elastomer. That is, in one embodiment of the present invention, the elastomer may include a mixture of multiple elastomers, a multi-stage polymeric elastomer, and / or a multi-layer elastomer.

[0156] (Surface cross-linked polymer)

[0157] The polymer particles (A) preferably have a surface crosslinked polymer outside the grafted portion formed by graft bonding to the elastomer and the elastomer. According to the above-mentioned constitution, (a) in the manufacture of the polymer particles (A), the anti-blocking property can be improved, and (b) the dispersibility of the polymer particles (A) of the thermosetting resin is better. As these reasons, there are no particular restrictions, it can be inferred as follows: by coating at least a portion of the elastomer with a surface crosslinked polymer, the exposure of the elastomer portion of the polymer particles (A) is reduced, and as a result, the elastomers are not easily adhered to each other, thereby improving the dispersibility of the polymer particles (A).

[0158] When the polymer particles (A) have a surface crosslinked polymer, the following effects can be further achieved: (a) reducing the viscosity of the resin composition, (b) increasing the crosslinking density of the elastomer, and (c) increasing the grafting efficiency of the grafted portion. The crosslinking density of the elastomer refers to the number of crosslinked structures of the entire elastomer.

[0159] The surface cross-linked polymer is composed of a polymer containing, as constituent units, 30 to 100% by weight of constituent units derived from a polyfunctional monomer and 0 to 70% by weight of constituent units derived from other vinyl monomers, with a total of 100% by weight.

[0160] As the multifunctional monomer that can be used for the polymerization of the surface cross-linked polymer, the monomers identical with the above-mentioned multifunctional monomers can be enumerated. Among these multifunctional monomers, the multifunctional monomer that can be preferably used as the polymerization of the surface cross-linked polymer can be enumerated as allyl methacrylate, (meth) ethylene glycol diester of acrylic acid, (meth) butylene glycol diester of acrylic acid, (meth) hexanediol diester of acrylic acid, cyclohexanedimethanol di(meth) acrylate and polyethylene glycol di(meth) acrylates. These multifunctional monomers can be used only one kind, and can also be used in combination of two or more kinds.

[0161] The polymer particles (A) may include a surface crosslinked polymer independently polymerized with the graft copolymer containing rubber, or a surface crosslinked polymer co-polymerized with the graft copolymer containing rubber. The polymer particles (A) may be a multi-stage polymer obtained by multi-stage polymerization of an elastomer, a surface crosslinked polymer, and a graft portion. In any of these embodiments, the surface crosslinked polymer may cover at least a portion of the elastomer.

[0162] The surface cross-linked polymer can also be regarded as a part of the elastomer. When the polymer particles (A) include the surface cross-linked polymer, for the grafted portion, (a) the elastomer other than the surface cross-linked polymer can be graft-bonded, (b) the surface cross-linked polymer can also be graft-bonded, and (c) both the elastomer other than the surface cross-linked polymer and the surface cross-linked polymer can be graft-bonded. When the polymer particles (A) include the surface cross-linked polymer, the volume average particle size of the elastomer refers to the volume average particle size of the elastomer including the surface cross-linked polymer.

[0163] The case (case D) of a multi-stage polymer obtained by sequentially polymerizing an elastomer, a surface cross-linked polymer and a grafted portion in multiple stages of polymerizing the polymer particles (A) is described. In case D, the surface cross-linked polymer may cover a portion of the elastomer, or may cover the entire elastomer. In case D, a portion of the surface cross-linked polymer may also enter the inside of the elastomer. According to case D, the grafted portion may cover a portion of the surface cross-linked polymer, or may cover the entire surface cross-linked polymer. In case D, a portion of the grafted portion may also enter the inside of the surface cross-linked polymer. In case D, the elastomer, the surface cross-linked polymer and the grafted portion may also have a layer structure. For example, a method in which the elastomer is the innermost layer (core layer), a layer of the surface cross-linked polymer exists as an intermediate layer on the outside of the elastomer, and a layer of the grafted portion exists as the outermost layer (shell layer) on the outside of the surface cross-linked polymer is one method of the present invention.

[0164] (Volume Average Particle Size (Mv) of Polymer Microparticles (A))

[0165] The volume average particle size (Mv) of the polymer microparticles (A) has a desired viscosity and can obtain a highly stable resin composition, so it is preferably 0.03 μm to 50.00 μm, more preferably 0.05 μm to 10.00 μm, more preferably 0.08 μm to 2.00 μm, further preferably 0.10 μm to 1.00 μm, further preferably 0.10 μm to 0.80 μm, and particularly preferably 0.10 μm to 0.50 μm. When the volume average particle size (Mv) of the polymer microparticles (A) is within the above range, there is also an advantage that the dispersibility of the polymer microparticles (A) in the matrix resin is good. In addition, in this specification, the "volume average particle size (Mv) of the polymer microparticles (A)" refers to the volume average particle size of the primary particles of the polymer microparticles (A) unless otherwise specified. The volume average particle size of the polymer particles (A) can be measured by using a dynamic light scattering particle size distribution measuring device or the like, using an aqueous latex containing the polymer particles (A) as a sample. The volume average particle size of the polymer particles (A) is described in detail according to the following examples. The volume average particle size of the polymer particles (A) can also be measured by cutting a cured product of the resin composition, photographing the cut surface using an electron microscope, and using the obtained photographed data (photographed image).

[0166] The number distribution of the particle size of the polymer fine particles (A) in the thermosetting resin preferably has a half value width of 0.5 to 1 times the volume average particle size in order to obtain a resin composition with low viscosity and easy handling.

[0167] (1-5. Method for producing polymer microparticles (A) (latex production process))

[0168] In one embodiment of the present invention, as a pre-stage of the resin mixing step, a step of producing polymer fine particles (A), in particular, a latex producing step of producing latex containing polymer fine particles (A) may be included. The latex refers to an aqueous latex.

[0169] For example, the polymer microparticles (A) can be produced by, after polymerizing an arbitrary polymer, graft-polymerizing the polymer constituting the graft portion in the presence of the polymer. Hereinafter, an example of producing the polymer microparticles (A) by, after polymerizing an elastomer, graft-polymerizing the polymer constituting the graft portion in the presence of the elastomer is given, to illustrate an example of a method for producing the polymer microparticles (A).

[0170] The polymer particles (A) can be manufactured by known methods such as emulsion polymerization, suspension polymerization, microsuspension polymerization, etc. Specifically, the polymerization of the elastomer of the polymer particles (A), the polymerization of the grafted portion (graft polymerization), and the polymerization of the surface cross-linked polymer are manufactured by known methods such as emulsion polymerization, suspension polymerization, microsuspension polymerization, etc. Among these, it is particularly easy to obtain the composition design of the polymer particles (A), the industrial production is easy, and the aqueous latex of the polymer particles (A) that can be preferably used in the manufacture of the present resin composition, and thus, as the manufacturing method of the polymer particles (A), emulsion polymerization is preferably used. Below, the manufacturing method of the elastomer, grafted portion, and arbitrary composition, i.e., the surface cross-linked polymer, which can be contained in the polymer particles (A) is described.

[0171] (Method for producing elastomer)

[0172] Consider the case where the elastomer contains at least one selected from diene rubber and (meth)acrylate rubber. In this case, the elastomer can be produced by methods such as emulsion polymerization, suspension polymerization, microsuspension polymerization, and as its production method, for example, the method described in WO2005 / 028546 can be used.

[0173] The elastomer may include a silicone rubber-based elastomer. In this case, the elastomer can be produced by, for example, emulsion polymerization, suspension polymerization, microsuspension polymerization, and the like. As a production method thereof, for example, the method described in WO2006 / 070664 can be used.

[0174] The elastic body is composed of a plurality of elastic bodies (e.g., elastic body 1, elastic body 2, ..., elastic body n ) is described below. In this case, elastomer 1, elastomer 2, ..., elastomer n By polymerizing the above methods separately, and then mixing them, an elastomer having multiple elastomers can be produced.n Multiple stage polymerizations can be performed sequentially to produce an elastomer having a variety of elastomers.

[0175] The multi-stage polymerization of elastomers is specifically described. For example, (1) elastomer 1 is polymerized to obtain elastomer 1; (2) then, in the presence of elastomer 1, elastomer 2 is polymerized to obtain a two-stage elastomer. 1+2 ; (3) Then, on the elastomer 1+2 In the presence of 1+2+3 ; (4) below, after the same process, in the elastic body 1+2+…+(n-1) In the presence of n Multi-stage polymer elastomer 1+2+…+n .

[0176] (Method for producing grafted portion)

[0177] The graft portion can be formed, for example, by polymerizing the monomer used for forming the graft portion by known free radical polymerization. (a) When a polymer particle precursor containing an elastomer or (b) an elastomer and a surface cross-linked polymer is obtained as an aqueous latex, the polymerization of the graft portion is preferably carried out by emulsion polymerization. The graft portion can be manufactured, for example, according to the method described in WO2005 / 028546.

[0178] The grafted part is composed of a plurality of grafted parts (e.g., grafted part 1, grafted part 2, ..., grafted part n ) is composed of, the method for producing the graft part is described. In this case, the graft part 1, the graft part 2, ..., the graft part n A grafted part having a plurality of grafted parts can be produced by polymerizing them separately using the above-mentioned method and then mixing them. n The multi-stage polymerization can be carried out sequentially to produce a graft part having a variety of graft parts.

[0179] The multi-stage polymerization of the grafted part is specifically described. For example, (1) the grafted part 1 is polymerized to obtain the grafted part 1; (2) then, the grafted part 2 is polymerized in the presence of the grafted part 1 to obtain the two-stage grafted part. 1+2 ; (3) Then, at the grafting portion 1+2 In the presence of 1+2+3 (4) below, after the same process, at the grafting part 1+2+…+(n-1) In the presence of n Polymerization to obtain multi-stage polymer grafting 1+2+…+n .

[0180] When the grafted portion is composed of multiple grafted portions, after the grafted portion having multiple grafted portions is polymerized, these grafted portions can be grafted and polymerized with an elastomer to produce polymer microparticles (A). In the presence of an elastomer, multiple polymers constituting multiple grafted portions on the elastomer can be sequentially grafted and polymerized in multiple stages to produce polymer microparticles (A).

[0181] (Method for producing surface cross-linked polymer)

[0182] The surface crosslinked polymer can be formed by polymerizing monomers for forming the surface crosslinked polymer by known radical polymerization. When the elastomer is obtained as an aqueous latex, the polymerization using the surface crosslinked polymer can be preferably performed by emulsion polymerization.

[0183] When the emulsion polymerization method is adopted as the method for producing the polymer fine particles (A), a known emulsifier (dispersant) can be used for the production of the polymer fine particles (A).

[0184] When the emulsion polymerization method is used as the method for producing the polymer microparticles (A), a thermal decomposition type initiator can be used in the production of the polymer microparticles (A). Examples of the thermal decomposition type initiator include known initiators such as 2,2'-azobisisobutyronitrile, hydrogen peroxide, potassium persulfate, and ammonium persulfate.

[0185] In the manufacture of polymer particles (A), redox initiators can also be used. The redox initiators are (a) organic peroxides and inorganic peroxides, (b) sodium formaldehyde sulfoxylate, glucose and other reducing agents as needed, and transition metal salts such as iron (II) sulfate as needed, and further chelating agents such as disodium ethylenediaminetetraacetate as needed, and further phosphorus-containing compounds such as sodium pyrophosphate as needed. Examples of the organic peroxides include tert-butyl peroxyisopropyl carbonate, p-menthane hydroperoxide, isopropylbenzene hydroperoxide, dicumyl peroxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, and tert-hexyl peroxide. Examples of the inorganic peroxides include hydrogen peroxide, potassium persulfate, and ammonium persulfate.

[0186] When a redox initiator is used, the peroxide can be polymerized at a low temperature without being substantially thermally decomposed, and the polymerization temperature can be set within a wide range. Therefore, it is preferred to use a redox initiator. Among the redox initiators, organic peroxides such as cumene hydroperoxide, dicumyl peroxide, p-menthane hydroperoxide, and tert-butyl hydroperoxide are preferably used as redox initiators. When the amount of the above initiator and the redox initiator are used, the amount of the reducing agent, transition metal salt, chelating agent, etc. can be used within a known range.

