Fuel cell battery

By using a hot-melt adhesive layer containing a specific ethylene-vinyl alcohol copolymer and polyamide in the fuel cell unit cell to bond the electrolyte membrane to the support frame, catalyst poisoning and hot-melt bonding caused by liquid adhesives are solved Solve the problem of agent peeling and achieve high durability and stability.

CN113675412BActive Publication Date: 2024-10-11TOYOTA JIDOSHA KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110515930.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-05-14
Filing Date
2021-05-12
Publication Date
2024-10-11
Estimated Expiration
2041-05-12

AI Technical Summary

Technical Problem

When using liquid adhesives in existing fuel cell units, the catalyst metal will be poisoned by decomposition gas and the output power will be reduced; when using hot-melt adhesives, they will easily peel off in a hydrothermal environment, resulting in insufficient durability.

Method used

A hot-melt adhesive layer containing 90 to 99 mol% of ethylene-vinyl alcohol copolymer or polyamide with 8 to 15 methylene groups in the main chain relative to the amide group is used to bond and bond the electrolyte membrane to the support frame. Perfluorosulfonic acid polymer and nylon materials enhance adhesion and durability.

Benefits of technology

It achieves high adhesion that is not easy to peel off in a hydrothermal environment and improves the durability and stability of the fuel cell unit.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113675412B_ABST
    Figure CN113675412B_ABST
Patent Text Reader

Abstract

The object of the present invention is to provide a fuel cell unit cell with high durability. The fuel cell unit cell with improved durability of the present invention is a fuel cell unit cell in which a membrane electrode assembly and a support frame are bonded to each other by a hot melt adhesive layer, the membrane electrode assembly having an electrolyte membrane and a pair of electrode catalyst layers stacked on both sides of the electrolyte membrane, the electrode catalyst layer being stacked on the inner side of the outer peripheral side of the electrolyte membrane on at least one side of the membrane electrode assembly, the hot melt adhesive layer bonding the outer peripheral side of the electrolyte membrane to the support frame, and the hot melt adhesive layer containing an ethylene-vinyl alcohol copolymer having a content of 90 to 99 mol% of units derived from ethylene, or a polyamide having 9 to 15 methylene groups in the main chain relative to one amide group, or a mixture thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to fuel cell units. Background Art

[0002] In recent years, fuel cells have been known that generate electricity by chemically reacting an anode gas such as hydrogen and a cathode gas such as oxygen.

[0003] A fuel cell as a constituent element of such a fuel cell is known to include a membrane electrode assembly having an electrolyte membrane and electrode catalyst layers disposed on both surfaces of the electrolyte membrane, and a gas diffusion layer and a separator disposed on both surfaces of the membrane electrode assembly.

[0004] The structure of a fuel cell unit cell may be a structure in which an electrode catalyst layer is stacked inside the outer peripheral side of an electrolyte membrane in a membrane electrode assembly, and the outer peripheral side of the electrolyte membrane and a support frame are bonded to each other with an adhesive.

[0005] Examples of the adhesive include liquid adhesives and hot-melt adhesives.

[0006] Patent Document 1 discloses a fuel cell using a liquid adhesive as an adhesive layer.

[0007] Furthermore, Patent Documents 2 to 4 disclose fuel cell units using a hot melt adhesive or the like as an adhesive layer.

[0008] More specifically, Citation 2 discloses using, as the adhesive, at least one hot-melt adhesive selected from the group consisting of ethylene vinyl acetate (EVA), polyamide, polyolefin, polyester, and a mixture thereof.

[0009] Furthermore, Citation 3 discloses using, as the adhesive, one or more hot-melt adhesives selected from polyurethane, ethylene-vinyl acetate polymer, and polyamide.

[0010] Furthermore, Citation Document 4 discloses the use of a cationic polymerization-type ultraviolet-curable adhesive as an adhesive.

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: Japanese Patent Application No. 2008-512828

[0014] Patent Document 2: Japanese Patent Application No. 2008-523574

[0015] Patent Document 3: Japanese Patent Application No. 2007-538358

[0016] Patent Document 4: Japanese Patent Application Publication No. 2016-201183 Summary of the invention

[0017] In a fuel cell unit cell having a structure in which an electrode catalyst layer is stacked on the inner side of the outer peripheral side surface of an electrolyte membrane on at least one side of a membrane electrode assembly, methods for bonding the outer peripheral side surface of the electrolyte membrane and a support frame to each other include methods using a liquid adhesive or a hot melt adhesive as described in Patent Documents 1 to 4.

