A method for preparing a perovskite solar cell using a copper indium oxide composite material as a hole transport layer

By using copper indium composite materials as the hole transport layer of perovskite solar cells, combined with hydrothermal methods and calcination processes, the problems of high material cost and environmental sensitivity of the hole transport layer materials in perovskite solar cells are solved, achieving Low-cost, large-area production and high-efficiency perovskite solar cell preparation.

CN113707819BActive Publication Date: 2024-10-15HARBIN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110995579.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-27
Publication Date
2024-10-15
Estimated Expiration
2041-08-27

AI Technical Summary

Technical Problem

The hole transport layer materials of existing perovskite solar cells are expensive and sensitive to air and water, and the preparation process is complex, making it difficult to achieve large-area and low-cost production.

Method used

The copper indium composite material is used as the hole transport layer. The copper indium composite material is prepared by hydrothermal method and calcination process, and combined with the perovskite film. As an important component of the perovskite solar cell, the preparation is simplified. process and reduce costs.

Benefits of technology

The low-cost preparation of copper indium composite materials is achieved, which reduces the overall cost of perovskite solar cells. It is resistant to air and water, is suitable for large-area production, and improves the photoelectric conversion efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113707819B_ABST
    Figure CN113707819B_ABST
Patent Text Reader

Abstract

A method for preparing a perovskite solar cell with a copper indium oxide composite material as a hole transport layer, which relates to a method for preparing a perovskite solar cell without an electron transport layer. The present invention mainly solves the problems of high cost and complex stacking of existing hole materials. The method of the present invention is as follows: 1. Cleaning treatment of indium tin oxide-doped FTO conductive glass; 2. Preparation of a perovskite film on FTO in step 1; 3. Preparation of a copper indium oxide composite material; 4. Preparation of a copper indium oxide composite material film as a hole transport layer on the surface of the perovskite film in step 2; 5. Preparation of an Ag electrode layer on the surface of the copper indium oxide composite material film in step 4. The perovskite solar cell prepared by the method of the present invention omits an electron transport layer by combining the copper indium oxide composite material film and the perovskite film, thereby reducing the preparation cost of the perovskite solar cell as much as possible. The present invention is applied to the field of solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of photovoltaic devices and relates to a method for preparing a perovskite solar cell using a copper indium oxide composite material as a hole transport layer. Background Art

[0002] In recent years, perovskite solar cells have been called "strong candidates for the next generation of photovoltaic cells" due to their high efficiency, low cost and simple preparation process. In just ten years, the conversion efficiency has increased from 3.8% to 25.5%, far exceeding the development efficiency of other photovoltaic cells.

[0003] The structure of perovskite solar cells is mainly mesoscopic structure, planar nip type and planar pin type structure. In the current main structure, it is difficult to avoid using expensive organic materials as transport layer materials. As for the hole transport layer, materials like Spiro-OMeTAD and PCMM are not only expensive, but also sensitive to air and water. When preparing and using them, some additives need to be added to suppress their sensitivity to air and water, even if the films prepared from these materials have good bonding with perovskite films. Inorganic transport materials such as copper oxide, cuprous oxide, and copper thiocyanate can replace them well. Not only are the element sources rich, but the prepared films are also inert to air and water, which is suitable for large-scale preparation. Summary of the invention

[0004] The main purpose of the present invention is to provide a method for preparing a perovskite solar cell using a copper indium oxide composite material as a hole transport layer, so as to overcome the problems of high cost of the hole transport layer of existing cells and complex cell stacking.