[0187] For the purpose of introducing a crosslinked structure into an elastomer, a grafted portion or a surface crosslinked polymer, a known chain transfer agent can be used within a known usage amount when a multifunctional monomer is used in the polymerization of the elastomer, the grafted portion or the surface crosslinked polymer. By using a chain transfer agent, the molecular weight and / or the degree of crosslinking of the obtained elastomer, the grafted portion or the surface crosslinked polymer can be easily adjusted.

[0188] In the production of polymer microparticles (A), a surfactant may be used in addition to the above components. The type and amount of the surfactant used are within known ranges.

[0189] In the production of the polymer microparticles (A), the polymerization temperature, pressure, deoxidation and other conditions of the polymerization can also be applied within known ranges.

[0190] (1-6. Resin (B))

[0191] The resin (B) is not particularly limited in other properties as long as it is a liquid, semisolid or solid having a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25° C. In addition, “the resin (B) has a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25° C.” means “the resin (B) at 25° C. has a viscosity of 100 mPa·s to 1,000,000 mPa·s”.

[0192] When the resin (B) is a liquid, the viscosity of the resin (B) at 25° C. is preferably 750,000 mPa·s or less, more preferably 700,000 mPa·s or less, more preferably 500,000 mPa·s or less, more preferably 350,000 mPa·s or less, more preferably 300,000 mPa·s or less, more preferably 250,000 mPa·s or less, more preferably 100,000 mPa·s or less, more preferably 75,000 mPa·s or less, more preferably 50,000 mPa·s or less, more preferably 30,000 mPa·s or less, more preferably 25,000 mPa·s or less, further preferably 20,000 mPa·s or less, and particularly preferably 15,000 mPa·s or less. According to the above configuration, the resin (B) has an advantage of excellent fluidity.

[0193] Furthermore, the viscosity of the resin (B) is more preferably 200 mPa·s or more, more preferably 300 mPa·s or more, more preferably 400 mPa·s or more, more preferably 500 mPa·s or more, further preferably 750 mPa·s or more, further preferably 1000 mPa·s or more, and particularly preferably 1500 mPa·s or more at 25°C. According to this configuration, the resin (B) does not penetrate into the polymer microparticles (A). Thus, the resin (B) can prevent the polymer microparticles (A) from fusing with each other.

[0194] The viscosity of resin (B) at 25°C is more preferably 100 mPa·s to 750,000 mPa·s, more preferably 100 mPa·s to 700,000 mPa·s, more preferably 100 mPa·s to 350,000 mPa·s, more preferably 100 mPa·s to 300,000 mPa·s, more preferably 100 mPa·s to 50,000 mPa·s, further preferably 100 mPa·s to 30,000 mPa·s, and particularly preferably 100 mPa·s to 15,000 mPa·s.

[0195] When the resin (B) is semi-solid, the resin (B) can be called semi-liquid, and the resin (B) can be called having a viscosity greater than 1000000 mPa·s. When the resin (B) is semi-solid or solid, the resin composition containing the obtained powder or granular material has the advantages of low viscosity and easy handling.

[0196] The viscosity of the resin (B) can be measured using a viscometer. The method for measuring the viscosity of the resin (B) will be described in detail with reference to the following examples.

[0197] Furthermore, the viscosity of the resin (B) is able to prevent the fusion of the polymer particles (A) by pouring the resin (B) into the polymer particles (A), and is therefore preferably 100 mPa·s or more at 25°C, further preferably 500 mPa·s or more, further preferably 1000 mPa·s or more, and particularly preferably 1500 mPa·s or more.

[0198] Furthermore, when the matrix resin is a thermosetting resin, the viscosity of the resin (B) at 25°C is preferably less than or equal to the value of the viscosity of the thermosetting matrix resin at 25°C plus 50,000 mPa·s. From the viewpoint of facilitating uniform mixing of the resin (B) and the thermosetting matrix resin, when the viscosity of the resin (B) at 25°C is greater than or equal to the viscosity of the thermosetting matrix resin at 25°C, the viscosity of the resin (B) at 25°C is more preferably less than or equal to the value of the viscosity of the thermosetting matrix resin at 25°C plus 20,000 mPa·s, more preferably less than or equal to 10,000 mPa·s, further preferably less than or equal to 5,000 mPa·s, and most preferably less than or equal to 0 mPa·s.

[0199] Furthermore, the resin (B) preferably has an endothermic peak at 25°C or lower in a thermogram of differential scanning calorimetry (DSC), and more preferably has an endothermic peak at 0°C or lower.

[0200] In addition, as resin (B), it can be a resin identical to the matrix resin, that is, a thermosetting resin, of the mixed object described later, or a resin different from the thermosetting resin. As an example, there is a case where resin (B) is used in the method for manufacturing a resin composition and the resin (B) is a resin of the same type as the matrix resin. In this case, the matrix resin and the resin (B) cannot be distinguished in the obtained resin composition. Therefore, from the appearance, the obtained resin composition only has a matrix resin outside the polymer particles (A). Next, there is a case where resin (B) is used in the method for manufacturing a resin composition and the resin (B) is a resin of a different type from the matrix resin. In this case, the matrix resin and the resin (B) can be identified in the obtained resin composition. In this case, the resin composition finally obtained can include resin (B) as a resin other than the matrix resin outside the polymer particles (A).

[0201] Resin (B) may be, for example, a thermosetting resin, a thermoplastic resin, or any combination of a thermosetting resin and a thermoplastic resin. When the resin composition contains resin (B), resin (B) has the effect of improving the dispersibility of polymer particles (A) in the thermosetting resin.

[0202] Examples of the thermosetting resin of the resin (B) include various thermosetting resins described below in the section of the matrix resin. The thermosetting resin in the resin (B) may be used alone or in combination of two or more.

[0203] The thermoplastic resin of the resin (B) includes, for example, a polymer containing a constituent unit derived from one or more monomers selected from aromatic vinyl monomers, vinyl cyanide monomers, and (meth)acrylate monomers as constituent units. In the resin (B), only one thermoplastic resin may be used, or two or more thermoplastic resins may be used in combination.

[0204] When the matrix resin to be mixed is a thermosetting resin, it is preferred that the resin (B) is of the same type as the thermosetting resin of the matrix resin because it does not affect various physical properties. That is, when the thermosetting resin of the matrix resin is an epoxy resin, the resin (B) is preferably an epoxy resin. That is, when the resin (B) is a thermosetting resin different from that of the matrix resin, the resin (B) is preferably compatible with the thermosetting resin of the matrix resin.

[0205] In addition, when the total amount of the above-mentioned polymer microparticles (A) and the above-mentioned resin (B) is set to 100 weight%, from the viewpoint of viscosity, it is more preferred that the polymer microparticles (A) are 10 to 60 weight% and the resin (B) is 90 to 40 weight%, further preferably that the polymer microparticles (A) are 20 to 50 weight% and the resin (B) is 80 to 50 weight%, and particularly preferably that the polymer microparticles (A) are 25 to 45 weight% and the resin (B) is 75 to 55 weight%.

[0206] (other)

[0207] In this specification, fats and fatty acid ethers are also included in resin (B). As fats and oils that can be preferably used as resin (B), epoxidized fats and oils such as epoxidized soybean oil and epoxidized linseed oil can be mentioned. As epoxidized soybean oil, commercial products can be used, for example, Adekacizer O-130P manufactured by ADEKA can be mentioned. As fatty acid ethers that can be preferably used as resin (B), epoxidized fatty acid ethers such as epoxidized fatty acid butyl ester, epoxidized fatty acid 2-ethylhexyl ester, epoxidized fatty acid octyl ether and epoxidized fatty acid alkyl ether can be mentioned.

[0208] Epoxidized fats and oils and epoxidized fatty acid ethers are sometimes referred to as epoxy plasticizers. That is, in this specification, epoxy plasticizers are also included in resin (B). Examples of epoxy plasticizers other than epoxidized fats and oils and epoxidized fatty acid ethers include diepoxystearyl epoxyhexahydrophthalate and di-2-ethylhexyl epoxyhexahydrophthalate.

[0209] The above-mentioned thermosetting resin, thermoplastic resin, mixture of thermosetting resin and thermoplastic resin, oil and fat and fatty acid ether can be mixed with antioxidants. In this specification, as long as it is mixed with the above-mentioned substances, the antioxidant is regarded as a part of resin (B). When only the antioxidant is used, the antioxidant is not regarded as resin (B).

[0210] The antioxidant is not particularly limited and includes, for example, (a) primary antioxidants such as phenolic antioxidants, amine antioxidants, lactone antioxidants, and hydroxydiamine antioxidants, and (b) secondary antioxidants such as sulfur antioxidants and phosphorus antioxidants.

[0211] As the above-mentioned phenolic antioxidant, hindered phenolic antioxidants can be mentioned. As hindered phenolic antioxidants, compounds having a hindered phenol structure or a sheet hindered phenol structure in the molecule can be mentioned. As the phenolic antioxidant, commercially available products can be used, for example, Irganox 245 manufactured by BASF Japan Co., Ltd. can be mentioned.

[0212] The amine antioxidant is not particularly limited, and conventionally known substances can be widely used. Specific examples of the amine antioxidant include amine-ketone compounds such as 2,2,4-trimethyl-1,2-dihydroquinoline polymers, 6-ethoxy-1,2-dihydro-2,2,4-trimethylquinoline, and a reaction product of diphenylamine and acetone.

[0213] The above-mentioned amine antioxidants include aromatic amine compounds. Examples of the aromatic amine compounds include naphthylamine antioxidants, diphenylamine antioxidants, and p-phenylenediamine antioxidants.

[0214] The lactone antioxidant, the hydroxydiamine antioxidant, and the sulfur antioxidant are not particularly limited, and conventionally known antioxidants can be widely used.

[0215] As the phosphorus antioxidant, there is no particular limitation, and conventionally known substances can be widely used. Phosphoric acid and phosphoric acid esters containing active hydrogen may have a negative impact on the storage stability of the resin composition containing the obtained powder and granules and the heat resistance of the cured product or molded body provided by the resin composition. Therefore, as the phosphorus antioxidant, phosphoric acid and phosphoric acid ester are contained in the molecule, preferably alkyl phosphite, aryl phosphite, alkyl aryl phosphite compounds, etc.

[0216] As the above-mentioned antioxidant, in addition, known substances can be used. As antioxidants, for example, various substances recorded in the "Antioxidant Handbook" (first edition issued on October 25, 1975) issued by Dacheng Society, the "Polymer Additive Handbook" (written by Haruna, the first edition issued on November 7, 2010) issued by CMC Publishing, etc. can be used.

[0217] The resin (B) is preferably selected from thermosetting resins, mixtures of thermosetting resins and antioxidants, thermoplastic resins, mixtures of thermoplastic resins and antioxidants, oils, mixtures of oils and antioxidants, fatty acid ethers, mixtures of fatty acid ethers and antioxidants, epoxy curing agents, and mixtures of epoxy curing agents and antioxidants. It is more preferably selected from epoxy resins, acrylic polymers, mixtures of epoxy resins and antioxidants, mixtures of acrylic polymers and antioxidants, and mixtures of epoxy plasticizers and antioxidants. It is further preferably selected from mixtures of epoxy resins and antioxidants, mixtures of acrylic polymers and antioxidants, and mixtures of epoxy plasticizers and antioxidants. It is particularly preferably a mixture of epoxy plasticizers and antioxidants. According to this configuration, there are the following advantages: (a) the resin composition containing the obtained powder and granules can provide a cured product or molded body with preferred heat resistance, and (b) the dispersibility of the polymer particles (A) in the matrix resin can be improved.

[0218] [2. Resin composition]

[0219] The resin composition according to one embodiment of the present invention is a resin composition comprising polymer particles (A) and resin (B), wherein the polymer particles (A) have a graft portion, the graft portion being composed of a polymer containing a constituent unit derived from one or more monomers selected from an aromatic vinyl monomer, a vinyl cyanide monomer, and a (meth)acrylate monomer, and the resin (B) is a resin (B) having a viscosity of 1000000 mPa·s at 25° C., and when the total of the polymer particles (A) and the resin (B) is 100% by weight, the polymer particles (A) are 30 to 70% by weight, and the resin (B) is 30 to 70% by weight. This resin composition can be, for example, the subject of the above-mentioned cleaning process. In other words, it can be referred to as a resin composition before the cleaning process.