[0018] However, although the liquid adhesive disclosed in Patent Document 1 is firmly bonded to the membrane electrode assembly, the volatile components in the liquid adhesive react with the catalyst metal such as platinum in the catalyst layer to generate decomposition gas. The decomposition gas can poison the catalyst metal and reduce the output power of the fuel cell.

[0019] Therefore, when a liquid adhesive is used, unnecessary steps such as a step for removing decomposed gas are generated in the manufacturing process of the fuel cell.

[0020] On the other hand, when the electrolyte membrane and the support frame are bonded using conventional hot melt adhesives, the hot melt adhesives are easily peeled off from the electrolyte membrane under the environment inside the fuel cell when the fuel cell is in use, that is, under a hydrothermal environment.

[0021] Therefore, when the electrolyte membrane and the support frame are bonded together using a conventional hot melt adhesive, sufficient durability of the fuel cell cannot be obtained.

[0022] An object of the present invention is to provide a fuel cell unit having high durability.

[0023] The inventors have found that the above-mentioned problems can be achieved by the following means:

[0024] Method 1

[0025] A fuel cell unit battery is a fuel cell unit battery in which a membrane electrode assembly and a support frame are bonded to each other through a hot melt adhesive layer.

[0026] The membrane electrode assembly comprises an electrolyte membrane and a pair of electrode catalyst layers stacked on both surfaces of the electrolyte membrane.

[0027] On at least one side of the membrane electrode assembly, the electrode catalyst layer is stacked on the inner side of the outer peripheral side of the electrolyte membrane, the hot melt adhesive layer bonds the outer peripheral side of the electrolyte membrane to the support frame, and

[0028] The hot-melt adhesive layer contains an ethylene-vinyl alcohol copolymer containing 90 to 99 mol% of units derived from ethylene, a polyamide having 9 to 15 methylene groups per amide group in the main chain, or a mixture thereof.

[0029] Method 2

[0030] The fuel cell according to aspect 1, wherein the electrolyte membrane contains a perfluorosulfonic acid polymer.

[0031] Method 3

[0032] The fuel cell according to Embodiment 2, wherein the perfluorosulfonic acid polymer is a polymer having repeating units represented by the following (A) to (C) or a combination thereof,

[0033] (A)

[0034]

[0035] (B)

[0036]

[0037] (C)

[0038]

[0039] Here, m is an integer greater than 1.

[0040] Method 4

[0041] The fuel cell according to any one of aspects 1 to 3, wherein the polyamide is nylon.

[0042] Method 5

[0043] The fuel cell according to Embodiment 4, wherein the polyamide is a polymer having repeating units represented by the following (P) and (Q) or a combination thereof,

[0044] (P)

[0045]

[0046] (Q)

[0047]

[0048] Method 6

[0049] The fuel cell according to any one of aspects 1 to 5, wherein the support frame is disposed on the outer periphery of the membrane electrode assembly and is spaced apart from the membrane electrode assembly.

[0050] Method 7

[0051] The fuel cell according to any one of aspects 1 to 6, wherein a pair of gas diffusion layers are stacked on both surfaces of the membrane electrode assembly.

[0052] The hot melt adhesive layer bonds the gas diffusion layer stacked on the electrode catalyst layer stacked on the inner side of the outer peripheral side of the electrolyte membrane among the pair of gas diffusion layers, the outer peripheral side of the electrolyte membrane, and the support frame to each other.

[0053] Method 8

[0054] The fuel cell according to aspect 7, wherein the pair of gas diffusion layers and the pair of separators are stacked in this order on both surfaces of the membrane electrode assembly.

[0055] According to the present invention, a fuel cell unit having high durability can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 FIG. 1 is a schematic diagram showing a portion of a fuel cell unit according to one embodiment of the present invention.

[0057] Explanation of symbols

[0058] 1 Fuel cell unit

[0059] 10 Membrane Electrode Assembly

[0060] 11 Electrolyte membrane

[0061] 12 and 13 Electrode catalyst layer

[0062] 20 Support frame

[0063] 30 Hot melt adhesive layer

[0064] 40 and 50 gas diffusion layer

[0065] 60 and 70 Spacers DETAILED DESCRIPTION

[0066] Hereinafter, embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the gist of the present invention.

