A blue light-proof high-brightness microlens composite film and preparation method thereof
By designing quadrilateral and octagonal convex structures in the microlens composite film and adding blue light absorbing particles to the prism structure, the existing anti-blue light film has been solved, and the range of 380nm to 450nm is achieved Effective protection and high brightness effects of blue light.
Patent Information
- Application Number
- CN202111222389.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-10-20
AI Technical Summary
The existing anti-blue light films have poor effects in protecting blue light, low transmittance, and color offset problems, especially for the blue light bands in the range of 380nm to 450nm.
A micro-lens composite film with high brightness of blue light is adopted, including a adhesive backing layer, a first substrate layer, an anti-blue prism structure layer, an adhesive layer and a second substrate layer, and four are provided on the micro-lens structure layer. Pyramid and octagonal raised structures, the prisms are arranged in a highly circular manner to improve light transmittance and anti-blue light effects, and blue-light absorbing particles are added to the prism structures to enhance protection.
Accurate barriers of high-energy short-wave blue light in bands below 450nm, alleviate color-shaping and yellowing phenomenon, improve the light transmittance and blue light resistance of the composite film, extend the service life, and ensure the high brightness and environmental stability of the product. sex.
Smart Images

Figure CN113835144B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of optical films, and in particular to a blue light-proof high-brightness microlens composite film and a preparation method thereof. Background Art
[0002] Medical research reports show that visible light with a wavelength between 500 and 800nm has basically no destructive effect on the retina, while blue light with a wavelength between 380 and 480nm, as the wavelength becomes shorter, the photon energy increases, the degree of damage to the retina increases rapidly, and blue light has the greatest destructive effect on the retina.
[0003] Currently, LED displays use red, green and blue primary colors as backlight sources, and the blue light wavelength range is 420 to 460nm. Therefore, the development of anti-blue light film requires selective protection for this band.
[0004] Existing blue light protection solutions: First, apply blue light protection film to the LCD screen; second, use blue light protection film on the backlight module; third, use software to filter blue light. However, each of the three solutions has the following defects:
[0005] First, it is easy to apply anti-blue light film to the LCD outer screen on small-size LCDs (mobile phones, computer monitors, PADs), but it is more difficult to apply film on large-size LCDs (large-size LCD TVs).
[0006] Second, the backlight module uses anti-blue light film. Currently, there are two types of anti-blue light optical films, one is a single-layer anti-blue light prism film, and the other is a single prism composite film, where the anti-blue light layer is set under the PET layer or between two layers of PET. Although these two types solve the blue light problem and reduce color difference, they sacrifice the transmittance and brightness of the backlight module.
[0007] Third, the software filters blue, and its eye protection effect is indeed significant, but the color cast is very yellowish.
[0008] In view of the shortcomings of the prior art such as low transmittance, serious color deviation, and no targeted protection, the present invention provides a high-brightness blue light protection microlens composite film and a preparation method thereof, which has high light transmittance, good blue light protection effect, more targeted blue light protection, and freer, more convenient, and simpler product matching with different needs, especially for the strongest excitation part of 380nm to 450nm LED, OLED and other fluorescent powders, and provides targeted and effective protection for the blue spectrum area that is most harmful to the human body. Summary of the invention
[0009] Aiming at the defects of poor blue light protection film and low transmittance in the prior art, the present invention provides a new blue light protection high-brightness microlens composite film and a preparation method thereof.
[0010] In order to solve the above technical problems, the present invention is implemented by the following technical solutions:
[0011] A blue light protection high-brightness microlens composite film comprises, from bottom to top, a back glue layer, a first substrate layer, an anti-blue light prism structure layer, an adhesive layer, and a second substrate layer stacked in sequence, and also comprises a microlens structure layer stacked on the second substrate layer, wherein a quadrangular pyramid structure and an octagonal convex structure are arrayed on the microlens structure layer, and four adjacent octagonal convex structures are surrounded to form a rhombus area, and the quadrangular pyramid structure is filled in the rhombus area, and the octagonal convex structure comprises a coaxially stacked octagonal base and a microlens, and prisms are arrayed on the blue light protection prism structure layer, and the heights of the prisms are cyclically arranged in a period of one high and N low in the horizontal and vertical directions, and N≥0, and the spacing between adjacent prisms is 50-60μm, and blue light absorbing particles with a particle size of 10-50nm are uniformly distributed in the prisms.