[0220] As described above, the present resin composition is obtained in a paste or crumb form according to the weight ratio of the polymer particles (A) and the resin (B). If it is in these shapes, the operability during the cleaning process is improved. For example, the specific gravity of the liquid resin composition is higher than that of water, so when it is left to stand and separate during the cleaning process, it becomes the lower layer. In this case, the cleaning operation is limited to only one time. Or when it is necessary to clean multiple times, it is necessary to temporarily move the resin composition into other containers, release the cleaning water, and return the resin composition to the cleaning tank again, and the operation becomes cumbersome.

[0221] On the other hand, if the resin composition is in a paste or crumb form, the resin composition can block the metal mesh, thereby facilitating the discharge of the washing water. In addition, it has the advantages of being able to perform repeated washing and requiring less equipment. In addition, if the resin composition is in the above-mentioned shape, it can be mixed and washed in addition to stirring, and the range of the device selection is wide.

[0222] The present resin composition can be produced by the method before the washing step is performed in the above-mentioned method for producing the resin composition.

[0223] The size of the resin composition is preferably 0.3 mm or more, more preferably 1 mm or more, and even more preferably 3 mm or more. If it is this size, the workability during the washing process, especially during drainage, is good.

[0224] In addition, in the present resin composition, the content of element S or P is preferably removed by 10% or more by one washing. In addition, the content of element S or P is more preferably removed by 15% or more by one washing, further preferably removed by 20% or more, particularly preferably removed by 25% or more, and most preferably removed by 30% or more.

[0225] Here, "cleaning once" refers to a cleaning process (1 time) in which, in the case of a paste, 1 part by weight of the resin composition is mixed with 1.5 parts by weight of ion exchange water at 90°C, and stirred for 30 minutes. In the case of crumbs, it refers to a cleaning process (1 time) in which 1 part by weight of the resin composition is kneaded with 0.3 parts by weight of ion exchange water at 30°C. Before and after this cleaning process (1 time), the content of the element S or P in the resin composition can be determined. In addition, the cleaning process (1 time) for determining "removing more than 10%" is not limited to the first cleaning, but may also be the cleaning after the second time. In addition, in the case of implementing multiple cleaning processes, it is preferred that "removing 10%" is used in all cleaning processes, and it may also be the case that "removing more than 10%" is used only in the cleaning process with the highest removal efficiency.

[0226] This resin composition can remove more than 10% of the element S or P as impurities by using one washing process as described above. Therefore, the number of washing processes for flushing impurities can be reduced. In addition, the small amount of element S and P means that there are fewer impurities from the emulsifier, and also means that there are fewer impurities and inclusions (water-soluble compounds) from the emulsifier, coagulant (inorganic salt), and metal soap. It is used for electronic materials and the like. This is because water-soluble compounds are the cause of corrosion of substrate wiring, component wires, or cause poor insulation and movement. In addition, this resin composition can be obtained, for example, by the above-mentioned method for manufacturing the resin composition.

[0227] (Organic Solvent)

[0228] The present resin composition contains substantially no organic solvent. “Contains substantially no organic solvent” means that the amount of the organic solvent in the resin composition is 100 ppm or less.

[0229] The amount of the organic solvent (also referred to as solvent content) contained in this resin combination is preferably below 100ppm, more preferably below 50ppm, further preferably below 25ppm, and particularly preferably below 10ppm.The amount of the organic solvent contained in this resin combination may also be referred to as the amount of the volatile component (wherein, removing water) contained in this resin combination.The amount of the organic solvent (volatile component) contained in this resin combination, for example, utilizes the resin combination of a prescribed amount of heating such as hot air dryers, by measuring the weight of the resin combination before and after heating, thereby can be used as the weight division of reduction to obtain.In addition, the amount of the organic solvent (volatile component) contained in this resin combination can be obtained by gas chromatography.In addition, in the manufacture of this resin combination, when an organic solvent is not used, the amount of the organic solvent contained in the resin combination obtained can be regarded as 0ppm.

[0230] Examples of the organic solvent that is not substantially contained in the present resin composition include (a) ethers such as methyl acetate, ethyl acetate, propyl acetate, and butyl acetate; (b) ketones such as acetone, methyl ethyl ketone, diethyl ketone, and methyl isobutyl ketone; (c) alcohols such as ethanol, (iso)propanol, and butanol; (d) tetrahydrofuran, tetrahydropyran, dihydrofuran, and dihydrofuran; (e) aromatic hydrocarbons such as benzene, toluene and xylene, and (f) chlorinated hydrocarbons such as methylene chloride and chloroform.

[0231] (Element S and P content)

[0232] The content of the elements S and P in the present resin composition can be measured using a fluorescent X-ray segmentation device or liquid chromatography. The elements S and P in the present resin composition are, for example, elements from an emulsifier. When the emulsifier is a sulfur-based emulsifier, the resin composition may contain the element S, and when the emulsifier is a phosphorus-based emulsifier, the resin composition may contain the element P. The content of the elements S and P in the present resin composition can also be said to be the residual emulsifier amount.

[0233] In the present resin composition, the content of the elements S and P in the resin composition measured using a fluorescent X-ray spectrometer is preferably 1000 ppm or less, more preferably 500 ppm or less, further preferably 100 ppm or less, further preferably 60 ppm or less, and particularly preferably 50 ppm or less.

[0234] (2-3. Other components)

[0235] In addition, the present resin composition is preferably a composition that does not pass through the metal mesh after 10 minutes on a metal mesh of 8 mesh at 25°C. In addition, it is more preferably a substance that does not pass through the metal mesh after 10 minutes on a metal mesh of 16 mesh at 25°C, and it is further preferably a substance that does not pass through the metal mesh after 10 minutes on a metal mesh of 30 mesh at 25°C, and it is preferably a substance that does not pass through the metal mesh after 10 minutes on a metal mesh of 50 mesh at 25°C. If it is the above-mentioned structure, the operability is good during the cleaning process, especially when draining water. Here, "not passing through the metal mesh" means that the resin that passes through the metal mesh after 10 minutes on the metal mesh is less than 5%.

[0236] The polymer microparticles (A) and the resin (B) are the same as those in the method for producing the resin composition, and the descriptions of the first embodiment can be cited. The polymer microparticles (A) are preferably a rubber-containing graft copolymer having an elastomer and a graft portion graft-bonded to the elastomer. In addition, the elastomer preferably comprises one or more selected from diene rubber, (meth)acrylate rubber, and silicone rubber elastomer.

[0237] The resin (B) is preferably a thermosetting resin. Among them, the thermosetting resin is preferably at least one of an ethylenically unsaturated monomer, an epoxy resin, a phenol resin, a polyol resin, and an amino formaldehyde resin (melamine resin).

[0238] According to the above structure, it is possible to improve fracture toughness, adhesive strength, surface impact resistance, etc. while maintaining the characteristics (heat resistance, rigidity, etc.) of the liquid curable resin.

[0239] [3. Resin composition (mixture of the present resin composition and a matrix resin)]

[0240] In one embodiment of the present invention, a resin composition obtained by mixing the above-mentioned resin composition with a matrix resin may be included. That is, the present resin composition includes the above-mentioned resin composition and a matrix resin.

[0241] (3-1. Matrix resin)

[0242] As the matrix resin, thermosetting resin can be suitably utilized. The thermosetting resin preferably comprises at least one thermosetting resin selected from the resin, epoxy resin, phenol resin, polyol resin and amino formaldehyde resin (melamine resin) of the polymer formed by polymerizing the ethylenic unsaturated monomer. In addition, as the thermosetting resin, the resin comprising the polymer formed by polymerizing the aromatic polyester raw material can also be cited. As the aromatic polyester raw material, free radical polymerizable monomers such as aromatic vinyl compounds, (meth) acrylic acid derivatives, cyanide vinyl compounds, maleimide compounds, ethylene phthalate, alkylene glycol, etc. can be cited. These thermosetting resins can be used only one kind, and can also be used in combination with two or more kinds.

[0243] (Ethylenically unsaturated monomer)

[0244] The ethylenically unsaturated monomer is not particularly limited as long as it has at least an ethylenically unsaturated bond in the molecule.

[0245] Examples of the ethylenically unsaturated monomer include acrylic acid, α-alkyl acrylic acid, α-alkyl acrylic acid ether, β-alkyl acrylic acid, β-alkyl acrylic acid ether, methacrylic acid, acrylic acid ether, methacrylic acid ether, vinyl acetate, vinyl ether, unsaturated ether, polyunsaturated carboxylic acid, polyunsaturated ether, maleic acid, maleic acid ether, maleic anhydride, and ethoxystyrene. These may be used alone or in combination of two or more.

[0246] (Epoxy resin)

[0247] The epoxy resin is not particularly limited as long as it has at least one epoxy bond in the molecule.

[0248] Specific examples of epoxy resins include bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol AD ​​epoxy resins, bisphenol S epoxy resins, glycidyl ether epoxy resins, glycidyl amine epoxy resins, novolac epoxy resins, glycidyl ether epoxy resins containing bisphenol A propylene oxide additives, hydrogenated bisphenol A (or F) epoxy resins, fluorinated epoxy resins, rubber-modified epoxy resins of polybutadiene or NBR, flame-retardant epoxy resins such as glycidyl ether of tetrabromobisphenol A, p-oxybenzoic acid glycidyl ether ether epoxy resins, m-aminophenol epoxy resins, diaminodiphenylmethane epoxy resins, urethane-modified epoxy resins having urethane bonds, various alicyclic epoxy resins, glycidyl ethers of polyols, hydantoin epoxy resins, petroleum resins, and epoxides of unsaturated polymers such as glycidyl ethers and amino group-containing glycidyl ether resins. Examples of the polyol include N,N-diglycidylaniline, N,N-diglycidyl-o-toluidine, triglycidyl isocyanurate, polyalkylene glycol diglycidyl ether, and glycerol. Examples of the epoxy resin include epoxy compounds obtained by addition reaction of bisphenol A (or F) or polybasic acids to the above-mentioned epoxy resins. The epoxy resin is not limited thereto, and commonly used epoxy resins may also be used. Only one of these epoxy resins may be used, or two or more of them may be used in combination.

[0249] The epoxy resins described above have at least two epoxy groups in one molecule, and are preferred in the curing of the resin composition because of their high reactivity and the ease with which the obtained cured product can be made into a three-dimensional mesh. In addition, as the epoxy resin, it is preferred that the epoxy resins having at least two epoxy groups in one molecule have a bisphenol type epoxy resin as the main component from the perspective of excellent economy and availability.

[0250] (Phenol resin)

[0251] The phenol resin is not particularly limited as long as it is a compound obtained by reacting phenols and aldehydes. As phenols, there are no particular limitations, and for example, phenols such as phenol, o-cresol, m-cresol, p-cresol, xylenol, p-tert-butylphenol, p-octylphenol, p-phenylphenol, bisphenol A, bisphenol F and resorcinol can be mentioned. As particularly preferred phenols, phenol and cresol can be mentioned.

[0252] As aldehydes, there are no particular limitations, and examples thereof include methanol, acetaldehyde, butyraldehyde, acrolein, and mixtures thereof. As aldehydes, substances that are sources of the above-mentioned aldehydes or solutions of these aldehydes may also be used. As aldehydes, methanol is preferred because of the ease of handling when reacting phenols with aldehydes.

[0253] The molar ratio (F / P) of phenols (P) to aldehydes (F) when reacting phenols with aldehydes (hereinafter, also referred to as the reaction molar ratio) is not particularly limited. When an acid catalyst is used in the reaction, the reaction molar ratio (F / P) is preferably 0.4 to 1.0, and more preferably 0.5 to 0.8. When an alkali catalyst is used in the reaction, the reaction molar ratio (F / P) is preferably 0.4 to 4.0, and more preferably 0.8 to 2.5. When the reaction molar ratio is above the lower limit, the yield will not be too low, and the molecular weight of the phenol resin obtained may be reduced. On the other hand, when the reaction molar ratio is below the upper limit, the molecular weight of the phenol resin will not become too large, and the softening point will not become too high, thereby obtaining sufficient fluidity when heated. In addition, when the reaction molar ratio is below the upper limit, the molecular weight is easy to control, and gelation or partial gelation caused by the reaction conditions may occur.

