Semiconductor device and method for forming the same
By using the combination of the first epitaxial layer and the second epitaxial layer in the MBC transistor, the interface defect problem caused by the increase in germanium content and doping concentration is solved, lower resistance and higher strainability are achieved, and multi-bridges are improved Performance of channel transistors.
Patent Information
- Application Number
- CN202111006744.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-05-17
- Filing Date
- 2021-08-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-08-30
AI Technical Summary
When the epitaxial components of existing multi-bridge channel (MBC) transistors improve performance, the increased germanium content may lead to interface defects and contact resistance, and the increase in doping concentration will also cause more defects, affecting device performance.
A first epitaxial layer and a second epitaxial layer are employed, wherein the first epitaxial layer is used to bond the channel member and reduce interface defects, and the second epitaxial layer has a higher germanium content and doping concentration to reduce resistance and improve strainability, The first epitaxial layer covers the side walls of the channel member and the substrate portion, and the second epitaxial layer forms a low resistance layer on the internal spacer.
By minimizing the volume of the first epitaxial layer and maximizing the volume of the second epitaxial layer, the parasitic resistance in the source/drain component is reduced, and the strainability and on-current performance of the channel member are improved.
Smart Images

Figure CN113809157B_ABST
Abstract
Description
Technical Field
[0001] Embodiments of the present application relate to semiconductor devices and methods of forming the same. Background Art
[0002] The semiconductor integrated circuit (IC) industry has experienced exponential growth. Technological advances in IC materials and design have produced multiple generations of ICs, each with smaller and more complex circuits than the previous generation. Over the course of IC evolution, functional density (i.e., the number of interconnected devices per chip area) has generally increased, while geometry size (i.e., the smallest component (or line) that can be produced using a manufacturing process) has decreased. This scaling down process generally provides benefits by increasing production efficiency and reducing associated costs. This scaling down has also increased the complexity of processing and manufacturing ICs.
[0003] For example, as integrated circuit (IC) technology develops to smaller technology nodes, multi-gate metal oxide semiconductor field effect transistors (multi-gate MOSFETs or multi-gate devices) have been introduced to improve gate control by increasing gate channel coupling, reducing off-state current, and reducing short channel effect (SCE). Multi-gate devices generally refer to devices having a gate structure or a portion thereof disposed above more than one side of a channel region. Fin field effect transistors (FinFETs) and multi-bridge channel (MBC) transistors are examples of multi-gate devices, which have become popular and promising candidate devices for high performance and low leakage applications. FinFETs have an elevated channel wrapped by a gate on more than one side (e.g., the top and sidewalls of the "fin" extending from the substrate of the gate wrapping semiconductor material). MBC transistors have a gate structure that can extend partially or completely around the channel region to provide access to the channel region on two or more sides. Because its gate structure surrounds the channel region, MBC transistors can also be referred to as surround gate transistors (SGTs) or full ring gate (GAA) transistors.
[0004] To improve the performance of MBC transistors, efforts have been devoted to developing strained channels and providing epitaxial features with reduced resistance.While conventional epitaxial features are generally adequate for their intended purposes, they are not satisfactory in all respects. Summary of the invention
[0005] Some embodiments of the present application provide a semiconductor device, comprising: a plurality of channel components arranged above a substrate; a plurality of internal spacer components interlaced with the plurality of channel components; a gate structure wrapping each of the plurality of channel components; and a source / drain component, comprising: a first epitaxial layer in contact with the substrate and the plurality of channel components, and a second epitaxial layer in contact with the first epitaxial layer and the plurality of internal spacer components, wherein the first epitaxial layer and the second epitaxial layer comprise silicon germanium, and wherein the germanium content of the second epitaxial layer is greater than the germanium content of the first epitaxial layer.
[0006] Other embodiments of the present application provide a semiconductor device, comprising: a plurality of silicon channel components disposed above a substrate; a plurality of dielectric internal spacer components interleaved with the plurality of silicon channel components, each of the plurality of silicon channel components comprising a rounded end; a gate structure wrapping each of the plurality of silicon channel components; and a source / drain component, comprising: a first epitaxial layer in contact with the substrate and the rounded ends of the plurality of silicon channel components, and a second epitaxial layer in contact with the first epitaxial layer and the plurality of dielectric internal spacer components, wherein the first epitaxial layer and the second epitaxial layer comprise silicon germanium, wherein the germanium content of the first epitaxial layer is between about 20% and about 30%, and wherein the germanium content of the second epitaxial layer is between about 50% and about 60%.
[0007] Some other embodiments of the present application provide a method for forming a semiconductor device, comprising: forming a stack above a substrate, wherein the stack includes a plurality of silicon layers interlaced with a plurality of silicon germanium layers; forming a fin structure from the stack and the substrate, the fin structure including a channel region and a source / drain region; forming a dummy gate stack above the channel region of the fin structure; depositing a gate spacer layer above the dummy gate stack; recessing the source / drain region to form a source / drain trench that exposes the sidewalls of the plurality of silicon layers and the plurality of silicon germanium layers; selectively and partially recessing the plurality of silicon germanium layers to form a plurality of internal spacer grooves; forming a plurality of internal spacer grooves in the plurality of internal spacer grooves; forming a plurality of internal spacer parts; depositing a first epitaxial layer in the source / drain trench, the first epitaxial layer contacting the plurality of silicon layers; depositing a second epitaxial layer over the first epitaxial layer, the second epitaxial layer contacting the plurality of internal spacer parts and the first epitaxial layer; depositing a third epitaxial layer on the second epitaxial layer; after depositing the third epitaxial layer, removing the pseudo gate stack; releasing the plurality of silicon layers in the channel region as a plurality of channel components; and forming a gate structure around each of the plurality of channel components, wherein the first epitaxial layer and the second epitaxial layer include silicon germanium, and wherein the germanium content of the second epitaxial layer is greater than the germanium content of the first epitaxial layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] The present invention can be best understood from the following detailed description when read in conjunction with the accompanying drawings. It should be emphasized that, in accordance with standard practice in the industry, the various components are not drawn to scale and are only used for illustration purposes. In fact, the size of the various components can be arbitrarily increased or reduced for clarity of discussion.
[0009] Figure 1 A flow chart of a method for forming a semiconductor device according to one or more aspects of the present invention is shown.
[0010] Figures 2 to 11 , FIG. 12A to FIG. 19A and FIG. 12B to FIG. 19B According to one or more aspects of the present invention, Figure 1 A partial cross-sectional view of a workpiece during a manufacturing process of the method. DETAILED DESCRIPTION
[0011] The following disclosure provides many different embodiments or examples for realizing the different features of the provided subject matter. Specific examples of components and arrangements are described below to simplify the present invention. Of course, these are merely examples and are not intended to limit the present invention. For example, in the following description, forming a first component above or on a second component may include an embodiment in which the first component and the second component are directly in contact with each other, and may also include an embodiment in which an additional component may be formed between the first component and the second component so that the first component and the second component may not be in direct contact. In addition, the present invention may repeat reference numerals and / or characters in various examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or configurations discussed.
[0012] For ease of description, spatially relative terms such as "below," "beneath," "lower," "above," "upper," etc. may be used herein to describe the relationship of one element or component to another (or additional) elements or components as shown in the figures. The spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein should be interpreted accordingly.