[0012] The first substrate layer and the second substrate layer of the present invention play a supporting role, the adhesive layer plays a connecting and compounding role, the back adhesive layer is used for bonding with other materials, and the anti-blue light prism structure layer has both optical brightening and widening optical viewing angle functions. The anti-blue light prism structure layer plays an important role in enhancing transmittance and preventing blue light.
[0013] Different from the traditional microlens structure, the present invention reuses the edge area of adjacent microlenses. An octagonal base is first stacked on the bottom of the microlens. The regular edge of the octagonal base can form a regular rhombus area, and then a quadrangular pyramid structure is arranged in these rhombus areas, thereby ensuring that the area of the microlens structure layer is 100% utilized, increasing the transmittance of the microlens structure layer, and improving the brightness of the present invention.
[0014] In order to prevent the blue light absorbing particles from being exposed on the surface of the film layer, resulting in poor service life and environmental stability, the present invention adds blue light absorbing particles to the anti-blue light prism structure layer, which can effectively improve the anti-blue light life and environmental stability of the composite film.
[0015] The present invention controls the particle size of blue light absorbing particles, absorbs most of the short-wave blue light without affecting the brightness of the screen to reduce damage to the human eye, so that the composite film has both excellent blue light protection effect and light transmittance, further achieves precise blocking of high-energy short-wave blue light in the band below 450nm, reduces color cast and yellowing, controls the color difference after filtering by the composite film, and completely overcomes the defects of the prior art.
[0016] Preferably, in the above-mentioned anti-blue light high-brightness microlens composite film, the bottom surface contour of the microlens coincides with the inscribed circle of the octagonal base, the diameter of the inscribed circle of the octagonal base is 100-120 μm, and the height of the microlens is cyclically arranged in a period of high and low in both the horizontal and vertical directions, and M ≥ 0, and the height of the octagonal convex structure is 6-12 μm.
[0017] The bottom surface contour of the microlens coincides with the inscribed circle of the octagonal base, which can maximize the coverage area of the microlens, maintain high brightness, and meet a higher overall optical effect.
[0018] The microlenses are arranged in a high-M-low cycle, which can resist pressure and scratch. The present invention adopts the above structure to reduce the risk of scratching other components and reduce bad appearance defects such as moiré interference.
[0019] Preferably, in the above-mentioned blue light protection and high-brightness microlens composite film, the side lengths of the quadrangular pyramid structure and the octagonal base are equal, and the height of the quadrangular pyramid structure is 6-10 μm.
[0020] The sides of the tetrahedral pyramid structure and the octagonal base are equal in length, which can ensure that all gaps between adjacent octagonal bases are filled, further ensuring the coverage of the microlens structure layer, thereby improving the brightness of the product.
[0021] In addition, the tetrahedral pyramid structure is not higher than the octagonal raised structure, which can effectively avoid scratching other components.
[0022] Preferably, in the above-mentioned anti-blue light high-brightness microlens composite film, when M≥1, the microlenses are cyclically arranged in a period of high M and low M, the octagonal base is stacked with microlenses of two heights and correspondingly forms a high octagonal convex structure and a low octagonal convex structure, and the low octagonal convex structure is equal in height to the quadrangular pyramid structure.
[0023] The microlens structure layer of the present invention is provided with octagonal protrusion structures of different heights, which can reduce the light interference problem and improve the brightness gain effect.
[0024] Preferably, in the above-mentioned blue light protection high-brightness microlens composite film, when N≥1, the prisms are arranged in a cycle of high N low, the top angle of the prism is not less than 90°, and the spacing between the high prism and the low prism is 50-60μm.
[0025] Since the high prisms will penetrate into the adhesive layer, resulting in a partial loss of brightness, but the low prisms can still maintain brightness. Therefore, the prisms of the present invention are arranged in a cycle of high N low, which can effectively improve the brightness and also ensure the peeling force.
[0026] The vertex angle of the prism is not less than 90°, so that the number of refraction and reflection of the incident light is small, which can reduce light loss and thus improve brightness.
[0027] Preferably, in the above-mentioned blue light protection and high-brightness microlens composite film, the apex of the high prism corresponds to the center of the octagonal base.
