Light emitting element and method for manufacturing the same
Patent Information
- Application Number
- CN202110648357.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-10
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-06-10
Smart Images

Figure CN113823722B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a light emitting element and a method for manufacturing the same. Background Art
[0002] Conventionally, there is a known technique for using a degenerately doped gallium nitride layer in a tunnel junction of a light emitting diode (LED) (for example, see Patent Document 1). The above-mentioned "degenerately doped" is considered to mean that the Fermi level and the conduction band overlap (degenerate) by doping with a high concentration of a dopant. Semiconductors with degenerate Fermi level and conduction band generally behave like metals, and have reduced resistance.
[0003] In addition, in the past, there is a known light-emitting element using p-type GaN as the material of the contact layer connected to the electrode on the p-side (see Patent Document 2). According to Patent Document 1, a p-type GaN layer or a p-type AlGaN layer can be used in the contact layer connected to the electrode on the p-side, but in order to improve the contact with the electrode on the p-side, it is preferred to use a p-type GaN layer.
[0004] In addition, a light-emitting element using a tunnel junction is known in the past (see Patent Document 3). In the light-emitting element described in Patent Document 1, a tunnel junction is formed between a p-type GaN layer and an n-type InGaN layer on the light-emitting layer, and the n-type InGaN layer is used as a p-side contact layer to connect the p-side electrode. Therefore, both the p-side contact layer and the n-side contact layer can use an n-type semiconductor, so that the n-side electrode and the p-side electrode can be formed from the same material.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent No. 5726405
[0008] Patent Document 2: Japanese Patent Application Publication No. 2019-110195
[0009] Patent Document 3: Japanese Patent No. 3786898 Summary of the invention
[0010] However, in n-type AlGaN using Si as a dopant, if the Si concentration is increased, the resistance will decrease like a general semiconductor until a certain concentration, but if the concentration exceeds a certain concentration, the resistance will start to increase. It is believed that this is because when the Si concentration exceeds a certain concentration, a compound defect of group III holes and Si is generated. Therefore, in the conventional method, even if the Si concentration is increased to degenerate the Fermi level and the conduction band, the resistance cannot be effectively reduced due to the compound defect of group III holes and Si.
[0011] Therefore, one of the objects of the present invention is to provide a light-emitting element and a method for manufacturing the same, wherein the light-emitting element has an n-type contact layer composed of AlGaN using Si as a dopant and has resistance effectively reduced by degeneration of the Fermi level and the conduction band.
[0012] In addition, since GaN or AlGaN with a low Al content absorbs deep ultraviolet light, if a contact layer composed of GaN or AlGaN with a low Al content is used in a deep ultraviolet light-emitting element, the light extraction efficiency is greatly reduced. Therefore, using the structure of the light-emitting element described in Patent Document 2, a deep ultraviolet light-emitting element with excellent light extraction efficiency cannot be obtained.
[0013] Therefore, another object of the present invention is to provide a light-emitting element that emits deep ultraviolet light, wherein the contact resistance between the electrode on the p-side and the contact layer of the light-emitting element is low and the absorption of light by the contact layer is suppressed.
[0014] In addition, GaN or InGaN strongly absorbs light in the deep ultraviolet region due to the size of their band gaps. Therefore, if the deep ultraviolet light-emitting element adopts the structure of the light-emitting element described in Patent Document 3, the p-type GaN layer or the n-type InGaN layer strongly absorbs the light emitted from the light-emitting layer, and the light extraction efficiency becomes low.
[0015] Therefore, another object of the present invention is to provide a light-emitting element emitting deep ultraviolet light using a tunnel junction, wherein the light-emitting element suppresses the absorption of light by an n-type layer and a p-type layer forming the tunnel junction.
[0016] In order to achieve the above object, one embodiment of the present invention provides the light-emitting elements of the following [1] to [4] and methods for producing the light-emitting elements of [5] and [6].
[0017] [1] A light-emitting element comprising: an n-type contact layer composed of AlGaN having a degenerate Fermi level and a conduction band, and a light-emitting layer composed of AlGaN stacked on the n-type contact layer, wherein the Al component of the n-type contact layer is greater than the Al component of the light-emitting layer by 10% or more and less than 70%, and the n-type contact layer contains a concentration of 4.0×10 19 cm -3 The following concentrations of Si.
[0018] [2] The light-emitting element according to [1] above, wherein the Al content of the n-type contact layer is 50% or more.
[0019] [3] The light-emitting element according to [1] or [2], wherein the concentration of Si contained in the n-type contact layer is 1.6×10 18 cm -3 above.
[0020] [4] The light-emitting element according to any one of [1] to [3], wherein the resistivity of the n-type contact layer is 5×10 -2 Ω·cm or less.
[0021] [5] A method for manufacturing a light-emitting element, comprising the following steps: forming an n-type contact layer composed of AlGaN with degenerate Fermi level and conduction band by vapor deposition, and forming a light-emitting layer composed of AlGaN on the n-type contact layer; the Al component of the n-type contact layer is greater than the Al component of the light-emitting layer by 10% or more and less than 70%, and the n-type contact layer contains a concentration of 4.0×10 19 cm -3 The Si concentration is below 1000 and the V / III ratio of the raw material gas of the n-type contact layer in the step of forming the n-type contact layer is in the range of 1000 to 3200.
[0022] [6] The method for manufacturing a light-emitting element according to [5] above, wherein a growth temperature of the n-type contact layer in the step of forming the n-type contact layer is 1150° C. or less.
[0023] In addition, another embodiment of the present invention provides the light-emitting elements of the following [7] to
[11] in order to achieve the above-mentioned object.
[0024] [7] A light-emitting element comprising: an n-type contact layer composed of n-type AlGaN, a light-emitting layer emitting deep ultraviolet light on the n-type contact layer, a current diffusion layer composed of AlGaN containing two-dimensional hole gas on the light-emitting layer, a p-type contact layer composed of p-type GaN or p-type AlGaN with an Al content of less than 35% connected to a portion of the upper surface of the current diffusion layer, an n-electrode connected to the n-type contact layer, and a p-electrode connected to the p-type contact layer.
[0025] [8] The light-emitting element according to [7] above, wherein the current diffusion layer comprises a first AlGaN layer composed of p-type AlGaN having an Al composition in the range of 50% to 70%, and a second AlGaN layer composed of p-type or i-type AlGaN having an Al composition in the range of 30% to 50% and provided directly on the first AlGaN layer,
[0026] The second AlGaN layer has the two-dimensional hole gas near the interface with the first AlGaN layer.
[0027] [9] The light-emitting element according to [7] or [8] above, wherein the area of the region of the upper surface of the current diffusion layer that contacts the p-type contact layer is in the range of 40% to 80% of the area of the entire region of the upper surface.
[0028]
[10] A light-emitting element according to any one of [7] to [9] above, wherein at least a portion of a region other than a region connected to the p-type contact layer on the upper surface of the current diffusion layer is covered by a passivation film made of an insulating material.
[0029]
[11] The light-emitting element according to any one of [7] to
[10] , wherein a light-reflecting layer is provided above a region of the upper surface of the current diffusion layer other than a region connected to the p-type contact layer.
[0030] In addition, another embodiment of the present invention provides the light-emitting elements of the following
[12] to
[16] in order to achieve the above-mentioned object.
[0031]
[12] A light-emitting element comprising: a first n-type contact layer composed of AlGaN, a light-emitting layer emitting deep ultraviolet light on the first n-type contact layer, a p-type layer composed of AlGaN on the light-emitting layer, a second n-type contact layer composed of AlGaN on the p-type layer, the second n-type contact layer forming a tunnel junction with the p-type layer and having a degenerate Fermi level and conduction band, an n-electrode connected to the first n-type contact layer, and a p-electrode connected to the second n-type contact layer; the Al content of the second n-type contact layer is in the range of 40% to 70%.
[0032]
[13] The light-emitting element according to
[12] above, wherein the p-type layer contains two-dimensional hole gas.
[0033]
[14] The light-emitting element according to
[12] or
[13] , wherein the n-type contact layer contains a concentration of 4.0×10 19 cm -3 The following concentrations of Si.
[0034]
[15] A light-emitting element according to any one of
[12] to
[14] above, wherein a portion of the n-electrode in contact with the first n-type contact layer and a portion of the p-electrode in contact with the second n-type contact layer are made of the same material.
[0035]
[16] The light-emitting element according to
[15] above, wherein the material is aluminum.
[0036] According to the present invention, a light emitting element having an n-type contact layer made of AlGaN using Si as a dopant and having resistance effectively reduced by degeneration of the Fermi level and the conduction band, and a method for manufacturing the same can be provided.
[0037] Furthermore, according to the present invention, a light-emitting element emitting deep ultraviolet light can be provided, in which the contact resistance between the p-side electrode and the contact layer is low and the absorption of light by the contact layer is suppressed.
[0038] In addition, according to the present invention, a light-emitting element emitting deep ultraviolet light using a tunnel junction can be provided, in which the absorption of light by an n-type layer and a p-type layer forming the tunnel junction is suppressed. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a vertical cross-sectional view of the light emitting element according to the first embodiment of the present invention.
[0040] Figure 2 It is a vertical cross-sectional view of a light emitting element according to a second embodiment of the present invention.
[0041] Figure 3 It is a vertical cross-sectional view of a modification of the light emitting element according to the second embodiment of the present invention.
[0042] Figure 4 It is a vertical cross-sectional view of a light emitting device including a light emitting element according to a second embodiment of the present invention as a light source.
[0043] Figure 5 It is a vertical cross-sectional view of a light emitting element according to a third embodiment of the present invention.
[0044] Figure 6 This is a graph showing the relationship between the Al composition and the resistivity of the n-type contact layer.
[0045] Figure 7 (a) to (c) are graphs showing the relationship between the Si concentration and the resistivity of the n-type contact layer.
[0046] Figure 8 (a) to (c) are graphs showing the temperature dependence of the resistivity, carrier concentration, and mobility of the n-type contact layer.
[0047] Fig. 9 This is a graph showing the relationship between the V / III ratio of the raw material gas of the n-type contact layer and the resistivity.
[0048] Fig.10 This is a graph showing the relationship between the growth temperature and resistivity of the n-type contact layer.
[0049] Fig.11 (a) to (c) show spectra of various n-type contact layers obtained by cathode luminescence measurement.
[0050] Fig.12 This is a graph showing the relationship between the Al component of the n-type contact layer and the transmittance of deep ultraviolet light with a wavelength of 280 nm.