[0013] In addition, when "about," "approximately," or the like is used to describe a value or a range of values, as understood by one of ordinary skill in the art, the term is intended to encompass values within a reasonable range that takes into account inherent variations during manufacturing. For example, based on known manufacturing tolerances associated with manufacturing components having properties associated with the values, the values or ranges of values encompass a reasonable range that includes the described values, such as within + / -10% of the described values. For example, a material layer having a thickness of "about 5 nm" may cover a range of sizes from 4.25 nm to 5.75 nm, where the manufacturing tolerance associated with the deposited material layer known to one of ordinary skill in the art is + / -15%. Further, the present invention may repeat reference numerals and / or characters in various instances. This repetition is for the purpose of simplicity and clarity and does not in itself indicate a relationship between the various embodiments and / or configurations discussed.
[0014] The present invention generally relates to multi-gate transistors and manufacturing methods, and more specifically to multilayer epitaxial components of MBC transistors. The channel region of the MBC transistor can be arranged in a nanowire channel member, a rod-shaped channel member, a nanosheet channel member, a nanostructure channel member, a columnar channel member, a rod-shaped channel member and / or other suitable channel configurations. Depending on the shape of the channel member, the MBC transistor may also be referred to as a nanowire transistor or a nanosheet transistor. Regardless of the shape, each of the channel members of the MBC transistor extends between two source / drain components and is coupled to two source / drain components. The ideal source / drain component of the MBC transistor introduces strain on the channel component and provides lower resistance. Although the germanium content in the source / drain component can be increased to enhance the strain on the channel component, a greater germanium content may result in more defects at the interface between the source / drain component and the channel component. Similarly, although the doping concentration in the source / drain component can be increased to reduce resistance, a greater dopant concentration may result in more defects at the interface between the source / drain component and the channel component. Defects at the interface may increase contact resistance.
[0015] The present invention provides an embodiment of a semiconductor device, wherein its source / drain component includes a first epitaxial layer to engage a channel member and a second epitaxial layer spaced apart from the channel member. The first epitaxial layer is used as a transition layer to engage the channel member and to reduce interface defects. The second epitaxial layer may have a doping concentration greater than the doping concentration of the first epitaxial layer to reduce resistance. At the same time, the second epitaxial layer may have a greater germanium content to improve the strain on the channel member. In order to improve the strain on the channel member and to reduce resistance, the first epitaxial layer is minimized and the second epitaxial layer is maximized, provided that the first epitaxial layer completely covers the exposed channel member. In some embodiments, the first epitaxial layer includes a channel sidewall portion and a substrate portion, and the substrate portion is formed to a thickness at which the substrate portion merges with one or more lower channel sidewall portions. Each of the channel members has a circular sidewall profile, and each of the channel sidewall portions is wrapped above the circular sidewall.
[0016] Various aspects of the present invention will now be described in more detail with reference to the accompanying drawings. In that regard, Figure 1 1 is a flow chart illustrating a method 100 of forming a semiconductor device from a workpiece according to an embodiment of the present invention. The method 100 is merely an example and is not intended to limit the present invention to that explicitly shown in the method 100. Additional steps may be provided before, during, and after the method 100, and some of the steps described may be replaced, eliminated, or moved for additional embodiments of the method. For simplicity, not all steps are described in detail herein. Figures 2 to 11 , FIG. 12A to FIG. 19A and FIG. 12B to FIG. 19B Describing method 100, Figures 2 to 11 , FIG. 12A to FIG. 19A and FIG. 12B to FIG. 19B is based on Figure 1 1 is a partial cross-sectional view of a workpiece 200 at different manufacturing stages of an embodiment of the method 100 in FIG. Because the workpiece 200 will be manufactured into a semiconductor device, the workpiece 200 may be referred to as a semiconductor device 200 herein as the context requires. To avoid, Figures 2 to 11 , FIG. 12A to FIG. 19A and FIG. 12B to FIG. 19B The X, Y and Z directions in FIG. 1 are perpendicular to each other. Throughout the present invention, the same reference numerals denote the same components unless otherwise specified.
[0017] refer to Figure 1 and Figure 2 , the method 100 includes a block 102, in which a stack 204 of alternating semiconductor layers is formed above a workpiece 200. Figure 2As shown in , workpiece 200 includes substrate 202. In some embodiments, substrate 202 may be a semiconductor substrate, such as a silicon (Si) substrate. Substrate 202 may include various doping configurations, depending on design requirements known in the art. In embodiments where the semiconductor device is p-type, an n-type doping profile (i.e., an n-type well or n-well) may be formed on substrate 202. In some embodiments, an n-type dopant for forming an n-type well may include phosphorus (P) or arsenic (As). In embodiments where the semiconductor device is n-type, a p-type doping profile (i.e., a p-type well or p-well) may be formed on substrate 202. In some embodiments, an n-type dopant for forming a p-type well may include boron (B) or gallium (Ga). Suitable doping may include ion implantation and / or diffusion processes of dopants. Substrate 202 may also include other semiconductors, such as germanium (Ge), silicon carbide (SiC), silicon germanium (SiGe), or diamond. Alternatively, substrate 202 may include a compound semiconductor and / or an alloy semiconductor. Additionally, the substrate 202 may optionally include an epitaxial layer (epitaxial layer), may be strained for performance enhancement, may include a silicon-on-insulator (SOI) or germanium-on-insulator (GeOI) structure, and / or may have other suitable enhancement features.
[0018] In some embodiments, the stack 204 includes sacrificial layers 206 of a first semiconductor composition interleaved with channel layers 208 of a second semiconductor composition. The first semiconductor composition and the second semiconductor composition may be different. In some embodiments, the sacrificial layers 206 include silicon germanium (SiGe) and the channel layers 208 include silicon (Si). It should be noted that the three (3) layers of the sacrificial layers 206 and the three (3) layers of the channel layers 208 are arranged alternately, as shown in FIG. Figure 2 , which is for illustrative purposes only and is not intended to limit the contents specifically recited in the claims. It is understood that any number of epitaxial layers can be formed in the stack 204. The number of layers depends on the desired number of channel components for the semiconductor device 200. In some embodiments, the number of channel layers 208 is between 2 and 10.
[0019] In some embodiments, all sacrificial layers 206 may have a substantially uniform first thickness between about 9 nm and about 10 nm, and all channel layers 208 may have a substantially uniform second thickness between about 6 nm and about 8 nm. The first thickness and the second thickness may be the same or different. As described in more detail below, the channel layer 208 or a portion thereof may be used as a channel member for a subsequently formed multi-gate device, and the thickness of each of the channel layers 208 is selected based on device performance considerations. The sacrificial layer 206 in the channel region may be ultimately removed and used to define the vertical distance between adjacent channel regions for a subsequently formed multi-gate device, and the thickness of each of the sacrificial layers 206 is selected based on device performance considerations.
[0020] The layers in stack 204 may be deposited using a molecular beam epitaxy (MBE) process, a vapor phase deposition (VPE) process, and / or other suitable epitaxial growth processes. As described above, in at least some examples, sacrificial layer 206 includes an epitaxially grown silicon germanium (SiGe) layer, and channel layer 208 includes an epitaxially grown silicon (Si) layer. In some embodiments, sacrificial layer 206 and channel layer 208 are substantially free of dopants (i.e., have approximately 0 cm -3 About 1x10 17 cm -3 of the extrinsic dopant concentration), wherein, for example, no intentional doping is performed during the epitaxial growth process of the stack 204.