[0067] The fuel cell unit battery of the present invention is a fuel cell unit battery in which a membrane electrode assembly and a support frame are bonded to each other by a hot melt adhesive layer, the membrane electrode assembly having an electrolyte membrane and a pair of electrode catalyst layers stacked on both sides of the electrolyte membrane, and on at least one side of the membrane electrode assembly, the electrode catalyst layer is stacked on the inner side of the outer peripheral side surface of the electrolyte membrane, the hot melt adhesive layer bonds the outer peripheral side surface of the electrolyte membrane and the support frame to each other, and the hot melt adhesive layer contains an ethylene-vinyl alcohol copolymer having an ethylene unit content of 90 to 99 mol%, or a polyamide having 8 to 15 methylene groups in the main chain relative to one amide group, or a mixture thereof.

[0068] use Figure 1 A specific example of the structure of the fuel cell unit of the present invention will be described.

[0069] Figure 1 FIG. 1 is a schematic diagram showing a portion of a fuel cell unit 1 according to an embodiment of the present invention.

[0070] like Figure 1 As shown, a fuel cell unit 1 according to an embodiment of the present invention is a fuel cell unit 1 in which a membrane electrode assembly 10 and a support frame 20 are bonded to each other via a hot melt adhesive layer 30 .

[0071] The membrane electrode assembly 10 includes an electrolyte membrane 11 and a pair of electrode catalyst layers 12 and 13 stacked on both surfaces of the electrolyte membrane 11. Of the electrode catalyst layers 12 and 13, one is an anode electrode catalyst layer and the other is a cathode electrode catalyst layer.

[0072] exist Figure 1 In the fuel cell unit cell 1 shown in accordance with an embodiment of the present invention, on one side of the membrane electrode assembly 10, the electrode catalyst layer 12 is stacked on the inner side of the outer peripheral side of the electrolyte membrane 11, and on the other side, the electrode catalyst layer 13 is stacked in a manner extending over the entire surface of the electrolyte membrane 11.

[0073] The hot-melt adhesive layer 30 bonds the outer peripheral side surface of the electrolyte membrane 11 and the support frame 20 to each other.

[0074] Furthermore, in the fuel cell 1 according to one embodiment of the present invention, in addition to the above-described configuration, a pair of gas diffusion layers 40 and 50 and a pair of separators 60 and 70 are provided.

[0075] Although not in Figure 1As shown in the figure, the fuel cell unit cell 1 according to one embodiment of the present invention, under the premise of the above structure, the hot melt adhesive layer 30 contains: an ethylene-vinyl alcohol copolymer with a unit content of 90 to 99 mol% from ethylene, or a polyamide with 8 to 15 methylene groups in the main chain relative to one amide group, or a mixture thereof.

[0076] It should be explained that Figure 1 The purpose is not to limit the composition of the fuel cell unit cell of the present invention. In particular, it should be noted that Figure 1 This is not intended to exclude a configuration in which, in the fuel cell 1 of the present invention, the electrode catalyst layer 13 is stacked on the inner side of the outer peripheral side surface of the electrolyte membrane 11 on the other side of the electrolyte membrane 11 .

[0077] Although not limited by the principle, the principle of the high durability of the fuel cell of the present invention is as follows.

[0078] As described above, as part of the structure of a fuel cell unit cell, on at least one side of the membrane electrode assembly, the electrode catalyst layer is stacked on the inner side of the outer peripheral side of the electrolyte membrane, and the hot melt adhesive layer bonds the outer peripheral side of the electrolyte membrane and the support frame to each other. In such a structure, the hot melt adhesive layer is directly bonded to the electrolyte membrane.

[0079] The electrolyte membrane that can be used for the fuel cell has a hydrophilic functional group. Therefore, it is considered that by using ethylene-vinyl alcohol copolymer or polyamide as a hot melt adhesive, high adhesion between the electrolyte membrane and the hot melt adhesive layer can be obtained.

[0080] On the other hand, if the hot melt adhesive layer contains a large amount of hydrophilic functional groups of ethylene-vinyl alcohol copolymer or polyamide, the hot melt adhesive layer will absorb water and swell in the hydrothermal environment when the fuel cell unit cell is used. If the hot melt adhesive layer swells, it will become easy to peel off from the electrolyte membrane.

[0081] Therefore, it is considered that if the amount of hydrophilic functional groups of the ethylene-vinyl alcohol copolymer or polyamide contained in the hot-melt adhesive layer is large, the durability of the fuel cell unit will be reduced.

[0082] In contrast, in the fuel cell unit cell of the present invention, the hot melt adhesive layer contains an ethylene-vinyl alcohol copolymer containing 90 to 99 mol% of units derived from ethylene, or a polyamide having 8 to 15 methylene groups in the main chain relative to one amide group, or a mixture thereof. Such ethylene-vinyl alcohol copolymers and polyamides have both hydrophilic functional groups that contribute to adhesion to the electrolyte membrane and significantly more methylene groups that are hydrophobic relative to the hydrophilic functional groups.