[0005] The preparation method of a perovskite solar cell using a copper indium oxide composite material as a hole transport layer of the present invention is carried out according to the following steps:

[0006] 1. Conductive glass pretreatment

[0007] The indium-doped tin oxide FTO conductive glass is cleaned and set aside for use;

[0008] 2. Preparation of perovskite thin films

[0009] Weigh 0.1 mol·L -1 ~1mol·L -1 Methylammonium iodide was dissolved in N, N-dimethylformamide to obtain a methylammonium iodide-N, N-dimethylformamide mixed solution. 0.1 mol·L -1 ~1mol·L -1Lead iodide is dissolved in N,N-dimethylformamide to obtain a lead iodide-N,N-dimethylformamide mixed solution, and then the methylammonium iodide-N,N-dimethylformamide mixed solution and the lead iodide-N,N-dimethylformamide mixed solution are mixed and stirred, and 1% to 10% by mass of cellulose acetate is added and stirred for 30 minutes, and the mixed solution is drop-coated on the FTO of step 1, and vacuum heat treatment is performed at 100°C to 150°C to obtain a perovskite film; (the concentrations of the methylammonium iodide-N,N-dimethylformamide mixed solution and the lead iodide-N,N-dimethylformamide mixed solution should be consistent, and the same volume should be weighed, but this is not enough. A certain mass fraction of cellulose acetate needs to be added to ensure that the obtained perovskite film has as good flatness as possible, and at a certain temperature, too low a solvent does not volatilize and does not form a crystalline phase; too high a perovskite is easy to decompose and affect the battery efficiency.)

[0010] 3. Preparation of copper indium oxide composite materials

[0011] Weigh 0.005mmol·mL -1 ~0.01mmol·mL -1 of copper sulfate and 0.001mmol·mL -1 ~0.005mmol·mL -1 The indium sulfate is dissolved in an ethanol-water system with a volume ratio of 60:2, and the mixture is stirred for 30 minutes. Potassium hydroxide is added at a molar ratio of copper sulfate: indium sulfate: potassium hydroxide of 1:1:1 to 1:1:5, and the mixture is stirred for 20 minutes. The mixed solution is transferred to a polytetrafluoroethylene kettle for hydrothermal reaction. The polytetrafluoroethylene kettle is cooled to 70°C in a vacuum drying oven, and then the polytetrafluoroethylene kettle is taken out and placed in a room temperature environment to cool to room temperature. The sample obtained by the hydrothermal reaction is first washed with deionized water for 5 to 10 times and then with ethanol for 5 to 10 times. The drying temperature is 40°C to 80°C. The solid sample obtained by drying is heat treated in a nitrogen atmosphere at 500°C to 800°C for 1h to 8h. , and obtain the copper indium oxide composite material; (the ratio of copper sulfate, indium sulfate and potassium hydroxide should be controlled at 1:1:5, only in this way can the copper ions and indium ions be completely precipitated for the next reaction, but this alone is not enough. The volume ratio of ethanol and water in the solvent system should be 60:2, so that an azeotrope can be formed at a certain temperature; the product of the hydrothermal reaction should be fully washed with deionized water and ethanol to remove other impurities such as sulfate in the sample. Ethanol can also dry the washed sample at a lower temperature; the dried sample can only be heat-treated in a nitrogen atmosphere at 500℃~800℃ for 1h~8h to obtain the copper indium oxide composite material, and the prepared perovskite solar cell has high efficiency.)

[0012] 4. Preparation of Copper Indium Oxide Composite Film

[0013] Take 10 mg mL-1 ~100mg·mL -1 Step 3: The copper indium oxide composite material is dispersed in a dispersant, and the dispersed liquid is droplet-coated on the surface of the perovskite film in step 2, and heat-treated to obtain a copper indium oxide composite material film; the prepared copper indium oxide composite material film is used as a hole transport layer, and the perovskite film is used as a light absorption layer and also as an n-type semiconductor, and together with the copper indium oxide composite material, they are important components of the perovskite solar cell, and neither is indispensable; (the dispersant should be selected with weak polarity, because the perovskite film is easily destroyed in a polar solvent, and the dispersant cannot react with the copper indium oxide composite material prepared in step 3, and can be volatilized and removed at a relatively low temperature that the perovskite film can accept.)

[0014] 5. Preparation of Ag Electrode

[0015] In step four, a layer of conductive silver paste is scraped or screen-printed on the surface of the copper indium oxide composite film to obtain a Ag electrode layer.