[0028] The vertex of the prism corresponds to the center of the octagonal base, which can reduce the number of refractions and reflections of the incident light, reduce light loss, and improve brightness.
[0029] Preferably, the method for preparing the above-mentioned blue light-proof high-brightness microlens composite film comprises the following steps:
[0030] S1: Laser engraving: Take a roll blank A made of copper or nickel, and use an ultra-precision engraving machine to engrave a quadrangular pyramid structure and an octagonal protrusion structure on the roll blank A to obtain a microlens structure mold, and then take a roll blank B made of copper or nickel, and use a diamond knife engraving process to engrave a prism structure on the roll blank B to obtain a prism structure mold;
[0031] In step S1, an ultra-precision engraving machine is used to engrave the microlens structure mold, which can fully guarantee the engraving accuracy, even reaching micron-level accuracy, with an extremely low deviation of only ±0.1μm, which plays an auxiliary function for subsequent alignment and bonding. The prism structure engraved by the diamond knife engraving process has a complete structure and a smooth surface, which is smoothly demolded during coating and has a longer service life.
[0032] S2: preparing an anti-blue light coating liquid: taking nano cerium oxide A, nano zinc oxide A, and solvent A in a weight ratio of 1:1:100 to 1:2:150, uniformly mixing and fully dispersing, stirring for 20 to 30 minutes, and setting the stirring speed to 1500rpm / min, then continuing to add acrylic resin A and continuing to stir for 40 minutes, the weight ratio of acrylic resin A to solvent A is 1.2:1 to 1.5:1, and finally adding photoinitiator A and continuing to stir for 10 minutes, the weight ratio of photoinitiator A to acrylic resin A is 0.07:1 to 0.1:1, and after stirring, an anti-blue light coating liquid is obtained, wherein nano cerium oxide A and nano zinc oxide A are used as blue light absorbing particles;
[0033] In step S2, the raw materials are added in the order mentioned above, and high-speed stirring is used to ensure that the materials are fully dissolved, the volatilization of the solvent is reduced, and the dispersion is uniform.
[0034] S3: Take the first substrate layer, use an ultra-precision coating machine to coat the anti-blue light coating liquid on the first substrate layer, and use a prism structure mold to transfer the prism structure to the first substrate layer, and then evaporate the solvent A at a temperature of 60 to 120° C., and then obtain the anti-blue light prism structure layer after light curing;
[0035] In step S3, the coating speed can reach 15-20 m / min by ultra-precision coating roller pressing, which effectively improves production capacity, has high transfer efficiency, few defects, and high yield. In addition, the present invention adopts a process of first thermal volatilization and then photocuring, which can fully remove the solvent and obtain a film layer with very uniform thickness after photocuring.
[0036] S4: preparing UV type acrylic resin: taking acrylate monomer and polyurethane acrylate oligomer, mixing and stirring until the acrylate monomer is completely dissolved, then adding photoinitiator B and continuing stirring for 10 minutes, finally adding dispersing aid and lubricant and continuing stirring for 5 minutes, to obtain a uniform and stable UV type acrylic resin, wherein the weight ratio of acrylate monomer, polyurethane acrylate oligomer, dispersing aid, photoinitiator B and lubricant is 40:55:2:5:0.5 to 35:60:2:6:0.5;
[0037] In step S4, the raw materials are added in the above order, and each component is effectively dispersed and dissolved by stirring and dispersing. The effect of the dispersing aid is to disperse each component so that no agglomeration and solidification problems will occur during use.
[0038] S5: Take the second substrate layer, use an ultra-precision coater to coat a UV-type acrylic resin on the second substrate layer, and use a micro-lens structure mold to transfer the quadrangular pyramid structure and the octagonal convex structure to the second substrate layer, and then perform UV light curing in a Class 100 clean room environment, wherein the wavelength of the UV lamp is 365nm, and the light curing time is 1 to 2s, to obtain a micro-lens structure layer;
[0039] In step S5, UV light curing can achieve the purpose of instant curing without volatile harmful gases, and the curing speed can reach 15-20 m / min. Coating in a Class 100 clean room environment can effectively reduce defects caused by foreign matter and improve yield.