[0021] Still reference Figure 1 , Figure 2 and Figure 3 , the method 100 includes a block 104, in which a fin structure 212 is formed from the stack 204 and the substrate 202. To pattern the stack 204, a hard mask layer 210 ( Figure 2 ) to form an etching mask. The hard mask layer 210 may be a single layer or a multilayer. For example, the hard mask layer 210 may include a pad oxide layer and a pad nitride layer above the pad oxide layer. The fin structure 212 may be patterned from the stack 204 and the substrate 202 using a photolithography process and an etching process. The photolithography process may include photoresist coating (e.g., spin coating), soft baking, mask alignment, exposure, post-exposure baking, photoresist development, rinsing, drying (e.g., spin drying and / or hard baking), other suitable photolithography techniques and / or combinations thereof. In some embodiments, the etching process may include dry etching (e.g., RIE etching), wet etching and / or other etching methods. As Figure 3 As shown in , the etching process in box 104 forms a trench that extends through the stack 204 and a portion of the substrate 202. The trench defines a fin structure 212. In some embodiments, a double patterning or multiple patterning process can be used to define a fin structure having a pitch that is smaller than that obtainable using a single, direct photolithography process, for example. For example, in one embodiment, a material layer is formed above a substrate and patterned using a photolithography process. Spacers are formed next to the patterned material layer using a self-aligned process. The material layer is then removed, and the remaining spacers or mandrels can then be used to pattern the fin structure 212 by etching the stack 204. As shown in FIG. Figure 3 As shown in FIG. 2 , the fin structure 212 together with the sacrificial layer 206 and the channel layer 208 therein extends vertically along the Z direction and longitudinally along the X direction.
[0022] An isolation component 214 is formed adjacent to the fin structure 212. In some embodiments, the isolation component 214 may be formed in a trench to isolate the fin structure 212 from an adjacent active area. The isolation component 214 may also be referred to as a shallow trench isolation (STI) component 214. As an example, in some embodiments, a dielectric layer is first deposited over the substrate 202, and the trench is filled with the dielectric layer. In some embodiments, the dielectric layer may include silicon oxide, silicon nitride, silicon oxynitride, fluorine-doped silicate glass (FSG), low-k dielectrics, combinations thereof, and / or other suitable materials. In various examples, the dielectric layer may be deposited by a CVD process, a sub-atmospheric pressure CVD (SACVD) process, a flowable CVD process, a spin coating process, and / or other suitable processes. The deposited dielectric material is then thinned and planarized, for example, by a chemical mechanical polishing (CMP) process. The planarized dielectric layer is further recessed or pulled back by a dry etching process, a wet etching process, and / or a combination thereof to form the STI component 214. After being recessed, the fin structure 212 rises above the STI feature 214 .
[0023] refer to Figure 1 , Figure 4 and Figure 5 The method 100 includes a block 106 in which a dummy gate stack 220 is formed above the channel region 212C of the fin structure 212. In some embodiments, a gate replacement process (or a gate-last process) is used, in which the dummy gate stack 220 ( Figure 4 and Figure 5 ) is used as a placeholder to undergo various processes and is removed and replaced by a functional gate structure. Other processes and configurations are also possible. Figure 5 In some embodiments shown in , the dummy gate stack 220 is formed above the fin structure 212 and the fin structure 212 can be divided into a channel region 212C located below the dummy gate stack 220 and a source / drain region 212SD not located below the dummy gate stack 220. The channel region 212C is adjacent to the source / drain region 212SD. Figure 5 As shown in FIG. 2 , the channel region 212C is disposed between two source / drain regions 212SD along the X direction.
[0024] Forming the dummy gate stack 220 may include depositing layers in the dummy gate stack 220 and patterning the layers. Figure 4, a dummy dielectric layer 216, a dummy electrode layer 218, and a gate top hard mask layer 222 may be blanket deposited over the workpiece 200. In some embodiments, the dummy dielectric layer 216 may be formed on the fin structure 212 using a chemical vapor deposition (CVD) process, an ALD process, an oxygen plasma oxidation process, or other suitable process. In some cases, the dummy dielectric layer 216 may include silicon oxide. Thereafter, a dummy electrode layer 218 may be deposited over the dummy dielectric layer 216 using a CVD process, an ALD process, or other suitable process. In some cases, the dummy electrode layer 218 may include polysilicon. For patterning purposes, a gate top hard mask layer 222 may be deposited over the dummy electrode layer 218 using a CVD process, an ALD process, or other suitable process. The gate top hard mask layer 222, the dummy electrode layer 218, and the dummy dielectric layer 216 may then be patterned to form a dummy gate stack 220, such as Figure 5 As shown in . For example, the patterning process may include a lithography process (e.g., photolithography or electron beam lithography), which may further include photoresist coating (e.g., spin coating), soft baking, mask alignment, exposure, post-exposure baking, photoresist development, rinsing, drying (e.g., spin drying and / or hard baking), other suitable lithography techniques and / or combinations thereof. In some embodiments, the etching process may include dry etching (e.g., RIE etching), wet etching and / or other etching methods. In some embodiments, the gate top hard mask layer 222 may include a silicon oxide layer 223 and a silicon nitride layer 224 above the silicon oxide layer 223. As shown in Figure 5 As shown in FIG. 2 , no dummy gate stack 220 is disposed over the source / drain region 212SD of the fin structure 212 .
[0025] refer to Figure 1 and Figure 6 , the method 100 includes a frame 108, wherein a gate spacer layer 226 is deposited over the dummy gate stack 220. In some embodiments, the gate spacer layer 226 is conformally deposited over the workpiece 200, including over the top surface and sidewalls of the dummy gate stack 220. The term "conformal" may be used herein to easily describe a layer having a substantially uniform thickness over various regions. The gate spacer layer 226 may be a single layer or multiple layers. At least one layer of the gate spacer layer 226 may include silicon carbonitride, silicon oxycarbide, silicon carbon oxynitride, or silicon nitride. The gate spacer layer 226 may be deposited over the dummy gate stack 220 using a process such as a CVD process, a sub-atmospheric pressure CVD (SACVD) process, an ALD process, or other suitable process. In one embodiment, the gate spacer layer 226 includes a first layer, a second layer disposed over the first layer, and a third layer disposed over the second layer. The first layer and the second layer include silicon oxynitride and the third layer includes silicon nitride.
[0026] refer to Figure 1and Figure 7 , the method 100 includes a frame 110, in which the source / drain region 212SD of the fin structure 212 is recessed to form a source / drain trench 228. In some embodiments, the source / drain region 212SD not covered by the dummy gate stack 220 and the gate spacer layer 226 is etched by dry etching or a suitable etching process to form the source / drain trench 228. For example, the dry etching process can be implemented with an oxygen-containing gas, a fluorine-containing gas (e.g., CF4, SF6, CH2F2, CHF3 and / or C2F6), a chlorine-containing gas (e.g., Cl2, CHCl3, CCl4 and / or BCl3), a bromine-containing gas (e.g., HBr and / or CHBR3), an iodine-containing gas, other suitable gases and / or plasmas and / or combinations thereof. Figure 7 In some embodiments shown in , the source / drain region 212SD of the fin structure 212 is recessed to expose the sidewalls of the sacrificial layer 206 and the channel layer 208. In some embodiments, the source / drain trenches 228 extend into the substrate 202 below the stack 204. Figure 7 2 shows a cross-sectional view of the workpiece 200 viewed along the Y direction at the source / drain region 212SD. Figure 7 As shown in FIG. 1 , the sacrificial layer 206 and the channel layer 208 in the source / drain region 212SD are removed in block 110 , exposing the substrate 202 .
