Secondary battery

By using the difference in the average surface roughness of the active substances of the first compound layer and the second compound layer in the winding electrode body, the problem of battery reaction is solved and the cycle characteristics of the battery is improved.

CN113826236BActive Publication Date: 2024-12-06PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202080021765.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-18
Filing Date
2020-03-06
Publication Date
2024-12-06
Estimated Expiration
2040-03-06

AI Technical Summary

Technical Problem

In the winding electrode body, the density difference between the first compound layer and the second compound layer causes uneven battery reactions and reduced circulation characteristics.

Method used

The active substance with different average surface roughness of the positive electrode and the negative electrode are used to reduce the density difference of the mixture layer and improve the circulation characteristics of the battery by making the average surface roughness of the first active substance greater than the average surface roughness of the second active substance.

Benefits of technology

With this electrode structure, uneven battery reactions are suppressed and the circulation characteristics of the secondary battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113826236B_ABST
    Figure CN113826236B_ABST
Patent Text Reader

Abstract

The object of the present invention is to improve the cycle characteristics in a secondary battery having a wound electrode body. A secondary battery as an example of an embodiment has a wound electrode body in which a positive electrode and a negative electrode are wound with a separator. The positive electrode has a positive electrode collector, a first positive electrode mixture layer formed on a first surface of the positive electrode collector facing the outside of the electrode body, and a second positive electrode mixture layer formed on a second surface of the positive electrode collector facing the inside of the electrode body. The first positive electrode mixture layer includes a first positive electrode active material, the second positive electrode mixture layer includes a second positive electrode active material, and the average surface roughness of the first positive electrode active material is greater than the average surface roughness of the second positive electrode active material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a secondary battery, and more particularly, to a secondary battery including a wound electrode assembly. Background Art

[0002] The electrodes that make up a wound electrode assembly include a current collector and a mixture layer formed on the surface of the current collector. The mixture layer includes a first mixture layer formed on the first surface of the current collector facing the inside of the electrode assembly, and a second mixture layer formed on the second surface of the current collector facing the outside of the electrode assembly. Patent Document 1 discloses a non-aqueous electrolyte secondary battery in which the active material filling density of the first negative electrode mixture layer is 5% to 20% lower than that of the second negative electrode mixture layer to improve battery cycle performance.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 6-290774 Summary of the Invention

[0006] Problems to be solved by the invention

[0007] However, in electrodes that constitute a wound electrode assembly, the second composite layer is stretched during winding, creating gaps between the active material particles, which tends to reduce the density of the second composite layer. On the other hand, the first composite layer is compressed during winding, reducing the gaps between the active material particles and increasing the density. In other words, a density difference is created between the first and second composite layers. As a result, it is believed that the battery reaction becomes uneven in the first and second composite layers, reducing the battery's cycle performance.

[0008] An object of the present invention is to improve the cycle characteristics of a secondary battery including a wound electrode assembly.

[0009] Means for solving problems

[0010] A secondary battery, one embodiment of the present invention, includes a wound electrode body formed by winding a positive electrode and a negative electrode with a separator interposed therebetween. The positive electrode and the negative electrode each include a current collector, a first material mixture layer formed on a first surface of the current collector facing inwardly of the electrode body, and a second material mixture layer formed on a second surface of the current collector facing outwardly of the electrode body. In at least one of the positive electrode and the negative electrode, the first material mixture layer includes a first active material, and the second material mixture layer includes a second active material. The first active material has a greater average surface roughness than the second active material.

[0011] Effects of the Invention

[0012] According to one embodiment of the present invention, the cycle characteristics of a secondary battery including a wound electrode assembly can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is a cross-sectional view of a secondary battery as an example of an embodiment.

[0014] Figure 2 This is a cross-sectional view of a positive electrode as an example of an embodiment.

[0015] Figure 3A This is a diagram showing the positive electrode active material (A) of Example 1.

[0016] Figure 3B This is a diagram for explaining a method for measuring the average surface roughness of the positive electrode active material (A) of Example 1.

[0017] Figure 4A This is a diagram showing the positive electrode active material (B) of Example 1.

[0018] Figure 4B This is a diagram for explaining a method for measuring the average surface roughness of the positive electrode active material (B) of Example 1. DETAILED DESCRIPTION

[0019] The present inventors have discovered that in a secondary battery with a wound electrode assembly, using a first active material in a first material mix layer facing the inside of the electrode assembly and a second active material in a second material mix layer facing the outside of the electrode assembly, and by making the average surface roughness of the first active material greater than that of the second active material, the battery's cycle performance can be significantly improved. It is believed that by employing this electrode structure, the density difference between the first and second material mix layers is reduced, which suppresses uneven battery reactions and, as a result, improves the battery's cycle performance.

