A method for improving Frit sintering effect

By preparing metal unit holes with gradually decreasing distribution density on the drive substrate, the problem of inconsistent sintering of laser welded Frit lines is solved, achieving uniform sintering of all parts of the Frit lines and improving sealing performance.

CN113707834BActive Publication Date: 2024-10-29TRULY HUIZHOU SMART DISPLAY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202110859465.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-28
Publication Date
2024-10-29
Estimated Expiration
2041-07-28

AI Technical Summary

Technical Problem

In the existing laser welding Frit technology, the sintering effect of Frit lines is inconsistent, resulting in bubbles or insufficient sintering in some areas, affecting the sealing performance.

Method used

Metal unit holes are prepared in the contact area of ​​the driving substrate. The distribution density gradually decreases along the Frit center line toward the periphery, forming a distribution pattern that is dense inside and sparse outside. The laser spot is reflected through the metal layer to compensate for the uneven laser energy and ensure that the Frit lines are uniform. The parts are sintered uniformly.

Benefits of technology

The consistency of the sintering effect in each part of the Frit line is achieved, the sealing performance is enhanced, and insufficient or excessive sintering caused by uneven energy during the laser welding process is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113707834B_ABST
    Figure CN113707834B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for improving Frit sintering effect, comprising the following steps: preparing a first inorganic film layer in a corresponding Frit contact area on a driving substrate; preparing a metal layer on the first inorganic film layer; processing the metal layer to form a plurality of unconnected metal unit holes, wherein the distribution density of the metal unit holes gradually decreases toward the periphery along the Frit center line, thereby forming a distribution pattern of the metal unit holes that is dense inside and sparse outside.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of display panel manufacturing, and specifically relates to a method for improving the sintering effect of Frit. Background Technology

[0002] The main purpose of encapsulating Active-Matrix Organic Light-Emitting Diodes (AMOLEDs) is to isolate external moisture and oxygen from the OLED panel, thus ensuring the lifespan of the OLED organic film. Currently, materials used in AMOLED encapsulation include Frit (glass powder), TFE (tetrafluoroethylene), and UV adhesive. AMOLED products are divided into Rigid and Flexible screens, the biggest difference being the encapsulation method. Rigid screens use Frit to seal the two glass substrates after bonding the encapsulation substrate and the driving substrate, while Flexible screens use a thin-film encapsulation method.

[0003] Encapsulation has a significant impact on the reliability of Rigid AMOLED products. Rigid AMOLED uses the Frit encapsulation process, which generally includes Frit screen printing, Frit high-temperature sintering, bonding of the encapsulation substrate and the driver substrate, and laser welding of the Frit. Laser welding of the Frit is a process that uses laser sintering technology to sinter the Frit, thereby isolating the OLED panel from the outside air. As the final and crucial step in the Frit encapsulation process, laser welding of the Frit plays a decisive role in Frit encapsulation technology.

[0004] The laser used for laser welding of fritters is generally a semiconductor laser. Semiconductor lasers produce a laser spot size of 800-1000 μm, with the laser energy decreasing from the center of the spot outwards. During laser welding of fritters, the operator typically aligns the center of the laser spot with the center of the fritter line, then selects an appropriate energy to melt the fritter. The fritter then cools rapidly, thus welding the two glass substrates together, forming a sealed space between them.

[0005] However, existing laser welding techniques for fritters have the following technical problems: Fritter lines are typically 300-600µm wide. When the laser is focused on the fritter, the fritter at the center of the laser spot absorbs more laser energy, while the fritter at the edge absorbs less. This results in inconsistent sintering across the fritter lines, potentially leading to two scenarios: 1. Bubbles appear on the fritter at the center of the laser spot, while the fritter at the edge sinters normally; 2. The fritter at the center of the laser spot sinters normally, while the fritter at the edge is under-sintered.

[0006] Terminology Definition

[0007] The "Frit centerline" described in this invention is defined as the centerline of the prepared Frit line along its width direction, on which the center of the laser spot falls.

[0008] The “contact area” described in this invention is defined as the area on the drive substrate covered by Frit after the packaging substrate and the drive substrate are bonded together, that is, the corresponding Frit contact area on the drive substrate.

[0009] In this invention, "distribution density" is defined as the ratio of the total area occupied by a single or multiple metal unit holes per unit area. The larger the ratio of the area occupied by the metal unit holes per unit area, the greater the distribution density. The area or shape of the multiple metal unit holes may be different.

[0010] In this invention, the "encapsulation substrate" is defined as a glass sheet with touch circuitry and sealing material.

[0011] In this invention, the "driving substrate" is defined as a glass sheet with a driving circuit and a light-emitting layer. Summary of the Invention

[0012] To address the technical problems existing in the prior art, the present invention provides a method for improving the sintering effect of Frit, which can achieve a consistent sintering effect in all parts of the Frit line during laser welding.

[0013] To achieve the above objectives, the present invention adopts the following technical solution: a method for improving Frit sintering effect, specifically including the following steps:

[0014] Step 1: Frit is formed on the packaging substrate using a screen printing process, and then sintered at high temperature for later use.