[0027] refer to Figure 1 , Figure 8 , Fig. 9 and Fig.10 , the method 100 includes block 112, in which an inner spacer feature 234 is formed. Although not explicitly shown, the operations in block 112 may include: selectively and partially removing the sacrificial layer 206 to form the inner spacer recess 230; depositing the inner spacer material 232 over the workpiece 200; and etching back the inner spacer material 232 to form the inner spacer feature 234 in the inner spacer recess 230. Figure 8206 is selectively and partially recessed to form an internal spacer recess 230, while the gate spacer layer 226, the exposed portion of the substrate 202, and the channel layer 208 are substantially unetched. In embodiments where the channel layer 208 is substantially composed of silicon (Si) and the sacrificial layer 206 is substantially composed of silicon germanium (SiGe), the selective recessing of the sacrificial layer 206 may be performed using a selective wet etching process or a selective dry etching process. The selectivity and partial recessing of the sacrificial layer 206 may include a SiGe oxidation process and subsequent SiGe oxide removal. In those embodiments, the SiGe oxidation process may include the use of ozone. In some other embodiments, the selective dry etching process may include the use of one or more fluorine-based etchants, such as fluorine gas or hydrofluorocarbons. The selective wet etching process may include APM etching (e.g., an ammonium hydroxide-hydrogen peroxide-water mixture).
[0028] After forming the internal spacer recess 230, the internal spacer material 232 is deposited over the workpiece 200, including over the internal spacer recess 230, such as Fig. 9 . The internal spacer material 232 may include a metal oxide, silicon oxide, silicon oxycarbonitride, silicon nitride, silicon oxynitride, carbon-rich silicon carbonitride, or a low-k dielectric material. The metal oxide may include aluminum oxide, zirconium oxide, tantalum oxide, yttrium oxide, titanium oxide, lanthanum oxide, or other suitable metal oxides. Although not explicitly shown, the internal spacer material 232 may be a single layer or multiple layers. In some embodiments, the internal spacer material 232 may be deposited using CVD, PECVD, SACVD, ALD, or other suitable methods. The internal spacer material 232 is deposited into the internal spacer recess 230 and over the sidewalls of the channel layer 208 exposed in the source / drain trench 228. Reference Fig.10 , and then etch back the deposited internal spacer material 232 to remove the internal spacer material 232 from the sidewalls of the channel layer 208 to form an internal spacer feature 234 in the internal spacer recess 230. In block 112, the internal spacer material 232 may also be removed from the top surface and / or sidewalls of the gate top hard mask layer 222 and the gate spacer layer 226. In some embodiments, the etch back operation performed in block 112 may include using hydrogen fluoride (HF), fluorine gas (F2), hydrogen (H2), ammonia (NH3), nitrogen trifluoride (NF3), or other fluorine-based etchants. Fig.10 As shown in , each of the inner spacer features 234 is in direct contact with the recessed sacrificial layer 206 and is disposed between two adjacent channel layers 208. In some cases, each of the inner spacer features 234 is between about 3 nm and about 5 nm measured along the X direction. Fig.10As shown in FIG, although the selective etching process and the etch-back process in box 112 are selective to the sacrificial layer 206 and the internal spacer material 232, the channel layer 208 is moderately etched and has rounded ends. In the depicted embodiment, the source / drain trenches 228 extend to a depth D in the substrate 202, and the depth D is between about 10 nm and about 12 nm.
[0029] refer to Figure 1 and Fig.11 , the method 100 includes a frame 114, in which a cleaning process 300 is implemented. The cleaning process 300 may include dry cleaning, wet cleaning, or a combination thereof. In some instances, the wet cleaning may include using standard cleaning 1 (RCA SC-1, a mixture of deionized (DI) water, ammonium hydroxide, and hydrogen peroxide), standard cleaning 2 (RCA SC-2, a mixture of DI water, hydrochloric acid, and hydrogen peroxide), SPM (sulfur peroxide mixture), and / or hydrofluoric acid for oxide removal. The dry cleaning process may include helium (He) and hydrogen (H2) treatment at a temperature between about 250° C. and about 550° C. and at a pressure between about 75 mTorr and about 155 mTorr. The hydrogen treatment may convert silicon on the surface into silane (SiH4), which may be pumped out for removal. In some embodiments, the cleaning process is configured to selectively remove or trim portions of the channel layer without substantially removing the internal spacer features 234. The cleaning process 300 may remove surface oxides and debris to ensure a clean semiconductor surface, which facilitates the growth of a high quality epitaxial layer in block 116 .
[0030] refer to Figure 1 , Fig. 12A and Fig. 12B , the method 100 includes block 116, where a first epitaxial layer 236 is deposited. Fig. 12AIn some embodiments shown in , the first epitaxial layer 236 can be epitaxially and selectively formed by the exposed sidewalls of the channel layer 208 and the exposed surface of the substrate 202, while the sidewalls of the sacrificial layer 206 remain covered by the internal spacer components 234. Suitable epitaxial processes for frame 116 include vapor phase epitaxy (VPE), ultra-high vacuum CVD (UHV-CVD), molecular beam epitaxy (MBE) and / or other suitable processes. The epitaxial growth process in frame 116 can use a gaseous precursor that interacts with the components of the substrate 202 and the channel layer 208. In some embodiments, the parameters of the epitaxial growth process in frame 116 are selected so that the first epitaxial layer 236 is not epitaxially deposited on the internal spacer components 234. According to the present invention, at the end of the operation in frame 116, at least some of the internal spacer components 234 remain exposed. That is, at least some of the internal spacer components 234 are not completely covered by the first epitaxial layer 236. In some cases, the first epitaxial layer 236 includes silicon germanium (SiGe) and is doped with a p-type dopant, such as boron (B). In some embodiments, the first epitaxial layer 236 includes a germanium (Ge) content between about 20% and about 30% and a silicon (Si) content between about 80% and about 70%. This germanium (Ge) content range is not unimportant. When the germanium content is greater than about 30%, the lattice mismatch between silicon and germanium may cause excessive defects at the interface between the first epitaxial layer 236 and the channel layer 208, which may cause increased resistance or device failure. When the germanium content is less than about 20%, the channel layer 208 may not be sufficiently strained to improve hole mobility. The concentration of the p-type dopant in the first epitaxial layer 236 may be about 1x10 20 Atom / cm 3 and about 4x10 20 Atom / cm 3 The p-type dopant concentration range is also not unimportant. When the p-type dopant concentration in the first epitaxial layer 236 is less than about 1×10 20 Atom / cm 3 When the doping concentration of the p-type dopant in the first epitaxial layer 236 is greater than about 4×10 20 Atom / cm 3 When the first epitaxial layer 236 is formed, the p-type dopant in the lattice gap may also cause excessive defects at the interface between the first epitaxial layer 236 and the channel layer 208, which may lead to an increase in resistance.