[0051] Fig.13 This is a graph showing the relationship between the Al composition and the resistivity of the n-type contact layer.
[0052] Fig.14 (a) to (c) are graphs showing the relationship between the Si concentration and the resistivity of the n-type contact layer.
[0053] Fig.15 (a) to (c) are graphs showing the temperature dependence of the resistivity, carrier concentration, and mobility of the n-type contact layer.
[0054] Fig.16 Shown are spectra (CL spectra) obtained by cathode luminescence measurement of various n-type contact layers.
[0055] Explanation of symbols
[0056] 1 Light-emitting element
[0057] 10 substrate
[0058] 11 Buffer layer
[0059] 12 n-type contact layer
[0060] 13. Luminescent layer
[0061] 14 Electron blocking layer
[0062] 15 p-type contact layer
[0063] 16 Transparent Electrode
[0064] 17 p electrode
[0065] 18 n electrode
[0066] 101, 102 Light-emitting element
[0067] 110 substrate
[0068] 111 Buffer layer
[0069] 112 n-type contact layer
[0070] 113 Luminous layer
[0071] 114 Current diffusion layer
[0072] 1141 First AlGaN layer
[0073] 1142 Second AlGaN layer
[0074] 1143 Upper surface
[0075] 1144 Two-dimensional cavitation gas
[0076] 115 p-type contact layer
[0077] 116 p electrode
[0078] 117 n electrode
[0079] 118 Passivation film
[0080] 119 Reflective layer
[0081] 211 Light-emitting element
[0082] 210 substrate
[0083] 211 Buffer layer
[0084] 212 n-type contact layer
[0085] 213 Luminous Layer
[0086] 214 Electron blocking layer
[0087] 215 p-type layer
[0088] 216 n-type contact layer
[0089] 217 p electrode
[0090] 218 n electrode DETAILED DESCRIPTION
[0091] [First embodiment]
[0092] (Constitution of Light Emitting Element)
[0093] Figure 1 1 is a vertical cross-sectional view of a light-emitting element 1 according to a first embodiment of the present invention. The light-emitting element 1 is a flip-chip mounted light-emitting diode (LED), and includes a substrate 10, a buffer layer 11 on the substrate 10, an n-type contact layer 12 on the buffer layer 11, a light-emitting layer 13 on the n-type contact layer 12, an electron blocking layer 14 on the light-emitting layer 13, a p-type contact layer 15 on the electron blocking layer 14, a transparent electrode 16 on the p-type contact layer 15, a p-electrode 17 connected to the transparent electrode 16, and an n-electrode 18 connected to the n-type contact layer 12.
[0094] It should be noted that the "upper" in the structure of the light emitting element 1 refers to the Figure 1 When the light emitting element 1 is placed in the direction shown, “upper” is the direction from the substrate 10 to the p-electrode 17 .
[0095] The substrate 10 is a growth substrate made of sapphire. The thickness of the substrate 10 is, for example, 900 μm. As a material for the substrate 10 , in addition to sapphire, AlN, Si, SiC, ZnO, etc. may be used.
[0096] The buffer layer 11 has, for example, a structure in which three layers, namely a core layer, a low-temperature buffer layer, and a high-temperature buffer layer, are stacked in sequence. The core layer is composed of undoped AlN grown at a low temperature, and is a layer that serves as a core for crystal growth. The thickness of the core layer is, for example, 10 nm. The low-temperature buffer layer is a layer composed of undoped AlN grown at a higher temperature than the core layer. The thickness of the low-temperature buffer layer is, for example, 0.3 μm. The high-temperature buffer layer is a layer composed of undoped AlN grown at a higher temperature than the low-temperature buffer layer. The thickness of the high-temperature buffer layer is, for example, 2.7 μm. By providing such a buffer layer 11, the density of threading dislocations of AlN is reduced.
[0097] The light emitting layer 13 is a layer stacked on the n-type contact layer 12. The light emitting layer 13 is composed of AlGaN, preferably having a multi-quantum well (MQW) structure. The Al component of the light emitting layer 13 (the Al component of the well layer when having the MQW structure) can be set according to the desired emission wavelength, for example, when the emission wavelength is about 280nm, it is set to 35-45%. Here, the percentage of the Al component is the ratio of the Al content to the total value of the Ga content and the Al content.
[0098] For example, the light emitting layer 13 has an MQW structure with two well layers, that is, a structure in which a first barrier layer, a first well layer, a second barrier layer, a second well layer, and a third barrier layer are stacked in this order. The first well layer and the second well layer are composed of n-type AlGaN. The first barrier layer, the second barrier layer, and the third barrier layer are composed of n-type AlGaN (including a material with an Al component of 100%, i.e., AlN) having a higher Al content than the first well layer and the second well layer.
[0099] As an example, the Al composition, thickness, and concentration of Si as a dopant in the first well layer and the second well layer are 40%, 2.4 nm, and 9×10 18 / cm 3 In addition, the Al composition, thickness, and Si concentration as a dopant of the first and second barrier layers are 55%, 19 nm, and 9×10 18 / cm 3 The Al composition, thickness, and Si concentration of the third barrier layer are 55%, 4 nm, and 5×10 18 / cm 3 .
[0100] The n-type contact layer 12 is composed of n-type AlGaN. The lower limit of the Al component of the n-type contact layer 12 is set to the lower limit of the range that can suppress the absorption of light emitted from the light-emitting layer 13. If the Al component of the n-type contact layer 12 is 10% or more greater than the Al component of the AlGaN constituting the light-emitting layer 13 (the Al component of the well layer when the light-emitting layer 13 has an MQW structure), it is possible to effectively suppress the light emitted from the light-emitting layer 13 from being absorbed by the n-type contact layer 12. If it is 15% or more greater, it can be suppressed more effectively. Therefore, it is preferred that the Al component of the n-type contact layer 12 is 10% or more greater than the Al component of the light-emitting layer 13, and more preferably 15% or more greater.
[0101] For example, when the Al content of the light emitting layer 13 is 35-45%, light having a wavelength of about 280 nm is emitted. If the Al content of the n-type contact layer 12 is 50% or more, absorption can be effectively suppressed, and if it is 55% or more, absorption can be suppressed more effectively.
[0102] In addition, the upper limit of the Al component of the n-type contact layer 12 is set to an upper limit of the range that can suppress the increase in resistance caused by the increase in the Al component. When the Al component is increased, the resistance of AlGaN is almost constant below 70%, but starts to increase if it exceeds 70%. Therefore, the Al component of the n-type contact layer 12 is set to be 70% or less.
[0103] Therefore, as a preferred example when the light emitting element 1 is an ultraviolet light emitting element, the Al component of the n-type contact layer 12 is in the range of 50% to 70%. In this case, it is desirable that the n-type contact layer 12 has Al x Ga 1-x The composition represented by N (0.5≤x≤0.7).
[0104] In addition, the n-type contact layer 12 contains Si at a concentration that makes the Fermi level and the conduction band degenerate. According to the non-patent document "A. Wolos et al., "Properties of metal-insulator transition and electron spinrelaxation in GaN:Si", PHYSICAL REVIEW B 83, 165206 (2011)", it is said that in GaN containing Si as a dopant, the Si concentration is 1.6×10 18 cm -3 At the above time, the Fermi level and the conduction band are degenerate. Since AlGaN is considered to exhibit almost the same behavior as GaN, it is considered that in the n-type contact layer 12, when the Si concentration is about 1.6×10 18 cm -3 Above this value, the Fermi level will also become degenerate with the conduction band.
[0105] In order to suppress the increase in resistance due to the increase in Si concentration, the concentration of Si contained in the n-type contact layer 12 was set to 4.0×10 19 cm -3 As described above, in AlGaN containing a high concentration of Si, although the Fermi level and the conduction band are usually degenerate, the resistance cannot be effectively reduced due to the influence of the compound defects of the III-group holes and Si. However, when the n-type contact layer 12 is formed under the conditions of the V / III ratio of the raw material gas involved in the present embodiment described later, if the Si concentration is 4.0×10 19 cm -3 Then, it is possible to suppress the increase in resistance which is considered to be caused by the influence of the complex defects of the group III holes and Si.
[0106] The details of the complex defects of group III holes and Si are not yet clear, but there is a theory that when Si does not enter the group III holes generated during the growth of AlGaN and remains in other locations, Si cannot function as a donor (releasing electrons) and releases 1 to 3 holes depending on its state, thereby increasing resistance.
[0107] According to the present embodiment, for example, by setting the Si concentration of the n-type contact layer 12 to 5×10 18 cm -3 ~4×10 19 cm -3 The growth temperature of the n-type contact layer 12 is set in the range of 850°C to 1100°C, and the V / III ratio of the raw material gas of the n-type contact layer 12 described later is set in the range of 1000 to 3200, so that the resistivity of the n-type contact layer 12 can be 5×10 -2 Ω·cm or less. In addition, it is considered that the lower limit of the resistivity of the n-type contact layer 12 under the conditions of the Si concentration of the n-type contact layer 12, the growth temperature, and the V / III ratio of the raw material gas is 1×10 -3 The thickness of the n-type contact layer 12 is, for example, 500 to 3000 nm.
[0108] The electron blocking layer 14 is composed of p-type AlGaN having a higher Al content than the third barrier layer. The electron blocking layer 14 suppresses the diffusion of electrons to the p-type contact layer 15. The Al content, thickness, and Mg concentration of the electron blocking layer 14 as a dopant are, for example, 80%, 25 nm, and 5×10 19 / cm 3 .
[0109] The p-type contact layer 15 has a structure in which a first p-type contact layer and a second p-type contact layer are stacked in this order. The first p-type contact layer and the second p-type contact layer are made of p-type GaN. The thickness of the first p-type contact layer and the concentration of Mg as a dopant are, for example, 700 nm and 2×10 19 / cm 3 The thickness of the second p-type contact layer and the concentration of Mg as a dopant are, for example, 60 nm and 1×10 20 / cm 3 .
[0110] A groove is provided in a part of the surface of the p-type contact layer 15. The groove penetrates the p-type contact layer 15 and the light emitting layer 13 and reaches the n-type contact layer 12. The n-electrode 18 is connected to the exposed surface of the n-type contact layer 12 by the groove.
