Method for forming a Li-ion battery cell

By using a mixture of polyethylene oxide and Li7La3Zr2O12 oxide for multiple charge/discharge cycle pretreatment in an all-solid Li-ion battery, a stable solid electrolyte interface is formed, which solves the problem of polymer instability at high potentials. It improves the electrochemical performance and energy density of the battery and meets the energy density needs of the automotive field.

CN113728480BActive Publication Date: 2024-10-11AMPERE
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202080029894.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-04-25
Filing Date
2020-04-02
Publication Date
2024-10-11
Estimated Expiration
2040-04-02

AI Technical Summary

Technical Problem

Existing polymer-based all-solid Li-ion batteries are unstable at high potentials and cannot meet the energy density needs of the automotive field.

Method used

A mixture including polyethylene oxide (PEO) and Li7La3Zr2O12 oxide is used as the solid electrolyte, and a stable solid electrolyte interface is formed through continuous multiple charge/discharge cycle pretreatment steps to improve the stability of the battery at a potential of 3.7V to 5V. sex.

Benefits of technology

Significantly improves the electrochemical performance and energy density of all-solid-state Li-ion batteries, extending battery life and providing better safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113728480B_ABST
    Figure CN113728480B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for forming a Li-ion battery cell comprising a cathode material, an anode material, a separator and an electrolyte, wherein the electrolyte comprises a mixture of polyethylene oxide and an oxide of the formula LivLasZnOn, characterized in that the method comprises the following consecutive cycling steps: (a) subjecting the battery cell to at least two consecutive charge and discharge cycles at a first cycle rate C / x, wherein the time limit of these charge / discharge steps is x / 2; (b) subjecting the battery cell to at least two consecutive charge and discharge cycles at a second charge rate C / y different from the first cycle rate, wherein y is less than x, and the time limit of these charge / discharge steps is y / 2; and (c) subjecting the battery cell to at least two consecutive charge and discharge cycles at a third cycle rate C / z different from the first charge rate and the second charge rate, wherein z is less than x and y, and the time limit of these charge / discharge steps is z / 2.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates generally to rechargeable lithium ion (Li-ion) batteries, and more particularly to a rechargeable lithium ion battery comprising polyethylene oxide and a rechargeable lithium ion battery having the formula Li7La3Zr2O 12 A battery cell of an all-solid-state Li-ion battery made of a mixture of oxides (PEO-LLZO).

[0002] More particularly, the present invention relates to methods for forming Li-ion battery cells including a PEO-LLZO mixture.

[0003] Electrochemical systems for energy storage have important applications in the field of portable electronic devices and electric vehicles. One of the most widely used battery technologies is based on the use of lithium ions.

[0004] Conventionally, a Li-ion battery is an assembly of one or more negative and positive electrodes (anode and cathode, respectively), an electrolyte, and a separator that prevents any contact between the electrodes.

[0005] Once the Li-ion cell is activated, ie, when the cell has been assembled and the cell is saturated with liquid electrolyte, a thermodynamic reaction occurs during the first cell charging cycle and the first Li-ion exchange between the electrodes occurs.

[0006] The products resulting from these reactions accumulate on the surface of the electrode to form a layer called the solid electrolyte interface (solid electrolyte interphase) or SEI layer. This layer is an essential element for the proper operation of Li-ion batteries because it conducts Li ions very well and has the advantage of preventing catalytic decomposition of the solvent of the liquid electrolyte.

[0007] The quality of the SEI determines the lifetime of the battery, and therefore its formation is an important step.

[0008] In new generations of batteries, the separator and the liquid electrolyte are replaced by solid electrolytes, such as polymers, inorganic compounds, amorphous materials or combinations of these various materials.

[0009] Since all-solid batteries do not include any flammable materials, they offer better safety.

[0010] In addition, the energy density of all-solid-state batteries is much greater than that of liquid electrolyte batteries.

[0011] The solid electrolyte is incorporated directly into the electrode in powder form during coating and is called catholyte in the cathode and anolyte in the anode.

[0012] However, manufacturing fully solid batteries on an industrial scale remains complex, and one intermediate solution is to use electrolytes made from materials that are both flexible and ion conductors, such as certain polymers, for example polyethylene oxide (PEO).

[0013] Although manufacturing batteries comprising polymers that conduct lithium ions is simple and well understood, these batteries have not been widely used because they encounter fundamental limitations.

[0014] In fact, these polymers are not stable at high potentials. For example, PEO is only stable at potentials up to 3.6 V. The potentials necessary for active materials forming electrodes to reach the energy densities required for applications in the automotive sector are now between 3.7 V and 5 V.