[0031] exist Fig. 12AIn the embodiment shown in , the first epitaxial layer 236 may include a first substrate portion 236B disposed on the substrate 202 and a first channel sidewall portion 236T in contact with the circular end of the channel layer 208. The first channel sidewall portion 236T is wrapped above the circular end and has a curved shape. In these embodiments, the first channel sidewall portion 236T is formed to a thickness such that the circular end is completely covered. In some cases, each of the first channel sidewall portions 236T has a thickness between about 4nm and about 6nm along the X direction. The first substrate portion 236B is not combined or merged with the first channel sidewall portion 236T. Therefore, each of the internal spacer components 234 is not completely covered by the first epitaxial layer 236. That is, although the internal spacer component 234 can be in contact with the first epitaxial layer 236, at least a portion of each of the internal spacer components 234 remains exposed. When measured from the bottom surface of the source / drain trench 228, the first substrate portion 236B has a first height (H1) along the Z direction. The first height (H1) is between about 12 nm and about 15 nm. Fig. 12A As shown in , because the first height ( H1 ) is greater than the depth D of the source / drain trench 228 into the substrate 202 , a portion of the first substrate portion 236B rises above the substrate 202 .
[0032] Fig. 12B An alternative embodiment of the first epitaxial layer 236 is shown in FIG. For clarity and ease of reference, the first epitaxial layer 236 in the alternative embodiment may be referred to as the alternative first epitaxial layer 2360. Fig. 12B As shown in , the optional first epitaxial layer 2360 may include a second substrate portion 2360B disposed on the substrate 202 and a second channel sidewall portion 2360T in contact with the circular end of the channel layer 208. The second channel sidewall portion 2360T wraps over the circular end and has a curved shape. In these embodiments, although the second channel sidewall portion 2360T is formed to a thickness that completely covers the circular end of the channel layer 208, the larger area of the exposed substrate 202 allows the second substrate portion 2360B to grow epitaxially faster. Therefore, the second substrate portion 2360B merges with the second channel sidewall portion 2360T in contact with the bottommost channel layer 208. As shown in FIG. Fig. 12BAs shown in , the second substrate portion 2360B is in contact not only with the substrate 202, but also with the rounded end of the bottommost channel layer 208. By extending between the substrate 202 and the bottommost channel layer 208, the second substrate portion 2360B also completely covers the bottommost internal spacer component 234. The bottommost internal spacer components 234 are those sandwiched vertically (along the Z direction) between the bottommost channel layer 208 and the substrate 202. Except for the bottommost internal spacer component 234, the optional first epitaxial layer 2360 does not completely cover other internal spacer components 234. In some cases, each of the second channel sidewall portions 2360T has a thickness between about 4nm and about 6nm along the X direction. When measured from the bottom surface of the source / drain trench 228, the second substrate portion 2360B has a second height (H2) along the Z direction. The second height (H2) is greater than the first height (H1) and is between about 15nm and about 20nm. As Fig. 12B As shown in , because the second height (H2) is greater than the depth D of the source / drain trench 228 into the substrate 202, a portion of the second substrate portion 2360B rises above the substrate 202.
[0033] refer to Figure 1 , Fig.13A and Fig. 13B , method 100 includes block 118, wherein Fig.13A The first epitaxial layer 236 or Fig. 13B A second epitaxial layer 238 is deposited over the optional first epitaxial layer 2360 in the frame 118. In some embodiments, the second epitaxial layer 238 can be epitaxially and selectively formed from the first epitaxial layer 236 (or the optional first epitaxial layer 2360). Suitable epitaxial processes of frame 118 include vapor phase epitaxy (VPE), ultra-high vacuum CVD (UHV-CVD), molecular beam epitaxy (MBE), and / or other suitable processes. The epitaxial growth process in frame 118 can use a gaseous precursor that interacts with the components of the first epitaxial layer 236 (or the optional first epitaxial layer 2360). The second epitaxial layer 238 is allowed to overgrow and merge over the inner spacer features 234 and substantially fill the source / drain trenches 228. In some embodiments, the second epitaxial layer 238 includes silicon germanium (SiGe) doped with a p-type dopant such as boron (B). Second epitaxial layer 238 serves as a low resistance layer and includes a doping concentration greater than the doping concentration in first epitaxial layer 236 (or optional first epitaxial layer 2360). In some cases, the doping concentration in second epitaxial layer 238 may be about 4×10 20 Atom / cm 3 and about 2x10 21 Atom / cm 3 When the doping concentration of the p-type dopant in the second epitaxial layer 238 is lower than 6×10 20 Atom / cm3 When the second epitaxial layer 238 is 2×10 , the second epitaxial layer 238 may not be sufficiently conductive to achieve a satisfactory drive current (ie, on-current). In addition, the solubility of the p-type dopant in the second epitaxial layer 238 may prevent the doping concentration of the p-type dopant from exceeding 2×10 21 Atom / cm 3 . The doping concentration in the second epitaxial layer 238 is limited by the solubility of boron (B) in the second epitaxial layer 238. Compared to the first epitaxial layer 236 (or the optional first epitaxial layer 2360), the second epitaxial layer 238 includes a greater germanium content to enhance the strain on the channel layer 208. In some embodiments, the second epitaxial layer 238 includes a germanium content between about 50% and about 60% and a silicon content between about 40% and about 50%. According to the present invention, the volume of the second epitaxial layer 238 is greater than the volume of the first epitaxial layer 236 (or the optional first epitaxial layer 2360). In this regard, the second epitaxial layer 238 is thicker than the first epitaxial layer 236 (or the optional first epitaxial layer 2360). In some embodiments, the second epitaxial layer 238 can have a thickness between about 11 nm and about 15 nm, measured along the X direction. Fig.13A and Fig. 13B In some embodiments shown in , the second epitaxial layer 238 is separated or spaced apart from the channel layer 208 and the substrate 202 by the first epitaxial layer 236 (or the optional first epitaxial layer 2360). The second epitaxial layer 238 may also be referred to as a second epitaxial component. Fig. 13B In the alternative embodiment shown in , the second epitaxial layer 238 is spaced apart from the bottommost inner spacer feature 234 because the bottommost inner spacer feature 234 is covered by the second substrate portion 2360B of the alternative first epitaxial layer 2360. Fig. 13B In the embodiment shown in FIG. 2 , the second epitaxial layer 238 is in contact with the other inner spacer features 234 .
[0034] refer to Figure 1 , Fig.14A and Fig. 14B, the method 100 may optionally include a frame 120, wherein a third epitaxial layer 240 is deposited on the second epitaxial layer 238. In some embodiments, the third epitaxial layer 240 may be epitaxially and selectively formed from the second epitaxial layer 238. Suitable epitaxial processes for frame 120 include vapor phase epitaxy (VPE), ultra-high vacuum CVD (UHV-CVD), molecular beam epitaxy (MBE), and / or other suitable processes. The epitaxial growth process in frame 120 may use a gaseous precursor that interacts with the components of the second epitaxial layer 238. In some embodiments, the third epitaxial layer 240 includes silicon germanium (SiGe) and is doped with a p-type dopant, such as boron (B). The third epitaxial layer 240 is used as a sacrificial layer when forming source / drain contact openings. In order to better serve as a sacrificial layer, the third epitaxial layer 240 is more etch-resistant by having a germanium content that is smaller than the germanium content of the second epitaxial layer 238 or even the germanium content of the first epitaxial layer 236 (or the optional first epitaxial layer 2360). In some cases, third epitaxial layer 240 has a germanium content between about 15% and about 20% and a silicon content between about 80% and about 85%. Likewise, to increase the etching resistance of third epitaxial layer 240, the doping concentration in third epitaxial layer 240 is less than the doping concentration of second epitaxial layer 238. In some cases, the doping concentration in third epitaxial layer 240 can be about 2×10 20 Atom / cm 3 and about 6x10 20 Atom / cm 3 Along the Z direction, the third epitaxial layer 240 has a thickness between about 2 nm and about 3 nm. Fig.14A and Fig. 14B , the first epitaxial layer 236 (or the optional first epitaxial layer 2360 ), the second epitaxial layer 238 , and the third epitaxial layer 240 (if formed) in the source / drain region 212SD may be collectively referred to as a source / drain feature 242 .