[0020] Below, an example embodiment of the present invention is described in detail. The drawings referenced in the description of the embodiment are schematic, so the dimensional ratios of the various components should be determined by referring to the following description. It should be noted that in this specification, unless otherwise specified, the description of "value A to value B" means that the value is greater than value A and less than value B.

[0021] In this embodiment, a secondary battery 10 is shown in which a wound electrode assembly 14 is housed in a bottomed cylindrical outer can 16. However, the outer can is not limited to a cylindrical outer can. For example, a rectangular outer can or an outer can made of a laminated sheet including a metal layer and a resin layer may be used. The electrode assembly may have a wound structure and may also be formed into a flat shape.

[0022] Figure 1 1 is a cross-sectional view of a secondary battery 10 as an example of an embodiment. Figure 1 As shown, the secondary battery 10 includes an electrode body 14, an electrolyte (not shown), and an outer can 16 for housing the electrode body 14 and the electrolyte. The electrode body 14 includes a positive electrode 11, a negative electrode 12, and a separator 13, and has a spirally wound structure in which the positive electrode 11 and the negative electrode 12 are interposed with the separator 13. The outer can 16 is a metal container with a bottom and a cylindrical shape that is open at one axial end. The opening of the outer can 16 is sealed by a sealing member 17. For ease of description, the sealing member 17 side of the secondary battery 10 is referred to as the top, and the bottom side of the outer can 16 is referred to as the bottom.

[0023] The electrolyte may be, for example, a non-aqueous electrolyte. The non-aqueous electrolyte comprises a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent include esters, ethers, nitriles, amides, and mixed solvents of two or more thereof. The non-aqueous solvent may contain a halogen-substituted substance in which at least a portion of the hydrogen atoms of these solvents is replaced by a halogen atom such as fluorine. It should be noted that the non-aqueous electrolyte is not limited to a liquid electrolyte and may also be a solid electrolyte. Examples of the electrolyte salt include lithium salts such as LiPF6. An example of a preferred secondary battery 10 is a non-aqueous electrolyte secondary battery such as a lithium ion battery.

[0024] The electrode assembly 14 is composed of an elongated positive electrode 11, an elongated negative electrode 12, two elongated separators 13, a positive electrode tab 20 joined to the positive electrode 11, and a negative electrode tab 21 joined to the negative electrode 12. To prevent lithium precipitation, the negative electrode 12 is formed slightly larger than the positive electrode 11. In other words, the negative electrode 12 is formed longer than the positive electrode 11 in both the length and width (short side) directions. The two separators 13 are formed to be at least slightly larger than the positive electrode 11 and are, for example, arranged to sandwich the positive electrode 11.

[0025] Insulating plates 18 and 19 are respectively arranged above and below the electrode body 14. Figure 1 In the illustrated example, the positive electrode tab 20 attached to the positive electrode 11 extends through a through-hole in the insulating plate 18 toward the sealing body 17, while the negative electrode tab 21 attached to the negative electrode 12 extends from the outside of the insulating plate 19 toward the bottom of the outer can 16. The positive electrode tab 20 is connected to the lower surface of an internal terminal plate 23 of the sealing body 17 by welding or the like. The top plate of the sealing body 17, or lid 27, which is electrically connected to the internal terminal plate 23, serves as the positive electrode terminal. The negative electrode tab 21 is connected to the inner bottom surface of the outer can 16 by welding or the like, with the outer can 16 serving as the negative electrode terminal.

[0026] The outer can 16 has a groove 22 formed, for example, by pressing the side surface from the outside, to support the sealing body 17. The groove 22 is preferably formed in an annular shape along the circumference of the outer can 16, and supports the sealing body 17 on its upper surface. A gasket 28 is provided between the outer can 16 and the sealing body 17 to hermetically seal the interior of the battery. Furthermore, the upper end of the outer can 16 is bent inward and riveted to the peripheral edge of the sealing body 17.

[0027] The sealing body 17 has a structure in which an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26 and a cover 27 are stacked in order from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected at their respective central portions, and the insulating member 25 is sandwiched between their respective peripheral portions. If the internal pressure of the battery rises due to abnormal heat, the lower valve body 24 is deformed and broken in a manner that pushes the upper valve body 26 upward toward the cover 27 side, thereby cutting off the current path between the lower valve body 24 and the upper valve body 26. If the internal pressure rises further, the upper valve body 26 breaks, and the gas is discharged from the opening of the cover 27.

[0028] Hereinafter, the positive electrode 11 , the negative electrode 12 , and the separator 13 constituting the electrode assembly 14 , particularly the positive electrode 11 , will be described in detail.