[0016] The present invention includes the following gain effects:

[0017] The preparation method provided by the present invention adopts a simple preparation process and provides a preparation method of a perovskite solar cell with a copper indium oxide composite material as a hole transport layer. Compared with the organic materials Spiro-OMeTAD and PCMM, the copper indium oxide composite material prepared by the present invention has greatly reduced costs and has a certain inertness to air and water. At the same time, the perovskite film, while serving as a light-absorbing layer, also plays the role of an n-type semiconductor, and is combined with the copper indium oxide composite film to form an important component of the perovskite solar cell, which is indispensable. There is no electron transport layer in the battery device, which further reduces the cost. The film preparation method is mainly scraping or dripping, which is suitable for large-scale production and has a good application prospect.

[0018] The copper indium oxide composite material prepared by the hydrothermal method and calcination has the following mechanism: 2+ andIn 3+ Copper oxide and indium hydroxide are obtained under the action of ethanol and mineralizer KOH, and the copper oxide and indium hydroxide are further reacted to obtain a composite material of copper indiumate and indium oxide.

[0019] Cu 2+ +In 3+ +CH3CH2OH+OH - →CuO+In(OH3)+H2O (1)

[0020] CuO+In(OH3)→In2O3+Cu2In2O5+H2O (2)

[0021] The structure of the perovskite solar cell device prepared by the present invention is FTO / perovskite film / copper indium oxide composite material / Ag. Light is irradiated on the perovskite film through the FTO conductive glass, and the perovskite film generates electron-hole pairs. The holes are collected by the copper indium oxide composite material film and concentrated on the Ag electrode layer, while the perovskite film plays the role of an n-type semiconductor to concentrate electrons on the FTO conductive layer, thereby forming a photocurrent and generating photoelectric conversion efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A 100000× SEM image and EDAX spectrum of a copper indium oxide composite material of a method for preparing a perovskite solar cell using a copper indium oxide composite material as a hole transport layer;

[0023] Figure 2 An XRD diagram of a copper indium oxide composite material for a method for preparing a perovskite solar cell using the copper indium oxide composite material as a hole transport layer;

[0024] Figure 3 A structural diagram of a perovskite solar cell device in a method for preparing a perovskite solar cell using a copper indium oxide composite material as a hole transport layer;

[0025] Figure 4 The LSV curve diagram of a perovskite solar cell device prepared from a copper indium oxide composite material with annealing times of 1 h, 3 h and 4 h in a method for preparing a perovskite solar cell using a copper indium oxide composite material as a hole transport layer; DETAILED DESCRIPTION

[0026] The drugs and testing instruments required in the preparation method of the present invention are shown in Tables 1-1 and 1-2 below;

[0027] Table 1-1 Reagents used in the experiment

[0028]

[0029]

[0030] Table 1-2 Instruments used in the experiment

[0031] Instrument Name model factory Analytical Balance MP6001 Shanghai Hengping Scientific Instrument Co., Ltd. Constant temperature heating magnetic stirrer CL-200 Gongyi Yuhua Instrument Co., Ltd. Electrochemical Analysis System Workstation DF-2002 Zhengzhou Du Fu Instrument Factory Tube resistance furnace SK-3-9K Harbin Longjiang Electric Furnace Factory Xenon lamp LSP-X500 Beijing Zhuoli Hanguang Instrument Co., Ltd. X-ray diffractometer X'Pert PRO Malvern Panalytical Instruments Ltd. Field Emission Scanning Electron Microscope FEI sirion200 FEI

[0032] Comparative Example 1:

[0033] 1. Conductive glass pretreatment

[0034] Clean the FTO conductive glass with cleaning powder once → Rinse the residual cleaning powder of FTO with distilled water 3 times → Ultrasonic clean FTO with dilute hydrochloric acid once, 15min → Rinse FTO with distilled water 3 times → Ultrasonic clean FTO with acetone once, 15min → Rinse FTO with distilled water 3 times → Ultrasonic clean FTO with anhydrous ethanol once, 15min → Rinse FTO with distilled water 3 times → Blow dry the FTO conductive glass for use;