[0254] (Polyol resin)

[0255] The polyol resin is a compound having two or more active hydrogen atoms at the terminal, and is a difunctional or higher functional polyol having a molecular weight of about 50 to 20000. Examples of the polyol resin include aliphatic alcohols, aromatic alcohols, polyether polyols, polyester polyols, polyolefin polyols, and acrylic polyols.

[0256] The aliphatic alcohol may be any of a dihydric alcohol or a trihydric alcohol or higher (a trihydric alcohol, a tetrahydric alcohol, etc.). Examples of the dihydric alcohol include ethylene glycol, propylene glycol, 1,3-propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, and other alkylene glycols (especially alkylene glycols having about 1 to 6 carbon atoms), and dehydrated condensates of two or more molecules (e.g., about 2 to 6 molecules) of the alkylene glycols (diethylene glycol, dipropylene glycol, tripropylene glycol, etc.). Examples of the trihydric alcohol include glycerol, trimethylolpropane, trimethylolethane, 1,2,6-hexanetriol, etc. (especially trihydric alcohols having about 3 to 10 carbon atoms). Examples of the tetrahydric alcohol include pentaerythritol, diglycerol, etc. In addition, sugars such as monosaccharides, oligosaccharides and polysaccharides can be mentioned.

[0257] Examples of the aromatic alcohol include bisphenols such as bisphenol A and bisphenol F; biphenyls such as dihydroxybiphenyl; polyphenols such as hydroquinone and phenol-methanol condensate; and naphthalene diol.

[0258] Examples of polyether polyols include random copolymers or block copolymers obtained by ring-opening polymerization of ethylene oxide, propylene oxide, butylene oxide, styrene oxide, etc., in the presence of one or more active hydrogen-containing initiators, and mixtures of these copolymers. Examples of initiators containing active hydrogen used in the ring-opening polymerization of polyether polyols include glycols such as ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, and bisphenol A; triols such as trimethylolethane, trimethylolpropane, and glycerol; sugars such as monosaccharides, oligosaccharides, and polysaccharides; sorbitol; and amines such as ammonia, ethylenediamine, urea, monomethyldiethanolamine, and monoethyldiethanolamine.

[0259] Examples of polyester polyols include polymers obtained by polycondensing (a) a polybasic acid such as maleic acid, fumaric acid, adipic acid, sebacic acid, phthalic acid, dodecanedioic acid, isophthalic acid, azelaic acid and / or anhydrides thereof, and (b) a polyol such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, neopentyl glycol, 3-methyl-1,5-pentanediol in the presence of an etherification catalyst at a temperature range of 150 to 270° C. Examples of (a) polyester polyols include ring-opening polymers such as ε-caprolactone and valerolactone, and (b) active hydrogen compounds having two or more active hydrogen atoms such as polycarbonate diol and castor oil.

[0260] Examples of the polyolefin polyol include polybutadiene polyol, polyisoprene polyol, and additives thereof.

[0261] Examples of acrylic polyols include (a) monomers containing a hydroxyl group such as ethyl hydroxy(meth)acrylate, butyl hydroxy(meth)acrylate, and vinylphenol; (b) copolymers of general-purpose monomers such as butyl n-(meth)acrylate and 2-ethylhexyl(meth)acrylate; and mixtures of these copolymers.

[0262] Among these polyol resins, polyether polyol is preferred because it can provide a cured product with a low viscosity and excellent workability of the obtained resin composition, and a good balance between hardness and toughness of the resin composition. In addition, polyester polyol is preferred because it can provide a cured product with excellent adhesion of the obtained resin composition.

[0263] (Amino formaldehyde resin)

[0264] The amino formaldehyde resin is not particularly limited as long as it is a compound obtained by reacting an amino compound and an aldehyde under a basic catalyst. Examples of the amino compound include melamine; 6-substituted guanamines such as guanamine, acetylguanamine, and benzoguanamine; amine-substituted triazine compounds such as CTUguanamine (3,9-bis[2-(3,5-diamino-2,4,6-triazaphenyl)ethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane) and CMTUguanamine (3,9-bis[(3,5-diamino-2,4,6-triazaphenyl)methyl]-2,4,8,10-tetraoxaspiro[5,5]undecane); and thioureas such as urea, thiourea, and ethylene urea. Furthermore, as the amino compound, a substituted melamine compound obtained by replacing the hydrogen of the amino group of melamine with an alkyl group, an alkenyl group and / or a phenyl group (described in U.S. Patent No. 5998573 (corresponding to Japanese Publication Gazette: Japanese Patent Laid-Open No. 9-143238)) and a substituted melamine compound obtained by replacing the hydrogen of the amino group of melamine with a hydroxyalkyl group, a hydroxyalkyloxyalkyl group and / or an aminoalkyl group (described in U.S. Patent No. 5322915 (corresponding to Japanese Publication Gazette: Japanese Patent Laid-Open No. 5-202157)) etc. can also be used. As the amino compound, among the above compounds, polyfunctional amino compounds, namely melamine, guanamine, acetylguanamine and benzoguanamine, are preferred because they are relatively inexpensive to produce industrially, and melamine is particularly preferred. The above amino compounds may be used alone or in combination of two or more. Furthermore, in addition to these amino compounds, (a) phenols such as phenol, cresol, alkylphenol, resorcinol, hydroquinone, and pyrogallol, and (b) aniline may be added and used.

[0265] Examples of the aldehydes include methanol, p-methanol, acetaldehyde, benzylaldehyde, and furfural. Methanol and p-methanol are preferred because they are inexpensive and have good reactivity with the amino compounds listed above. In the production of the aminoformaldehyde resin, the aldehyde is preferably used in an amount of 1.1 to 6.0 moles, particularly preferably 1.2 to 4.0 moles, per mole of effective aldehyde group in the p-amino compound.

[0266] (Physical properties of thermosetting resin)

[0267] The properties of the thermosetting resin are not particularly limited. The thermosetting resin preferably has a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25°C. The viscosity of the thermosetting resin is more preferably 50,000 mPa·s or less at 25°C, further preferably 30,000 mPa·s or less, and particularly preferably 15,000 mPa·s or less. According to the above-mentioned structure, the thermosetting resin has the advantage of excellent fluidity. At 25°C, a thermosetting resin having a viscosity of 100 mPa·s to 1,000,000 mPa·s can be said to be a liquid.

[0268] The greater the fluidity of the thermosetting resin, the better, in other words, the smaller the viscosity, the better. In the thermosetting resin, it is difficult to disperse the polymer particles (A) in the state of primary particles. In the past, it was very difficult to disperse the polymer particles (A) in the state of primary particles in a thermosetting resin having a viscosity of 1000000 mPa·s or less at 25°C. However, the resin composition involved in one embodiment of the present invention has the following advantages: the polymer particles (A) having the above-mentioned structure are well dispersed in a thermosetting resin having a viscosity of 1000000 mPa·s or less at 25°C.

[0269] Furthermore, the viscosity of the thermosetting resin is preferably 100 mPa·s or more, further preferably 500 mPa·s or more, further preferably 1000 mPa·s or more, and particularly preferably 1500 mPa·s or more at 25°C, since the thermosetting resin can be incorporated into the polymer particles (A) to prevent fusion of the polymer particles (A).

[0270] The thermosetting resin may have a viscosity greater than 1,000,000 mPa·s. The thermosetting resin may be semi-solid (semi-liquid) or solid. When the thermosetting resin has a viscosity greater than 1,000,000 mPa·s, the resulting resin composition has the advantage of being less viscous and easier to handle.

[0271] The thermosetting resin preferably has an endothermic peak at 25° C. or lower, and more preferably has an endothermic peak at 0° C. or lower in a thermogram by differential scanning calorimetry (DSC). According to the above configuration, the thermosetting resin has an advantage of excellent fluidity.

[0272] (3-2. Mixing ratio of the present resin composition and the matrix resin, etc.)

[0273] The mixing ratio of the present resin composition and the matrix resin is preferably 0.5 to 50% by weight of the present resin composition and 50 to 99.5% by weight of the matrix resin, more preferably 1 to 35% by weight of the present resin composition and 65 to 99% by weight of the matrix resin, particularly preferably 1.5 to 25% by weight of the present resin composition and 75 to 98.5% by weight of the matrix resin, and most preferably 2.5 to 20% by weight of the present resin composition and 80 to 97.5% by weight of the matrix resin, when the total of the present resin composition and the matrix resin is set to 100% by weight.

[0274] When the matrix resin is a thermosetting resin, the state thereof is not particularly limited as long as it is fluid when mixed with the present resin composition, and may be solid at room temperature, but is preferably liquid from the viewpoint of workability.

[0275] The temperature when the present resin composition is mixed with the thermosetting matrix resin is generally the temperature at which the thermosetting matrix resin becomes flowable, but the resin (B) can flow at the temperature at which the thermosetting matrix resin is flowable, so it becomes easy to evenly mix the resin (B) with the thermosetting matrix resin. On the contrary, when the thermosetting matrix resin is liquid and the epoxy resin in the present resin composition added thereto is solid, it becomes difficult to evenly mix the two. It should be noted that in this specification, when the thermosetting matrix resin is liquid at 25°C, it can be interpreted as "the viscosity of the thermosetting matrix resin at 25°C is greater than the viscosity of the resin (B) at 25°C".

[0276] (3-3. Other optional ingredients)

[0277] In the mixture of the present resin composition and the matrix resin, from the viewpoint of improving the anti-blocking property and the dispersibility to the thermosetting matrix resin, it is preferred to further include an anti-blocking agent. As long as the anti-blocking agent plays the above-mentioned effect, there is no particular restriction. As an anti-blocking agent, an anti-blocking agent composed of inorganic particles such as silicon dioxide, titanium oxide, aluminum oxide, zirconium oxide, aluminum silicate, diatomaceous earth, zeolite, kaolin, talc, calcium carbonate, calcium phosphate, barium sulfate, magnesium hydrosilicate, etc. can be cited; an anti-blocking agent composed of organic particles; grease-based anti-blocking agents such as polyethylene wax, higher fatty acid amide, metal soap, and organic oil. Among these, an anti-blocking agent composed of particles is preferably an anti-blocking agent composed of organic particles. As an anti-blocking agent, as a constituent unit, it is particularly preferred that the anti-blocking agent is composed of organic particles of a polymer of constituent units of more than one monomer selected from aromatic vinyl monomers, vinyl cyanide monomers, and (meth) acrylate monomers.

[0278] The anti-blocking agent composed of microparticles is usually formed by dispersing microparticles in a liquid or in a colloidal state. The volume average particle size (Mv) of the microparticles in the anti-blocking agent is usually less than 10 μm, preferably 0.05 to 10 μm. The content of the anti-blocking agent is preferably 0.01 to 5.0% by weight, more preferably 0.5 to 3.0% by weight, relative to the total weight of the resin composition and the base resin.

[0279] The mixture of the present resin composition and the matrix resin may contain other arbitrary components other than the above-mentioned components as required. As other arbitrary components, colorants such as curing agents, pigments and dyes, extender pigments, ultraviolet absorbers, antioxidants, thermal stabilizers (gelation inhibitors), plasticizers, leveling agents, defoamers, silane coupling agents, antistatic agents, flame retardants, lubricants, viscosity reducers, low shrinkage agents, inorganic fillers, organic fillers, thermoplastic resins, desiccants and dispersants can be cited.

[0280] Anti-blocking agents and additives (the above-mentioned other optional components) can be appropriately added in any step of the method for producing the present resin composition. For example, anti-blocking agents and the above-mentioned additives can be added to the aqueous suspension before or after the polymer particles (A) are solidified, or can be added to the present resin composition or a mixture of the present resin composition and a matrix resin.

[0281] The mixture of the present resin composition and the matrix resin may further contain a known thermosetting resin other than the matrix resin, and may further contain a known thermoplastic resin.