[0015] The document US 2018 / 0006326 describes an all-solid-state Li-ion battery comprising a polymer material. In particular, a battery comprising PEO and a Li 6.5 Ln3Z 21.5 Ta 0.5 o 12 Oxide battery electrodes.

[0016] However, this document does not disclose a method for forming a battery cell that can stabilize the polymer to improve battery performance at high potentials.

[0017] The object of the present invention is therefore to overcome these drawbacks and to propose a method for forming an all-solid Li-ion battery cell comprising a PEO-LLZO solid electrolyte, conferring stability to the polymer at high potentials between 3.7 V and 5 V.

[0018] Therefore, a method for forming a Li-ion battery cell comprising a cathode material, an anode material and a solid electrolyte is proposed, wherein the electrolyte comprises polyethylene oxide and a Li7La3Zr2O 12 The method comprises the following consecutive cycle steps: (a) subjecting the battery cell to at least two consecutive charge / discharge cycles at a first cycle rate C / x, wherein the time limit of these charge / discharge steps is x / 2; (b) subjecting the battery cell to at least two consecutive charge / discharge cycles at a second charge rate C / y different from the first cycle rate, wherein y is less than x, and the time limit of these charge / discharge steps is y / 2; and (c) subjecting the battery cell to at least two consecutive charge / discharge cycles at a third cycle rate C / z different from the first charge rate and the second charge rate, wherein z is less than x and y, and the time limit of these charge / discharge steps is z / 2.

[0019] A charge / discharge cycle means a step comprising charging and then discharging. Thus, a continuous charge / discharge cycle means a cycle comprising charging and then discharging followed by one or more other cycles, each cycle also comprising charging and discharging.

[0020] The method for forming a battery cell according to the present invention can stabilize the composite electrolyte and improve the electrochemical performance of an all-solid Li-ion battery.

[0021] Other objects, advantages and features will become apparent from the following description provided for illustrative purposes only, with reference to the accompanying drawings, in which:

[0022] [ Figure 1 ] shows the variation of voltage with capacity of a battery cell that has not undergone any preconditioning during five consecutive charge / discharge cycles at a cycle rate of C / 20.

[0023] [ Figure 2 ] shows the variation of the capacity of a battery cell that has not undergone any preconditioning with the number of charge / discharge cycles at different cycle rates.

[0024] [ Figure 3 ] shows the variation of voltage with the capacity of a battery cell during a cycling step of preconditioning the battery cell according to the first embodiment.

[0025] [ Figure 4 ] shows the variation of voltage at different cycle rates with the capacity of a battery cell that has undergone preconditioning according to the first embodiment.

[0026] [ Figure 5 ] shows the variation of the capacity of a battery cell that has undergone preconditioning according to the first embodiment with the number of charge / discharge cycles at different cycle rates.

[0027] [ Figure 6 ] shows the variation of voltage with capacity of a battery cell during a pre-processing cycling step according to a second embodiment.

[0028] [ Figure 7 ] shows the variation of voltage at different cycle rates with the capacity of a battery cell that has undergone preconditioning according to the second embodiment.

[0029] [ Figure 8 ] shows the capacity of a battery cell that has undergone preconditioning according to the second embodiment as a function of the number of charge / discharge cycles at different cycle rates.

[0030] All-solid-state Li-ion batteries generally include a cathode, an anode, and a solid electrolyte.

[0031] The formation method according to the present invention relates to a Li-ion battery cell including a solid electrolyte comprising polyethylene oxide (PEO) and a Li7La3Zr2O 12 A mixture of oxides of (LLZO).

[0032] Preferably, the anode comprises lithium metal.

[0033] According to a preferred embodiment, the electrolyte comprises a lithium salt, such as lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).

[0034] The cathode is prepared by mixing the active material, the cathode electrolyte and a filler of the active material.

[0035] Preferably, the active material comprises a material of formula LiNiMnCoO2, corresponding to a mixture of nickel, manganese and cobalt, for example NMC622.

[0036] The filler of the active material may include carbon black, for example carbon black C65.

[0037] The cathode electrolyte preferably comprises polyethylene oxide and a 12 mixture of oxides.

[0038] Preferably, the cathode electrolyte further comprises lithium bis(trifluoromethanesulfonyl)imide, thereby advantageously forming a PEO-LiTFSI:LLZO mixture.

[0039] The method for forming a Li-ion battery cell according to the present invention comprises a step of pre-treating the battery cell, which comprises at least three consecutive steps (a), (b) and (c).