[0015] Step 2: Prepare the first inorganic film layer in the contact area on the driving substrate;

[0016] Step 3: Prepare a metal layer on the first inorganic film layer;

[0017] Step 4: Multiple non-connected metal unit holes are formed on the metal layer. The shape of the metal unit holes can be square, rectangular, circular, etc. The distribution density of the metal unit holes gradually decreases from the center line of Frit outwards, thus forming a distribution pattern of denser inside and sparser outside of the metal unit holes.

[0018] Step 5: Prepare a second inorganic film layer on the end face of the metal layer away from the first inorganic film layer. The second inorganic film layer will fill the pores of the metal unit.

[0019] Step 6: Deposit organic material onto the driving substrate by vapor deposition, apply UV adhesive to the edge of the end face of the encapsulation substrate where Frit is provided, and then bond the driving substrate containing vapor deposition material to the encapsulation substrate containing UV adhesive and Frit in a protective gas environment (e.g., nitrogen). After bonding, cure the UV adhesive.

[0020] Step 7: After the UV adhesive has cured, laser welding is performed.

[0021] Because a metal layer is disposed beneath the film layer in contact with the driving substrate, the metal unit hole distribution density is higher below the Fri at the center of the laser spot, resulting in a smaller metal layer area below the Fri at the center of the laser spot. Conversely, the metal unit hole distribution density is lower below the Fri at the edge of the laser spot, resulting in a larger metal layer area below the Fri at the edge of the laser spot. By gradually decreasing the distribution density of the metal unit holes along the Fri's center line outwards, the metal layer area gradually increases along the Fri's center line outwards. The metal layer can reflect the laser spot. Therefore, during laser welding, the Fri at the edge of the laser spot receives more laser spot reflection compensation than the Fri at the center of the laser spot, thus preventing insufficient sintering of the Fri at the edge of the laser spot. Therefore, this metal unit hole distribution design enables the Fri to achieve a consistent sintering effect across all parts of the Fri line during laser welding, thereby improving the Fri sintering effect and enhancing the Fri's sealing performance compared to existing technologies.

[0022] In one embodiment, the first inorganic film layer comprises SiN x Or SiO2.

[0023] In one embodiment, the metal layer includes Mo, and the metal layer also functions as a trace and capacitor electrode on the driving substrate.

[0024] In one embodiment, the metal layer is a Ti-Al-Ti layered composite metal layer, which serves as both an ELVDD / ELVSS and a reset voltage line on the driving substrate. When the metal layer is a Ti-Al-Ti layered composite metal layer, the second inorganic film layer can be omitted. That is, step five is omitted.

[0025] In one embodiment, the second inorganic film layer comprises SiN x Or SiO2. When the second inorganic film layer includes SiN x At that time, the thickness of the second inorganic film layer does not exceed When the second inorganic film layer includes SiO2, the thickness of the second inorganic film layer does not exceed

[0026] This invention provides a method for improving the sintering effect of Frit. The method involves preparing a metal layer including metal unit holes in the contact area on a driving substrate. The distribution density of the metal unit holes gradually decreases from the center line of Frit outwards, forming a denser inner and sparser outer distribution. This allows the unevenness of laser energy between the inner and outer parts to be improved by compensating for the reflection of the laser spot by the metal layer located below Frit during laser welding. Furthermore, the differentiated distribution density of the metal unit holes results in different reflections of the laser spot by regions with different distribution densities, thereby improving the sintering effect of Frit under the same laser spot.

[0027] The following description is based on specific embodiments. Attached Figure Description

[0028] The accompanying drawings further illustrate the invention, but the embodiments in the drawings do not constitute any limitation on the invention.

[0029] Figure 1 This is a front view of a packaging substrate provided in an embodiment of the present invention.

[0030] Figure 2 This is a schematic diagram of the structure after the driving substrate and the packaging substrate are bonded together in one embodiment of the present invention.

[0031] Figure 3 This is a partial front view of the contact area on a driving substrate provided in an embodiment of the present invention.

[0032] Figure 4 for Figure 3 A sectional view of part A in the middle.

[0033] Figure 5 for Figure 3 Sectional view of part B in the middle.

[0034] In the figures, the reference numerals are: 1. Packaging substrate; 2. Frit; 3. Driving substrate; 41. First inorganic film layer; 42. Second inorganic film layer; 51. Metal layer; 52. Metal unit hole; 6. UV adhesive. Detailed Implementation

[0035] It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.

[0036] In this embodiment, the preparation process of the metal unit hole includes the following steps:

[0037] Step 1: Deposit a metal layer on the first inorganic film layer. The metal layer is deposited by evaporation deposition, sputtering deposition or printing.

[0038] Step 2: Coat the metal layer with photoresist, the thickness of which is 1-10μm, and then print. After printing, bake and cure at a temperature of 70-200℃.

[0039] Step 3: Cover the surface of the baked and cured metal layer with a mask that sets the shape of the metal unit hole, then partially expose the photoresist with ultraviolet light, and then place it in a developing solution for development.