[0282] 〔4.Cured material〕

[0283] The cured product according to one embodiment of the present invention is a cured product obtained by curing the resin composition described in the section [3. Resin composition (mixture of the present resin composition and a matrix resin)]. Hereinafter, it is simply referred to as the present cured product.

[0284] The cured product has the above-mentioned structure, and thus after being applied to a metal plate or the like, rust is unlikely to form even when cured. In addition, the cured product has (a) a beautiful surface, (b) high rigidity and high elastic modulus, and (c) excellent toughness and adhesion.

[0285] 〔5. Other uses〕

[0286] The above-mentioned resin composition, the mixture of the resin composition and the matrix resin (hereinafter referred to as the resin composition, etc.) can be used for various purposes, and these uses are not particularly limited. The resin composition, etc. are preferably used for adhesives, coating materials, adhesives for reinforcing fibers, composite materials, modeling materials for 3D printers, sealants, electronic substrates, ink adhesives, wood chip adhesives, adhesives for rubber chips, foam adhesives, adhesives for castings, bed materials and rock bed consolidation materials for ceramics, urethane foams and other purposes. As urethane foams, automotive sheets, automotive interior parts, sound absorbing materials, vibration damping materials, shock absorbers (impact absorbing materials), heat insulating materials, bed material cushioning pads for construction, etc. can be cited.

[0287] Among the above-mentioned uses, the present resin composition and the like are more preferably used as an adhesive, a coating material, an adhesive for reinforcing fibers, a composite material, a modeling material for a 3D printer, a sealant, and an electronic substrate.

[0288] (5-1. Adhesive)

[0289] The adhesive agent according to one embodiment of the present invention includes the present resin composition described above, etc. The adhesive agent according to one embodiment of the present invention has the above-described configuration and thus has excellent adhesiveness.

[0290] The adhesive according to one embodiment of the present invention is simply referred to as the present adhesive.

[0291] The present adhesive can be preferably used for various applications such as automobile interior materials, general woodworking, furniture, interior decoration, wall materials, and food packaging.

[0292] This adhesive has good adhesion to various covering materials such as cold-rolled steel, aluminum, polyester (FRP) reinforced with glass fiber, panels of cured products of thermosetting resins such as epoxy resin reinforced with carbon fiber, panels of thermoplastic resin sheets reinforced with carbon fiber, seat molding adhesive (SMC), acrylonitrile-butadiene-styrene copolymer (ABS), polyvinyl chloride (PVC), polycarbonate, polypropylene, TPO, wood and glass.

[0293] The adhesive has excellent adhesive properties and flexibility not only at low temperatures (about -20°C) to room temperature but also at high temperatures (about 80°C). Therefore, the adhesive is preferably used as a structural adhesive.

[0294] Structural adhesives using this adhesive can be used, for example, as adhesives for structural parts in automobiles and vehicles (Shinkansen, trams, etc.), civil engineering, construction, building materials, woodworking, electrical, products, aircraft, and aerospace industries. In particular, automotive-related uses include bonding interior materials such as ceilings, doors, and sheets, and bonding exterior materials such as automotive lighting fixtures such as lamps and shopping malls.

[0295] The present adhesive can be produced using the present resin composition, etc. The method for producing the present adhesive is not particularly limited, and a known method can be used.

[0296] (5-2. Coating material)

[0297] A coating material according to one embodiment of the present invention includes the present resin composition, etc. Since the coating material according to one embodiment of the present invention has the above-mentioned configuration, it is possible to provide a coating film having excellent load resistance and wear resistance.

[0298] The coating material according to one embodiment of the present invention may also be referred to as the present coating material.

[0299] When the present coating material is applied to a bed or corridor, for example, the construction method used can be generally applied. For example, after applying a primer to the substrate adjusted by the substrate, the present coating material is evenly applied using an iron, a roller, a rake, a spray gun, etc. according to the construction conditions. After the present coating material is applied, it is cured to obtain a paving film with good performance. The coating film obtained by curing the present coating material can be called a coating film with excellent load resistance and wear resistance.

[0300] The viscosity of the resin composition used for the coating material can be adjusted depending on the construction method of the coating material. For example, when an iron or a rake is used for the construction of the coating material, the viscosity of the resin composition used for the coating material can be generally adjusted to about 500 to 9000 cps / 25°C. When a roller or a spray is used for the construction of the coating material, the viscosity of the resin composition used for the coating material can be generally adjusted to about 100 to 3000 cps / 25°C.

[0301] There is no particular limitation on the substrate (in other words, the material of the bed or porch) to which the coating material is applied. Specifically, (a) inorganic substrates such as concrete walls, concrete slabs, concrete blocks, CMU (Concrete Masonry Unit), mortar boards, ALC (Autoclaved Light-weight Concrete) boards, gypsum boards (Dens Glass Gold: manufactured by Georgia Pacific, etc.), and stone slabs, (b) wooden substrates (wood, plywood, OSB (Oriented Strand Board), etc.), asphalt, modified asphalt waterproof sheets, ethylene-propylene-diene rubber (EPDM) waterproof sheets, TPO waterproof sheets, plastics, FRP, urethane foam insulation materials, and (c) metal substrates such as metal panels.

[0302] The situation of applying this coating material to a metal substrate or porous substrate is described. After the above-mentioned coating, the laminate obtained by curing the coating material has excellent corrosion resistance to the above-mentioned substrate. In addition, the coating film obtained by curing the coating material after the above-mentioned coating can give excellent crack resistance and load resistance to the substrate. Thus, the mode of applying this coating material to a metal substrate or porous substrate is a particularly preferred mode.

[0303] The coating method of the present coating material is not particularly limited, and the coating can be carried out by a known coating method such as iron, rake, brush, roller, air spray, airless spray, etc.

[0304] The use of the coating material is not particularly limited, and examples thereof include automobiles, electrical equipment, office machines, building materials, wood, coating beds, paving, heavy food protection, concrete food protection, waterproofing of roofs and roots, corrosion resistance of roofs and roots, waterproofing of underground waterproofing, automobile repair, can coating, external coating, intermediate coating, internal coating, primer, electroplating coating, high weather resistance coating, non-yellowing coating, etc. When used as a coating material for coating beds and paving, it can be used in factories, laboratories, warehouses, clean rooms, etc.

[0305] The present coating material can be produced using the present resin composition, etc. The method for producing the present coating material is not particularly limited, and a known method can be used.

[0306] (5-3. Composite materials)

[0307] The composite material according to one embodiment of the present invention is a composite material containing the present resin composition as a binder for reinforcing fibers. The composite material according to one embodiment of the present invention has the above-mentioned structure and therefore has advantages of excellent toughness and impact resistance.

[0308] The composite material according to one embodiment of the present invention is also simply referred to as this composite material.

[0309] This composite material can include reinforcing fibers. As the above-mentioned reinforcing fibers, there is no particular limitation, and glass fibers, long glass fibers, carbon fibers, natural fibers, metal fibers, thermoplastic resin fibers, boron fibers, aramid fibers, polyethylene fibers, Ceylon reinforcing fibers, etc. can be enumerated. Among these reinforcing fibers, glass fibers and carbon fibers are particularly preferred.

[0310] The manufacturing method (molding method) of the composite material is not particularly limited, and examples thereof include an autoclave molding method using a prepreg, a filament winding molding method, a hand lay-up molding method, a vacuum bag molding method, a resin injection molding (RTM) method, a vacuum assisted resin injection molding (VARTM) method, a pull molding method, an injection molding method, a sheet winding molding method, a spraying method, a BMC (Bulk Molding Compound) method, an SMC (Sheet Molding Compound) method, and the like.

[0311] In particular, when carbon fiber is used as a reinforcing fiber, as a method for manufacturing the present composite material, it is preferred to use an autoclave molding method using prepreg, a filament winding molding method, a hand lay-up molding method, a vacuum bag molding method, a resin injection molding (RTM) method, a vacuum assisted resin injection molding (VARTM) method, etc.

[0312] The use of the composite material is not particularly limited, and examples thereof include aircraft, spacecraft, automobiles, bicycles, ships, weapons, windmills, sporting goods, containers, building materials, waterproof materials, printed circuit boards, and electrical insulating materials.

[0313] The composite material can be produced using the resin composition. For more details about the composite material, reinforcing fibers, production method (molding method), production conditions (molding conditions), compounding ingredients, uses, etc., there are U.S. Patent Publication No. 2006 / 0173128, U.S. Patent Publication No. 2012 / 0245286, JP-A-2002-530445 (International Publication No. WO2000 / 029459), JP-A-55-15762 0 (U.S. Patent No. 4,251,428), Japanese Patent Publication No. 2013-504007 (International Publication No. WO2011 / 028271), Japanese Patent Publication No. 2007-125889 (U.S. Publication No. 2007 / 0098997), and Japanese Patent Publication No. 2003-220661 (U.S. Publication No. 2003 / 0134085).

[0314] (5-4. Modeling materials for 3D printers)

[0315] A modeling material for a 3D printer according to an embodiment of the present invention includes the present resin composition, etc. The modeling material for a 3D printer according to an embodiment of the present invention has the above-mentioned structure and thus has advantages of excellent toughness and impact resistance.

[0316] The modeling material of the 3D printer according to one embodiment of the present invention is also simply referred to as the modeling material.

[0317] The use of the modeling material is not particularly limited, and examples thereof include prototypes for the purpose of verifying the appearance and function of products before actually manufacturing them, aircraft parts, building parts, and medical equipment parts.

[0318] The present modeling material can be produced using the present resin composition, etc. The method for producing the present modeling material is not particularly limited, and a known method can be used.

[0319] (5-5. Sealant)

[0320] The sealant according to one embodiment of the present invention is formed by using the present resin composition, etc. The sealant according to one embodiment of the present invention has the above-mentioned configuration, and thus has advantages of excellent toughness and impact resistance.

[0321] The sealant according to one embodiment of the present invention is also simply referred to as the present sealant.

[0322] The use of the sealing agent is not particularly limited, and examples thereof include sealing of various electrical devices such as semiconductors and power devices.

[0323] The present sealant is produced using the present resin composition, etc. The method for producing the present sealant is not particularly limited, and a known method can be used.

[0324] (5-6. Electronic substrate)

[0325] The electronic substrate according to one embodiment of the present invention is formed by using the above-mentioned present resin composition, etc. The electronic substrate according to one embodiment of the present invention has the above-mentioned structure and thus has advantages of excellent toughness and impact resistance.

[0326] The electronic substrate according to one embodiment of the present invention is also simply referred to as this electronic substrate.

[0327] The application of the electronic substrate is not particularly limited, and examples thereof include printed circuits, printed wiring, printed wiring boards, printed circuit boards, printed circuit mounted products, printed wiring boards, and printed boards.

[0328] The present electronic substrate can be produced from the present resin composition etc. using the present resin composition etc. There are no particular limitations on the method for producing the present electronic substrate, and a known method can be used.

[0329] 〔Summary〕

[0330] One embodiment of the present invention includes the following invention.

[0331] (1) A method for producing a resin composition, comprising a washing step of washing the resin composition with water, wherein the resin composition comprises polymer microparticles (A) and a resin (B), wherein the polymer microparticles (A) have a graft portion, the graft portion being composed of a polymer comprising constituent units derived from one or more monomers selected from an aromatic vinyl monomer, a vinyl cyanide monomer, and a (meth)acrylate monomer, and the resin (B) is a liquid, semisolid, or solid having a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25° C.

[0332] When the total of the polymer fine particles (A) and the resin (B) is 100% by weight, the polymer fine particles (A) are 1 to 70% by weight, and the resin (B) is 30 to 99% by weight.

[0333] (2) A method for producing a resin composition according to (2), further comprising a coagulation step of obtaining the resin composition as an agglomerate comprising polymer particles (A) and resin (B) from latex using at least one method selected from the group consisting of a coagulant, shearing, and freezing.

[0334] (3) A method for producing a resin composition according to (2), wherein the above-mentioned coagulation step includes the following steps: a first coagulation step of obtaining agglomerates containing polymer particles (A) from a latex containing polymer particles (A); an intermediate washing step of washing the agglomerates obtained in the above-mentioned first coagulation step with water; and a second coagulation step of mixing the agglomerates after the above-mentioned intermediate washing step with a resin (B) to obtain agglomerates containing polymer particles (A) and resin (B).