[0083] Therefore, the hot-melt adhesive layer used in the fuel cell unit cell of the present invention is bonded to the electrolyte membrane and is less likely to absorb water and expand in a hydrothermal environment.

[0084] More specifically, the ethylene-vinyl alcohol copolymer contained in the hot melt adhesive layer of the fuel cell unit cell of the present invention has high adhesion to the electrolyte membrane due to the hydrophilic functional group, namely, the hydroxyl group (-OH). On the other hand, the content of the unit derived from ethylene is 90 to 99 mol%, that is, the hydrophobic methylene group (-CH 2 Therefore, the proportion of hydroxyl groups that react with water in a hydrothermal environment is small, and the degree of expansion of the hot-melt adhesive layer is small.

[0085] In addition, the polyamide contained in the hot melt adhesive layer of the fuel cell unit cell of the present invention has high adhesion to the electrolyte membrane due to the hydrophilic functional group, namely, the amide group (-CO-NH-). On the other hand, the main chain has 8 to 15 methylene groups per amide group, that is, the hydrophobic methylene group (-CH 2 Therefore, there are fewer amide groups that react with water in a hydrothermal environment, and the degree of expansion of the hot-melt adhesive layer is small.

[0086] As described above, the fuel cell of the present invention has high durability because the heat-melting layer is unlikely to be peeled off from the electrolyte membrane even in a hydrothermal environment.

[0087] 《Hot-melt adhesive layer》

[0088] The hot melt adhesive layer bonds the outer peripheral side of the electrolyte membrane to the support frame. The hot melt adhesive layer contains an ethylene-vinyl alcohol copolymer containing 90 to 99 mol% of ethylene-derived units, or a polyamide having 8 to 15 methylene groups per amide group in the main chain, or a mixture thereof.

[0089] The shape of the hot melt adhesive layer is not particularly limited, and can be, for example, a sheet. In addition, the hot melt adhesive layer can have a multilayer structure. The hot melt adhesive layer can contain a rubber filler, a cross-linking component, a plasticizer, a heat stabilizer, an anti-hydrolysis agent, and / or a compatibilizer.

[0090] The thickness of the hot melt adhesive layer may be, for example, 10 to 100 μm. The thickness of the hot melt adhesive layer may be 10 μm or more, 20 μm or more, 30 μm or more, or 40 μm or less, and 100 μm or less, 90 μm or less, 70 μm or less, or 50 μm or less.

[0091] 〈Ethylene-vinyl alcohol copolymer〉

[0092] In the ethylene-vinyl alcohol copolymer used for the heat-melting layer of the fuel cell unit cell of the present invention, the content of the unit derived from ethylene is 90 to 99 mol%.

[0093] By setting the content of the units derived from ethylene to 90 mol % or more, the methylene groups (—CH 2 -) is significantly more than the hydroxyl group (-OH) in the polymer, so the expansion caused by water absorption by the heat-fusible layer can be suppressed in the hydrothermal environment when the fuel cell is used. Therefore, the heat-fusible layer can be suppressed from peeling off from the electrolyte membrane.

[0094] On the other hand, by setting the content of the units derived from ethylene to 99 mol % or less, the heat-fusible layer can be bonded to the electrolyte membrane via the hydroxyl group (—OH) in the polymer.

[0095] The content of units derived from ethylene in the ethylene-vinyl alcohol copolymer used in the hot melt layer of the fuel cell unit battery of the present invention can be more than 90 mol%, more than 91 mol%, more than 93 mol%, or more than 94 mol%, and can be less than 99 mol%, less than 98 mol%, less than 97 mol%, or less than 96 mol%.

[0096] In addition, the content of the unit derived from vinyl alcohol in the ethylene-vinyl alcohol copolymer of the hot melt layer of the fuel cell unit cell of the present invention can be 1 mol% to 10 mol%. The content of the unit derived from vinyl alcohol can be 1 mol% or more, 2 mol% or more, 3 mol% or more, or 4 mol% or more, and can be 10 mol% or less, 9 mol% or less, 8 mol% or less, or 7 mol% or less.

[0097] 〈Polyamide〉

[0098] The polyamide used for the heat-melting layer of the fuel cell unit cell of the present invention is a polyamide having 8 to 15 methylene groups in the main chain relative to one amide group.