[0035] refer to Figure 1 , Fig.15A and Fig. 15B , the method 100 includes a block 122, wherein the workpiece 200 is annealed in an annealing process 400. In some embodiments, the annealing process 400 may include a rapid thermal annealing (RTA) process, a laser spike annealing process, a rapid annealing process, or a furnace annealing process. The annealing process 400 may include a peak annealing temperature between about 900° C. and about 1000° C. In these embodiments, the peak annealing temperature may be maintained for a duration measured in seconds or microseconds. Through the annealing process 400, a desired electron contribution of a p-type dopant in a semiconductor body, such as silicon germanium (SiGe) or germanium (Ge), may be obtained. The annealing process 400 may generate vacancies that promote the movement of the p-type dopant from an interstitial position to a substitutional lattice position and reduce damage or defects in the lattice of the semiconductor body.
[0036] refer to Figure 1 , FIG. 16A to FIG. 19A and FIG. 16B to FIG. 19B The method 100 includes block 124, where further processing is performed. Such further processing may include, for example, depositing a contact etch stop layer (CESL) 244 (e.g., Fig.16A and Fig. 16B ), an interlayer dielectric (ILD) layer 246 is deposited over the CESL 244 (as shown in Fig.16A and Fig. 16B ), removing the dummy gate stack 220 (as shown in Fig.17A and Fig. 17B ), the sacrificial layer 206 in the channel region 212C is selectively removed to release the channel layer 208 as a channel member 2080 (as shown in Fig.18A and Fig.18B ), and forming a gate structure 252 (as shown in Fig.19A and Fig.19B ). Now refer to Fig.16A and Fig. 16B , a CESL 244 is formed before forming the ILD layer 246. In some instances, the CESL 244 includes silicon nitride, silicon oxynitride, and / or other materials known in the art. The CESL 244 may be formed by an ALD, a plasma enhanced chemical vapor deposition (PECVD) process, and / or other suitable deposition processes. The ILD layer 246 is then deposited over the CESL 244. In some embodiments, the ILD layer 246 includes a material such as tetraethyl orthosilicate (TEOS) oxide, undoped silicate glass, or doped silicon oxide, such as borophosphosilicate glass (BPSG), fused silica glass (FSG), phosphosilicate glass (PSG), boron-doped silica glass (BSG), and / or other suitable dielectric materials. The ILD layer 246 may be deposited by a PECVD process or other suitable deposition techniques. In some embodiments, after forming the ILD layer 246, the workpiece 200 may be annealed to improve the integrity of the ILD layer 246. Fig.16A As shown in FIG. 2 , the CESL 244 may be disposed directly on the top surface of the third epitaxial layer 240 .
[0037] Still reference Fig.16A and Fig. 16B After depositing the CESL 244 and the ILD layer 246, the workpiece 200 may be planarized by a planarization process to expose the dummy gate stack 220. For example, the planarization process may include a chemical mechanical planarization (CMP) process. The exposure of the dummy gate stack 220 allows the dummy gate stack 220 to be removed and the channel layer 208 to be released. Fig.17A and Fig. 17B . In some embodiments, removing the dummy gate stack 220 creates a gate trench 248 above the channel region 212C. Removing the dummy gate stack 220 may include one or more etching processes that are selective to the material of the dummy gate stack 220. For example, the removal of the dummy gate stack 220 may be performed using a selective wet etch, a selective dry etch, or a combination thereof that is selective to the dummy gate stack 220. After removing the dummy gate stack 220, the sidewalls of the channel layer 208 and the sacrificial layer 206 located in the channel region 212C are exposed in the gate trench 248.
[0038] refer to Fig.17A , Fig. 17B , Fig.18A and Fig.18B After removing the dummy gate stack 220, the method 100 may include an operation of selectively removing the sacrificial layer 206 between the channel layers 208 in the channel region 212C. Selectively removing the sacrificial layer 206 releases Fig.17A and Fig. 17B The channel layer 208 in the Fig.18A and Fig.18B 2080 shown in . The selective removal of sacrificial layer 206 also leaves a space 250 between channel members 2080. The selective removal of sacrificial layer 206 can be achieved by selective dry etching, selective wet etching or other selective etching processes. Example selective dry etching processes can include using one or more fluorine-based etchants, such as fluorine gas or hydrofluorocarbons. Example selective wet etching processes can include APM etching (e.g., a mixture of ammonium hydroxide-hydrogen peroxide-water).
[0039] refer to Fig.19A and Fig.19B, the method 100 may include further operations to form a gate structure 252 to wrap each of the channel members 2080. In some embodiments, the gate structure 252 is formed within the gate trench 248 and into the space 250 left by removing the sacrificial layer 206. In this regard, the gate structure 252 wraps each of the channel members 2080. The gate structure 252 includes a gate dielectric layer 254 and a gate electrode layer 256 above the gate dielectric layer 254. In some embodiments, although not explicitly shown in the figure, the gate dielectric layer 254 includes an interface layer and a high-K gate dielectric layer. High-K dielectric materials as used and described herein include dielectric materials with high dielectric constants, such as dielectric constants greater than thermal silicon oxide (~3.9). The interface layer may include a dielectric material, such as silicon oxide, hafnium silicate, or silicon oxynitride. The interface layer may be formed by chemical oxidation, thermal oxidation, atomic layer deposition (ALD), chemical vapor deposition (CVD), and / or other suitable methods. The high-K gate dielectric layer may include hafnium oxide. Alternatively, the high-K gate dielectric layer may include other high-K dielectric materials, such as titanium oxide (TiO2), hafnium zirconium oxide (HfZrO), tantalum oxide (Ta2O5), hafnium silicon oxide (HfSiO4), zirconium dioxide (ZrO2), zirconium oxide silicon (ZrSiO2), lanthanum oxide (La2O3), aluminum oxide (Al2O3), zirconium oxide (ZrO), yttrium oxide (Y2O3), SrTiO3 (STO), BaTiO3 (BTO), BaZrO, hafnium lanthanum oxide (HfLaO), lanthanum silicon oxide (LaSiO), aluminum silicon oxide (AlSiO), hafnium tantalum oxide (HfTaO), hafnium titanium oxide (HfTiO), (Ba, Sr)TiO3 (BST), silicon nitride (SiN), silicon oxynitride (SiON), combinations thereof, or other suitable materials. The high-K gate dielectric layer may be formed by ALD, physical vapor deposition (PVD), CVD, oxidation, and / or other suitable methods.