[0040] S6: preparing adhesive: taking UV type adhesive, butanone A, and leveling agent in a weight ratio of 2:8:0.01 to 3:7:0.02, mixing and stirring, and then adding butanone B or ethyl acetate A to dilute until the solid content reaches 10-20%, and then continuing to stir at high speed for 30 minutes, and the speed is set to 1500 rpm / min, to obtain a uniform and stable adhesive;
[0041] In step S6, the adhesive does not use conventional resin, but only uses a combination of solvent and UV type adhesive, so that the solid content is relatively low, only 10-20%, and no solid remains, so that the blue light absorption is more sufficient.
[0042] S7: The adhesive is coated on the other side of the second substrate layer by a slit or concave coating method, the wet thickness after coating is 30-50 μm, and then placed in an oven at 40-70° C. for drying for 2-3 min, the air inlet and exhaust flow rate of the oven is set to 30,000-35,000 cubic meters per hour, and the dry thickness of the adhesive after drying is 2-5 μm;
[0043] In step S7, by coating with slits or dimples and the above-mentioned drying method, an adhesive with uniform and stable thickness can be obtained, thereby reducing problems such as stripes caused by uneven thickness.
[0044] S8: coating of adhesive layer: acrylic resin B, polyurethane monomer, photoinitiator C, PBMA diffusion particles, ethyl acetate B, butyl acetate, and composite auxiliary agent are mixed and stirred in a weight ratio of 4:5:0.1:0.01:1:1:0.01 to 4:5:0.1:0.01:2:2:0.01 to obtain adhesive coating, which is coated on one side of the first substrate layer, and then cured by light or heat to obtain an adhesive layer;
[0045] In step S8, the adhesive coating prepared by the above formula has a good dispersion effect during coating, and the adhesive layer finally prepared has the advantages of high compressive strength, high wear resistance and good antistatic effect.
[0046] S9: Lamination: The anti-blue light prism structure layer and the second substrate layer are aligned and laminated, and the peak of the prism penetrates the adhesive layer. The layers are laminated by roller pressing and cured by high-pressure mercury lamp or LED lamp. The curing energy is 2000-3000mj / cm 3 , and finally rolled up to obtain a blue light-proof and high-brightness microlens composite film.
[0047] In step S9, the above-mentioned pressing method is adopted, and the peak of the prism penetrates 2-3 um in height, which can ensure the brightness of the microlens composite film and the peeling force of the product, and reduce the occurrence of defects such as delamination.
[0048] Preferably, in the above-mentioned method for preparing a blue light-proof high-brightness microlens composite film, in step S6, the adhesive also includes nano cerium oxide B and nano zinc oxide B, and the weight ratio of the UV type adhesive, nano cerium oxide B, and nano zinc oxide B is 2:1:1 to 3:2:2.
[0049] Since the solid content of the adhesive is only 10-20%, nano-cerium oxide B and nano-zinc oxide B can be fully dissolved and dispersed after being introduced into the adhesive.
[0050] Preferably, in the above-mentioned method for preparing a blue light-proof high-brightness microlens composite film, in step S8, the back adhesive coating also includes nano cerium oxide C and nano zinc oxide C, and the weight ratio of the acrylic resin B, nano cerium oxide C, and nano zinc oxide C is 4:3:3 to 4:4:4.
[0051] Adding nano cerium oxide C and nano zinc oxide C to the back adhesive coating can absorb blue light, help cover blemishes, and has a simple preparation and production process.
[0052] Preferably, in the above-mentioned method for preparing a blue light-proof high-brightness microlens composite film, in step S9, a laser alignment device is used for alignment and pressing, and the prism is coaxially arranged with the octagonal base.
[0053] The laser marking device is used for precise marking and pressing, which achieves excellent alignment effect. The top angle of the lower prism is coaxial with the center of the octagonal base, which helps to improve the brightness of the product.