[0040] Step (a) includes subjecting the battery cell to at least two consecutive charge / discharge cycles at a first cycle rate C / x, and the time limit of each charge / discharge step is x / 2; step (b) includes subjecting the battery cell to at least two consecutive charge / discharge cycles at a second charge rate C / y different from the first cycle rate, wherein y is less than x, and the time limit of each charge / discharge step is y / 2; and step (c) includes subjecting the battery cell to at least two consecutive charge / discharge cycles at a third cycle rate C / z different from the first charge rate and the second charge rate, wherein z is less than x and y, and the time limit of each charge / discharge step is z / 2.

[0041] Surprisingly, it was found that a pre-treatment of the battery cell comprising at least the three steps (a), (b) and (c) described above allows the formation of a SEI on the surface of the battery cell, the quality of which contributes to stabilizing the polymer used to provide the battery cell.

[0042] In particular, it is observed that the stability of the polymer is improved at high battery operating potentials between 3.7 V and 5 V. As a result, the battery performance, and in particular the energy density, is improved.

[0043] Advantageously, successive circulation steps are performed at an increasing circulation rate.

[0044] Advantageously, the circulation rate during circulation step (a) is C / 40 and the circulation rate during circulation step (b) is C / 20.

[0045] The cycle rate or "charge or discharge rate" is expressed as C / n, where C is the battery capacity in Ah, ie the amount of electrical energy that can be returned after a full charge, and n refers to the time in h.

[0046] Advantageously, the circulation rate during the circulation step (c) is C / 10.

[0047] Preferably, the method for forming a Li-ion battery cell further comprises a continuous step (d) comprising subjecting the battery cell to at least two consecutive charge / discharge cycles at a fourth cycle rate different from the first charge rate, the second charge rate, and the third charge rate.

[0048] Advantageously, the circulation rate during the circulation step (d) is C / 5.

[0049] According to a preferred embodiment, the method for forming a Li-ion battery cell further comprises a continuous step (e), which comprises subjecting the battery cell to at least two consecutive charge / discharge cycles at a fifth cycle rate different from the first charge rate, the second charge rate, the third charge rate, and the fourth charge rate.

[0050] Advantageously, the circulation rate during the circulation step (e) is C / 2.

[0051] Preferably, one or more of the cycling steps (a), (b), (c), (d) and (e) comprises subjecting the battery cell to at least five consecutive charge / discharge cycles.

[0052] The duration of each charge / discharge cycle carried out at a cycle rate C / n during the various pre-treatment steps is preferably equal to n / 2.

[0053] The invention is illustrated in a non-limiting manner by the following example of a method for forming a Li-ion battery cell.

[0054] Example 1

[0055] 1. Preparation of battery cells

[0056] Solid electrolyte

[0057] The electrolyte used is a mixture of polyethylene oxide (PEO), Li7La3Zr2o 12 The LLZO was prepared by using the oxide of LLZO and the lithium salt, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).

[0058] The volume percentage of PEO-LiTFSI was 90 vol%, and the volume percentage of LLZO oxide was 10 vol%.

[0059] anode

[0060] The anode is formed from lithium metal.

[0061] cathode

[0062] The cathode is prepared by mixing the active material, the cathode electrolyte and the electron conductor.

[0063] Formula: LiNi 0.6 Mn 0.2 Co 0.2 NMC622 of o2 is selected as active material and corresponds to a nickel-manganese-cobalt mixture comprising 60 mol % of nickel, 20 mol % of manganese and 20 mol % of cobalt.

[0064] Carbon black C65 was selected as the electron conductor.

[0065] In addition, the cathode includes a cathode electrolyte, which includes polyethylene oxide, a Li7La3Zr2O 12 oxide and lithium bis(trifluoromethanesulfonyl)imide to form a PEO-LiTFSI:LLZO mixture.

[0066] The proportions of NMC622, carbon black C65 and cathode electrolyte in the cathode are shown in Table 1. Assume that for NMC622, The capacity is 166mAh / g. The amount of NMC622 present at the cathode is adjusted so as to obtain 1.6±0.6mAh.cm -2 surface capacity.

[0067] [Table 1]

[0068] NMC622 Carbon Black Catholyte Weight percentage (wt%) 74 6 20 Volume percentage (vol%) 50 10 40

[0069] Battery Cell Assembly

[0070] A 16 mm diameter electrolyte disk and a 13 mm diameter cathode disk were assembled and then added to a 14 mm diameter anode disk to form the battery cell.