[0099] By making the main chain of the polyamide have 8 to 15 methylene groups per amide group, the methylene groups (-CH 2 -) is significantly more than the amide group (-CO-NH-) in the polymer, so the expansion caused by water absorption by the heat-fusible layer can be suppressed in the hydrothermal environment when the fuel cell is used. Therefore, the heat-fusible layer can be suppressed from peeling off from the electrolyte membrane.

[0100] On the other hand, by providing polyamide with an amide group (—CO—NH—), the heat-fusible layer can be bonded to the electrolyte membrane.

[0101] In the hot-melt layer polyamide used for the fuel cell unit battery of the present invention, the number of methylene groups in the main chain relative to one amide group can be more than 8, more than 9, more than 10, or more than 12, and can be less than 15, less than 14, less than 13, or less than 12.

[0102] The polyamide that can be used for the hot melt layer of the fuel cell unit cell of the present invention can be, for example, nylon, and more specifically, can be a polymer formed by polymerization of one or more monomers having a repeating unit of -HN-(CH2)n-CO- (here, n is an integer of 8 to 15).

[0103] More specifically, the polyamide that can be used for the heat-melting layer of the fuel cell unit cell of the present invention may be a polymer having repeating units represented by, for example, the following (P) and (Q) or a combination thereof.

[0104] (P)

[0105]

[0106] (Q)

[0107] 《Membrane Electrode Assembly》

[0108] The fuel cell of the present invention has a membrane electrode assembly having an electrolyte membrane and a pair of electrode catalyst layers stacked on both sides of the electrolyte membrane. In addition, on at least one side of the membrane electrode assembly, the electrode catalyst layer is stacked inside the outer peripheral side surface of the electrolyte membrane.

[0109] 〈Electrolyte membrane〉

[0110] As the material of the electrolyte membrane, any material that can be used for the electrolyte layer of a fuel cell unit cell can be used. Such a material can be, for example, a fluorine-based polymer having ion conductivity, more specifically, an ion exchange polymer having proton conductivity containing perfluorosulfonic acid, i.e., a perfluorosulfonic acid polymer.

[0111] The perfluorosulfonic acid polymer may be a polymer having repeating units represented by the following (A) to (C) or a combination thereof.

[0112]

[0113] (A)

[0114]

[0115] (B)

[0116]

[0117] (C)

[0118]

[0119] Here, m is an integer greater than 1.

[0120] 〈Electrode Catalyst Layer〉

[0121] Examples of the electrode catalyst layer include an anode catalyst layer and a cathode catalyst layer. The anode catalyst layer and the cathode catalyst layer may be catalyst layers in which a catalyst metal is supported on a carrier.

[0122] The catalyst metal may be any catalyst metal used for a fuel cell catalyst. Examples of such a catalyst metal include Pt, Pd, Rh, and alloys containing these.

[0123] The carrier may be any carrier used for a fuel cell catalyst, and may be, for example, a carbon carrier, more specifically, carbon particles formed of glassy carbon, carbon black, activated carbon, coke, natural graphite, or artificial graphite.

[0124] Support frame

[0125] The support frame can be formed of any material having electrical insulation and airtightness. Examples of such materials include thermosetting resins and thermoplastic resins, and preferably thermoplastic resins such as polyethylene, polypropylene, cyclic polyolefin resins, polyphenylene ether resins, polyethylene naphthalate resins (PEN), polyetherimide, polyimide, polyphenylsulfone (PPS), polyethersulfone, polyphenylsulfone, and polysulfone.

[0126] The support frame may be disposed on the outer periphery of the membrane electrode assembly and spaced apart from the membrane electrode assembly.

[0127] Other Compositions

[0128] The fuel cell of the present invention may include a gas diffusion layer and a separator as a configuration other than the above. The fuel cell of the present invention may include a pair of gas diffusion layers and a pair of separators stacked in this order on both surfaces of the membrane electrode assembly.

[0129] In such a configuration, the hot melt adhesive layer can bond the gas diffusion layer stacked on the electrode catalyst layer on the inner side of the outer peripheral side of the electrolyte membrane, the outer peripheral side of the electrolyte membrane, and the support frame to each other. In addition, the hot melt layer can further bond the gas diffusion layers to each other.