[0029] [positive electrode]

[0030] The positive electrode 11 includes a positive electrode current collector 30, a positive electrode mixture layer 31 (first positive electrode mixture layer) formed on a first surface 30A of the positive electrode current collector 30 facing the inner side of the electrode body 14, and a positive electrode mixture layer 32 (second positive electrode mixture layer) formed on a second surface 30B of the positive electrode current collector 30 facing the outer side of the electrode body 14. The positive electrode current collector 30 can be made of a foil of a metal such as aluminum or an aluminum alloy that is stable within the potential range of the positive electrode 11, or a film having the metal disposed on the surface. The thickness of the positive electrode current collector 30 is, for example, not less than 5 μm and not more than 20 μm. The positive electrode mixture layers 31 and 32 include a positive electrode active material, a conductive agent, and a binder. The thickness of the positive electrode mixture layers 31 and 32 is, for example, substantially the same as each other, preferably not less than 50 μm and not more than 150 μm, and more preferably not less than 80 μm and not more than 120 μm.

[0031] The positive electrode mixture layer 31 contains a first positive electrode active material, and the positive electrode mixture layer 32 contains a second positive electrode active material. That is, the positive electrode mixture layers 31 and 32 contain positive electrode active materials having different average surface roughnesses. The compositions of the first positive electrode active material and the second positive electrode active material may be the same or different. The content of the positive electrode active material in the positive electrode mixture layers 31 and 32 may be the same or different. Furthermore, the types and contents of the conductive agent and binder may be the same or different in the positive electrode mixture layers 31 and 32. The positive electrode 11 can be manufactured, for example, as follows: a first positive electrode mixture slurry containing a first positive electrode active material is applied to the surface of the positive electrode collector 30 on one side becoming the first surface 30A, and a second positive electrode mixture slurry containing a second positive electrode active material is applied to the surface of the other side becoming the second surface 30B of the positive electrode collector 30. After the coating is dried to remove the dispersion medium, the coating is compressed to form positive electrode mixture layers 31 and 32 on each surface of the positive electrode collector 30.

[0032] The first positive electrode active material and the second positive electrode active material are both composed of a lithium transition metal composite oxide as a main component. As the metal elements contained in the lithium transition metal composite oxide, Ni, Co, Mn, Al, B, Mg, Ti, V, Cr, Fe, Cu, Zn, Ga, Sr, Zr, Nb, In, Sn, Ta, Mo, Ce, K, W, etc. can be mentioned. The lithium transition metal composite oxide preferably contains at least one selected from Ni, Co, and Mn. An example of a suitable lithium transition metal composite oxide is a composite oxide containing Ni, Co, and Mn, or a composite oxide containing Ni, Co, and Al. It should be noted that inorganic compound particles such as aluminum oxide and compounds containing lanthanide elements can be fixed to the surface of the composite oxide particles.

[0033] The volume-based median particle size (hereinafter referred to as "D50") of the first positive electrode active material and the second positive electrode active material is, for example, substantially the same, preferably 4 μm or more and 30 μm or less, more preferably 10 μm or more and 25 μm or less. D50 is the particle size at which the volume cumulative value in the particle size distribution measured by the laser diffraction scattering method becomes 50%, also known as the 50% particle size or median particle size. The first positive electrode active material and the second positive electrode active material are, for example, secondary particles formed by the aggregation of primary particles, and the primary particles are composed of crystallites.

[0034] The average particle size of the primary particles is preferably 1 μm or more and 5 μm or less. If the average particle size of the primary particles is less than 1 μm, the surface roughness of the secondary particles sometimes becomes too large. On the other hand, if the average particle size of the primary particles exceeds 5 μm, the particle size of the secondary particles sometimes becomes too large. The particle size of the primary particles is measured using a scanning electron microscope (SEM). Specifically, the particles of the positive electrode active material are observed by SEM at a magnification of 2000 times, and 10 particles are randomly selected from the SEM image of the obtained particles to observe the grain boundaries, etc., to obtain the longest diameter of each primary particle, and the average value of the 10 particles is used as the average particle size.

[0035] The average surface roughness of the first positive electrode active material contained in the positive electrode mixture layer 31 is greater than the average surface roughness of the second positive electrode active material contained in the positive electrode mixture layer 32. The average surface roughness of the first positive electrode active material is preferably 2.3% to 20%, more preferably 2.3% to 6.6%. On the other hand, the average surface roughness of the second positive electrode active material contained in the positive electrode mixture layer 32 is preferably 1% to 6.2%. Compared to the first positive electrode active material, the second positive electrode active material has smoother particle surfaces with fewer irregularities.