[0035] 2. Preparation of perovskite thin films

[0036] Weigh 0.5 mol·L -1 Methylammonium iodide was dissolved in N, N-dimethylformamide to obtain a methylammonium iodide-N, N-dimethylformamide mixed solution. The mixture was stirred for 1 h and 0.5 mol·L -1 Lead iodide is dissolved in N, N-dimethylformamide to obtain a lead iodide-N, N-dimethylformamide mixed solution, which is stirred for 1 hour, and then the methylammonium iodide-N, N-dimethylformamide mixed solution and the lead iodide-N, N-dimethylformamide mixed solution are mixed and stirred, and 10% by mass of cellulose acetate is added and stirred for 30 minutes, and the mixed solution is drop-coated on the FTO in step 1, and vacuum heat treatment is performed at 120° C. to obtain a perovskite film;

[0037] 3. Preparation of copper indium oxide composite materials

[0038] Weigh 0.0096mmol·mL -1 of copper sulfate and 0.0048mmol·mL -1 Indium sulfate was dissolved in an ethanol-water system, mixed and stirred for 30 minutes, potassium hydroxide was added at a molar ratio of copper sulfate: indium sulfate: potassium hydroxide of 1:1:5, stirred for 20 minutes, and the mixed solution was transferred to a polytetrafluoroethylene kettle and reacted at 160°C for 12 hours, the polytetrafluoroethylene kettle was cooled to 70°C in a vacuum drying oven, and then the polytetrafluoroethylene kettle was taken out and placed in a room temperature environment to cool to room temperature. The sample obtained by the hydrothermal reaction was first centrifugally washed with deionized water for 8 times, and then centrifugally washed with ethanol for 8 times, and dried at 40°C. The solid sample obtained by drying was heat-treated at 800°C in a nitrogen atmosphere for 3 hours to obtain an indium acid copper composite material;

[0039] 4. Preparation of Copper Indium Oxide Composite Film

[0040] Take 100 mg mL -1Step 3: Dispersing the copper indium oxide composite material in isopropanol, applying the dispersed liquid droplets on the surface of the perovskite film in step 2, and heat treating at 80° C. for 10 minutes to obtain a copper indium oxide composite material film; the prepared copper indium oxide composite material film is used as a hole transport layer, and the perovskite film is used as a light absorption layer and also as an n-type semiconductor, and together with the copper indium oxide composite material, they are important components of the perovskite solar cell, and neither of them can be missing;

[0041] 5. Preparation of Ag Electrode

[0042] In step four, a layer of conductive silver paste is scraped or screen-printed on the surface of the copper indium oxide composite film to obtain a Ag electrode layer.

[0043] Example 1: The solid sample obtained by drying in step 3 was heat treated in a nitrogen atmosphere at 800°C for 1 hour. The other steps were the same as those in comparative example 1. The efficiency of the perovskite solar cell prepared in this way was 0.18%, the corresponding open circuit voltage was 148.7 mV, and the short circuit current density was 4.73 mA·cm -2 , the filling factor is 25.1%.

[0044] Example 2: The solid sample obtained by drying in step 3 was heat treated in a nitrogen atmosphere at 800°C for 4 hours. The other steps were the same as those in comparative example 1. The efficiency of the perovskite solar cell prepared in this way was 0.33%, the open circuit voltage was 291.6 mV, and the short circuit current density was 4.39 mA cm -2 , the filling factor is 25.7%.

[0045] The efficiency and other parameters of the battery prepared in Comparative Example 1 are shown in Tables 1-3. The open circuit voltage and short circuit current density of the battery device prepared in Comparative Example 1 are 422.3 mV and 6.36 mA·cm -2 , the fill factor is 24.9%, and the photoelectric conversion efficiency is 0.67%. Compared with the battery device parameters prepared in Examples 1 and 2, whether it is open circuit voltage, short circuit current density or battery efficiency, the battery device efficiency prepared in Comparative Example 1 is the highest.