[0111] The transparent electrode 16 is made of, for example, a conductive oxide transparent to visible light, such as IZO, ITO, ICO, or ZnO. It should be noted that when the light emitted from the light-emitting layer 13 is ultraviolet light (light below 365 nm), much of it is absorbed by the p-type contact layer 15 made of GaN, does not pass through the transparent electrode 16, and does not reflect light at the p-electrode 17. However, in the case of using a p-type contact layer 15 made of GaN as a thin film or a p-type contact layer 15 made of AlGaN, and in the case of using a transparent electrode 16 as a thin film or a transparent electrode 16 made of a material transparent to ultraviolet light, their absorption of ultraviolet light can be suppressed, so that light output can be greatly improved. The p-electrode 17 is made of, for example, Ni / Au. The n-electrode 18 is made of, for example, Ti / Al / Ni, V / Al / Ni, V / Al / Ru, etc.
[0112] The light emitting element 1 may be a face-mounted type. In addition, the characteristic configuration of the n-type contact layer 12 and the like of the light emitting element 1 may also be applied to light emitting elements other than LEDs such as laser diodes.
[0113] (Method for manufacturing light emitting element)
[0114] An example of a method for manufacturing the light-emitting element 1 involved in the first embodiment of the present invention is described below. In each layer of the light-emitting element 1 formed by vapor deposition, as Ga raw material gas, Al raw material gas, and N raw material gas, for example, trimethylgallium, trimethylaluminum, and ammonia are used respectively. In addition, as the raw material gas of Si belonging to the n-type dopant and the raw material gas of Mg belonging to the p-type dopant, for example, silane gas and bis(cyclopentadienyl)magnesium gas are used respectively. In addition, as the carrier gas, for example, hydrogen gas and nitrogen gas are used. In addition, the growth temperature of each layer in this embodiment is the temperature of the heating heater of the film forming device, and the surface temperature of the substrate 10 is about 100°C lower than the temperature of the heating heater.
[0115] First, a substrate 10 is prepared, and a buffer layer 11 is formed thereon. In forming the buffer layer 11, first, a core layer composed of AlN is formed by sputtering. The growth temperature is, for example, 880°C. Next, a low-temperature buffer layer and a high-temperature buffer layer composed of AlN are sequentially formed on the core layer by MOCVD. The growth conditions of the low-temperature buffer layer are, for example, a growth temperature of 1090°C and a growth pressure of 50 mbar. In addition, the growth conditions of the high-temperature buffer layer are, for example, a growth temperature of 1270°C and a growth pressure of 50 mbar.
[0116] Next, an n-type contact layer 12 composed of AlGaN containing Si is formed on the buffer layer 11 by MOCVD. In forming the n-type contact layer 12, in order to reduce the resistance of the n-type contact layer 12, the V / III ratio of the raw material gas of the n-type contact layer 12 is set in the range of 1000 to 3200. Here, the V / III ratio refers to the ratio of the number of atoms of the III group element (Ga, Al) and the V group element (N) in the raw material gas.
[0117] In addition, in the formation of the n-type contact layer 12, the growth temperature of the n-type contact layer 12 is preferably set to 1150° C. or less. By setting the growth temperature to 1150° C. or less, the increase in resistance caused by the increase in growth temperature can be suppressed. This is believed to be because the evaporation of the group III elements, especially Ga, which is easy to evaporate, can be suppressed, and the excessive generation of group III holes can be suppressed, thereby suppressing the increase in resistance caused by the influence of the composite defects of group III holes and Si.
[0118] In addition, in the formation of the n-type contact layer 12, it is preferred to set the growth temperature of the n-type contact layer 12 to 850° C. or higher. When the growth temperature is lower than 850° C., since ammonia, which is a raw material of the group V element N, is difficult to decompose, the supply amount of ammonia must be increased, and the V / III ratio must be set to an abnormally high value. In addition, when the growth temperature is low, there is a problem of C mixing from the group III raw material, so it is preferred to set the growth temperature to a temperature that can avoid this problem, for example, 850° C. or higher.
[0119] In addition, the growth pressure of the n-type contact layer 12 is set to, for example, 20 to 200 mbar.
[0120] Next, the light emitting layer 13 is formed on the n-type contact layer 12 by MOCVD. The light emitting layer 13 is formed by stacking the first barrier layer, the first well layer, the second barrier layer, the second well layer, and the third barrier layer in this order. The growth conditions of the light emitting layer 13 are, for example, a growth temperature of 975° C. and a growth pressure of 400 mbar.
[0121] Next, the electron blocking layer 14 is formed on the light emitting layer 13 by MOCVD. The growth conditions of the electron blocking layer 14 are, for example, a growth temperature of 1025° C. and a growth pressure of 50 mbar.
[0122] Next, a p-type contact layer 15 is formed on the electron blocking layer 14 by MOCVD. The p-type contact layer 15 is formed by stacking the first p-type contact layer and the second p-type contact layer in this order. The growth conditions of the first p-type contact layer are, for example, a growth temperature of 1050° C. and a growth pressure of 200 mbar. The growth conditions of the second p-type contact layer are, for example, a growth temperature of 1050° C. and a growth pressure of 100 mbar.
[0123] Next, a predetermined region on the surface of the p-type contact layer 15 is dry-etched to form a groove having a depth reaching the n-type contact layer 12 .
[0124] Next, transparent electrode 16 is formed on p-type contact layer 15. Next, p-electrode 17 is formed on transparent electrode 16, and n-electrode 18 is formed on n-type contact layer 12 exposed at the bottom of the groove. Transparent electrode 16, p-electrode 17, and n-electrode 18 are formed by sputtering, vapor deposition, or the like.
[0125] (Effects of the First Embodiment)
[0126] According to the first embodiment of the present invention, the amount of compound defects of group III holes and Si can be suppressed, thereby obtaining an n-type contact layer composed of AlGaN that effectively reduces resistance by degeneration of the Fermi level and the conduction band. By reducing the resistance of the n-type contact layer, the output of the light-emitting element to the forward current can be increased.
[0127] [Second embodiment]
[0128] (Constitution of Light Emitting Element)
[0129] Figure 21 is a vertical cross-sectional view of a light emitting element 101 according to a second embodiment of the present invention. The light emitting element 101 is a deep ultraviolet light emitting diode (LED) of a flip chip mounting type. Here, deep ultraviolet refers to a wavelength region of 200 to 300 nm.
[0130] The light-emitting element 101 includes: a substrate 110, a buffer layer 111 on the substrate 110, an n-type contact layer 112 on the buffer layer 111, a light-emitting layer 113 on the n-type contact layer 112, an electron blocking layer 120 on the light-emitting layer 113, a current diffusion layer 114 on the electron blocking layer 120, a p-type contact layer 115 connected to a portion of an upper surface 1143 of the current diffusion layer 114, a p-electrode 116 connected to the p-type contact layer 115, and an n-electrode 117 connected to the n-type contact layer 112.
[0131] It should be noted that the "upper" in the structure of the light emitting element 101 refers to the Figure 2 When the light emitting element 101 is placed in the direction shown, “upper” is the direction from the substrate 110 to the p-electrode 116 .
[0132] The substrate 110 is a growth substrate made of sapphire. The thickness of the substrate 110 is, for example, 900 μm. As a material for the substrate 110 , in addition to sapphire, AlN, Si, SiC, ZnO, etc. can be used.
[0133] The buffer layer 111 has, for example, a structure in which three layers, namely a core layer, a low-temperature buffer layer, and a high-temperature buffer layer, are stacked in sequence. The core layer is composed of undoped AlN grown at a low temperature, and is a layer that serves as the core of crystal growth. The thickness of the core layer is, for example, 10 nm. The low-temperature buffer layer is a layer composed of undoped AlN grown at a higher temperature than the core layer. The thickness of the low-temperature buffer layer is, for example, 0.3 μm. The high-temperature buffer layer is a layer composed of undoped AlN grown at a higher temperature than the low-temperature buffer layer. The thickness of the high-temperature buffer layer is, for example, 2.7 μm. By providing such a buffer layer 111, the density of threading dislocations of AlN is reduced. It should be noted that the AlN constituting the buffer layer 111 may be n-type.
[0134] The light emitting layer 113 is composed of AlGaN, preferably having a multi-quantum well (MQW) structure. The Al component of the light emitting layer 113 (the Al component of the well layer when having the MQW structure) can be set according to the desired emission wavelength in the deep ultraviolet region (200 to 300 nm), for example, when the emission wavelength is 270 to 290 nm, it is set to about 35 to 45%. Here, the percentage of the Al component is the ratio of the Al content to the total value of the Ga content and the Al content.
[0135] For example, the light emitting layer 113 has an MQW structure with two well layers, that is, a structure in which a first barrier layer, a first well layer, a second barrier layer, a second well layer, and a third barrier layer are stacked in this order. The first well layer and the second well layer are composed of n-type AlGaN. The first barrier layer, the second barrier layer, and the third barrier layer are composed of n-type AlGaN (including a substance with an Al component of 100%, i.e., AlN) having a higher Al content than the first well layer and the second well layer.
[0136] As an example, the Al composition, thickness, and concentration of Si as a dopant in the first well layer and the second well layer are 40%, 2.4 nm, and 9×10 18 / cm 3 In addition, the Al composition, thickness, and Si concentration as a dopant of the first and second barrier layers are 55%, 19 nm, and 9×10 18 / cm 3 The Al composition, thickness, and Si concentration of the third barrier layer are 55%, 4 nm, and 5×10 18 / cm 3 .
[0137] The n-type contact layer 112 is composed of n-type AlGaN. The lower limit of the Al component of the n-type contact layer 112 is set to the lower limit of the range that can suppress the absorption of light emitted from the light emitting layer 113. For example, if the Al component of the n-type contact layer 112 is 50% or more, it is possible to suppress the absorption of deep ultraviolet light with a wavelength of 270 to 290 nm and light with a longer wavelength than the wavelength, and if it is 55% or more, it is possible to suppress the absorption more effectively.
[0138] In addition, the upper limit of the Al component of the n-type contact layer 112 is set to the upper limit of the range that can suppress the increase in resistance caused by the increase in the Al component. When the Al component is increased, the resistance of AlGaN is almost constant below 70%, but starts to increase if it exceeds 70%. Therefore, it is preferable to set the Al component of the n-type contact layer 112 to be below 70%.
[0139] Therefore, as a preferred example, the Al component of the n-type contact layer 112 is in the range of 50% to 70%. x Ga 1-x The composition represented by N (0.5≤x≤0.7).
[0140] In addition, the n-type contact layer 112 preferably contains Si at a concentration that makes the Fermi level and the conduction band degenerate (overlap). A semiconductor whose Fermi level and conduction band are degenerate behaves like a metal and has low resistance.