[0036] The second positive electrode active material particles have smooth surfaces, making it easier for the particles to pack tightly together during compression during the manufacturing process of the positive electrode 11. This results in a higher density for the positive electrode mixture layer 32 containing the second positive electrode active material. On the other hand, in the positive electrode mixture layer 31 containing the first positive electrode active material particles, which have rougher surfaces, the particles become stuck together during the compression process, making it difficult to pack tightly together. Consequently, the density tends to be lower than that of the positive electrode mixture layer 32. By winding the positive electrode 11, which has a density difference (positive electrode mixture layer 31 density < positive electrode mixture layer 32 density), with the negative electrode 12 and separator 13, the positive electrode mixture layer 31 is compressed, resulting in a higher density, while the positive electrode mixture layer 32 is stretched, resulting in a lower density. Therefore, it is believed that in the positive electrode 11, the density of the positive electrode mixture layer 31 is approximately the density of the positive electrode mixture layer 32, improving the battery's cycle performance.

[0037] The surface roughness of the positive electrode active material was measured based on SEM images of particles using the method described in International Publication No. 2011 / 125577. The surface roughness was calculated using the following formula.

[0038] Surface roughness = (maximum change in particle radius per 1°) / (longest particle diameter)

[0039] The average surface roughness is calculated by averaging the surface roughness of 10 randomly selected particles. The details of the method for measuring the average surface roughness will be described later.

[0040] The circularity of the first positive electrode active material and the second positive electrode active material is, for example, substantially the same as each other, and from the viewpoint of the filling property in the mixture layer, is preferably 0.85 or more, more preferably 0.88 or more. The circularity of the positive electrode active material is an index of sphericity when the particle is projected onto a two-dimensional plane, and is measured by placing the sample into a measurement system and irradiating the sample flow with a stroboscopic light to obtain a particle image. The calculation formula of circularity is as follows. It should be noted that when the particle image is a perfect circle, the circularity is 1.

[0041] Circularity = (circumference of a circle with the same area as the particle image) / (circumference of the particle image)

[0042] As described above, the first positive electrode active material and the second positive electrode active material are composed of lithium transition metal composite oxides, for example, x Ni y M 1-y The invention is composed of a composite oxide having a layered rock salt type crystal structure represented by O2. In the formula, 0.1≤x≤1.2, 0.3<y<1, and M is at least one metal element selected from Ni, Co, Mn, Al, B, Mg, Ti, V, Cr, Fe, Cu, Zn, Ga, Sr, Zr, Nb, In, Sn, Ta, Mo, Ce, K, and W.

[0043] Lithium transition metal composite oxides can be synthesized from a lithium raw material or by ion-exchanging sodium for lithium after synthesizing a sodium transition metal composite oxide. Sodium transition metal composite oxides are synthesized using a sodium raw material and a transition metal compound such as nickel. By setting the calcination temperature to 600°C to 1100°C during the synthesis of sodium transition metal composite oxides, a composite oxide with an undistorted crystal structure can be synthesized. Furthermore, the lithium transition metal composite oxides obtained by ion exchange are generally spherical and have an average surface roughness of 20% or less.

[0044] As the sodium raw material, at least one selected from sodium (metallic sodium) and sodium compounds can be used. Specifically, oxides such as Na2O, Na2O2, salts such as Na2CO3, NaNO3, hydroxides such as NaOH, etc. can be exemplified. Among them, NaNO3 is preferred. The transition metal compound can be, for example, any of oxides, salts, hydroxides, and oxyhydroxides. In the case of nickel compounds, oxides such as Ni3O4, Ni2O3, NiO2, salts such as NiCO3, NiCl2, hydroxides such as Ni(OH)2, oxyhydroxides such as NiOOH, etc. can be exemplified. Among them, NiO2 and Ni(OH)2 are preferred.

[0045] The mixture of the sodium raw material and the transition metal compound can be prepared using a conventionally known mixer. The sodium transition metal composite oxide can be synthesized by calcining the mixture in the atmosphere or in an oxygen stream. The calcination temperature is appropriately set according to the composition of the mixture, and is preferably 600° C. to 1100° C. For example, when the calcination temperature is 600° C. to 1100° C., the calcination time is preferably 1 hour to 50 hours. After calcination, the calcined product is preferably pulverized as needed.

[0046] The average surface roughness of the positive electrode active material can be adjusted by, for example, changing the firing temperature during the synthesis of the sodium transition metal composite oxide. The average surface roughness of the positive electrode active material tends to increase as the firing temperature decreases within the temperature range of 600°C to 1100°C. As a specific example, in a sodium transition metal composite oxide composed of Na 0.95 Ni 0.35 Co 0.35 Mn 0.3 In the case of O 2 expression, if the firing temperature is set to 500° C. or higher and 1100° C. or lower, the average surface roughness can be adjusted within a range of 1% or higher and 20% or lower.