[0040] The gate electrode layer 256 of the gate structure 252 may include a single layer or optionally include a multilayer structure, such as a metal layer (work function metal layer) having a selected work function to enhance device performance, a liner layer, a wetting layer, an adhesion layer, a metal alloy or various combinations of metal silicides. As an example, the gate electrode layer 256 may include titanium nitride (TiN), titanium aluminum (TiAl), titanium aluminum nitride (TiAlN), tantalum nitride (TaN), tantalum aluminum (TaAl), tantalum aluminum nitride (TaAlN), tantalum aluminum carbide (TaAlC), tantalum carbonitride (TaCN), aluminum (Al), tungsten (W), nickel (Ni), titanium (Ti), ruthenium (Ru), cobalt (Co), platinum (Pt), tantalum carbide (TaC), tantalum silicon nitride (TaSiN), copper (Cu), other refractory metals or other suitable metal materials or combinations thereof. In various embodiments, the gate electrode layer 256 may be formed by ALD, PVD, CVD, electron beam evaporation or other suitable processes. In various embodiments, a CMP process may be performed to remove excess metal, thereby providing a substantially planar top surface of the gate structure 252. The gate structure 252 includes a portion between the channel members 2080 in the channel region 212C.
[0041] refer to Fig.19A and Fig.19B At the end of the operations in block 124, transistor 260 is substantially formed. Transistor 260 includes channel members 2080 vertically stacked in the Z direction. Each of channel members 2080 is wrapped by gate structure 252. Channel members 2080 extend in the X direction or are sandwiched between two source / drain features 242. Each of source / drain features 242 includes a first epitaxial layer 236 (or Fig.19B 236 ), a second epitaxial layer 238 in contact with the first epitaxial layer 236 , and a third epitaxial layer 240 (if formed). The second epitaxial layer 238 is spaced apart from the channel member 2080 by the first epitaxial layer 236 (or the optional first epitaxial layer 2360 ).
[0042] Although not intended to be limiting, one or more embodiments of the present invention provide many benefits for semiconductor devices and their formation. For example, embodiments of the present invention provide a transistor including a vertical stack of channel components extending between two source / drain components. Each of the source / drain components includes a first epitaxial layer, a second epitaxial layer above the first epitaxial layer, and a third epitaxial layer above the second epitaxial layer. The first epitaxial layer engages the channel component and serves as a transition layer between the channel component and the second epitaxial layer. The volume or thickness of the first epitaxial layer is just enough to cover the rounded end of the channel layer. By minimizing the volume or thickness of the first epitaxial layer, the volume or thickness of the second epitaxial layer can be maximized. Compared with the first epitaxial layer, the second epitaxial layer has a greater germanium content to exert stress on the channel component and has a greater dopant concentration to reduce resistance. The third epitaxial layer has a lower germanium content than the second epitaxial layer to serve as a sacrificial layer when forming a source / drain contact opening. Embodiments of the present invention reduce parasitic resistance in the source / drain component.
[0043] In one exemplary aspect, the present invention relates to a semiconductor device. The semiconductor device includes: a plurality of channel components disposed above a substrate; a plurality of internal spacer components interlaced with the plurality of channel components; a gate structure wrapping each of the plurality of channel components; and a source / drain component. The source / drain component includes: a first epitaxial layer in contact with the substrate and the plurality of channel components; and a second epitaxial layer in contact with the first epitaxial layer and the plurality of internal spacer components. The first epitaxial layer and the second epitaxial layer include silicon germanium. The germanium content of the second epitaxial layer is greater than the germanium content of the first epitaxial layer.
[0044] In some embodiments, the germanium content of the first epitaxial layer is between about 20% and about 30%, and the germanium content of the second epitaxial layer is between about 50% and about 60%. In some embodiments, the first epitaxial layer and the second epitaxial layer are doped with boron (B), and the boron doping concentration of the second epitaxial layer is greater than the boron doping concentration of the first epitaxial layer. In some cases, the semiconductor device may further include a third epitaxial layer disposed above the second epitaxial layer. The third epitaxial layer includes silicon germanium, and the germanium content of the third epitaxial layer is less than the germanium content of the second epitaxial layer. In some embodiments, the germanium content of the third epitaxial layer is less than the germanium content of the first epitaxial layer. In some cases, the first epitaxial layer includes a substrate portion in contact with the substrate, and the substrate portion completely covers the bottommost inner spacer component of the plurality of inner spacer components. In some embodiments, each of the plurality of channel components includes a rounded end. The substrate portion of the first epitaxial layer completely covers the rounded end of the bottommost channel component of the plurality of channel components. In some cases, the plurality of inner spacer components are in contact with the second epitaxial layer except for the bottommost inner spacer component.
[0045] In another exemplary aspect, the present invention relates to a semiconductor device. The semiconductor device includes: a plurality of silicon channel members disposed above a substrate; a plurality of dielectric internal spacer members interlaced with the plurality of silicon channel members, each of the plurality of silicon channel members including a rounded end; a gate structure wrapping each of the plurality of silicon channel members; and a source / drain member. The source / drain member includes: a first epitaxial layer in contact with the substrate and the rounded ends of the plurality of silicon channel members, and a second epitaxial layer in contact with the first epitaxial layer and the plurality of dielectric internal spacer members. The first epitaxial layer and the second epitaxial layer include silicon germanium. The germanium content of the first epitaxial layer is between about 20% and about 30%, and the germanium content of the second epitaxial layer is between about 50% and about 60%.
[0046] In some embodiments, the first epitaxial layer and the second epitaxial layer are doped with boron (B), and the boron doping concentration of the second epitaxial layer is greater than the boron doping concentration of the first epitaxial layer. In some embodiments, the semiconductor device may further include a third epitaxial layer disposed above the second epitaxial layer. The third epitaxial layer includes silicon germanium, and the germanium content of the third epitaxial layer is between about 15% and about 20%. In some cases, the first epitaxial layer includes a substrate portion in contact with the substrate and a channel sidewall portion in contact with a plurality of silicon channel components, and the substrate portion completely covers the bottommost dielectric internal spacer component of the plurality of dielectric internal spacer components. In some embodiments, the channel sidewall portion of the first epitaxial layer is wrapped over the circular ends of the plurality of silicon channel components. In some embodiments, the channel sidewall portion of the first epitaxial layer includes a curved shape. In some cases, in addition to the bottommost dielectric internal spacer component, the plurality of dielectric internal spacer components are in contact with the second epitaxial layer.
[0047] In yet another exemplary aspect, the invention relates to a method. The method includes: forming a stack above a substrate, wherein the stack includes multiple silicon layers interlaced with multiple silicon germanium layers; forming a fin structure from the stack and the substrate, the fin structure including a channel region and a source / drain region; forming a dummy gate stack above the channel region of the fin structure; depositing a gate spacer layer above the dummy gate stack; recessing the source / drain region to form a source / drain trench that exposes the sidewalls of the multiple silicon layers and the multiple silicon germanium layers; selectively and partially recessing the multiple silicon germanium layers to form multiple internal spacer grooves; forming multiple internal spacer components in the multiple internal spacer grooves; depositing a first epitaxial layer in the source / drain trench, the first epitaxial layer contacting the multiple silicon layers; depositing a second epitaxial layer above the first epitaxial layer, the second epitaxial layer contacting the multiple internal spacer components and the first epitaxial layer; depositing a third epitaxial layer on the second epitaxial layer; after depositing the third epitaxial layer, removing the dummy gate stack; releasing the multiple silicon layers in the channel region as multiple channel components; and forming a gate structure around each of the multiple channel components. The first epitaxial layer and the second epitaxial layer include silicon germanium, and a germanium content of the second epitaxial layer is greater than a germanium content of the first epitaxial layer.