[0141] According to the non-patent document "A. Wolos et al., "Properties of metal-insulator transition and electron spin relaxation in GaN:Si", PHYSICAL REVIEW B 83, 165206 (2011)", in GaN containing Si as a dopant, the Si concentration is 1.6×10 18 cm -3 When the Si concentration is about 1.6×10 18 cm -3 Above this value, the Fermi level will also become degenerate with the conduction band.
[0142] On the other hand, in n-type AlGaN using Si as a dopant, if the Si concentration is increased, the resistance will decrease like a general semiconductor up to a certain concentration, but if the concentration exceeds a certain concentration, the resistance will start to increase. Therefore, in order to suppress the increase in resistance caused by the increase in Si concentration, it is preferable to set the Si concentration contained in the n-type contact layer 112 to 4.0×10 19 cm -3 the following.
[0143] It is believed that the increase in resistance with increasing Si concentration in n-type AlGaN using Si as a dopant is caused by the generation of compound defects of group III holes and Si when the Si concentration exceeds a certain concentration. The details of the compound defects of group III holes and Si are not clear, but there is a theory that when Si does not enter the group III holes generated during the growth of AlGaN but remains in other positions, Si cannot function as a donor (emit electrons) and instead emits 1 to 3 holes depending on its state, thereby increasing resistance.
[0144] The thickness of the n-type contact layer 112 is, for example, 0.3 to 3 μm.
[0145] The electron blocking layer 120 is composed of p-type AlGaN having a higher Al content than the third barrier layer of the light emitting layer 113. The electron blocking layer 120 can suppress the diffusion of electrons to the current diffusion layer 114. The Al content, thickness, and Mg concentration of the electron blocking layer 120 as a dopant are, for example, 80% or more, 25 nm, and 1×10 18 ~1×10 20 cm -3 .
[0146] The current diffusion layer 114 is composed of AlGaN containing two-dimensional hole gas 1144. The current diffusion layer 114 has a p-type first AlGaN layer 1141 and a p-type or i-type second AlGaN layer 1142 directly provided on the first AlGaN layer 1141, and the second AlGaN layer 1142 has two-dimensional hole gas 1144 near the interface with the first AlGaN layer 1141.
[0147] The Al composition of the first AlGaN layer 1141 is higher than that of the second AlGaN layer 1142. In order to suppress absorption of deep ultraviolet light emitted from the light emitting layer 113, the Al composition of the first AlGaN layer 1141 and the second AlGaN layer 1142 is preferably 30% or more.
[0148] For example, the Al content of the first AlGaN layer 1141 is in the range of 50% to 70%, and the Al content of the second AlGaN layer 1142 is in the range of 30% to 50%. x Ga 1-x N (0.5≤x≤0.7), the second AlGaN layer 1142 has Al x Ga 1-x It should be noted that when the thickness of the second AlGaN layer 1142 is large (for example, about 50 nm or more), it is necessary to consider that the deep ultraviolet light emitted from the light-emitting layer 113 is absorbed by the second AlGaN layer 1142, so it is preferred that the Al component of the second AlGaN layer 1142 is 40% or more.
[0149] By stacking the second AlGaN layer 1142 on a layer with a band gap energy larger than that of the second AlGaN layer 1142 and a thickness of 5×10 17 cm -3 In the first AlGaN layer 1141 doped with Mg at a concentration above Mg, the Fermi level and the valence band are degenerate in the band bending region near the interface between the second AlGaN layer 1142 and the first AlGaN layer 1141 , thereby generating two-dimensional hole gas 1144 .
[0150] The current diffusion layer 114 contains the two-dimensional hole gas 1144, so that holes migrate with high mobility in the two-dimensional hole gas 1144, and thus the current effectively diffuses in the in-plane direction of the current diffusion layer 114. Here, the two-dimensional hole gas can be observed as a high-concentration p-type region by cross-sectional SCM (Scanning Capacitance Microscopy). That is, if a high-concentration p-type region is observed near the interface between the second AlGaN layer 1142 and the first AlGaN layer 1141, it can be determined that the two-dimensional hole gas is generated.
[0151] The thickness of the first AlGaN layer 1141 is, for example, 5 to 50 nm. The thickness of the second AlGaN layer 1142 is, for example, 5 to 100 nm.
[0152] The p-type contact layer 115 is composed of p-type GaN or p-type AlGaN with an Al content of 35% or less. x Ga 1-x Therefore, the contact resistance between the p-type contact layer 115 and the p-electrode 116 can be suppressed to be low.
[0153] On the other hand, since GaN and AlGaN with an Al content of less than 35% have a high absorption rate for deep ultraviolet light, light emitted from the light-emitting layer 113 and directed toward the p-type contact layer 115 is strongly absorbed by the p-type contact layer 115. For example, when the Al content of the p-type contact layer 115 is 35%, the transmittance of light with a wavelength of 280 nm is about 90% when the thickness is 20 nm, and when the thickness is large enough, almost all light with a wavelength of less than about 290 nm is absorbed. In addition, when the Al content of the p-type contact layer 115 is 30%, the transmittance of light with a wavelength of 280 nm is about 80% when the thickness is 20 nm, and when the thickness is large enough, almost all light with a wavelength of less than about 310 nm is absorbed.
[0154] Therefore, in the light emitting element 101, the p-type contact layer 115 is formed only on a part of the upper surface 1143 of the current diffusion layer 114, so that the absorption of deep ultraviolet light emitted from the light emitting layer 113 by the p-type contact layer 115 is suppressed to a low level. In order to more effectively suppress the absorption of ultraviolet light by the p-type contact layer 115, the area of the upper surface 1143 that contacts the p-type contact layer 115 is preferably 80% or less of the area of the entire upper surface 1143, and more preferably 50% or less.
[0155] It should be noted that when a pss substrate (Patterned Sapphire Substrate) having a concave-convex pattern on the surface is used as the substrate 110, since more light travels back and forth in the light-emitting element 101, the effect of the present invention of suppressing the absorption of light by the p-type contact layer 115 is particularly beneficial.
[0156] The p-type contact layer 115 is connected to the current diffusion layer 114 only in a portion of the upper surface 1143, but since the current diffusion layer 114 containing the two-dimensional hole gas 1144 efficiently diffuses the current in the in-plane direction, it is possible to ensure the uniformity of the luminous intensity within the plane of the light-emitting layer 113. In order to further improve the uniformity of the luminous intensity within the plane of the light-emitting layer 113, it is preferred that the area of the upper surface 1143 that contacts the p-type contact layer 115 is greater than 40% of the area of the entire area of the upper surface 1143.
[0157] The thickness of the p-type contact layer 115 is, for example, 4 to 30 nm.
[0158] The p-electrode 116 is made of, for example, Ni / Au, and the n-electrode 117 is made of, for example, Ti / Al / Ni, V / Al / Ni, V / Al / Ru, or the like.
[0159] In addition, if Figure 2 As shown, preferably, at least a portion of, and more preferably the entire area other than the area connected to the p-type contact layer 115 on the upper surface 1143 of the current diffusion layer 114 is covered with a passivation film 118 made of an insulating material such as SiO2 or SiN. By using the passivation film 118, the generation of surface leakage current flowing on the upper surface 1143 of the current diffusion layer 114 can be suppressed, and the current can flow efficiently in the two-dimensional hole gas 1144.
[0160] In addition, it is preferable to provide a reflective layer 119 above the region other than the region contacting the p-type contact layer 115 of the upper surface 1143 of the current diffusion layer 114. The reflective layer 119 is made of a material having a high reflectivity to deep ultraviolet light, such as aluminum, rhodium, or ruthenium. By using the reflective layer 119 to reflect the light emitted from the light-emitting layer 113, the light extraction efficiency of the light-emitting element 101 can be improved. The reflective layer 119 can be, for example, Figure 2 As shown, it is buried inside the passivation film 118.
[0161] It should be noted that the characteristic configurations of the current diffusion layer 114 , the p-type contact layer 115 , and the like of the light emitting element 101 can also be applied to light emitting elements other than LEDs, such as vertical laser diodes such as VCSEL type.
[0162] (Method for manufacturing light emitting element)
[0163] An example of a method for manufacturing the light-emitting element 101 according to the second embodiment of the present invention is described below. In the formation of each layer of the light-emitting element 101 by vapor deposition, trimethylgallium, trimethylaluminum, and ammonia are used as Ga raw material gas, Al raw material gas, and N raw material gas, for example. In addition, silane gas and bis(cyclopentadienyl)magnesium gas are used as raw material gas of Si, which is an n-type dopant, and Mg, which is a p-type dopant. In addition, hydrogen gas and nitrogen gas are used as carrier gas.
[0164] First, prepare a substrate 110, and form a buffer layer 111 thereon. In the formation of the buffer layer 111, first, a core layer composed of AlN is formed. For example, the core layer is formed by MOCVD at a growth temperature of 880°C. In addition, the core layer can be formed by a sputtering method. Next, a low-temperature buffer layer and a high-temperature buffer layer composed of AlN are sequentially formed on the core layer by the MOCVD method. The growth conditions of the low-temperature buffer layer are, for example, a growth temperature of 1090°C and a growth pressure of 50 mbar. In addition, the growth conditions of the high-temperature buffer layer are, for example, a growth temperature of 1270°C and a growth pressure of 50 mbar.
[0165] Next, an n-type contact layer 112 made of AlGaN containing Si is formed on the buffer layer 111 by MOCVD. The growth conditions of the n-type contact layer 112 are, for example, a growth temperature of 980° C. and a growth pressure of 50 mbar.
[0166] Next, a light emitting layer 113 is formed on the n-type contact layer 112 by MOCVD. The light emitting layer 113 is formed by stacking the first barrier layer, the first well layer, the second barrier layer, the second well layer, and the third barrier layer in this order. The growth conditions of the light emitting layer 113 are, for example, a growth temperature of 975° C. and a growth pressure of 400 mbar.
[0167] Next, the electron blocking layer 120 is formed on the light emitting layer 113 by MOCVD. The growth conditions of the electron blocking layer 120 are, for example, a growth temperature of 1000° C. and a growth pressure of 50 mbar.
[0168] Next, a first AlGaN layer 1141 and a second AlGaN layer 1142 constituting the current diffusion layer 114 are formed on the electron blocking layer 120 by MOCVD. The growth conditions of the first AlGaN layer 1141 are, for example, a growth temperature of 950 to 1000° C. (as a typical example, 980° C.) and a growth pressure of 50 mbar. The growth conditions of the second AlGaN layer 1142 are, for example, a growth temperature of 950 to 1000° C. (as a typical example, 980° C.) and a growth pressure of 50 mbar.