[0046] Table 1-3 Test parameters of solar cells assembled from copper indium oxide composite materials prepared with different annealing times

[0047] Annealing time <![CDATA[V oc mV]]> <![CDATA[J sc mA cm -2 ]]> FF% η% 1 148.7 4.73 25.1 0.18 3 422.3 6.36 24.9 0.67 4 291.6 4.39 25.7 0.33

[0048] The above comparative examples and embodiments were tested for performance

[0049] 1) Scanning electron microscope (SEM) test: The surface morphology of the copper indium oxide composite material was observed by scanning electron microscope (SEM), the instrument model was FEI sirion200, the acceleration voltage was 0.2-30 kV, the resolution was 20 kV, the prepared sample was dried, and then adhered to a sample holder coated with conductive glue for testing.

[0050] 2) X-ray diffractometer (XRD) test. The characteristic peaks of the crystal structure of the sample were observed by XRD test. The instrument was X'Pert PRO measuring instrument of Malvern Panalytical, Netherlands. The basic parameters were as follows: the negative electrode material was Cu; the wavelength of K-Alpha1 was 1.5405, the wavelength of K-Alpha2 was 1.5444; the ratio of K-Alpha2 / K-Alpha1 was 0.5; the slit was selected to be 0.19 mm, the scanning range was 10-90°, and the scanning step length was 2θ=0.01313.

[0051] 3) Linear scanning test (LSV test). Use the xenon lamp solar simulator LSP-X500 and the electrochemical workstation DF-2002, and the test light source intensity is AM 1.5G (100mW·cm -2 ) The prepared perovskite solar cell was subjected to LSV test, with a test voltage range of -1000mV to 1000mV, a test current range of 50mA, a standing time of 2s, and test parameters including open circuit voltage, short circuit current density and fill factor.

[0052] Figure 1 The present invention discloses a method for preparing a perovskite solar cell using a copper indium oxide composite material as a hole transport layer. The 100000× SEM image and EDAX spectrum image of a copper indium oxide composite material are provided. The sample contains copper indium oxide with irregular flaky structure and spherical granular indium oxide in the 100000× SEM image. The atomic ratios of O, Cu and In elements are compared in the EDAX spectrum. Compared with the atomic ratio of O:In:Cu of 5:2:2 in copper indium oxide, the ratio of In and O elements is higher, and the sample contains both copper indium oxide and indium oxide.

[0053] Figure 2 The XRD diagram of the copper indium oxide composite material of a method for preparing a perovskite solar cell using the copper indium oxide composite material as a hole transport layer; Figure 2 As shown, the characteristic peaks of copper indium oxide and indium oxide exist in the XRD test, which can explain the high proportion of O and In elements in EDAX, thereby further proving the successful preparation of copper indium oxide-indium oxide composite materials.

[0054] The structure of the perovskite solar cell device prepared by the preparation method of the present invention is as follows Figure 3 As shown, its structure is FTO / perovskite film / copper indium oxide composite film / Ag.

[0055] The preparation method of the present invention studies the influence of different heat treatment times on the efficiency of the prepared thin film and assembled into solar cells. The corresponding spectrum is as follows: Figure 4 As shown. The test results after calculation show that when the annealing time is 1h, the open circuit voltage is 148.7mV and the short circuit current density is 4.73mA·cm -2 , the fill factor is 25.1%, the photoelectric conversion efficiency is 0.18%; when the annealing time is 3h, the open circuit voltage is 422.3mV, and the short circuit current density is 6.36mA·cm -2 , the fill factor is 24.9%, the photoelectric conversion efficiency is 0.67%; when the annealing time is 4h, the open circuit voltage is 291.6mV, and the short circuit current density is 4.39mA·cm -2 , the filling factor is 25.7%, and the photoelectric conversion efficiency is 0.33%. After comparing the annealing time of 3h, the copper indium oxide composite material prepared, made into a thin film and assembled into a solar cell device, has the highest open circuit voltage and short circuit current density, and the filling factor is not much different, which ultimately makes the efficiency of the solar cell device the highest.