[0047] As a method for ion-exchanging sodium for lithium, a method of adding a molten salt bed of a lithium salt to a sodium transition metal composite oxide and heat-treating the mixture can be mentioned. The lithium salt is, for example, at least one selected from lithium nitrate, lithium sulfate, lithium chloride, lithium carbonate, lithium hydroxide, lithium iodide, and lithium bromide. Alternatively, sodium can be ion-exchanged for lithium by immersing a sodium-containing transition metal oxide in a solution containing a lithium salt. The temperature during the ion exchange treatment is preferably 150°C to 400°C. The treatment time is preferably 2 to 20 hours, more preferably 5 to 15 hours.

[0048] It should be noted that in the lithium transition metal composite oxide synthesized by the above ion exchange method, the ion exchange is sometimes not completely carried out and a certain amount of sodium remains. In this case, the lithium transition metal composite oxide is composed of the general formula Li xu Na x(1-u) Ni y M 1-y Here, u is the ion exchange rate, preferably 0.95<u≤1.

[0049] Examples of the conductive agent contained in the positive electrode mixture layers 31 and 32 include carbon materials such as carbon black, acetylene black, Ketjen black, and graphite. Examples of the binder contained in the positive electrode mixture layers 31 and 32 include fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, and polyolefin. These resins may also be used in combination with cellulose derivatives such as carboxymethyl cellulose (CMC) or its salts, polyethylene oxide (PEO), and the like.

[0050] [negative electrode]

[0051] The negative electrode 12 includes a negative electrode current collector 40 and a negative electrode mixture layer 41 formed on both sides of the negative electrode current collector 40. The negative electrode current collector 40 can be made of a foil of a metal such as copper or a copper alloy that is stable within the potential range of the negative electrode 12, or a film having the metal disposed on the surface. The thickness of the negative electrode current collector 40 is, for example, not less than 5 μm and not more than 20 μm. The negative electrode mixture layer 41 contains a negative electrode active material and a binder. The thickness of the negative electrode mixture layer 41 is preferably not less than 50 μm and not more than 150 μm, more preferably not less than 80 μm and not more than 120 μm, measured on one side of the negative electrode current collector 40. The negative electrode 12 can be manufactured as follows: a negative electrode mixture slurry containing a negative electrode active material and a binder is applied to the negative electrode current collector 40, the coating is dried to remove the dispersion medium, and then the coating is compressed to form the negative electrode mixture layer 41 on both sides of the negative electrode current collector 40.

[0052] In this embodiment, the first negative electrode mixture layer formed on the first surface of the negative electrode current collector 40 facing the inner side of the electrode body 14 and the second negative electrode mixture layer formed on the second surface of the negative electrode current collector 40 facing the outer side of the electrode body 14 are composed of the same material. In other words, the negative electrode mixture layer 41 formed on the first and second surfaces of the negative electrode current collector 40 contains the same negative electrode active material. However, similarly to the positive electrode 11, in the negative electrode 12, the average surface roughness of the first negative electrode active material contained in the first negative electrode mixture layer can be greater than the surface roughness of the second negative electrode active material contained in the second negative electrode mixture layer. Alternatively, only the negative electrode 12 can have a structure including these two mixture layers.

[0053] In the negative electrode mixture layer 41, the negative electrode active material includes, for example, a carbon-based active material that reversibly occludes and releases lithium ions. Preferred carbon-based active materials include natural graphites such as flaky graphite, bulk graphite, and amorphous graphite, and artificial graphites such as bulk artificial graphite (MAG) and graphitized mesocarbon microbeads (MCMB). Alternatively, the negative electrode active material may be a Si-based active material composed of at least one of Si and a Si-containing compound, or a combination of a carbon-based active material and a Si-based active material.

[0054] The binder contained in the negative electrode mixture layer 41 can be a fluororesin such as PTFE and PVdF, PAN, polyimide, acrylic resin, polyolefin, etc., similarly to the case of the positive electrode 11, and preferably styrene-butadiene rubber (SBR) can be used. In addition, the negative electrode mixture layer 41 can contain CMC or its salt, polyacrylic acid (PAA) or its salt, PVA, etc. CMC or its salt functions as a thickener to adjust the negative electrode mixture slurry to an appropriate viscosity range, and also functions as a binder similar to SBR.