[0169] Next, the p-type contact layer 115 is formed on the current diffusion layer 114 by MOCVD. The growth conditions of the p-type contact layer 115 are, for example, a growth temperature of 1000 to 1100° C. (typically, 1050° C.) and a growth pressure of 50 mbar.
[0170] Next, a predetermined region on the surface of the p-type contact layer 115 is dry-etched in two steps to form a groove reaching the n-type contact layer 112 for connecting the n-electrode 117 and pattern the p-type contact layer 115 on the current diffusion layer 114 .
[0171] Next, p-electrode 116 is formed on p-type contact layer 115, and n-electrode 117 is formed on n-type contact layer 112 exposed at the bottom surface of the groove. P-electrode 116 and n-electrode 117 are formed by sputtering, vapor deposition or the like.
[0172] (Variation Example)
[0173] Figure 3 1 is a vertical cross-sectional view of a light emitting element 102 which is a modified example of the light emitting element 101 according to the second embodiment of the present invention. The light emitting element 102 is different from the light emitting element 101 in the planar shape of the p-type contact layer 115 .
[0174] The p-type contact layer 115 of the light emitting element 102 has a ring-shaped planar shape. The upper surface 1143 of the current diffusion layer 114 is covered with a passivation film 118 inside the region connected to the ring-shaped p-type contact layer 115 , and a light reflecting layer 119 is provided on the passivation film 118 .
[0175] As shown in the example of the light emitting element 102 , the planar shape of the p-type contact layer 115 of the light emitting element according to this embodiment can be appropriately changed to, for example, a circle, a ring, a mesh, etc., depending on the purpose of the light emitting element.
[0176] (Application example)
[0177] Figure 4 1 is a vertical cross-sectional view of a light emitting device 103 having the light emitting element 101 according to the second embodiment of the present invention as a light source. The light emitting device 103 has a multilayer wiring structure called a build-up structure and is an example of a light emitting device having the light emitting element 101 as a light source.
[0178] In the light emitting device 103, the p-electrodes 116 of the plurality of light emitting elements 101 are connected to the p-pad electrode 133 via the bonding electrode 131, and the n-electrodes 117 of the plurality of light emitting elements 101 are connected to the n-pad electrode 134 via the bonding electrode 132. Then, by applying a voltage between the p-pad electrode 133 and the n-pad electrode 134, the plurality of light emitting elements 101 emit light.
[0179] In the light emitting device 103 , the bonding electrodes 131 and 132 are wired inside the insulating layers 135 and 136 , and the light reflecting layer 119 is buried in the insulating layer 135 covering the light emitting element 101 .
[0180] (Effects of the Second Embodiment)
[0181] According to the above-mentioned second embodiment of the present invention, by reducing the area of the p-type contact layer with a high absorption rate of deep ultraviolet light and using a diffusion layer to efficiently diffuse the current in the in-plane direction, a light-emitting element can be provided in which the contact resistance between the electrode on the p-side and the contact layer is low and the absorption of light by the contact layer is suppressed.
[0182] [Third embodiment]
[0183] (Constitution of Light Emitting Element)
[0184] Figure 5 2 is a vertical cross-sectional view of a light emitting element 201 according to a third embodiment of the present invention. The light emitting element 201 is a deep ultraviolet light emitting diode (LED) of a flip chip mounting type. Here, deep ultraviolet refers to a wavelength region of 200 to 300 nm.
[0185] The light-emitting element 201 includes: a substrate 210, a buffer layer 211 on the substrate 210, an n-type contact layer 212 on the buffer layer 211, a light-emitting layer 213 on the n-type contact layer 212, an electron blocking layer 214 on the light-emitting layer 213, a p-type layer 215 on the electron blocking layer 214, an n-type contact layer 216 on the p-type layer 215, a p-electrode 217 connected to the n-type contact layer 216, and an n-electrode 218 connected to the n-type contact layer 212.
[0186] It should be noted that the "upper" in the structure of the light emitting element 201 refers to the Figure 5 When the light emitting element 201 is placed in the direction shown, “upper” is the direction from the substrate 210 to the p-electrode 217 .
[0187] The substrate 210 is a growth substrate made of sapphire. The thickness of the substrate 210 is, for example, 900 μm. As a material for the substrate 210 , in addition to sapphire, AlN, Si, SiC, ZnO, etc. can be used.
[0188] The buffer layer 211 has, for example, a structure in which three layers, namely a core layer, a low-temperature buffer layer, and a high-temperature buffer layer, are stacked in order. The core layer is composed of undoped AlN grown at a low temperature, and is a layer that serves as a core for crystal growth. The thickness of the core layer is, for example, 10 nm. The low-temperature buffer layer is a layer composed of undoped AlN grown at a higher temperature than the core layer. The thickness of the low-temperature buffer layer is, for example, 0.3 μm. The high-temperature buffer layer is a layer composed of undoped AlN grown at a higher temperature than the low-temperature buffer layer. The thickness of the high-temperature buffer layer is, for example, 2.7 μm. By providing such a buffer layer 211, the density of threading dislocations of AlN is reduced.
[0189] The light emitting layer 213 is composed of AlGaN, preferably having a multi-quantum well (MQW) structure. The Al component of the light emitting layer 213 (the Al component of the well layer when having the MQW structure) can be set according to the desired emission wavelength in the deep ultraviolet region (200 to 300 nm), for example, when the emission wavelength is 270 to 290 nm, it is set to about 40 to 50%. Here, the percentage of the Al component is the ratio of the Al content to the total value of the Ga content and the Al content.
[0190] For example, the light emitting layer 213 has an MQW structure with two well layers, that is, a structure in which a first barrier layer, a first well layer, a second barrier layer, a second well layer, and a third barrier layer are stacked in order. The first well layer and the second well layer are composed of n-type AlGaN. The first barrier layer, the second barrier layer, and the third barrier layer are composed of n-type AlGaN (including a material with an Al component of 100%, i.e., AlN) having a higher Al content than the first well layer and the second well layer.
[0191] As an example, the Al composition, thickness, and concentration of Si as a dopant in the first well layer and the second well layer are 40%, 2.4 nm, and 9×10 1 cm -3 In addition, the Al composition, thickness, and Si concentration as a dopant of the first and second barrier layers are 55%, 19 nm, and 9×10 18 cm -3 The Al composition, thickness, and Si concentration of the third barrier layer are 55%, 4 nm, and 5×10 18 cm -3 .
[0192] The n-type contact layer 212 and the n-type contact layer 216 are composed of n-type AlGaN. In order to suppress the absorption of deep ultraviolet light emitted from the light-emitting layer 213, the Al content of the n-type contact layer 212 and the n-type contact layer 216 is preferably higher than that of the light-emitting layer 213, for example, preferably in the range of 50% to 70%. In this case, it is ideal that the n-type contact layer 212 and the n-type contact layer 216 have Al x Ga 1-x The composition represented by N (0.5≤x≤0.7).
[0193] If the Al content of the n-type contact layer 212 and the n-type contact layer 216 is 50% or more, high transmittance can be ensured for deep ultraviolet light with a wavelength of 270 to 290 nm and light with a longer wavelength than the wavelength. In addition, if the Al content of the n-type contact layer 212 and the n-type contact layer 216 is 55% or more, a higher transmittance can be ensured, and if it is 60% or more, a further higher transmittance can be ensured.
[0194] In addition, if the Al content of the n-type contact layer 212 and the n-type contact layer 216 is 70% or less, the resistance can be suppressed to a low level. When the Al content is increased, the resistance of AlGaN is almost constant below 70%, but starts to increase if it exceeds 70%. Therefore, the Al content of the n-type contact layer 212 and the n-type contact layer 216 is set to 70% or less.
[0195] On the other hand, in order to allow carriers to efficiently pass between the n-type contact layer 216 and the p-type layer 215, it is preferred that the Al component of the n-type contact layer 216 be as low as possible, and when the passing of carriers is emphasized, the Al component is set to be lower than the Al component of the light-emitting layer 213 within a range that suppresses the absorption of deep ultraviolet light to a certain extent. Therefore, the Al component of the n-type contact layer 216 is set, for example, within a range of 40% to 70%. The tunnel junction between the n-type contact layer 216 and the p-type layer 215 will be described below.
[0196] In addition, the n-type contact layer 212 and the n-type contact layer 216 contain Si at a concentration that makes the Fermi level and the conduction band degenerate (overlap). A semiconductor whose Fermi level and conduction band are degenerate behaves like a metal, and the resistance is reduced.
[0197] According to the non-patent document "A. Wolos et al., "Properties of metal-insulator transition and electron spin relaxation in GaN:Si", PHYSICAL REVIEW B 83, 165206 (2011)", it is said that in GaN containing Si as a dopant, the Si concentration is 1.6×10 18 cm-3 At this time, the Fermi level and the conduction band are degenerate. Since AlGaN is considered to exhibit almost the same behavior as GaN, it is considered that the n-type contact layer 212 and the n-type contact layer 216 have a Si concentration of about 1.6×10 18 cm -3 Above this value, the Fermi level will also become degenerate with the conduction band.
[0198] On the other hand, in n-type AlGaN using Si as a dopant, if the Si concentration is increased, the resistance will decrease like a general semiconductor until a certain concentration, but if the concentration exceeds a certain value, the resistance will start to increase. Therefore, in order to suppress the increase in resistance caused by the increase in Si concentration, it is preferred to set the Si concentration contained in the n-type contact layer 212 and the n-type contact layer 216 to 4.0×10 19 cm -3 the following.
[0199] It is believed that the increase in resistance with increasing Si concentration in n-type AlGaN using Si as a dopant is caused by the generation of compound defects of group III holes and Si when the Si concentration exceeds a certain concentration. The details of the compound defects of group III holes and Si are not clear, but there is a theory that when Si does not enter the group III holes generated during the growth of AlGaN but remains in other positions, Si cannot function as a donor (emit electrons) and instead emits 1 to 3 holes depending on its state, thereby increasing resistance.
[0200] The thickness of the n-type contact layer 212 is, for example, 500 to 2000 nm. The thickness of the n-type contact layer 216 is, for example, 25 to 200 nm.
[0201] The electron blocking layer 214 is a layer for suppressing diffusion of electrons toward the n-type contact layer 216, and is made of, for example, undoped AlN. The thickness of the electron blocking layer 214 is, for example, 2 nm.