[0054] Compared with the prior art, the high-brightness blue light-proof microlens composite film finally prepared by the present invention has high brightness, low light interference, and significant blue light-proof effect, and the production process is simple, which greatly improves the brightness of the product and makes the product more competitive. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 The structure of the present invention is schematically shown Figure 1 ;
[0056] Figure 2 The structure of the present invention is schematically shown Figure 2 ;
[0057] Figure 3 The structure of the present invention is schematically shown Figure 3 ;
[0058] Figure 4 Schematic diagram of the structure of the microlens structure layer in the present invention. DETAILED DESCRIPTION
[0059] The following is combined with Figure 1-4 The present invention is further described in detail with specific embodiments, but they are not intended to limit the present invention:
[0060] Example 1
[0061] A blue light protection high-brightness microlens composite film comprises, from bottom to top, a back glue layer 1, a first substrate layer 2, an anti-blue light prism structure layer 3, an adhesive layer 6, and a second substrate layer 4 which are stacked in sequence, and also comprises a microlens structure layer 5 stacked on the second substrate layer 4, wherein the microlens structure layer 5 is arrayed with a quadrangular pyramid structure 51 and an octagonal protrusion structure, and four adjacent octagonal protrusion structures are surrounded to form a rhombus area, wherein the quadrangular pyramid structure 51 is filled in the rhombus area, and the octagonal protrusion structure comprises a coaxially stacked octagonal base 53 and a microlens 52, wherein the anti-blue light prism structure layer 3 is arrayed with prisms 31, wherein the height of the prisms 31 is cyclically arranged in a period of one high and N low in both the horizontal and vertical directions, and N≥0, the spacing between adjacent prisms 31 is 50μm, and blue light absorbing particles with a particle size of 10nm are uniformly distributed in the prisms 31.
[0062] Preferably, the bottom surface contour of the microlens 52 coincides with the inscribed circle of the octagonal base 53, the inscribed circle diameter of the octagonal base 53 is 100 μm, the height of the microlens 52 is cyclically arranged in a period of high and low in both the horizontal and vertical directions, and M ≥ 0, and the height of the octagonal protrusion structure is 6 μm.
[0063] Preferably, the side lengths of the quadrangular pyramid structure 51 and the octagonal base 53 are equal, and the height of the quadrangular pyramid structure 51 is 6 μm.
[0064] Preferably, when M≥1, the microlenses 52 are arranged cyclically in a period of high M and low, the octagonal base 53 is stacked with microlenses 52 of two heights to form a high octagonal convex structure 531 and a low octagonal convex structure 532 accordingly, and the low octagonal convex structure 532 is equal to the height of the quadrangular pyramid structure 51.
[0065] Preferably, when N≥1, the prisms 31 are arranged in a cyclical manner with a period of high and low, the vertex angle of the prisms 31 is not less than 90°, and the spacing between the high prisms 31 and the low prisms 31 is 50 μm.
[0066] Preferably, the vertex of the tall prism 31 corresponds to the center of the octagonal base 53 .
[0067] As a preference, the method comprises the following steps:
[0068] S1: Laser engraving: Take a roll blank A made of copper or nickel, and use an ultra-precision engraving machine to engrave a quadrangular pyramid structure 51 and an octagonal protrusion structure on the roll blank A to obtain a microlens structure mold, then take a roll blank B made of copper or nickel, and use a diamond knife engraving process to engrave a prism 31 structure on the roll blank B to obtain a prism structure mold;
[0069] S2: prepare anti-blue light coating liquid: take nano cerium oxide A, nano zinc oxide A, and solvent A in a weight ratio of 1:1:100, mix them evenly, fully disperse them, stir for 20 minutes, and set the stirring speed to 1500rpm / min, then continue to add acrylic resin A and continue stirring for 40 minutes, the weight ratio of acrylic resin A to solvent A is 1.2:1, finally add photoinitiator A and continue stirring for 10 minutes, the weight ratio of photoinitiator A to acrylic resin A is 0.07:1, and after stirring, the anti-blue light coating liquid is prepared, wherein nano cerium oxide A and nano zinc oxide A are used as blue light absorbing particles;
[0070] S3: Take the first substrate layer 2, use an ultra-precision coating machine to coat the anti-blue light coating liquid on the first substrate layer 2, and use a prism structure mold to transfer the prism 31 structure to the first substrate layer 2, and then evaporate the solvent A at a temperature of 60 to 120° C., and then obtain the anti-blue light prism structure layer 3 after light curing;
[0071] S4: preparing UV type acrylic resin: taking acrylate monomer and polyurethane acrylate oligomer, mixing and stirring until the acrylate monomer is completely dissolved, then adding photoinitiator B and continuing stirring for 10 minutes, finally adding dispersing aid and lubricant and continuing stirring for 5 minutes, to obtain a uniform and stable UV type acrylic resin, wherein the weight ratio of acrylate monomer, polyurethane acrylate oligomer, dispersing aid, photoinitiator B and lubricant is 40:55:2:5:0.5;
[0072] S5: Take the second substrate layer 4, use an ultra-precision coater to coat UV acrylic resin on the second substrate layer 4, and use a microlens structure mold to transfer the quadrangular pyramid structure 51 and the octagonal convex structure to the second substrate layer 4, and then perform UV light curing in a Class 100 clean room environment, wherein the wavelength of the UV lamp is 365nm, and the light curing time is 1s, to obtain a microlens structure layer 5;
[0073] S6: preparing adhesive: taking UV type glue, butanone A, and leveling agent in a weight ratio of 2:8:0.01, mixing and stirring, and then adding butanone B or ethyl acetate A to dilute until the solid content reaches 10%, and then continue to stir at high speed for 30 minutes, and the speed is set to 1500rpm / min to obtain a uniform and stable adhesive;
[0074] S7: The adhesive is coated on the other side of the second substrate layer 4 by a slit or micro-concave coating method, and the wet thickness after coating is 30 μm. Then, the adhesive is placed in an oven at 40° C. for drying for 2 min. The air inlet and exhaust flow rate of the oven is set to 30,000 cubic meters per hour. After drying, the adhesive has a dry thickness of 2 μm.