[0130] For example, Figure 1As shown in FIG. 1 , a fuel cell unit cell 1 according to an embodiment of the present invention includes a pair of gas diffusion layers 40 and 50 and a pair of separators 60 and 70. Figure 1 In the embodiment, a pair of gas diffusion layers 40 and 50 are stacked on both sides of the membrane electrode assembly 10. The hot melt adhesive layer 30 bonds the gas diffusion layer 40 stacked on the electrode catalyst layer 12 stacked on the inner side of the outer peripheral side of the electrolyte membrane 11, the outer peripheral side of the electrolyte membrane 11, the support frame 20, and the separator 60 to each other.

[0131] Gas Diffusion Layer

[0132] One of the pair of gas diffusion layers is an anode gas diffusion layer, and the other is a cathode gas diffusion layer.

[0133] The material of the gas diffusion layer may be any material that can be used for the gas diffusion layer of the fuel cell catalyst. Such a material may include, for example, a porous body having conductivity. Such a porous body may include, more specifically, a carbon porous body such as carbon paper, carbon cloth, and glassy carbon, or a metal porous body such as a metal mesh and a foamed metal.

[0134] 〈Isolator〉

[0135] The material of the separator may be any material that can be used for separators of fuel cell units, and may be an airtight conductive material. Examples of such materials include dense carbon that is airtight by compressing carbon, and pressed metal plates.

[0136] 《Method for manufacturing fuel cell unit cell》

[0137] The fuel cell unit cell of the present invention can be manufactured according to a known manufacturing method except that the hot melt adhesive layer is formed as described above. It should be noted that the temperature applied to the hot melt adhesive layer when the outer periphery of the electrolyte membrane is bonded to the support frame by the hot melt adhesive layer can be appropriately set according to the material used for the hot melt adhesive layer, for example, it can be within a temperature range of 80°C or more and less than the melting point of the material used for the hot melt adhesive layer.

[0138] Example

[0139] 《Examples 1 to 4 and Comparative Examples 1 to 12》

[0140] <Example 1>

[0141] The adhesive layer sheet of Example 1 was prepared by cutting a 40 μm thick sheet made of an ethylene-vinyl alcohol copolymer (EVOH, melting point 105° C.) containing 95 mol % of units derived from ethylene into a rectangle of 10 mm in length and 40 mm in width.

[0142] In addition, this sheet was formed by using a casting method.

[0143] <Example 2>

[0144] An adhesive layer sheet of Example 2 was prepared in the same manner as in Example 1 except that EVOH (melting point: 110° C.) having an ethylene-derived unit content of 90 mol% was used as the material of the hot-melt adhesive layer sheet.

[0145] <Example 3>

[0146] An adhesive layer sheet of Example 3 was prepared in the same manner as in Example 1 except that a sheet having a thickness of 40 μm and made of nylon 12 (melting point: 178° C.) was used as the hot-melt adhesive layer sheet.

[0147] In addition, the sheet having a thickness of 40 μm formed of nylon 12 (melting point 178° C.) was molded by extrusion molding.

[0148] <Example 4>

[0149] An adhesive layer sheet of Example 4 was prepared in the same manner as in Example 3 except that a sheet having a thickness of 40 μm and made of nylon 11 (melting point: 187° C.) was used as the hot-melt adhesive layer sheet.

[0150] <Example 5>

[0151] An adhesive layer sheet of Example 5 was prepared in the same manner as in Example 3 except that a sheet having a thickness of 40 μm and made of nylon 9 (melting point: 306° C.) was used as the hot-melt adhesive layer sheet.

[0152] <Comparative Example 1>

[0153] An adhesive layer sheet of Comparative Example 1 was prepared in the same manner as in Example 3 except that a 40 μm thick sheet made of EVOH (melting point 173° C.) having an ethylene-derived unit content of 38 mol% was used as the hot-melt adhesive layer sheet.

[0154] <Comparative Example 2>

[0155] An adhesive layer sheet of Comparative Example 2 was prepared in the same manner as in Example 1 except that a 40 μm-thick sheet made of EVOH (melting point 121° C.) having an ethylene-derived unit content of 81 mol % was used as the hot-melt adhesive layer sheet.

[0156] <Comparative Examples 3 to 6>

[0157] Adhesive layer sheets of Comparative Examples 3 to 6 were prepared in the same manner as in Example 3 except that sheets with a thickness of 40 μm formed from Admer (AT2937, manufactured by Mitsui Chemicals, melting point 141°C), Admer (AT3363, manufactured by Mitsui Chemicals, melting point 120°C), Admer (QF551, manufactured by Mitsui Chemicals, melting point 140°C) and Admer (QF500, manufactured by Mitsui Chemicals, melting point 165°C) were used in sequence as hot-melt adhesive layer sheets.