[0202] The p-type layer 215 is composed of p-type AlGaN, for example, having a structure in which a p-type electron blocking layer and a p-type cladding layer are stacked in sequence. When the p-type electron blocking layer is composed of AlGaN, the p-type cladding layer is composed of AlGaN or GaN having a lower Al content than the p-type electron blocking layer, and when the p-type electron blocking layer is composed of AlN, the p-type cladding layer is composed of AlGaN. The thickness of the p-type electron blocking layer is, for example, 10 to 50 nm. In addition, the thickness of the p-type cladding layer is, for example, 2 to 200 nm.
[0203] For example, when the p-type electron blocking layer and the p-type cladding layer are composed of AlGaN, the Al composition, thickness, and Mg concentration as a dopant of the p-type electron blocking layer are 80%, 25 nm, and 1×10 20cm -3 The Al composition, thickness, and Mg concentration of the p-type cladding layer as a dopant are, for example, 35%, 5 nm, and 1×10 19 cm -3 .
[0204] To suppress absorption of deep ultraviolet light emitted from the light emitting layer 213, the Al composition of the p-type electron blocking layer and the p-type cladding layer is preferably higher than that of the light emitting layer 213. In this case, the Al composition of the p-type cladding layer is preferably 50% or more, for example, 50 to 60%.
[0205] On the other hand, in order to allow carriers to effectively travel between the n-type contact layer 216 and the p-type layer 215, it is preferred that the Al composition of the p-type electron blocking layer and the p-type cladding layer be as low as possible. When the travel of carriers is important, the Al composition of the p-type cladding layer can be set to be lower than the Al composition of the light-emitting layer 213 within a range that suppresses the absorption of deep ultraviolet light to a certain extent. The tunnel junction between the n-type contact layer 216 and the p-type layer 215 will be described below.
[0206] The n-type contact layer 216, whose Fermi level and conduction band are degenerate, forms a tunnel junction with the p-type layer 215. In the region of the energy band bending near the interface between the p-type layer 215 and the n-type contact layer 216, n-type and p-type carriers are distributed at high concentrations, so when a forward voltage is applied between the p-electrode 217 and the n-electrode 218, electrons pass through the potential barrier and migrate from the p-type layer 215 to the n-type contact layer 216, causing the light-emitting element 201 to emit light.
[0207] In addition, near the interface between the p-type layer 215 and the n-type contact layer 216 , when the Fermi level and the valence band are degenerate to generate two-dimensional hole gas, the potential barrier between the p-type layer 215 and the n-type contact layer 216 becomes thinner, tunneling is easily generated, and the operating voltage of the light-emitting element 201 can be reduced.
[0208] In order to form a two-dimensional hole gas, for example, a stack of different first layers with an Al content of 10% or more and a second layer thereon, each composed of p-type AlN, AlGaN, or AlGaInN, is used as the p-type layer 215. At this time, by making the Al content of the second layer larger than that of the first layer, electron boiling occurs at the interface between the first layer and the second layer, and on the other hand, holes boil at the interface between the second layer and the n-type contact layer 216 to form a two-dimensional hole gas. In addition, the p-type layer 215 can have a structure (superlattice structure) in which a plurality of thin first layers and second layers are alternately stacked. In this case, a two-dimensional hole gas can also be formed near each interface between the first layer and the second layer. In addition, at this time, the Al content of one of the first layer and the second layer can be increased. Here, in order to increase the amount of carrier injection into the light-emitting layer 213, it is preferred to dope Mg in the p-type layer 215.
[0209] It should be noted that two-dimensional vacancy gas can be observed as a high-concentration p-type region by cross-sectional SCM (Scanning Capacitance Microscopy) observation. That is, if a high-concentration p-type region is observed near the interface between the p-type layer 215 and the n-type contact layer 216, it can be determined that two-dimensional vacancy gas is generated.
[0210] A groove is provided in a part of the surface of the n-type contact layer 216. The groove penetrates the n-type contact layer 216, the p-type layer 215 and the light emitting layer 213 to reach the n-type contact layer 212, and the n-electrode 218 is connected to the exposed surface of the n-type contact layer 212 by the groove.
[0211] In the light emitting element 201, the n-type contact layer 212 connected to the n-electrode 218 and the n-type contact layer 216 connected to the p-electrode 217 are both made of n-type AlGaN. Therefore, the material of the portion of the n-electrode 218 in contact with the n-type contact layer 212 and the portion of the p-electrode 217 in contact with the n-type contact layer 216 can be the same substance. When the p-electrode 217 and the n-electrode 218 are respectively made of a single material, the material of the n-electrode 218 and the p-electrode 217 can be the same substance.
[0212] Therefore, similarly to the n-electrode 218, the p-electrode 217 may also use aluminum having a high reflectivity to deep ultraviolet light. Therefore, the portion of the n-electrode 218 in contact with the n-type contact layer 212 and the portion of the p-electrode 217 in contact with the n-type contact layer 216 are preferably made of aluminum.
[0213] The p-electrode 217 and the n-electrode 218 are composed of, for example, V / Al / NiAu or V / Al / Ru / Au. In this case, in order to increase the reflectivity, it is preferable that the V layer is as thin as possible.
[0214] Note that since p-type AlGaN cannot make ohmic contact with aluminum having a low work function, aluminum cannot be used as the material of the p-electrode when a contact layer made of p-type AlGaN is connected to the p-electrode as in conventional general light-emitting elements.
[0215] It should be noted that the characteristic configuration of the n-type contact layer 216 and the like of the light emitting element 201 can also be applied to light emitting elements other than LEDs, such as laser diodes.
[0216] (Method for manufacturing light emitting element)
[0217] An example of a method for manufacturing the light-emitting element 201 according to the third embodiment of the present invention is described below. In the formation of each layer of the light-emitting element 201 by vapor deposition, trimethylgallium, trimethylaluminum, and ammonia are used as Ga raw material gas, Al raw material gas, and N raw material gas, for example. In addition, silane gas and bis(cyclopentadienyl)magnesium gas are used as raw material gas of Si, which is an n-type dopant, and Mg, which is a p-type dopant. In addition, hydrogen gas and nitrogen gas are used as carrier gas.
[0218] First, a substrate 210 is prepared, and a buffer layer 211 is formed thereon. In the formation of the buffer layer 211, first, a core layer composed of AlN is formed by sputtering. The growth temperature is, for example, 880°C. Next, a low-temperature buffer layer and a high-temperature buffer layer composed of AlN are sequentially formed on the core layer by MOCVD. The growth conditions of the low-temperature buffer layer are, for example, a growth temperature of 1090°C and a growth pressure of 50 mbar. In addition, the growth conditions of the high-temperature buffer layer are, for example, a growth temperature of 1270°C and a growth pressure of 50 mbar.
[0219] Next, an n-type contact layer 212 made of AlGaN containing Si is formed on the buffer layer 211 by MOCVD. The growth conditions of the n-type contact layer 212 are, for example, a growth temperature of 980° C. and a growth pressure of 50 mbar.
[0220] In order to suppress the increase in resistance of the n-type contact layer 212, the V / III ratio of the raw material gas of the n-type contact layer 212 is preferably set in the range of 1000 to 3200, and the growth temperature is preferably set below 1100°C. Here, the V / III ratio refers to the ratio of the number of atoms of the III-group element (Ga, Al) and the V-group element (N) in the raw material gas. In addition, since ammonia, which is a raw material of N, is easily decomposed, it is preferred to set the growth temperature above 850°C. In addition, the growth pressure of the n-type contact layer 212 is set at, for example, 20 to 200 mbar. It should be noted that when the growth temperature of the n-type contact layer 212 is set relatively low (close to 850°C), in order to suppress the acquisition of C, it is preferred to make the V / III ratio of the raw material gas larger than the above range, for example, increased to about 10000. If C is taken into the n-type contact layer 212 , C acts as an acceptor to compensate for carriers. Also, since C increases impurity scattering and reduces carrier mobility, there is a possibility that the n-type contact layer 212 will have a high resistance.
[0221] Next, a light emitting layer 213 is formed on the n-type contact layer 212 by MOCVD. The light emitting layer 213 is formed by stacking the first barrier layer, the first well layer, the second barrier layer, the second well layer, and the third barrier layer in this order. The growth conditions of the light emitting layer 213 are, for example, a growth temperature of 975° C. and a growth pressure of 400 mbar.
[0222] Next, the electron blocking layer 214 is formed on the light emitting layer 213 by MOCVD. The growth conditions of the electron blocking layer 214 are, for example, a growth temperature of 975° C. and a growth pressure of 400 mbar.
[0223] Next, a p-type layer 215 is formed on the electron blocking layer 214 by MOCVD. The p-type layer 215 is formed by stacking the p-type electron blocking layer and the p-type cladding layer in this order. The growth conditions of the p-type electron blocking layer are, for example, a growth temperature of 1025° C. and a growth pressure of 50 mbar. The growth conditions of the p-type cladding layer are, for example, a growth temperature of 980° C. and a growth pressure of 50 mbar.
[0224] After the p-type layer 215 is formed, it is preferable to perform an annealing process to remove hydrogen from the p-type layer 215 in order to activate Mg contained in the p-type layer 215 .
[0225] Next, an n-type contact layer 216 is formed on the p-type layer 215 by MOCVD. The growth conditions of the n-type contact layer 216 are, for example, a growth temperature of 980° C. and a growth pressure of 50 mbar.
[0226] In addition, similarly to the n-type contact layer 212, in order to suppress the increase in the resistance of the n-type contact layer 212, the V / III ratio of the raw material gas of the n-type contact layer 212 is preferably set in the range of 1000 to 3200, and the growth temperature is preferably set to 1100° C. or less. In addition, in order to facilitate the decomposition of ammonia as a raw material of N, the growth temperature is preferably set to 850° C. or more. In addition, the growth pressure of the n-type contact layer 212 is set, for example, to 20 to 200 mbar.
[0227] Here, when hydrogen is removed from the p-type layer 215 by annealing, the growth temperature of the n-type contact layer 216 is preferably set to 900° C. or less in order to suppress hydrogen from re-entering the p-type layer 215 and deactivating Mg.
[0228] Next, a predetermined region on the surface of the n-type contact layer 216 is dry-etched to form a groove having a depth reaching the n-type contact layer 212 .