Claims

1. A method for preparing a perovskite solar cell using a copper indium oxide composite material as a hole transport layer, characterized in that The preparation method of the perovskite solar cell using the copper indium oxide composite material as the hole transport layer is carried out according to the following steps:

1. Conductive glass pretreatment The indium-doped tin oxide FTO conductive glass is cleaned and set aside for use; 2. Preparation of perovskite thin films According to the concentration of 0.5 mol·L -1 Weigh methylammonium iodide and dissolve it in N,N-dimethylformamide to obtain a methylammonium iodide-N,N-dimethylformamide mixed solution with a concentration of 0.5 mol·L -1 Weigh lead iodide and dissolve it in N, N-dimethylformamide to obtain a lead iodide-N, N-dimethylformamide mixed solution, then mix and stir the methylammonium iodide-N, N-dimethylformamide mixed solution and the lead iodide-N, N-dimethylformamide mixed solution, add 1% to 10% by mass of cellulose acetate and continue stirring for 30 minutes, drop-coat the mixed solution on the FTO in step 1, and perform vacuum heat treatment at 100° C. to 150° C. to obtain a perovskite film; 3. Preparation of copper indium oxide composite materials The concentration is 0.0096mmol·mL -1 Weigh copper sulfate and adjust the concentration to 0.0048mmol·mL -1 Weigh indium sulfate, dissolve it in an ethanol-water system, mix and stir for 30 minutes, add potassium hydroxide according to a copper: indium: potassium molar ratio of 1:1:1 to 1:1:5, stir for 20 minutes, transfer the mixed solution to a polytetrafluoroethylene kettle for hydrothermal reaction, cool the polytetrafluoroethylene kettle to 70°C in a vacuum drying oven, take out the polytetrafluoroethylene kettle and place it in a room temperature environment to cool to room temperature, centrifuge and wash the sample obtained by the hydrothermal reaction, dry it, and heat-treat the solid sample obtained by drying to obtain an indium copper oxide composite material; the heat treatment condition is heat treatment at 800°C in a nitrogen atmosphere for 3 hours; 4. Preparation of Copper Indium Oxide Composite Film According to the concentration of 10mg mL -1 ~100mg·mL -1 The copper indium oxide composite material of step 3 is weighed and dispersed in a dispersant, and the dispersed liquid is dropwise applied to the surface of the perovskite film of step 2, and heat-treated to obtain a copper indium oxide composite material film; the prepared copper indium oxide composite material film is used as a hole transport layer, and the perovskite film is used as a light absorption layer and also as an n-type semiconductor, and together with the copper indium oxide composite material, they are important components of the perovskite solar cell, and neither of them can be missing; 5. Preparation of Ag Electrode In step four, a layer of conductive silver paste is scraped or screen-printed on the surface of the copper indium oxide composite film to obtain a Ag electrode layer.

2. The method for preparing a perovskite solar cell using a copper indium oxide composite material as a hole transport layer according to claim 1, characterized in that In the ethanol-water system in step 3, the volume ratio of ethanol:water is 2:

60.

3. The method for preparing a perovskite solar cell using a copper indium oxide composite material as a hole transport layer according to claim 1, characterized in that In step 3, the centrifugal washing is first washed with deionized water for 5 to 10 times and then washed with ethanol for 5 to 10 times, and the drying temperature is 40°C to 80°C.

4. The method for preparing a perovskite solar cell using a copper indium oxide composite material as a hole transport layer according to claim 1, characterized in that In step 4, the dispersant is isopropanol and the heat treatment temperature is 60°C to 120°C.

5. A perovskite solar cell prepared by the preparation method according to any one of claims 1 to 2.

6. The perovskite solar cell according to claim 5, characterized in that The device structure is: FTO / perovskite film / copper indium oxide composite material / Ag.