[0158] <Comparative Examples 7 to 12>

[0159] Adhesive layer sheets of Comparative Examples 7 to 12 were prepared in the same manner as in Example 3 except that sheets having a thickness of 40 μm were used in sequence as hot-melt adhesive layer sheets, respectively, which were formed from low-density polyethylene (LDPE, melting point 108°C), polymethyl methacrylate resin (PMMA, melting point 160°C), ethylene / vinyl acetate copolymer (ethylene 90 mol%, melting point 100°C), nylon 6 (melting point 225°C), methyl methacrylate / ethylene copolymer (ethylene 9 mass%, melting point 100°C) and nylon 66 (melting point 269°C).

[0160] <Comparative Example 13>

[0161] 150 g of lauryl acrylate, 50 g of methyl methacrylate, 60 g of vinyl ester resin and 4 g of photoinitiator were put into a glass bottle and stirred with a stirrer until uniform, thereby preparing an adhesive of Comparative Example 13.

[0162] Tensile test

[0163] <Adhesive layer sheets of Examples 1 to 4 and Comparative Examples 1 to 12>

[0164] Nafion (registered trademark, manufactured by DuPont) having a thickness of 25 μm as an electrolyte membrane was cut into a rectangular shape having a length of 10 mm and a width of 30 mm to prepare an electrolyte membrane sheet.

[0165] The adhesive layer sheet and the electrolyte membrane sheet of Example 1 were overlapped with each other in the longitudinal end portions with a length of 10 mm and a width of 10 mm, and hot pressed at 1 MPa, 100°C, and 1 minute to bond the adhesive layer sheet and the electrolyte membrane sheet by heat compression to prepare a test piece.

[0166] The thermocompression-bonded test piece was placed in a vial and immersed in hot water at 95°C for 500 hours. After that, the test piece was cooled to 25°C, the adhesive layer was reinforced with Kapton tape, and then a tensile test was performed at 25°C at 10 mm / min until the electrolyte membrane broke or the electrolyte membrane and the adhesive layer peeled off.

[0167] It should be noted that in the tensile test, the adhesive layer sheet and the electrolyte membrane sheet were clamped at the end portion of 10 mm long and 10 mm wide on the side where they were not bonded to each other. The adhesive layer sheets of Examples 2 to 4 and Comparative Examples 1 to 12 were subjected to tensile tests in the same manner as the adhesive layer sheet of Example 1.

[0168] <Adhesive of Comparative Example 13>

[0169] The adhesive of Comparative Example 13 was applied to the entire surface of one side of a polyethylene terephthalate (PET) film having a thickness of 50 μm, and the surface of the adhesive layer sheet of Comparative Example 13 on the side on which the adhesive was applied was in contact with the electrolyte membrane sheet, and the portions of the ends in the longitudinal direction with a length of 10 mm and a width of 10 mm overlapped each other. Next, the overlapping portion was irradiated with ultraviolet light (wavelength: 365 nm) from an LED at 400 mW × 5 seconds, and the adhesive layer sheet and the electrolyte membrane sheet were bonded by ultraviolet curing.

[0170] The bonded test piece was placed in a vial and immersed in 95°C hot water for 500 hours. After that, the test piece was cooled to 25°C, the adhesive layer was reinforced with Kapton tape, and then a tensile test was performed at 25°C at 10 mm / min until the adhesive layer broke or the electrolyte membrane and the adhesive layer peeled off.

[0171] Gas generation test

[0172] <Adhesive layer sheets of Examples 1 to 4 and Comparative Examples 1 to 12>

[0173] A catalyst carrier carrying platinum as a catalyst metal, Nafion (registered trademark, manufactured by DuPont) as an electrolyte, ion exchange water and 1-propanol were dispersed and mixed in carbon black as a conductive carrier using a bead mill to obtain a catalyst ink.

[0174] The obtained catalyst ink was applied on one surface of a polytetrafluoroethylene (PTFE) sheet using a spray coating device and dried to form a catalyst layer having a thickness of 10 μm, thereby producing an electrode sheet for a fuel cell.

[0175] Using Nafion (registered trademark, manufactured by DuPont) as an electrolyte membrane, a fuel cell electrode sheet was bonded to one side of the electrolyte membrane so that the catalyst layer was in contact, thereby producing a membrane electrode assembly. The bonding was performed by hot pressing at 100°C, 10 minutes, and 0.8 MPa.