[0229] Next, p-electrode 217 is formed on n-type contact layer 216, and n-electrode 218 is formed on n-type contact layer 212 exposed at the bottom surface of the groove. P-electrode 217 and n-electrode 218 are formed by sputtering, vapor deposition or the like.
[0230] (Effects of the Third Embodiment)
[0231] According to the third embodiment of the present invention, a tunnel junction structure that suppresses absorption of deep ultraviolet light can be formed by using an n-type contact layer 216 composed of AlGaN with a high Al content, in which the Fermi level and the conduction band are degenerate. In addition, by using the n-type contact layer 216 as a contact layer of the p-electrode 217, the material of the p-electrode 217 can use a material with a high reflectivity to deep ultraviolet light, such as aluminum with a low work function.
[0232] Therefore, a large amount of light emitted from the light-emitting layer 213 and transmitted to the p-electrode 217 side is not absorbed by the n-type contact layer 216, but is transmitted and efficiently reflected by the p-electrode 217 and taken out from the substrate 210 side, so that the light-emitting element 201 has a high light extraction efficiency.
[0233] Example 1
[0234] The following describes the evaluation results of the characteristics of the n-type contact layer 12 involved in the first embodiment described above. In this embodiment, the n-type contact layer 12 was formed on the substrate 10 with the buffer layer 11 interposed therebetween under various conditions described below, and these n-type contact layers 12 were evaluated. The following Table 1 shows the composition and growth conditions of the substrate 10, buffer layer 11, and n-type contact layer 12 involved in this embodiment.
[0235] [Table 1]
[0236]
[0237] In this embodiment, the resistivity, carrier concentration, and mobility of the n-type contact layer 12 were measured by hole effect measurement, and the Si concentration was measured by secondary ion mass spectrometry (SIMS).
[0238] Figure 6 : is a graph showing the relationship between the Al composition and the resistivity of the n-type contact layer 12 . Figure 6 It is shown that if the Al content of the n-type contact layer 12 exceeds about 70%, the resistance increases. Figure 6 The numerical values of the plotted points and the growth temperature of the n-type contact layer 12 and the V / III ratio of the raw material gas to which each plotted point relates.
[0239] [Table 2]
[0240]
[0241] Figure 7 (a) to (c) are graphs showing the relationship between the Si concentration and the resistivity of the n-type contact layer 12 . Figure 7 The growth temperature of the n-type contact layer 12 and the V / III ratio of the raw material gas in (a) are 1013° C. and 1058, respectively. Figure 7 The growth temperature of the n-type contact layer 12 and the V / III ratio of the raw material gas involved in (b) are 1013° C. and 1587, respectively. Figure 7 The growth temperature of the n-type contact layer 12 and the V / III ratio of the raw material gas in (c) are 1083° C. and 1058, respectively. Figure 7 (a) to (c) show that if the Si concentration of the n-type contact layer 12 exceeds about 4.0×10 19 cm -3 The resistance increases. The following Table 3 shows Figure 7 The values of the plotted points.
[0242] [Table 3]
[0243]
[0244] according to Figure 7 From (a) to (c) and Table 3, it can be seen that, for example, in order to make the resistivity of the n-type contact layer 12 5×10 -2 Ω·cm or less, when the growth temperature of the n-type contact layer 12 and the V / III ratio of the raw material gas are 1013°C and 1058, respectively, the Si concentration is set to 1.2×10 19 ~4.0×10 19 cm -3 That is, when the growth temperature of the n-type contact layer 12 and the V / III ratio of the raw material gas are 1013°C and 1587, respectively, the Si concentration is set to 2.1×10 19 ~3.2×10 19 cm -3 That is, when the growth temperature of the n-type contact layer 12 and the V / III ratio of the raw material gas are 1083°C and 1058, respectively, the Si concentration is set to 5.4×10 18 ~2.7×10 19 cm -3 That's it.
[0245] Figure 8 (a) to (c) are graphs showing the temperature dependence of the resistivity, carrier concentration, and mobility of the n-type contact layer 12 . Figure 8 (a) to (c) show that the Si concentration is 2.10×10 19 cm -3 3.20×10 19cm -3 4.30×10 19 cm -3 The measured values of the three types of n-type contact layers 12 are as follows. The Si concentration is 2.10×10 19 cm -3 The growth temperature of the n-type contact layer 12 and the V / III ratio of the raw material gas are 1013°C and 1587, respectively, and the Si concentration is 3.20×10 19 cm -3 The growth temperature of the n-type contact layer 12 and the V / III ratio of the raw material gas are 1013°C and 1587, respectively, and the Si concentration is 4.30×10 19 cm -3 The growth temperature of the n-type contact layer 12 and the V / III ratio of the raw material gas are 1043° C. and 1587, respectively.
[0246] In n-type AlGaN, where the Fermi level and conduction band are degenerate, there is almost no temperature dependence of carrier concentration. Figure 8 In (b), when the Si concentration is 2.10×10 19 cm -3 3.20×10 19 cm -3 4.30×10 19 cm -3 In any of the n-type contact layers 12 , the temperature dependence of the carrier concentration is small, and therefore it can be determined that the Fermi level and the conduction band are degenerate.
[0247] On the other hand, even when the Fermi level and the conduction band are degenerate, if there are complex defects of group III holes and Si, the defects will cause carrier scattering, so the mobility depends on the temperature. Figure 8 In (c), when the Si concentration is 2.10×10 19 cm -3 3.20×10 19 cm -3 In the n-type contact layer 12, there is almost no temperature dependence of mobility, but when the Si concentration is 4.30×10 19 cm -3 The n-type contact layer 12 has a large temperature dependence of mobility. This is considered to be due to the high Si concentration and the presence of a large number of complex defects of group III holes and Si.
[0248] In addition, according to Figure 8 In (a), when the Si concentration is 2.10×10 19 cm -3 3.20×10 19 cm -3In the n-type contact layer 12, the resistivity has almost no temperature dependence, but when the Si concentration is 4.30×10 19 cm -3 The n-type contact layer 12 has a large temperature dependence of resistivity.
[0249] In the case of AlGaN where the Fermi level and conduction band are not degenerate, the resistivity also depends on temperature, but is determined by Figure 8 In (b), it can be confirmed that when the Si concentration is 4.30×10 19 cm -3 The n-type contact layer 12 is degenerate, so it is considered that the Si concentration is 4.30×10 19 cm -3 The temperature dependence of the resistivity of the n-type contact layer 12 is caused by the presence of a large number of compound defects of group III holes and Si.
[0250] Fig. 9 This is a graph showing the relationship between the V / III ratio of the raw material gas of the n-type contact layer 12 and the resistivity. Fig. 9 The growth temperature of the n-type contact layer 12 is 1013°C. Fig. 9 It is shown that the resistivity is minimum when the V / III ratio of the raw material gas of the n-type contact layer 12 is about 1500, and low resistivity can be obtained when the V / III ratio of the raw material gas is in the range of 1000 to 3200. The following Table 4 shows Fig. 9 The values of the plotted points.
[0251] [Table 4]
[0252]
[0253] Fig.10 It is a graph showing the relationship between the growth temperature and resistivity of the n-type contact layer 12 . Fig.10 It is shown that the resistance starts to increase when the growth temperature of the n-type contact layer 12 is about 1100 to 1150°C. The following Table 5 shows Fig.10 The numerical values of the plotted points and the V / III ratio of the raw material gas of the n-type contact layer 12 associated with each plotted point.
[0254] [Table 5]
[0255]
[0256] Fig.11(a) to (c) show the spectra (CL spectra) obtained by cathode luminescence measurement of various n-type contact layers 12. The peak with a photon energy of about 2.4 eV in the CL spectrum of the n-type contact layer 12 is caused by the luminescence due to the recombination defects of group III holes and Si. The greater the intensity of the peak, the more recombination defects of group III holes and Si.
[0257] The peak at a photon energy of about 3.2 eV is due to light emission from C at the group V site, and the peak at a photon energy of about 4.9 eV is due to light emission corresponding to the band gap.
[0258] Fig.11 (a) in FIG. 1 shows the change in the shape of the CL spectrum of the n-type contact layer 12 due to the Si concentration. Fig.11 In (a), for the peak due to the combined defect of group III holes and Si, the peak is 18 ~3.0×10 19 cm -3 No ions were found in the n-type contact layer 12. 19 cm -3 A weak peak appears in the n-type contact layer 12. When the Si concentration is 6.0×10 19 cm -3 A strong peak appears in the n-type contact layer 12.
[0259] Since the more compound defects of group III holes and Si are, the greater the resistance of the n-type contact layer 12 is, the greater the resistance of the n-type contact layer 12 is. Fig.11 The result obtained by (a) is similar to that obtained by Figure 7 The results obtained in (a) to (c) are consistent, that is, if the Si concentration of the n-type contact layer 12 exceeds about 4.0×10 19 cm -3 The resistance increases.
[0260] Fig.11 (b) shows the change in the shape of the CL spectrum of the n-type contact layer 12 due to the V / III ratio of the raw material gas. Fig.11 In (b), the peak caused by the composite defect of group III holes and Si is not confirmed in the n-type contact layer 12 whose V / III ratio of the raw material gas is 1100-1600, but can be confirmed in the n-type contact layer 12 whose V / III ratio of the raw material gas is 3200.
[0261] Since the more compound defects of group III holes and Si are, the greater the resistance of the n-type contact layer 12 is, the greater the resistance of the n-type contact layer 12 is. Fig.11 The result obtained by (b) is similar to that obtained by Fig. 9The obtained results are consistent, that is, when the V / III ratio of the raw material gas of the n-type contact layer 12 is in the range of 1000 to 3200, a low resistivity can be obtained.
[0262] Fig.11 (c) in FIG. 1 shows the change in the shape of the CL spectrum of the n-type contact layer 12 as a function of the growth temperature. Fig.11 In (c), the peak due to the composite defect of group III holes and Si is not confirmed in the n-type contact layer 12 grown at a temperature of 1010 to 1080°C, but is confirmed in the n-type contact layer 12 grown at a temperature of 1170°C.
[0263] Since the more compound defects of group III holes and Si are, the greater the resistance of the n-type contact layer 12 is, the greater the resistance of the n-type contact layer 12 is. Fig.11 The result obtained by (c) is similar to that obtained by Fig.10 The obtained results are consistent, that is, the resistance starts to increase when the growth temperature of the n-type contact layer 12 is about 1100 to 1150° C.