[0055] [Spacer]

[0056] A porous sheet having ion permeability and insulating properties can be used for the separator 13. Specific examples of porous sheets include microporous films, woven fabrics, and non-woven fabrics. Preferred materials for the separator 13 include olefin resins such as polyethylene and polypropylene, and cellulose. The separator 13 can have either a single-layer structure or a laminated structure. A heat-resistant layer or the like can also be formed on the surface of the separator 13.

[0057] Example

[0058] Hereinafter, the present invention will be further described with reference to examples, but the present invention is not limited to these examples.

[0059] <Example 1>

[0060] [Preparation of positive electrode mixture slurry (A)]

[0061] To obtain the general formula Na 0.95 Ni 0.35 Co 0.35 Mn 0.3 Sodium nitrate, nickel oxide, cobalt oxide, and manganese oxide were mixed in the form of a composite oxide represented by O2, and the mixture was calcined at 750°C for 35 hours to obtain a sodium transition metal composite oxide. A molten salt bed containing lithium nitrate and lithium hydroxide at a molar ratio of 61:39 was added, which was 5 times the equivalent of the obtained sodium transition metal composite oxide. The mixture was heat-treated at 200°C for 10 hours to ion-exchange the sodium in the composite oxide with lithium, and then washed with water to obtain a lithium transition metal composite oxide.

[0062] The obtained lithium transition metal composite oxide was subjected to crystal structure identification using a powder X-ray diffraction (XRD) analyzer (RINT2200, manufactured by Rigaku Corporation, with a Cu-Kα radiation source), and the crystal structure was found to be a layered rock salt type. In addition, the composition was analyzed using an inductively coupled plasma (ICP) emission spectrometer (iCAP6300, manufactured by Thermo Fisher Scientific Corporation), and the composition was found to be Li 0.95 Ni 0.35 Co 0.35 Mn 0.3 O2. The lithium transition metal composite oxide is classified to obtain a positive electrode active material (A).

[0063] 92 parts by mass of the positive electrode active material (A), 5 parts by mass of carbon powder, and 3 parts by mass of PVdF were mixed, and N-methyl-2-pyrrolidone was used as a dispersion medium to prepare a positive electrode mixture slurry (A).

[0064] [Preparation of positive electrode mixture slurry (B)]

[0065] A positive electrode active material (B) was synthesized in the same manner as that for the positive electrode active material (A) except that the calcination temperature during the synthesis of the sodium transition metal composite oxide was changed from 750°C to 1100°C, thereby preparing a positive electrode mixture slurry (B).

[0066] [About positive electrode active materials (A, B)]

[0067] like Figure 3A and Figure 4A As schematically shown in Figure 2, the positive electrode active material (B) has a smoother particle surface with fewer irregularities than the positive electrode active material (A). The D50 of the positive electrode active material (A) is 10.5 μm, with an average surface roughness of 4.5%. The D50 of the positive electrode active material (B) is 10.0 μm, with an average surface roughness of 1.1%.

[0068] [Production of positive electrode]

[0069] Positive electrode mixture slurry (A) is applied to one side of a positive electrode current collector formed of aluminum foil, and positive electrode mixture slurry (B) is applied to the other side of the positive electrode current collector. After drying, the coating is compressed using a roller and cut into a predetermined electrode size. This produces a positive electrode having a positive electrode mixture layer (A) formed on one side of the positive electrode current collector and a positive electrode mixture layer (B) formed on the other side.

[0070] [Production of negative electrode]

[0071] As the negative electrode active material, graphite powder is used. 99 parts by mass of the negative electrode active material and 1 part by mass of CMC are dry-mixed, water is added to the mixed powder to prepare an aqueous dispersion with a solid content concentration of 50% by mass. In the aqueous dispersion, a dispersion of SBR is added in an amount of 1% by mass relative to the negative electrode active material to prepare a negative electrode mixture slurry. The negative electrode mixture slurry is applied to both sides of a negative electrode collector consisting of copper foil, and after the coating is dried, the coating is compressed using a roller and cut into a specified electrode size to produce a negative electrode having a negative electrode mixture layer formed on both sides of the negative electrode collector.

[0072] [Production of Electrode Body]

[0073] The positive electrode and the negative electrode are wound around a core having a curvature radius of 1.5 mm via a separator having a thickness of 20 μm formed of a polyethylene microporous film, and a tape is applied to the outermost surface to produce a cylindrical wound electrode body. At this time, the positive electrode is wound with the positive electrode mixture layer (A) facing the core side. It should be noted that an aluminum positive electrode lead is welded to the exposed portion of the positive electrode collector, and a nickel negative electrode lead is welded to the exposed portion of the negative electrode collector.