[0176] The adhesive layer sheet of Example 1 was overlapped on the catalyst layer side of the membrane electrode assembly and heated at 100°C and 1 MPa for 1 minute by hot pressing to bond the adhesive layer sheet to obtain a test piece. The overlapped portion of the catalyst electrode layer of the membrane electrode assembly and the adhesive layer sheet of Example 1 was 5 mm long and 2.5 mm wide.

[0177] The test piece was clamped with a glass epoxy material, fixed with a restraining pressure of 1 MPa, placed in a headspace crimp sample bottle (round bottom, 10 mL), and sealed. Then, it was heated to 100°C for 5 minutes, and then the amount of generated carbon dioxide (ppm) was quantified using a gas chromatograph.

[0178] The adhesive layer sheets of Examples 2 to 4 and Comparative Examples 1 to 12 were subjected to a gas generation test in the same manner as the adhesive layer sheet of Example 1.

[0179] <Adhesive of Comparative Example 13>

[0180] By the same method as the gas generation test of the adhesive layer sheet in Example 1, a membrane electrode assembly was produced.

[0181] The adhesive of Comparative Example 13 was applied to the catalyst layer side of the membrane electrode assembly by screen printing to obtain a test piece of 10 mm×50 mm and 50 μm thickness. The test piece was subjected to the same gas generation test as the adhesive layer sheet of Example 1 to evaluate the amount of carbon dioxide (ppm) generated.

[0182] "result"

[0183] The type of adhesive layer or adhesive in each example and the results of the tensile test and the gas generation test on each example are shown in Table 1 below.

[0184] [Table 1]

[0185] Table 1

[0186]

[0187] It should be noted that "OK" in "Tensile Test" in Table 1 means that the adhesive sheet broke during the tensile test. The breaking of the adhesive sheet means that the adhesive sheet and the electrolyte membrane are firmly bonded. In addition, "NG" in "Tensile Test" in Table 1 means that the electrolyte membrane and the adhesive layer sheet peeled off during the tensile test. The peeling of the electrolyte membrane and the adhesive layer sheet indicates that the bonding between the adhesive sheet and the electrolyte membrane is relatively weak.

[0188] "OK" in "Gas Generation Test" in Table 1 means that the amount of carbon dioxide generated is less than 1000 ppm. In addition, "NG" in "Gas Generation Test" in Table 1 means that the amount of carbon dioxide generated is 1000 ppm or more. The amount of carbon dioxide generated being 1000 ppm or more means that the volatile components of the adhesive are decomposed by platinum as a catalyst metal.

[0189] As shown in Table 1, the adhesive layer sheets of Comparative Examples 1 to 12 were all "NG" in the tensile test, whereas the adhesive layer sheets of Examples 1 to 4 were all "OK" in the tensile test.

[0190] As shown in Table 1, the adhesive layer sheets of Examples 1 to 4 and Comparative Examples 1 to 12 were all "OK" in the gas generation test.

Claims

1. A fuel cell unit battery, wherein a membrane electrode assembly and a support frame are bonded to each other via a hot melt adhesive layer, The membrane electrode assembly includes an electrolyte membrane and a pair of electrode catalyst layers stacked on both sides of the electrolyte membrane. On at least one side of the membrane electrode assembly, the electrode catalyst layer is stacked on the inner side of the outer peripheral side of the electrolyte membrane, the hot melt adhesive layer bonds the outer peripheral side of the electrolyte membrane and the support frame to each other, and The hot melt adhesive layer contains an ethylene-vinyl alcohol copolymer having a content of 90 to 99 mol % of units derived from ethylene. The support frame is disposed on the outer periphery of the membrane electrode assembly and is spaced apart from the membrane electrode assembly.

2. The fuel cell unit cell according to claim 1, in, The electrolyte membrane contains a perfluorosulfonic acid polymer.

3. The fuel cell unit cell according to claim 2, in, The perfluorosulfonic acid polymer is a polymer having repeating units represented by the following (A) to (C) or a combination thereof, (A) (B) (c) Here, m is an integer greater than 1.

4. The fuel cell unit cell according to any one of claims 1 to 3, in, A pair of gas diffusion layers are stacked on both surfaces of the membrane electrode assembly. The hot melt adhesive layer bonds the gas diffusion layer stacked on the electrode catalyst layer stacked on the inner side of the outer peripheral side of the electrolyte membrane among the pair of gas diffusion layers, the outer peripheral side of the electrolyte membrane, and the support frame to each other.

5. The fuel cell unit cell according to claim 4, in, The pair of gas diffusion layers and the pair of separators are stacked in this order on both surfaces of the membrane electrode assembly.