[0264] Example 2
[0265] The following describes the evaluation results of the characteristics of the n-type contact layer 212 involved in the third embodiment described above. In this embodiment, the n-type contact layer 212 is formed on the substrate 210 with the buffer layer 211 interposed therebetween under various conditions described below, and these n-type contact layers 212 are evaluated. The following Table 6 shows the composition and growth conditions of the substrate 210, buffer layer 211, and n-type contact layer 212 involved in this embodiment.
[0266] [Table 6]
[0267]
[0268] In this embodiment, the resistivity, carrier concentration and mobility of the n-type contact layer 212 are measured by hole effect measurement, the Si concentration is measured by secondary ion mass spectrometry (SIMS), and the transmittance is measured by a spectrophotometer.
[0269] Fig.12 : is a graph showing the relationship between the Al component of the n-type contact layer 212 and the transmittance of deep ultraviolet light with a wavelength of 280 nm. Fig.12 The thickness of the n-type contact layer 212 involved is 500 nm. Fig.12It is shown that if the Al content of the n-type contact layer 212 is 50% or more, the transmittance of deep ultraviolet light with a wavelength of 280nm exceeds 50%, if the Al content is 55% or more, the transmittance of deep ultraviolet light with a wavelength of 280nm exceeds 70%, and if the Al content is 60% or more, the transmittance of deep ultraviolet light with a wavelength of 280nm is almost 100%. This result also applies to the n-type contact layer 216 composed of the same n-type AlGaN as the n-type contact layer 212. The following Table 7 shows Fig.12 The values of the plotted points.
[0270] [Table 7]
[0271] Al composition Transmittance 0% 0.0% 8% 0.0% 20% 0.1% 29% 0.2% 33% 8.3% 40% 21.2% 63% 100.0%
[0272] Fig.13 : is a graph showing the relationship between the Al composition and the resistivity of the n-type contact layer 212 . Fig.13 It is shown that if the Al content of the n-type contact layer 212 exceeds about 70%, the resistance increases. This result also applies to the n-type contact layer 216 composed of the same n-type AlGaN as the n-type contact layer 212. The following Table 8 shows Fig.13 The values of the plotted points.
[0273] [Table 8]
[0274]
[0275] Fig.14 (a) to (c) are graphs showing the relationship between the Si concentration and the resistivity of the n-type contact layer 212 . Fig.14 (a) Fig.14 (b) Fig.14 The growth temperature of the n-type contact layer 212 and the V / III ratio of the raw material gas involved in (c) are different. Fig.14 (a) to (c) show that if the Si concentration of the n-type contact layer 212 exceeds about 4.0×10 19 cm - 3, the resistance increases.
[0276] Based on this result, it can be said that if the Al content of the n-type contact layer 212 is 50% or more, high transmittance can be ensured for deep ultraviolet light in the wavelength region of 270 to 290 nm close to 280 nm and light with a longer wavelength than this. In addition, if the Al content is 55% or more, higher transmittance can be ensured, and if the Al content is 60% or more, even higher transmittance can be ensured. This result also applies to the n-type contact layer 216 composed of the same n-type AlGaN as the n-type contact layer 212. The following Table 9 shows Fig.14 The values of the plotted points.
[0277] [Table 9]
[0278]
[0279] Fig.15 (a) to (c) are graphs showing the temperature dependence of the resistivity, carrier concentration, and mobility of the n-type contact layer 212 . Fig.15 (a) to (c) show that the Si concentration is 2.10×10 19 cm -3 3.20×10 19 cm -3 4.30×10 19 cm -3 The measured values of these three types of n-type contact layers 212 are shown in FIG.
[0280] In n-type AlGaN, where the Fermi level and conduction band are degenerate, there is almost no temperature dependence of carrier concentration. Fig.15 In (b), when the Si concentration is 2.10×10 19 cm -3 3.20×10 19 cm -3 4.30×10 19 cm -3 In any of the n-type contact layers 212 , the temperature dependence of the carrier concentration is small, and therefore it can be determined that the Fermi level and the conduction band are degenerate.
[0281] On the other hand, even when the Fermi level and the conduction band are degenerate, if there are complex defects of group III holes and Si, carriers will be scattered by the defects, so the mobility depends on the temperature. Fig.15 In (c), when the Si concentration is 2.10×10 19 cm -3 3.20×10 19 cm -3 In the n-type contact layer 212, there is almost no temperature dependence of mobility, but when the Si concentration is 4.30×10 19 cm -3 The n-type contact layer 212 has a large temperature dependence of mobility. This is considered to be because the Si concentration is high, so there are a large number of complex defects of group III holes and Si.
[0282] In addition, according to Fig.15 In (a), when the Si concentration is 2.10×10 19 cm -3 3.20×10 19 cm -3In the n-type contact layer 212, the resistivity has almost no temperature dependence, but when the Si concentration is 4.30×10 19 cm -3 The n-type contact layer 212 has a large temperature dependence of resistivity.
[0283] In the case of AlGaN where the Fermi level and conduction band are not degenerate, the resistivity also depends on temperature, but is determined by Fig.15 It can be confirmed from (b) that the Si concentration is 4.30×10 19 cm -3 The n-type contact layer 212 is degenerate, so it is considered that the Si concentration is 4.30×10 19 cm -3 The temperature dependence of the resistivity of the n-type contact layer 212 is caused by the presence of a large number of compound defects of group III holes and Si.
[0284] Fig.16 Spectra (CL spectra) obtained by cathode luminescence measurement of various n-type contact layers 212 are shown. The peak with a photon energy of about 2.4 eV in the CL spectrum of the n-type contact layer 212 is caused by luminescence due to the recombination defects of group III holes and Si. The greater the intensity of the peak, the more recombination defects of group III holes and Si.
[0285] The peak at a photon energy of about 3.2 eV is due to light emission from C at the group V site, and the peak at a photon energy of about 4.9 eV is due to light emission corresponding to the band gap.
[0286] Fig.16 The shape of the CL spectrum of the n-type contact layer 212 changes with the Si concentration. Fig.16 For the peaks due to the combined defects of group III holes and Si, when the Si concentration is 4.0×10 18 ~3.0×10 19 cm -3 No ions were found in the n-type contact layer 212. 19 cm -3 A weak peak appears in the n-type contact layer 212. When the Si concentration is 6.0×10 19 cm -3 A strong peak appears in the n-type contact layer 212.
[0287] Since the more compound defects of group III holes and Si are, the greater the resistance of the n-type contact layer 212 is, the greater the resistance of the n-type contact layer 212 is. Fig.16 The results obtained are similar to those obtained by Fig.14 The results obtained in (a) to (c) are consistent, that is, if the Si concentration of the n-type contact layer 212 exceeds about 4.0×1019 cm -3 , the resistance increases.
[0288] The above embodiments and examples of the present invention are described, but the present invention is not limited to the above embodiments and examples, and various modifications can be implemented without departing from the scope of the main purpose of the invention. In addition, the constituent elements of the above embodiments and examples can be arbitrarily combined without departing from the scope of the main purpose of the invention.
[0289] In addition, the above-described embodiments and examples do not limit the invention involved in the scope of the patent application. In addition, it should be noted that in the means for solving the problems of the invention, not all combinations of features described in the embodiments and examples are necessary.
Claims
1. A light emitting element, comprising: The n-type contact layer is composed of n-type AlGaN. a light-emitting layer emitting deep ultraviolet light on the n-type contact layer, A current diffusion layer composed of AlGaN containing two-dimensional hole gas on the light-emitting layer, a p-type contact layer connected to a portion of the upper surface of the current diffusion layer and composed of p-type GaN or p-type AlGaN having an Al content of 35% or less, an n-electrode connected to the n-type contact layer, and a p-electrode connected to the p-type contact layer; In the cathode luminescence measurement of the n-type contact layer, no peak due to the complex defect of group III holes and Si was confirmed; An area of a region of the upper surface of the current diffusion layer that contacts the p-type contact layer is in a range of 40% to 80% of an area of the entire upper surface.
2. The light-emitting element according to claim 1, wherein The current diffusion layer comprises: a first AlGaN layer composed of p-type AlGaN having an Al content in the range of 50% to 70%, and a second AlGaN layer directly disposed on the first AlGaN layer and composed of p-type or i-type AlGaN having an Al content in the range of 30% to 50%; The second AlGaN layer has the two-dimensional hole gas near the interface with the first AlGaN layer.
3. The light-emitting element according to claim 1 or 2, wherein: At least a portion of a region other than a region connected to the p-type contact layer on the upper surface of the current diffusion layer is covered with a passivation film made of an insulating material.
4. The light-emitting element according to claim 1 or 2, wherein: A light reflecting layer is provided above a region of the upper surface of the current diffusion layer other than a region connected to the p-type contact layer.
5. A light emitting element comprising: A first n-type contact layer composed of AlGaN, a light-emitting layer emitting deep ultraviolet light on the first n-type contact layer, a p-type layer composed of AlGaN on the light-emitting layer, the p-type layer having a superlattice structure in which a plurality of first layers each composed of AlGaN and a plurality of second layers having an Al composition different from that of the first layers are alternately stacked, and the Al composition of the second layers is greater than that of the first layers, A second n-type contact layer on the p-type layer, which forms a tunnel junction with the p-type layer, has a degenerate Fermi level and a conduction band, and is made of AlGaN; an n-electrode connected to the first n-type contact layer, and a p-electrode connected to the second n-type contact layer; Two-dimensional hole gas is contained at the interface between the p-type layer and the second n-type contact layer, and at each interface between the plurality of first layers and the plurality of second layers of the p-type layer. The Al content of the second n-type contact layer is in the range of 40% to 70%; In the cathode luminescence measurement of the first n-type contact layer and the second n-type contact layer, no peak due to the recombination defect of the group III holes and Si was confirmed.
6. The light emitting element according to claim 5, wherein The second n-type contact layer has a concentration of 4.0×10 19 cm -3 Si is contained at the following concentrations.
7. The light-emitting element according to claim 5 or 6, wherein: A portion of the n-electrode in contact with the first n-type contact layer and a portion of the p-electrode in contact with the second n-type contact layer are made of the same material.
8. The light-emitting element according to claim 7, wherein The material is aluminum.
Citation Information
Patent Citations
Nitride semiconductor light-emitting element
JP2019110195A
Nitride semiconductor light-emitting element and process for production thereof
CN102334204A
Ultraviolet semiconductor light emitting device and manufacturing method thereof
CN102810609A
Light emitting diode and preparation method thereof
CN103367594A
Light emitting device inserted with current homogenizing structure and manufacturing method thereof
CN103811610A