[0040] Step 4: Etch the surface of the developed metal layer, etching the area corresponding to the metal unit hole to the upper surface of the first inorganic film layer.

[0041] Step 5: Immerse the etched drive substrate in a solvent to separate the photoresist from the metal layer.

[0042] Materials for the metal layer include Au, Ag, Cu, Al, Fe, Ni, Mo, and metal alloys.

[0043] In this embodiment, the shape of the metal unit hole is square, and the area of ​​the metal unit hole varies depending on its location. Specifically, the area of ​​the metal unit hole in the center of the Frit is larger, and the area of ​​the metal unit hole in the periphery of the Frit is smaller. This arrangement is conducive to forming a distribution pattern of dense inside and sparse outside.

[0044] The method for improving the Frit sintering effect provided in this embodiment is applicable to AMOLED packaging, and the method for improving the Frit sintering effect provided in this embodiment can be implemented using existing laser curing equipment.

[0045] The method for improving Frit sintering effect provided in this embodiment specifically includes the following steps:

[0046] Step 1, as follows Figure 1As shown, Frit 2 is formed on the packaging substrate 1 by screen printing process, and then high temperature sintering is performed. After high temperature sintering, UV adhesive 6 is coated on the edge of the end face of the packaging substrate 1 where Frit is provided. UV adhesive 6 surrounds Frit 2. Frit 2 has a width of 0.3-0.7mm and a height of 4-6μm.

[0047] Step 2: Prepare the first inorganic film layer 41 in the contact area on the driving substrate 3;

[0048] Step 3: Prepare a metal layer 51 on the first inorganic film layer 41;

[0049] Step four: Form multiple non-connected metal unit holes 52 in the metal layer 51, such as... Figure 3-5 As shown, the distribution density of the metal unit aperture 52 is along the center line of Frit 2 (corresponding to...). Figure 3 The dotted lines in the middle gradually decrease in size towards the outer direction, thus forming a dense inner and sparse outer distribution pattern of the metal unit holes 52;

[0050] Step 5: Prepare a second inorganic film layer 42 on the end face of the metal layer 51 away from the first inorganic film layer 41. The second inorganic film layer 42 will fill the metal unit hole 52.

[0051] Step six: The driving substrate 3 is vapor-deposited with an organic material. Then, in a protective gas environment (e.g., nitrogen), the driving substrate 3 containing the vapor-deposited material is bonded to the encapsulation substrate 1 containing UV adhesive 6 and Frit 2. Figure 2 As shown, UV adhesive 6 is cured after bonding;

[0052] Step 7: After UV adhesive 6 has cured, laser welding is performed. The laser is focused onto Frit 2. The metal layer 51 can reflect the laser beam. Therefore, during laser welding, Frit 2 at the edge of the laser beam receives more compensation from the laser beam reflection compared to Frit 2 at the center of the laser beam, thus preventing incomplete sintering of Frit 2 at the edge of the laser beam. Frit 2 at the center of the laser beam sinters normally, and Frit 2 at the edge of the laser beam also sinters normally due to the compensation from the laser beam reflection.

[0053] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0054] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A method for improving Frit sintering effect, characterized in that: The method comprises the following steps: A first inorganic film layer is prepared in the corresponding Frit contact area on the driving substrate, wherein the first inorganic film layer includes SiN x or SiO2; preparing a metal layer on the first inorganic film layer; A plurality of unconnected metal unit holes are formed on the metal layer, and the distribution density of the metal unit holes gradually decreases from the Frit center line to the peripheral direction, thereby forming a distribution mode of the metal unit holes that is dense inside and sparse outside. By gradually decreasing the distribution density of the metal unit holes from the Frit center line to the peripheral direction, the area of ​​the metal layer gradually increases from the Frit center line to the peripheral direction, and the metal layer can play the function of reflecting the laser spot. Therefore, when laser welding is performed, the Frit at the edge of the laser spot can obtain more compensation for the reflection of the laser spot than the Frit at the center of the laser spot, thereby preventing the Frit at the edge of the laser spot from being insufficiently sintered; Prepare a second inorganic film layer on the end surface of the metal layer away from the first inorganic film layer, and the second inorganic film layer will fill the metal unit hole; If the second inorganic film layer includes SiN x , the thickness of the second inorganic film layer does not exceed 3000 angstroms; if the second inorganic film layer includes SiO2, the thickness of the second inorganic film layer does not exceed 2000 angstroms.

2. The method according to claim 1, characterized in that The metal layer includes metal Mo.

3. The method according to claim 1, characterized in that: The metal layer is a Ti-Al-Ti layered composite metal layer.

Citation Information

Patent Citations

  • Organic light emitting diode (OLED) display unit and OLED display device adopting display unit

    CN102931214A

  • Substrate packaging structure and packaging method

    CN103871323A

  • Display device and packaging method thereof

    CN103943648A

  • Organic light-emitting display panel and production method thereof and display device

    CN107579167A

  • OLED display panel and manufacturing method thereof

    CN108389981A