[0074] [Preparation of non-aqueous electrolyte]

[0075] In a mixed solvent of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate at a volume ratio of 20:60:20, vinylene carbonate was dissolved at a concentration of 2% by mass. Then, LiPF6 was dissolved at a concentration of 1.3 mol / L to prepare a non-aqueous electrolyte.

[0076] [Battery Production]

[0077] The electrode assembly was housed in a bottomed cylindrical outer can. The positive electrode lead was welded to the sealing member, and the negative electrode lead was welded to the inner surface of the bottom of the outer can. The non-aqueous electrolyte was then injected into the outer can, and the opening of the outer can was sealed with the sealing member to produce a non-aqueous electrolyte secondary battery (65 mm in height, 18 mm in diameter, and a designed capacity of 3000 mAh).

[0078] <Example 2>

[0079] A positive electrode and a nonaqueous electrolyte secondary battery were produced in the same manner as in Example 1 except that the calcination temperature during the synthesis of the sodium transition metal composite oxide was changed from 1100° C. to 900° C. in the synthesis of the positive electrode active material (B).

[0080] <Example 3>

[0081] A positive electrode and a nonaqueous electrolyte secondary battery were produced in the same manner as in Example 1 except that the calcination temperature during the synthesis of the sodium transition metal composite oxide was changed from 1100°C to 800°C in the synthesis of the positive electrode active material (B).

[0082] <Example 4>

[0083] A positive electrode and a nonaqueous electrolyte secondary battery were prepared in the same manner as in Example 1 except that the calcination temperature during the synthesis of the sodium transition metal composite oxide was changed from 750°C to 600°C in the synthesis of the positive electrode active material (A).

[0084] <Example 5>

[0085] A positive electrode and a nonaqueous electrolyte secondary battery were produced in the same manner as in Example 4 except that the calcination temperature during the synthesis of the sodium transition metal composite oxide was changed from 1100° C. to 800° C. in the synthesis of the positive electrode active material (B).

[0086] <Example 6>

[0087] In the synthesis of the positive electrode active material (A), the calcination temperature during the synthesis of the above-mentioned sodium transition metal composite oxide was changed from 750°C to 550°C. In the synthesis of the positive electrode active material (B), the calcination temperature during the synthesis of the above-mentioned sodium transition metal composite oxide was changed from 1100°C to 600°C. Otherwise, the positive electrode and the non-aqueous electrolyte secondary battery were prepared using the same method as in Example 1.

[0088] <Example 7>

[0089] A positive electrode and a nonaqueous electrolyte secondary battery were prepared in the same manner as in Example 1 except that the calcination temperature during the synthesis of the sodium transition metal composite oxide was changed from 750°C to 900°C in the synthesis of the positive electrode active material (A).

[0090] <Comparative Example 1>

[0091] A positive electrode and a nonaqueous electrolyte secondary battery were prepared in the same manner as in Example 1 except that the calcination temperature during the synthesis of the sodium transition metal composite oxide was changed from 1100°C to 750°C in the synthesis of the positive electrode active material (B).

[0092] <Comparative Example 2>

[0093] A positive electrode and a nonaqueous electrolyte secondary battery were prepared in the same manner as in Comparative Example 1 except that the calcination temperature during the synthesis of the sodium transition metal composite oxide was changed from 750°C to 1100°C in the synthesis of the positive electrode active material (A).

[0094] <Comparative Example 3>

[0095] A positive electrode and a nonaqueous electrolyte secondary battery were prepared in the same manner as in Comparative Example 1 except that the calcination temperature during the synthesis of the sodium transition metal composite oxide was changed from 750°C to 900°C in the synthesis of the positive electrode active material (A).

[0096] <Comparative Example 4>

[0097] A positive electrode and a non-aqueous electrolyte secondary battery were prepared in the same manner as in Example 6 except that the calcination temperature during the synthesis of the sodium transition metal composite oxide was changed from 600°C to 550°C in the synthesis of the positive electrode active material (B).

[0098] <Comparative Example 5>

[0099] A positive electrode and a nonaqueous electrolyte secondary battery were prepared in the same manner as in Example 1 except that the calcination temperature during the synthesis of the sodium transition metal composite oxide was changed from 750°C to 1100°C in the synthesis of the positive electrode active material (A).

[0100] For each positive electrode active material and non-aqueous electrolyte secondary battery of the examples and comparative examples, evaluation was carried out by the following method. The evaluation results are shown in Table 1.

[0101] [Average surface roughness]

[0102] From the particle images obtained by SEM observation (magnification 2000 times) of each positive electrode active material, 10 particles were randomly selected, and the maximum value of the change amount per 1° of the particle radius and the longest diameter of the particle were measured. The surface roughness was calculated by the following formula.