[0335] (4) The method for producing a resin composition according to any one of (1) to (3), wherein the washing step includes a step of kneading with a kneader or stirring with a stirrer.

[0336] (5) The method for producing a resin composition according to any one of (1) to (4), wherein the intermediate washing step includes a step of washing the aggregates obtained in the first coagulation step with water having a temperature lower than the glass transition temperature of the polymer fine particles (A).

[0337] (6) The method for producing a resin composition according to any one of (1) to (5), wherein the temperature of water in the washing step is 60° C. or lower.

[0338] (7) A resin composition comprising polymer particles (A) and a resin (B), wherein the polymer particles (A) have a graft portion, the graft portion being composed of a polymer comprising a constituent unit derived from one or more monomers selected from an aromatic vinyl monomer, a vinyl cyanide monomer and a (meth)acrylate monomer, and the resin (B) is a liquid, semi-solid or solid resin (B) having a viscosity of 100 mPa·s to 1,000,000 mPa·s at 25° C., and when the total of the polymer particles (A) and the resin (B) is taken as 100 weight %, the polymer particles (A) account for 30 to 70 weight % and the resin (B) account for 30 to 70 weight %.

[0339] (8) The resin composition according to (7), wherein the content of the element S or P is removed by 10% or more in one washing.

[0340] (9) The resin composition according to (7) or (8), wherein the resin composition does not pass through a metal mesh of 8 mesh after being placed on a metal mesh of 8 mesh at 25° C. for 10 minutes.

[0341] (10) The resin composition according to any one of (7) to (9), wherein the polymer fine particles (A) are rubber-containing graft copolymers having an elastomer and the graft portion graft-bonded to the elastomer.

[0342] (11) The resin composition according to (10), wherein the elastomer comprises one or more selected from the group consisting of diene rubber, (meth)acrylate rubber, and silicone rubber elastomer.

[0343] (12) The resin composition according to any one of (7) to (11), wherein the resin (B) comprises a thermosetting resin.

[0344] Example

[0345] Hereinafter, one embodiment of the present invention will be described in more detail according to examples and comparative examples, but the present invention is not limited thereto. One embodiment of the present invention can be appropriately changed and implemented within the scope suitable for the above or the following purport, and they are all included in the technical scope of the present invention. It should be noted that in the following examples and comparative examples, "parts" and "%" refer to parts by weight or weight %.

[0346] [Evaluation method]

[0347] First, the evaluation methods of the resin compositions produced according to Examples and Comparative Examples will be described in order.

[0348] <Measurement of volume average particle size>

[0349] The volume average particle size (Mv) of the elastomer or polymer microparticles (A) dispersed in the aqueous latex is measured using Nanotrac Wave II-EX150 (manufactured by Micro Track Bell Co., Ltd.). A liquid obtained by diluting the aqueous latex with deionized water is used as a measurement sample. The measurement is performed by inputting water and the refractive index of the elastomer or polymer microparticles (A) obtained in each manufacturing example, and adjusting the sample concentration in a measurement time of 120 seconds and a loading index in the range of 1 to 20.

[0350] <Differential Scanning Calorimetry (DSC) of Resin (B)>

[0351] The resin (B) used in the following examples and comparative examples, i.e., liquid epoxy resin (JER828 manufactured by Mitsubishi Chemical Corporation), was subjected to differential scanning calorimetry using DSC7020 (manufactured by Hitachi High Tech Science Co., Ltd.). The heating rate was set to 10°C / min. As a result, it was found that the liquid epoxy resin had an endothermic peak at -15°C.

[0352] <Viscosity measurement>

[0353] The viscosity of the resin (B) used in the following examples and comparative examples, i.e., the liquid epoxy resin (Mitsubishi Chemical Corporation, JER828), or the obtained resin composition was measured. The device used was a digital viscometer DV-II+Pro type manufactured by Brookfield. In addition, according to the viscosity range, the spindle CPE-52 was used to measure the viscosity at a measurement temperature of 25°C by changing the Shear Rate (slip speed) as needed. The result was that the liquid epoxy resin was 12000 mPa·s.

[0354] <Measurement of Solvent Content in Resin Composition>

[0355] The amount of solvent contained in the obtained resin composition was measured using gas chromatography (GC-2014, manufactured by Shimadzu Corporation).

[0356] <Measurement of Residual S Amount or Residual P Amount in Resin Composition>

[0357] The amount of residual S or residual P in the resin composition was measured. Specifically, the fluorescence X-ray segmentation device SPECTRO XEPOS (manufactured by SPECTRO) was used for measurement. In addition, when sodium dodecylbenzenesulfonate (DBS) was used as an emulsifier, only the amount of residual S was measured. When sodium polyoxyethylene lauryl ether phosphate was used as an emulsifier, only the amount of residual P was measured.

[0358] 1. Polymerization of elastomers

[0359] Preparation Example 1-1: Preparation of polybutadiene rubber latex (R-1)

[0360] In the pressure polymerizer, 200 parts of deionized water, 0.03 parts of tripotassium phosphate, 0.002 parts of disodium ethylenediaminetetraacetate (EDTA), 0.001 parts of iron sulfate heptahydrate, and 1.55 parts of sodium dodecylbenzene sulfonate (SDBS) as an emulsifier were added. Next, the gas inside the pressure polymerizer was replaced with nitrogen while stirring the added raw materials, thereby fully removing oxygen from the inside of the pressure polymerizer. Thereafter, 100 parts of butadiene (Bd) were added to the pressure polymerizer, and the temperature inside the pressure polymerizer was raised to 45°C. Thereafter, 0.03 parts of hydrogen peroxide p-menthane (PHP) was added to the pressure polymerizer, and then 0.10 parts of sodium formaldehyde sulfoxylate (SFS) was added to the pressure polymerizer to start polymerization. At 15 hours from the start of polymerization, devolatilization was performed under reduced pressure, and the polymerization was terminated by devolatilizing and removing the monomers remaining when not used for polymerization. During the polymerization, PHP, EDTA and ferrous sulfate 7-hydrate salt are added to the pressure-resistant polymerization vessel in any amount and at any time. By the polymerization, an aqueous latex (R-1) containing an elastomer with polybutadiene rubber as the main component is obtained. The volume average particle size of the elastomer contained in the obtained aqueous latex is 90 nm.

[0361] Preparation Example 1-2: Preparation of polybutadiene rubber latex (R-2)

[0362] 7 parts of the polybutadiene rubber latex (R-1) obtained above, 200 parts of deionized water, 0.03 parts of tripotassium phosphate, 0.002 parts of EDTA and 0.001 parts of ferrous sulfate 7 hydrate are added to a pressure polymerizer in fixed composition. Next, the gas inside the pressure polymerizer is replaced with nitrogen while stirring the added raw materials, and oxygen is fully removed from the inside of the pressure polymerizer. Thereafter, 3 parts of Bd9 are added to the pressure polymerizer, and the temperature inside the pressure polymerizer is raised to 45°C. Thereafter, 0.02 parts of PHP are added to the pressure polymerizer, and then 0.10 parts of SFS are added to the pressure polymerizer to start polymerization. By devolatilizing under reduced pressure at the 30th hour from the start of polymerization, the monomers remaining when not used for polymerization are devolatilized and removed, thereby completing the polymerization. During the polymerization, PHP, EDTA, ferrous sulfate 7 hydrate and SDBS are added to the pressure polymerizer in any amount and at any time. By this polymerization, an aqueous latex (R-2) containing an elastomer having polybutadiene rubber as a main component was obtained. The volume average particle size of the elastomer contained in the obtained aqueous latex was 195 nm.

[0363] Preparation Example 1-3: Preparation of polystyrene-butadiene rubber latex (R-3)

[0364] In a pressure polymerizer, 160 parts of deionized water, 0.002 parts of EDTA, 0.001 parts of ferrous sulfate 7-hydrate, 0.029 parts of polyoxyethylene lauryl ether phosphoric acid, and 0.003 parts of sodium hydroxide are added. Here, polyoxyethylene lauryl ether phosphoric acid becomes polyoxyethylene lauryl ether sodium phosphate in the presence of sodium hydroxide, and functions as an emulsifier. Next, the gas inside the pressure polymerizer is replaced with nitrogen on the basis of stirring the raw materials added, so as to fully remove oxygen from the inside of the pressure polymerizer. Thereafter, 76.5 parts of Bd and 23.5 parts of styrene (St) are added to the pressure polymerizer, and the temperature inside the pressure polymerizer is raised to 45°C. Thereafter, 0.03 parts of PHP are added to the pressure polymerizer, and then 0.05 parts of SFS are added to the pressure polymerizer to start polymerization. At 20 hours from the start of polymerization, devolatilization was performed under reduced pressure, and the polymerization was terminated by devolatilization of the monomers remaining in the case of polymerization. During the polymerization, PHP, polyoxyethylene lauryl ether phosphate and sodium hydroxide were added to the pressure-resistant polymerization vessel in any amount and at any time. By means of this polymerization, an aqueous latex (R-3) containing an elastomer with polystyrene-butadiene rubber as the main component was obtained. The volume average particle size of the elastomer contained in the obtained aqueous latex was 192 nm.

[0365] Preparation Example 1-4: Preparation of polybutadiene rubber latex (R-4)

[0366] 200 parts by weight of deionized water, 0.03 parts by weight of tripotassium phosphate, 0.002 parts by weight of disodium ethylenediaminetetraacetate (EDTA), 0.001 parts by weight of ferrous sulfate 7-hydrate, and 1.55 parts by weight of sodium dodecylbenzenesulfonate (SDBS) as an emulsifier were added to the pressure polymerizer. Next, the gas inside the pressure polymerizer was replaced with nitrogen while stirring the added raw materials, thereby fully removing oxygen from the inside of the pressure polymerizer. Thereafter, 100 parts by weight of butadiene (Bd) was added to the pressure polymerizer, and the temperature inside the pressure polymerizer was raised to 45°C. Thereafter, 0.03 parts by weight of p-menthane hydrogen peroxide (PHP) was added to the pressure polymerizer, and then 0.10 parts by weight of sodium formaldehyde sulfoxylate (SFS) was added to the pressure polymerizer to start polymerization. Devolatilization is carried out under reduced pressure at 15 hours from the start of polymerization, and the polymerization is terminated by devolatilizing and removing the monomers that do not remain when not used for polymerization. During the polymerization, PHP, EDTA, and ferrous sulfate·7 water and salt are added to the pressure-resistant polymerization vessel in any amount and at any time. By means of this polymerization, an aqueous latex (R-4) containing an elastomer with polybutadiene rubber as the main component is obtained. The volume average particle size of the elastomer contained in the obtained aqueous latex is 70nm.

[0367] 2. Preparation of polymer microparticles (A) (polymerization of grafted part)

[0368] Preparation Example 2-1: Preparation of polymer microparticle latex (L-1)

[0369] 250 parts of the above-mentioned polybutadiene rubber latex (R-2) (including 87 parts of elastomer with polybutadiene rubber as the main component) and 50 parts of deionized water are added to a glass reactor. Here, the above-mentioned glass reactor has a thermometer, a stirrer, a reflux cooler, a nitrogen gas inlet and a monomer addition device. The gas in the glass reactor is replaced with nitrogen, and the raw materials added at 60°C are stirred. Next, 0.004 parts of EDTA, 0.001 parts of ferrous sulfate 7 hydrate and 0.2 parts of SFS are added to the glass reactor and stirred for 10 minutes. Thereafter, a mixture of 12.5 parts of methyl methacrylate (MMA), 0.5 parts of St and 0.035 parts of tert-butyl hydroperoxide (BHP) is continuously added to the glass reactor for 80 minutes. Thereafter, 0.013 parts of BHP are added to the glass reactor, and the mixture in the glass reactor is stirred for 1 hour to complete the polymerization. By the above operation, an aqueous latex (L-1) containing polymer particles (A) and an emulsifier is obtained. The polymerization conversion rate of the monomer component is 99% or more. The volume average particle size of the polymer particles (A) contained in the obtained aqueous latex is 200nm. The solid concentration (concentration of polymer particles (A)) of the obtained aqueous latex (L-1) is 30%.