[0048] In some embodiments, the method may further include: performing a cleaning process to trim the plurality of silicon layers after forming the plurality of internal spacer components and before depositing the first epitaxial layer. In some embodiments, the first epitaxial layer has a germanium content between about 20% and about 30%, and the second epitaxial layer has a germanium content between about 50% and about 60%. In some embodiments, the third epitaxial layer includes silicon germanium, and the germanium content of the third epitaxial layer is less than the germanium content of the second epitaxial layer. In some cases, the first epitaxial layer includes a substrate portion in contact with the substrate, and the substrate portion completely covers the bottommost internal spacer component of the plurality of internal spacer components.
[0049] The features of several embodiments are summarized above so that those of ordinary skill in the art can better understand aspects of the present invention. Those of ordinary skill in the art should understand that they can easily use the present invention as a basis to design or modify other processes and structures for implementing the same purpose and / or achieving the same advantages as the embodiments introduced herein. Those of ordinary skill in the art should also be aware that such equivalent constructions do not deviate from the spirit and scope of the present invention, and that they can make various changes, substitutions and modifications herein without departing from the spirit and scope of the present invention.
Claims
1. A semiconductor device, comprising: a plurality of channel members disposed above the substrate; a plurality of internal spacer components interleaved with the plurality of channel members, each of the plurality of channel members including a convex rounded end; a gate structure wrapping each of the plurality of channel members; as well as Source / drain components, including: a first epitaxial layer in contact with the substrate and the circular ends of the plurality of channel members, and a second epitaxial layer in contact with the first epitaxial layer and the plurality of inner spacer features, Wherein, the first epitaxial layer and the second epitaxial layer include silicon germanium, The germanium content of the second epitaxial layer is greater than the germanium content of the first epitaxial layer.
2. The semiconductor device according to claim 1, in, The germanium content of the first epitaxial layer is between 20% and 30%, The germanium content of the second epitaxial layer is between 50% and 60%.
3. The semiconductor device according to claim 1, in, The first epitaxial layer and the second epitaxial layer are doped with boron (B), The boron doping concentration of the second epitaxial layer is greater than the boron doping concentration of the first epitaxial layer.
4. The semiconductor device according to claim 1, further comprising: a third epitaxial layer, disposed above the second epitaxial layer, Wherein, the third epitaxial layer comprises silicon germanium, The germanium content of the third epitaxial layer is less than the germanium content of the second epitaxial layer.
5. The semiconductor device according to claim 4, wherein: The germanium content of the third epitaxial layer is less than the germanium content of the first epitaxial layer.
6. The semiconductor device according to claim 1, in, The first epitaxial layer includes a substrate portion in contact with the substrate, wherein the substrate portion completely covers a bottommost inner spacer component of the plurality of inner spacer components.
7. The semiconductor device according to claim 6, in, The substrate portion of the first epitaxial layer completely covers the rounded end of a bottommost channel member of the plurality of channel members.
8. The semiconductor device according to claim 6, wherein: The plurality of inner spacer features are in contact with the second epitaxial layer except for the bottommost inner spacer feature.
9. A semiconductor device comprising: a plurality of silicon channel members disposed above the substrate; a plurality of dielectric inner spacer features interleaved with the plurality of silicon channel members, each of the plurality of silicon channel members including a convex rounded end; a gate structure surrounding each of the plurality of silicon channel members; as well as Source / drain components, including: a first epitaxial layer in contact with the substrate and the rounded ends of the plurality of silicon channel members, and a second epitaxial layer in contact with the first epitaxial layer and the plurality of dielectric inner spacer features, Wherein, the first epitaxial layer and the second epitaxial layer include silicon germanium, Wherein, the germanium content of the first epitaxial layer is between 20% and 30%, The germanium content of the second epitaxial layer is between 50% and 60%.
10. The semiconductor device according to claim 9, in, The first epitaxial layer and the second epitaxial layer are doped with boron (B), The boron doping concentration of the second epitaxial layer is greater than the boron doping concentration of the first epitaxial layer.
11. The semiconductor device according to claim 9, further comprising: a third epitaxial layer, disposed above the second epitaxial layer, Wherein, the third epitaxial layer comprises silicon germanium, Wherein, the germanium content of the third epitaxial layer is between 15% and 20%.
12. The semiconductor device according to claim 9, in, The first epitaxial layer includes a substrate portion in contact with the substrate and a channel sidewall portion in contact with the plurality of silicon channel members, wherein the substrate portion completely covers a bottommost dielectric inner spacer component of the plurality of dielectric inner spacer components.
13. The semiconductor device according to claim 12, in, The channel sidewall portions of the first epitaxial layer wrap over the rounded ends of the plurality of silicon channel members.
14. The semiconductor device according to claim 12, in, The channel sidewall portion of the first epitaxial layer includes a curved shape.
15. The semiconductor device according to claim 12, in, The plurality of dielectric inner spacer features are in contact with the second epitaxial layer except for the bottommost dielectric inner spacer feature.
16. A method of forming a semiconductor device, comprising: forming a stack over a substrate, wherein the stack includes a plurality of silicon layers interleaved with a plurality of silicon germanium layers; forming a fin structure by the stack and the substrate, the fin structure comprising a channel region and a source / drain region; forming a dummy gate stack over the channel region of the fin structure; depositing a gate spacer layer over the dummy gate stack; recessing the source / drain regions to form source / drain trenches exposing sidewalls of the plurality of silicon layers and the plurality of silicon germanium layers; selectively and partially recessing the plurality of silicon germanium layers to form a plurality of inner spacer recesses and forming each of the plurality of silicon layers with a convex rounded end; forming a plurality of inner spacer members in the plurality of inner spacer grooves; depositing a first epitaxial layer in the source / drain trench, the first epitaxial layer contacting the plurality of silicon layers and the rounded ends of the plurality of silicon layers; depositing a second epitaxial layer over the first epitaxial layer, the second epitaxial layer contacting the plurality of inner spacer features and the first epitaxial layer; depositing a third epitaxial layer on the second epitaxial layer; After depositing the third epitaxial layer, removing the dummy gate stack; releasing the plurality of silicon layers in the channel region as a plurality of channel members; and forming a gate structure around each of the plurality of channel members, Wherein, the first epitaxial layer and the second epitaxial layer include silicon germanium, The germanium content of the second epitaxial layer is greater than the germanium content of the first epitaxial layer.
17. The method according to claim 16, further comprising: After forming the plurality of inner spacer features and before depositing the first epitaxial layer, a cleaning process is performed to trim the plurality of silicon layers.
18. The method according to claim 16, in, The germanium content of the first epitaxial layer is between 20% and 30%, The germanium content of the second epitaxial layer is between 50% and 60%.
19. The method according to claim 16, in, The third epitaxial layer includes silicon germanium, The germanium content of the third epitaxial layer is less than the germanium content of the second epitaxial layer.
20. The method according to claim 16, wherein: The first epitaxial layer includes a substrate portion in contact with the substrate, wherein the substrate portion completely covers a bottommost inner spacer component of the plurality of inner spacer components.