[0071] 2. Constant current cycling, evaluation and results

[0072] A series of five charge / discharge cycles were performed at a rate of C / 20 on the battery cell obtained according to the formation method described in paragraph 1. The cycle tests were performed at 70°C and in a voltage window between 2.7V and 4.2V.

[0073] exist Figure 1 , curves A, B, C, D, and E correspond to the variation of voltage with battery cell capacity during the first, second, third, fourth, and fifth charge / discharge cycles, respectively.

[0074] Note that the voltage is unstable during the charge cycle above 3.7 V. During discharge, the capacity reaches an average of 43 mA.hg -1 Or just the expected experimental capacity of a battery cell including NMC622 as active material (166mA.hg -1 )’s 26%.

[0075] The cell was subjected to five additional charge / discharge cycles at a cycle rate of C / 20, during which the capacity slowly increased until it reached 85 mA.hg -1 .

[0076] exist Figure 2 As can be seen in the figure, the figure shows the change of battery cell capacity with the number of cycles at C / 20, C / 10, C / 5, C / 2 and 1C rates. The value of the discharge capacity at C / 20 is similar to that at the cycle rate C / 10, but gradually decreases with the increase of the capacity level C, that is, it is about 20mA.hg at C / 2 and 1C. -1 .

[0077] The voltage instability observed during the first charge / discharge cycle can be explained by the degradation of the composite electrolyte, and in particular the polyethylene oxide.

[0078] Example 2

[0079] 1. Preparation of battery cells

[0080] The method for preparing a battery cell described in detail in Example 1 was reproduced to carry out the method for preparing a battery cell in Example 2. Furthermore, an additional step of pre-treating the battery cell as further described below was performed.

[0081] Preprocessing

[0082] A battery cell was prepared according to a first embodiment of pretreatment. According to the first step (a), two charge / discharge cycles were performed at a first cycle rate C / 40.

[0083] Each charge / discharge cycle of step (a) was performed for 20 hours.

[0084] In the second step (b), two charge / discharge cycles are performed at a second cycle rate C / 20, wherein each cycle is performed for 10 hours.

[0085] Finally, in the final third step (c), two charge / discharge cycles are performed at a third cycle rate C / 10, wherein each cycle is performed for 5 hours.

[0086] Figure 3 The variation of voltage with the capacity of the battery cell during the cycling step of the pretreatment according to the first embodiment is shown in . It can be seen that the results obtained during this pretreatment show a better stability compared to the results in Example 1. The voltage reached is 3.8V.

[0087] 2. Constant current cycling, evaluation and results

[0088] After preconditioning the cells, charge and discharge tests were performed at cycle rates of C / 20, C / 10, C / 5, C / 2, and 1C. Figure 4 and Figure 5 The variation of voltage with the capacity of the battery cell at different rates and the variation of the capacity of the battery cell with the number of charge / discharge cycles are shown in FIG.

[0089] During charging, the voltage curve as a function of capacity at cycle rates C / 20 and C / 10 showed better stability than the battery cell in Example 1 without preconditioning, reaching 3.9 V and 3.8 V, respectively.

[0090] At cycle rates C / 5 and C / 2, the voltage instability persists but is still lower than in Example 1 without pretreatment.

[0091] 120mA.hg was obtained when discharging at a cycle rate of C / 20 -1 This represents a significant increase in capacity relative to the unpreconditioned cells.

[0092] Thus, the pre-treatment described in Example 2 enables the performance of the battery cell to be improved.

[0093] Example 3

[0094] 1. Preparation of battery cells

[0095] The method for preparing a battery cell described in detail in Example 1 was reproduced to carry out the method for preparing a battery cell in Example 3. In addition, the steps of pre-treating the battery cell presented in more detail below were performed.

[0096] Preprocessing

[0097] A battery cell was prepared according to the second embodiment of the pretreatment. Five charge / discharge cycles were performed according to the first step (a) at a first cycle rate C / 40. Each charge / discharge cycle of step (a) was performed for 20 hours.

[0098] In the second step (b), five charge / discharge cycles are performed at a second cycle rate C / 20, wherein each cycle is performed for 10 hours.

[0099] In the third step (c), five charge / discharge cycles are performed at a third cycle rate C / 10, wherein each cycle is performed for 5 hours.

[0100] In the fourth step (d), five charge / discharge cycles are performed at a fourth cycle rate C / 5, wherein each cycle is performed for 2 hours.

[0101] In the fifth step (e), five charge / discharge cycles are performed at a fifth cycle rate C / 2, wherein each cycle is performed for 1 hour.