[0370] Preparation Example 2-2: Preparation of polymer microparticle latex (L-2)

[0371] 250 parts of the above-mentioned polystyrene-butadiene rubber latex (R-3) (including 87 parts of an elastomer with polystyrene-butadiene rubber as the main component) and 50 parts of deionized water are added to a glass reactor. Here, the above-mentioned glass reactor has a thermometer, a stirrer, a reflux cooler, a nitrogen gas inlet and a monomer addition device. The gas in the glass reactor is replaced with nitrogen, and the raw materials added at 60°C are stirred. Next, 0.004 parts of EDTA, 0.001 parts of ferrous sulfate 7 hydrate and 0.2 parts of SFS are added to the glass reactor and stirred for 10 minutes. Thereafter, a mixture of 12.5 parts of MMA, 0.5 parts of St and 0.035 parts of BHP is continuously added to the glass reactor for 80 minutes. Thereafter, 0.013 parts of BHP are added to the glass reactor, and the stirring of the mixture in the glass reactor is further continued for 1 hour to complete the polymerization. By the above operation, an aqueous latex (L-2) containing polymer particles (A) and an emulsifier is obtained. The polymerization conversion rate of the monomer component is 99% or more. The volume average particle size of the polymer particles (A) contained in the obtained aqueous latex is 200nm. The solid content concentration (concentration of polymer particles (A)) of the obtained aqueous latex (L-2) is 30%.

[0372] Preparation Example 2-3: Preparation of polymer microparticle latex (L-3)

[0373] 250 parts by weight of the above-mentioned polybutadiene rubber latex (R-4) (including 83 parts by weight of an elastomer having polybutadiene rubber as a main component) are put into a glass reactor. Here, the above-mentioned glass reactor has a thermometer, a stirrer, a reflux cooler, a nitrogen inlet and a monomer addition device. The gas in the glass reactor is replaced with nitrogen, and the raw materials put in at 60°C are stirred. Next, 0.004 parts by weight of EDTA, 0.001 parts by weight of ferrous sulfate 7 hydrate and 0.20 parts by weight of SFS are added to the glass reactor and stirred for 10 minutes. Thereafter, a mixture of 0.8 parts by weight of methyl methacrylate (MMA), 5.4 parts by weight of styrene (St), 3.9 parts by weight of acrylonitrile (AN), 6.9 parts by weight of glycidyl methacrylate (GMA) and 0.043 parts by weight of tert-butyl hydroperoxide (BHP) is continuously added to the glass reactor for 120 minutes. Thereafter, 0.013 parts by weight of BHP was added to the glass reactor, and further, the mixture in the glass reactor was stirred for 1 hour to complete the polymerization. By the above operation, an aqueous latex (L-3) containing polymer particles (A) was obtained. The polymerization conversion rate of the monomer component was 99% or more. The volume average particle size of the polymer particles (A) contained in the obtained aqueous latex was 80 nm. The solid content concentration (concentration of polymer particles (A)) of the obtained aqueous latex (L-3) was 30%.

[0374] (Example 1)

[0375] 20 g of 24% sodium sulfate is added to 333 g of aqueous latex (L-1), and the mixture is mixed with a spatula to obtain a latex containing aggregates containing polymer particles (A). Thereafter, the aggregates and the water component are separated from the latex. Thereafter, (a1) the obtained aggregates are mixed with 500 g of ion exchange water, and the mixture is stirred at 30°C for 30 minutes, and (a2) the obtained mixture is subjected to reduced pressure filtration to remove the washing water from the mixture. The above-mentioned operations (a1) and (a2) are further repeated twice (a total of 3 times) to obtain aggregates. The obtained aggregates and 150 g of resin (B), i.e., liquid epoxy resin (JER828 manufactured by Mitsubishi Chemical Corporation. The same shall apply hereinafter) are added and kneaded using a continuous kneader to obtain aggregates containing polymer particles (A) and resin (B), i.e., a resin composition. Thereafter, (b1) the obtained resin composition (agglomerate) and 375 g of ion exchange water are mixed, and the mixture is stirred at 90°C for 30 minutes, and (b2) the oil-water separation is performed from the obtained mixture, and the washing water is removed to take out the resin composition. The above operations (b1) and (b2) are further repeated twice (a total of 3 times) to obtain a washed resin composition. The obtained resin composition is subjected to vacuum devolatilization at 115°C to remove water. After measuring the residual S amount of the obtained resin composition, the result is 50 ppm. In addition, the weight ratio of polymer particles (A) to resin (B) is 40:60, and the resin composition is in a paste state.

[0376] (Comparative Example 1)

[0377] 20 g of 24% sodium sulfate was added to 333 g of aqueous latex (L-1), and the mixture was mixed with a spatula to obtain a latex containing aggregates containing polymer microparticles (A). Thereafter, the aggregates and the water component were separated from the latex. Thereafter, (1) the obtained aggregates were mixed with 500 g of ion exchange water, and the mixture was stirred at 30°C for 30 minutes, and (2) the obtained mixture was subjected to reduced pressure filtration to remove the washing water from the mixture. The above operations (1) and (2) were further repeated 5 times (a total of 6 times) to obtain aggregates. The obtained aggregates and 150 g of resin (B), i.e., liquid epoxy resin, were added and kneaded using a continuous kneader to obtain aggregates containing polymer microparticles (A) and resin (B), i.e., a resin composition. The obtained resin composition was vacuum devolatilized at 115°C to remove water. The residual S content of the obtained resin composition was measured, and the result was 150 ppm. The weight ratio of the polymer fine particles (A) to the resin (B) was 40:60, and the resin composition was in a paste form.

[0378] (Example 2)

[0379] 20 g of 24% sodium sulfate was added to 150 g of liquid epoxy resin, which is resin (B), and the mixture was mixed with a spatula. 333 g of aqueous latex (L-1) was added to the obtained mixture, and the mixture was mixed with a spatula to obtain a latex containing an aggregate of polymer particles (A) and resin (B), which is a resin composition. Thereafter, the resin composition and the water component were separated from the latex. Thereafter, 100 g of the obtained resin composition (aggregate) and 150 g of ion exchange water were mixed, and the mixture was stirred at 90°C for 30 minutes. The oil and water were separated from the obtained mixture, and the washed resin composition was taken out. The obtained resin composition was vacuum devolatilized at 115°C to remove water. After measuring the residual S content of the obtained resin composition, the result was 375 ppm. In addition, the weight ratio of polymer particles (A) to resin (B) was 40:60, and the resin composition was in a paste state.

[0380] (Example 3)

[0381] 20 g of 24% sodium sulfate and 333 g of aqueous latex (L-1) were added to 300 g of resin (B), i.e., liquid epoxy resin, and mixed with a scraper to obtain a latex containing an aggregate of polymer particles (A) and resin (B), i.e., a resin composition. Thereafter, the resin composition and the water component were separated from the latex. Thereafter, 100 g of the obtained resin composition (agglomerate) and 150 g of ion exchange water were mixed, the mixture was stirred at 90°C for 30 minutes, the oil and water were separated from the obtained mixture, and the washed resin composition was taken out. The obtained resin composition was vacuum devolatilized at 115°C to remove water. The amount of residual S in the obtained resin composition was measured, and the result was 563 ppm. In addition, the weight ratio of polymer particles (A) to resin (B) was 25:75, and the resin composition was liquid.

[0382] (Comparative Example 2)

[0383] 20 g of 24% sodium sulfate was added to 25 g of liquid epoxy resin, i.e., resin (B), and mixed with a spatula. 333 g of aqueous latex (L-1) was added to the obtained mixture, and mixed with a spatula to obtain a latex containing an agglomerate of polymer particles (A) and resin (B), i.e., a resin composition. Thereafter, the resin composition and the water component were separated from the latex. Thereafter, 100 g of the obtained resin composition (agglomerate) and 150 g of ion exchange water were mixed, and the mixture was stirred at 90°C for 30 minutes, and the oil-water separation was performed from the obtained mixture, and the washed resin composition was taken out. The obtained resin composition was subjected to vacuum devolatilization at 115°C to remove water. The amount of residual S in the obtained resin composition was measured, and the result was 740 ppm. In addition, the weight ratio of polymer particles (A) to resin (B) was 80:20, and the resin composition was in the form of powder.

[0384] (Example 4)

[0385] 333 g of aqueous latex (L-1) was stirred at 12000 rpm using a homomixer, and 150 g of resin (B), i.e., liquid epoxy resin, was added to the homomixer and stirred for further 30 minutes. The obtained mixture was frozen and placed in a -20°C freezer for 12 hours to obtain a frozen latex (L-1). The frozen latex (L-1) was immersed in warm water at 50°C for thawing. From the thawed latex (L-1), the agglomerates containing polymer particles (A) and resin (B), i.e., the resin composition, and the water component were separated. 200 g of the obtained resin composition (agglomerate) and 300 g of ion exchange water were mixed, and the mixture was stirred at 90°C for 30 minutes. The oil and water were separated from the obtained mixture, and the washed resin composition was taken out. The obtained resin composition was vacuum devolatilized at 115°C to remove water. The residual S content of the obtained resin composition was measured, and the result was 66 ppm. The weight ratio of the polymer fine particles (A) to the resin (B) was 40:60, and the resin composition was in a paste form.

[0386] (Example 5)

[0387] Using a homomixer, 333 g of the aqueous latex (L-1) was stirred at 12000 rpm, and 66.7 g of the resin (B), i.e., a liquid epoxy resin, was added to the homomixer and stirred for further 30 minutes. The obtained mixture was frozen and placed in a -20°C freezer for 12 hours to obtain a frozen latex (L-1). The frozen latex (L-1) was immersed in warm water at 50°C to thaw. From the thawed latex (L-1), the agglomerates containing polymer particles (A) and resin (B), i.e., the resin composition, and the water component were separated. The operation of supplying 100 g of the obtained resin composition (agglomerate) and 30 g of ion exchange water to a continuous kneader and the operation of centrifugal dehydration of the obtained mixture were repeated for a total of 7 cycles to obtain a washed resin composition. The obtained resin composition was vacuum devolatilized at 115°C to remove water. The residual S content of the obtained resin composition was measured, and the result was 68 ppm. The weight ratio of the polymer fine particles (A) to the resin (B) was 60:40, and the resin composition was in the form of chips.

[0388] (Example 6)

[0389] 333 g of aqueous latex (L-1) was stirred at 6000 rpm using a high shear emulsifier, and 66.7 g of resin (B), i.e., liquid epoxy resin, was added to the high shear emulsifier and stirred for further 90 minutes. From the obtained mixture (latex), the agglomerates containing polymer particles (A) and resin (B), i.e., the resin composition and the water component were separated. The operation of supplying 100 g of the obtained resin composition (agglomerate) and 60 g of ion exchange water to a continuous kneader and the operation of centrifugal dehydration of the obtained mixture were repeated for a total of 3 cycles to obtain a washed resin composition. The obtained resin composition was vacuum devolatilized at 115°C to remove water. The amount of residual S in the obtained resin composition was measured and the result was 60 ppm. In addition, the weight ratio of polymer particles (A) to resin (B) was 60:40, and the resin composition was in the form of crumbs.

[0390] (Example 7)

[0391] Using a high shear emulsifier, 333 g of the aqueous latex (L-1) was stirred at 6000 rpm, and 150 g of the resin (B), i.e., a liquid epoxy resin, was added to the high shear emulsifier and stirred for further 90 minutes. From the obtained mixture (latex), the agglomerates containing the polymer particles (A) and the resin (B), i.e., the resin composition, and the water component were separated. The operation of supplying the obtained resin composition (agglomerate) and 100 g of ion exchange water to a continuous kneader and the operation of centrifugal dehydration of the obtained mixture were repeated for a total of 3 cycles to obtain a washed resin composition. The obtained resin composition was vacuum devolatilized at 115°C to remove water. The amount of residual S in the obtained resin composition was measured and the result was 41 ppm. In addition, the weight ratio of the polymer particles (A) to the resin (B) was 40:60, and the resin composition was in a paste state.