[0103] Surface roughness = (Maximum value of the change amount per 1° of the particle radius) / (Longest diameter of the particle)

[0104] The change amount per 1° of the particle radius is an absolute value, and its maximum value is the maximum value among the change amounts per 1° measured for the entire circumference of the active material particles.

[0105] Figure 3B It is a diagram showing the peripheral shape obtained from the particle image of the positive electrode active material (A) of Example 1. Figure 4B It is a diagram showing the peripheral shape obtained from the particle image of the positive electrode active material (B) of Example 1. In Figure 3B and Figure 4B The distance from the center position C to each point Pi on the periphery of the particle was measured as the particle radius ri. The center position C is the position that bisects the longest diameter of the particle. The peripheral position of the particle where the particle radius ri is the maximum was taken as the reference point P0 (θ = 0). The angle formed by the line segment CP0 connecting this reference point P0 and the center position C and the line segment CPi formed by other peripheral points Pi of the particle and the center position C was defined as θ, and the particle radius ri at each θ of 1° was obtained. The average surface roughness was calculated by averaging the surface roughness of 10 randomly selected particles.

[0106] [D50]

[0107] The D50 of each positive electrode active material was measured using a laser diffraction scattering type particle size distribution measuring device (manufactured by HORIBA, LA-750) with water as the dispersion medium.

[0108] [Circularity]

[0109] The circularity of each positive electrode active material was measured using a flow-type particle image analysis device (manufactured by Sysmex, FPIA-2100). The number of target particles was set to 5000 or more, and ion-exchanged water added with polyoxyethylene sorbitan monolaurate was used as the dispersion medium.

[0110] [Cycle characteristics (capacity retention rate)]

[0111] Each battery of the example and the comparative example was charged and discharged under the following conditions in a temperature environment of 25° C., and the capacity retention rate was determined.

[0112] <Charge and Discharge Conditions>

[0113] After constant current charging at a constant current of 0.3 It = 900 mA until the battery voltage reached 4.2 V, constant voltage charging was performed at a voltage of 4.2 V until the current value reached 150 mA. Then, constant current discharge was performed at a constant current of 900 mA until the battery voltage reached 2.75 V. This charge and discharge cycle was repeated for 1000 cycles, and the capacity retention rate was calculated using the following formula.

[0114] Capacity retention rate (%) = 1000th cycle discharge capacity ÷ 1st cycle discharge capacity × 100 [Table 1]

[0115]

[0116] As shown in Table 1, the batteries of the examples all had higher capacity retention rates than the batteries of the comparative examples and exhibited excellent cycle characteristics.

[0117] Description of Reference Numerals

[0118] 10: Secondary battery, 11: Positive electrode, 12: Negative electrode, 13: Separator, 14: Electrode body, 16: Outer can, 17: Sealing body, 18, 19: Insulating plate, 20: Positive electrode connector, 21: Negative electrode connector, 22: Groove, 23: Internal terminal plate, 24: Lower valve body, 25: Insulating member, 26: Upper valve body, 27: Cover, 28: Gasket, 30: Positive electrode collector, 30A: First side, 30B: Second side, 31, 32: Positive electrode mixture layer, 40: Negative electrode collector, 41: Negative electrode mixture layer.

Claims

1. A secondary battery comprising a wound electrode body in which a positive electrode and a negative electrode are wound with a separator interposed therebetween, The positive electrode and the negative electrode each include a current collector, a first mixture layer formed on a first surface of the current collector facing the inner side of the electrode body, and a second mixture layer formed on a second surface of the current collector facing the outer side of the electrode body. In at least one of the positive electrode and the negative electrode, the first mixture layer includes a first active material, the second mixture layer includes a second active material, and the first active material has an average surface roughness greater than an average surface roughness of the second active material.

2. The secondary battery according to claim 1, wherein The average surface roughness of the first active material is 2.3% or more and 20% or less, and the average surface roughness of the second active material is 1% or more and 6.6% or less.

3. The secondary battery according to claim 1 or 2, wherein: The volume-based median diameter of the first active material and the second active material is 4 μm or more and 30 μm or less.

4. The secondary battery according to claim 1 or 2, wherein: The positive electrode includes the first mixture layer and the second mixture layer.

5. The secondary battery according to claim 3, wherein The positive electrode includes the first mixture layer and the second mixture layer.

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery

    JP1994290774A

  • Modified natural graphite particle and method for producing same

    WO2011125577A1

  • Positive-electrode active material, positive electrode, battery, battery pack, electronic device, electric vehicle, electricity storage device, and electric power system

    EP3373367A1

  • Current collector, negative electrode and battery

    JP2007273182A

  • Power storage device

    JP2014110105A