[0102] Figure 6 The variation of voltage with the capacity of the battery cell during the cycling step of the pretreatment according to the second embodiment is shown in FIG. It can be seen that the results obtained during this pretreatment not only show very good stability compared to the results in Example 1, but also show higher stability relative to the battery cell in Example 2. The voltage reached is 4.2V.

[0103] 2. Constant current cycling, evaluation and results

[0104] After preconditioning the cells, charge and discharge tests were performed at cycle rates of C / 20, C / 10, C / 5, C / 2, and 1C. Figure 7 and Figure 8 The variation of voltage with the capacity of the battery cell at different rates and the variation of the capacity of the battery cell with the number of charge / discharge cycles are shown in FIG.

[0105] Regardless of the charging rate (C / 20 to C / 2), the potential of the battery cell can reach 4.2V during charging, and the polarization increases at a charging rate of 1C.

[0106] In discharge, 150 mA hg was obtained at a cycle rate of C / 20. -1 The average capacity at C / 10 is 91% of the expected experimental capacity, and 81% at C / 10. Thus, the performance of the cell is significantly improved relative to the performance of the cell that has not undergone any preconditioning.

Claims

1. A method for forming a lithium ion battery cell comprising a cathode material, an anode material and a solid electrolyte, the electrolyte comprising polyethylene oxide and a Li7La3Zr2O 12 A mixture of oxides, characterized in that The method comprises the following consecutive cyclic steps: (a) subjecting the battery cell to at least two consecutive charge / discharge cycles at a first cycle rate C / x, wherein the time limit of each charge / discharge step is x / 2; (b) subjecting the battery cell to at least two consecutive charge / discharge cycles at a second cycle rate C / y different from the first cycle rate, wherein y is less than x and the time limit of each charge / discharge step is y / 2; and (c) subjecting the battery cell to at least two consecutive charge / discharge cycles at a third cycle rate C / z different from the first cycle rate and the second cycle rate, wherein z is less than x and y, and the time limit of each charge / discharge step is z / 2, Here, x, y, z refer to the time in h.

2. The method according to claim 1, characterized in that The first cycle rate is C / 40, which is applied to perform charging / discharging for 20 h.

3. The method according to claim 1 or 2, characterized in that The second cycle rate was C / 20, which was applied for 10 h of charge / discharge.

4. The method according to claim 1 or 2, characterized in that: The third cycle rate is C / 10, which is applied to perform charge / discharge for 5 h.

5. The method according to claim 1 or 2, characterized in that: The method further comprises the following looping steps: (d) subjecting the battery cell to at least two consecutive charge / discharge cycles at a fourth cycle rate that is different from the first cycle rate, the second cycle rate, and the third cycle rate.

6. The method according to claim 5, characterized in that The fourth cycle rate is C / 5, which is applied to perform charging / discharging for 2.5 h.

7. The method according to claim 5, characterized in that The method further comprises the following looping steps: (e) subjecting the battery cell to at least two consecutive charge / discharge cycles at a fifth cycle rate that is different from the first cycle rate, the second cycle rate, the third cycle rate, and the fourth cycle rate.

8. The method according to claim 7, characterized in that The fifth cycle rate is C / 2, and is applied to perform charge / discharge for 1 h.

9. The method according to claim 7, characterized in that One or more of the cycling steps (a), (b), (c), (d), and (e) include subjecting the battery cell to at least five consecutive charge / discharge cycles.

10. The method according to claim 1 or 2, characterized in that: These successive cycling steps are performed at increasing cycling rates.

11. The method according to claim 1 or 2, characterized in that: The electrolyte includes lithium bis(trifluoromethanesulfonyl)imide LiTFSI.

12. The method according to claim 1 or 2, characterized in that: The cathode includes a cathode electrolyte including polyethylene oxide and an oxide Li7La3Zr2O 12 mixture.

13. The method according to claim 12, characterized in that The cathode electrolyte includes lithium bis(trifluoromethanesulfonyl)imide LiTFSI.

14. The method according to claim 1 or 2, characterized in that: The method includes a cathode having a mixture of nickel-manganese-cobalt active materials, carbon black, and a cathode electrolyte comprising polyethylene oxide and Li7La3Zr2O 12 mixture.

Citation Information

Patent Citations

  • Electrode compositions for solid-state batteries

    US20180006326A1

  • Positive plate of lithium ion secondary battery, and battery including the same

    CN101197436A

  • Solid electrolyte material, and electrolyte layer and lithium ion battery comprising solid electrolyte material

    CN105098234A

  • Lithium ion battery and formation method thereof

    CN107959071A

  • Composite polymer solid electrolyte and preparation method thereof

    CN108448167A