[0392] (Example 8)

[0393] 333 g of aqueous latex (L-2) was supplied to a metal surface at -30°C and scraped off after 1 minute to obtain a frozen latex (L-2). The frozen latex (L-2) was thawed at room temperature. The thawed latex (L-2) and 66.7 g of resin (B), i.e., liquid epoxy resin, were kneaded using a continuous kneader. Next, the agglomerates containing polymer particles (A) and resin (B), i.e., the resin composition and the water component were separated from the latex. The operation of supplying 100 g of the obtained resin composition (agglomerate) and 60 g of ion exchange water to a continuous kneader and the operation of centrifugal dehydration of the obtained mixture were repeated for a total of 3 cycles to obtain a washed resin composition. The obtained resin composition was vacuum devolatilized at 115°C to remove water. The residual P content of the obtained resin composition was measured and the result was 58 ppm. In addition, the weight ratio of polymer particles (A) to resin (B) was 60:40, and the resin composition was in the form of crumbs.

[0394] (Comparative Example 3)

[0395] 333 g of aqueous latex (L-2) was supplied to a metal surface at -30°C and scraped off after 1 minute to obtain a frozen latex (L-2). The frozen latex (L-2) was thawed at room temperature. From the thawed latex (L-2), the aggregates containing polymer particles (A) and the water component were separated. The operation of supplying the obtained aggregates and 100 g of ion exchange water to a continuous kneader and the operation of supplying the obtained mixture to a centrifugal dehydration were repeated for a total of 3 cycles to obtain a washed aggregate. Thereafter, 100 g of the obtained aggregates and 66.7 g of resin (B), i.e., liquid epoxy resin, were kneaded using a continuous kneader. Next, the aggregates containing polymer particles (A) and resin (B), i.e., the resin composition, and the water component were separated from the latex. The obtained resin composition (aggregate) was vacuum devolatilized at 115°C to remove water. The residual P content of the obtained resin composition was measured, and the result was 120 ppm. The dispersibility of the obtained resin composition was evaluated.

[0396] (Example 9)

[0397] 20 g of 24% sodium sulfate was added to 150 g of the liquid epoxy resin (ie, resin (B)), and the mixture was mixed with a spatula. 333 g of aqueous latex (L-3) was added to the obtained mixture, and the mixture was mixed with a spatula to obtain a latex containing an agglomerate of polymer particles (A) and resin (B), namely, a resin composition. Thereafter, the resin composition and the water component were separated from the latex. Thereafter, 100 g of the obtained resin composition (agglomerate) and 150 g of ion exchange water were mixed, and the mixture was stirred at 50°C for 30 minutes, and the oil-water separation was performed from the obtained mixture, and the washed resin composition was taken out. The viscosity at the washing temperature was 110,000 mPa·s. After performing this operation a total of 3 times, the obtained resin composition was vacuum-devolatilized at 115°C to remove water. The amount of residual S in the obtained resin composition was measured, and the result was 504 ppm. The weight ratio of the polymer fine particles (A) to the resin (B) was 40:60, and the resin composition was in a paste form.

[0398] (Example 10)

[0399] 20 g of 24% sodium sulfate was added to 178 g of liquid epoxy resin, i.e., resin (B), and mixed with a spatula. 333 g of aqueous latex (L-3) was added to the obtained mixture, and mixed with a spatula to obtain a latex containing an aggregate of polymer particles (A) and resin (B), i.e., a resin composition. Thereafter, the resin composition and the water component were separated from the latex. Thereafter, 100 g of the obtained resin composition (agglomerate) and 150 g of ion exchange water were mixed, and the mixture was stirred at 50°C for 30 minutes, and oil-water separation was performed from the obtained mixture to take out the washed resin composition. After performing this operation a total of 3 times, the obtained resin composition was vacuum devolatilized at 115°C to remove water. The amount of residual S in the obtained resin composition was measured, and the result was 720 ppm. In addition, the weight ratio of polymer particles (A) to resin (B) was 36:64, and the resin composition was in a paste state.

[0400] (Example 11)

[0401] 20 g of 24% sodium sulfate was added to 150 g of liquid epoxy resin, which was resin (B), and the mixture was mixed with a spatula. 333 g of aqueous latex (L-3) was added to the obtained mixture, and the mixture was mixed with a spatula to obtain a latex containing an aggregate of polymer particles (A) and resin (B), i.e., a resin composition. Thereafter, the resin composition and the water component were separated from the latex. Thereafter, 100 g of the obtained resin composition (agglomerate) and 150 g of ion exchange water were mixed, the mixture was stirred at 30°C for 30 minutes, the oil and water were separated from the obtained mixture, and the washed resin composition was taken out. After performing this operation three times in total, the obtained resin composition was vacuum devolatilized at 115°C to remove water. The amount of residual S in the obtained resin composition was measured, and the result was 126 ppm. In addition, the weight ratio of polymer particles (A) to resin (B) was 40:60, and the resin composition was in a paste state.

[0402] (Comparative Example 4)

[0403] 20 g of 24% sodium sulfate was added to 25 g of liquid epoxy resin, which was resin (B), and the mixture was mixed with a spatula. 333 g of aqueous latex (L-3) was added to the obtained mixture, and the mixture was mixed with a spatula to obtain a latex containing an aggregate of polymer particles (A) and resin (B), i.e., a resin composition. Thereafter, the resin composition and the water component were separated from the latex. Thereafter, 100 g of the obtained resin composition (agglomerate) and 150 g of ion exchange water were mixed, the mixture was stirred at 50°C for 30 minutes, the oil and water were separated from the obtained mixture, and the washed resin composition was taken out. After performing this operation three times in total, the obtained resin composition was vacuum devolatilized at 115°C to remove water. The amount of residual S in the obtained resin composition was measured, and the result was 1300 ppm. In addition, the weight ratio of polymer particles (A) to resin (B) was 80:20, and the resin composition was in the form of powder.

[0404] Next, an experiment was conducted on the case where the temperature of water in the washing step was low.

[0405] (Example 12)

[0406] 20 g of 24% sodium sulfate was added to 150 g of liquid epoxy resin (ie, resin (B)), and the mixture was mixed with a spatula. 333 g of aqueous latex (L-1) was added to the obtained mixture, and the mixture was mixed with a spatula to obtain a latex containing an aggregate of polymer particles (A) and resin (B), i.e., a resin composition. Thereafter, the resin composition and the water component were separated from the latex. Thereafter, 100 g of the obtained resin composition (aggregate) and 150 g of ion exchange water were mixed, and the mixture was stirred at 50°C for 30 minutes, and the oil-water separation was performed from the obtained mixture, and the washed resin composition was taken out. The obtained resin composition was vacuum devolatilized at 115°C to remove water. The residual S content of the obtained resin composition was measured, and the result was 103 ppm. In addition, the weight ratio of polymer particles (A) to resin (B) was 40:60, and the resin composition was in a paste state.

[0407] (Example 13)

[0408] 20 g of 24% sodium sulfate was added to 150 g of liquid epoxy resin, i.e., resin (B), and mixed with a spatula. 333 g of aqueous latex (L-1) was added to the obtained mixture, and mixed with a spatula to obtain a latex containing an agglomerate of polymer particles (A) and resin (B), i.e., a resin composition. Thereafter, the resin composition and the water component were separated from the latex. Thereafter, 100 g of the obtained resin composition (agglomerate) and 150 g of ion exchange water were mixed, the mixture was stirred at 30°C for 30 minutes, oil and water were separated from the obtained mixture, and the washed resin composition was taken out. The obtained resin composition was vacuum devolatilized at 115°C to remove water. The amount of residual S in the obtained resin composition was measured, and the result was 53 ppm. In addition, the weight ratio of polymer particles (A) to resin (B) was 40:60, and the resin composition was in a paste state.

[0409] The results are shown in Table 1 below.

[0410] [Table 1]

[0411]

[0412] As described above, by comparing Example 1 and Comparative Example 1, Example 2 and Comparative Example 2, and Example 8 and Comparative Example 3, it is found that impurities can be reduced by performing the cleaning step which is one embodiment of the present invention.

[0413] In addition, in Example 2, the washing process of mixing 100 g of the resin composition with 150 g of ion exchange water at 90° C. for 30 minutes was set as one time, and in Example 5, the washing process of mixing 100 g of the resin composition and 30 g of ion exchange water was set as one time, and the content of element S in each washing and the removal rate before and after the washing process were calculated. The results are shown in Table 2.

[0414] [Table 2]

[0415]

[0416] (Example 14)

[0417] The resin composition containing 40% by weight of polymer microparticles (A) obtained from the aqueous latex (L-1) and 60% by weight of the resin (B), i.e., a liquid epoxy resin, was in a paste state. In addition, when the resin composition was placed on an 8-mesh metal mesh at 25° C. for 10 minutes, the amount of resin that did not pass through the metal mesh was 0%.

[0418] (Example 15)

[0419] The resin composition containing 60% by weight of polymer microparticles (A) obtained from the aqueous latex (L-1) and 40% by weight of the resin (B), i.e., a liquid epoxy resin, was in the form of crumbs. In addition, when the resin composition was placed on a metal mesh of 8 mesh at 25°C for 10 minutes, 1% of the resin passed through the metal mesh.

[0420] (Comparative Example 5)

[0421] The resin composition containing 20% ​​by weight of polymer microparticles (A) obtained from the aqueous latex (L-1) and 80% by weight of the resin (B), i.e., a liquid epoxy resin, was in liquid form. Moreover, after being placed on a 8-mesh metal mesh at 25° C. for 10 minutes, 90% of the particles passed through the metal mesh.

[0422] In addition, in the present example and the comparative example, no organic solvent was used in the production process, and therefore, the amount of residual organic solvent in the resin composition was 0 ppm.

[0423] Industrial Applicability

[0424] According to one embodiment of the present invention, a thermosetting resin can be blended and the composition can be suitably used in various applications such as an adhesive and a coating material.

Claims

1. A method for producing a resin composition, comprising a washing step of washing the following resin composition with water, The resin composition comprises polymer particles (A) and a resin (B), The polymer microparticles (A) have a grafted portion, the grafted portion is composed of a polymer containing constituent units derived from one or more monomers selected from aromatic vinyl monomers, vinyl cyanide monomers and (meth)acrylate monomers, and the volume average particle size thereof measured by a dynamic light scattering (DLS) particle size distribution measuring device is 0.03 μm to 10.00 μm, and the resin (B) is a liquid or semisolid having a viscosity of 100 mPa·s to 1000000 mPa·s at 25° C., When the total of the polymer fine particles (A) and the resin (B) is 100 wt %, the polymer fine particles (A) are 1 to 70 wt %, and the resin (B) is 30 to 99 wt %. The method further comprises a coagulation step before the washing step, wherein the coagulation step is a step of obtaining the resin composition as a coagulation body containing polymer microparticles (A) and resin (B) from latex by using at least one method selected from the group consisting of a coagulant, shearing, and freezing. Furthermore, the agglomeration step includes the following steps: A first coagulation step of obtaining coagulates containing polymer particles (A) from a latex containing polymer particles (A); In the second coagulation step, the coagulation obtained in the first coagulation step and the resin (B) are mixed to obtain coagulations containing the polymer fine particles (A) and the resin (B).

2. The method for producing a resin composition according to claim 1, wherein Include: The intermediate washing step is to wash the aggregates obtained in the first aggregation step with water.

3. The method for producing a resin composition according to claim 1, wherein The washing step includes a step of kneading with a kneader or stirring with a stirrer.

4. The method for producing a resin composition according to claim 2, wherein The washing step includes a step of kneading with a kneader or stirring with a stirrer.

5. The method for producing a resin composition according to claim 2 or 4, wherein: The intermediate washing step includes a step of washing the aggregates obtained in the first aggregation step with water having a temperature lower than the glass transition temperature of the polymer fine particles (A).

6. The method for producing a resin composition according to any one of claims 1 to 4, wherein The temperature of water in the washing step is 60° C. or lower.

7. The method for producing a resin composition according to claim 5, wherein: The temperature of the water in the intermediate washing step is 60° C. or lower.

Citation Information

Patent Citations

  • Melamine-formaldehyde polycondensate

    JP1993202157A

  • Epoxy resin composition

    JP1996183836A

  • New amino resin composition

    JP1997143238A

  • Polyisocyanurate compositions and composite materials

    JP2002530445A

  • Pultrusion systems and process

    US20060173128A1