[0075] S8: coating of adhesive layer 1: acrylic resin B, polyurethane monomer, photoinitiator C, PBMA diffusion particles, ethyl acetate B, butyl acetate, and composite auxiliary agent are mixed and stirred in a weight ratio of 4:5:0.1:0.01:1:1:0.01 to prepare adhesive coating, and the mixture is coated on one side of the first substrate layer 2, and then cured by light or heat to prepare adhesive layer 1;
[0076] S9: Lamination: The blue light protection prism structure layer 3 and the second substrate layer 4 are aligned and laminated, and the peak of the prism 31 penetrates the adhesive layer 6, and the layers are cured by a high-pressure mercury lamp or LED lamp through a roller lamination method, and the curing energy is 2000mj / cm 3 , and finally rolled up to obtain a blue light-proof and high-brightness microlens composite film.
[0077] Preferably, in step S6, the adhesive further comprises nano cerium oxide B and nano zinc oxide B, and the weight ratio of the UV adhesive, nano cerium oxide B and nano zinc oxide B is 2:1:1.
[0078] Preferably, in step S8, the adhesive coating further comprises nano cerium oxide C and nano zinc oxide C, and the weight ratio of the acrylic resin B, nano cerium oxide C and nano zinc oxide C is 4:3:3.
[0079] Preferably, in step S9, a laser marking device is used to perform marking and pressing, and the prism 31 and the octagonal base 53 are coaxially arranged.
[0080] Example 2
[0081] A blue light protection high-brightness microlens composite film comprises, from bottom to top, a back glue layer 1, a first substrate layer 2, an anti-blue light prism structure layer 3, an adhesive layer 6, and a second substrate layer 4 which are stacked in sequence, and also comprises a microlens structure layer 5 stacked on the second substrate layer 4, wherein the microlens structure layer 5 is arrayed with a quadrangular pyramid structure 51 and an octagonal protrusion structure, and four adjacent octagonal protrusion structures are surrounded to form a rhombus area, wherein the quadrangular pyramid structure 51 is filled in the rhombus area, and the octagonal protrusion structure comprises a coaxially stacked octagonal base 53 and a microlens 52, wherein the blue light protection prism structure layer 3 is arrayed with prisms 31, wherein the height of the prisms 31 is cyclically arranged in a period of one high and N low in both the horizontal and vertical directions, and N≥0, the spacing between adjacent prisms 31 is 55 μm, and blue light absorbing particles with a particle size of 30 nm are uniformly distributed in the prisms 31.
[0082] Preferably, the bottom surface contour of the microlens 52 coincides with the inscribed circle of the octagonal base 53, the inscribed circle diameter of the octagonal base 53 is 110 μm, the height of the microlens 52 is cyclically arranged in a period of high and low in both the horizontal and vertical directions, and M ≥ 0, and the height of the octagonal protrusion structure is 9 μm.
[0083] Preferably, the side lengths of the quadrangular pyramid structure 51 and the octagonal base 53 are equal, and the height of the quadrangular pyramid structure 51 is 8 μm.
[0084] Preferably, when M≥1, the microlenses 52 are arranged cyclically in a period of high M and low, the octagonal base 53 is stacked with microlenses 52 of two heights to form a high octagonal convex structure 531 and a low octagonal convex structure 532 accordingly, and the low octagonal convex structure 532 is equal to the height of the quadrangular pyramid structure 51.
[0085] Preferably, when N≥1, the prisms 31 are arranged in a cyclical manner with a period of high and low, the vertex angle of the prisms 31 is not less than 90°, and the spacing between the high prisms 31 and the low prisms 31 is 55 μm.
[0086] Preferably, the vertex of the tall prism 31 corresponds to the center of the octagonal base 53 .
[0087] As a preference, the method comprises the following steps:
[0088] S1: Laser engraving: Take a roll blank A made of copper or nickel, and use an ultra-precision engraving machine to engrave a quadrangular pyramid structure 51 and an octagonal protrusion structure on the roll blank A to obtain a microlens structure mold, then take a roll blank B made of copper or nickel, and use a diamond knife engraving process to engrave a prism 31 structure on the roll blank B to obtain a prism structure mold;
[0089] S2: prepare anti-blue light coating liquid: take nano cerium oxide A, nano zinc oxide A, and solvent A in a weight ratio of 1:1.5:125, mix them evenly, fully disperse them, stir for 25 minutes, and set the stirring speed to 1500rpm / min, then continue to add acrylic resin A and continue stirring for 40 minutes, the weight ratio of acrylic resin A to solvent A is 1.4:1, finally add photoinitiator A and continue stirring for 10 minutes, the weight ratio of photoinitiator A to acrylic resin A is 0.08:1, and after stirring, the anti-blue light coating liquid is obtained, wherein nano cerium oxide A and nano zinc oxide A are used as blue light absorbing particles;
[0090] S3: Take the first substrate layer 2, use an ultra-precision coating machine to coat the anti-blue light coating liquid on the first substrate layer 2, and use a prism structure mold to transfer the prism 31 structure to the first substrate layer 2, and then evaporate the solvent A at a temperature of 60 to 120° C., and then obtain the anti-blue light prism structure layer 3 after light curing;
[0091] S4: preparing UV type acrylic resin: taking acrylate monomer and polyurethane acrylate oligomer, mixing and stirring until the acrylate monomer is completely dissolved, then adding photoinitiator B and continuing stirring for 10 minutes, finally adding dispersing aid and lubricant and continuing stirring for 5 minutes, to obtain a uniform and stable UV type acrylic resin, wherein the weight ratio of acrylate monomer, polyurethane acrylate oligomer, dispersing aid, photoinitiator B and lubricant is 38:58:2:5.5:0.5;
[0092] S5: Take the second substrate layer 4, use an ultra-precision coater to coat the UV type acrylic resin on the second substrate layer 4, and use a microlens structure mold to transfer the quadrangular pyramid structure 51 and the octagonal convex structure to the second substrate layer 4, and then perform UV light curing in a Class 100 clean room environment, wherein the wavelength of the UV lamp is 365nm, and the light curing time is 1.5s, to obtain a microlens structure layer 5;
[0093] S6: preparing adhesive: taking UV type adhesive, butanone A, and leveling agent in a weight ratio of 2.5:7.5:0.01, mixing and stirring, and then adding butanone B or ethyl acetate A to dilute until the solid content reaches 15%, and then continue to stir at high speed for 30 minutes, and the speed is set to 1500rpm / min to obtain a uniform and stable adhesive;
[0094] S7: The adhesive is coated on the other side of the second substrate layer 4 by a slit or concave coating method, the wet thickness after coating is 40 μm, and then placed in an oven at 40-70° C. for drying for 2.5 min, the air inlet and exhaust flow rate of the oven is set to 32,000 cubic meters per hour, and the dry thickness of the adhesive after drying is 3.5 μm;
[0095] S8: coating of adhesive layer 1: acrylic resin B, polyurethane monomer, photoinitiator C, PBMA diffusion particles, ethyl acetate B, butyl acetate, and composite auxiliary agent are mixed and stirred in a weight ratio of 4:5:0.1:0.01:1:1.5:0.01 to prepare adhesive coating, and the mixture is coated on one side of the first substrate layer 2, and then cured by light or heat to prepare adhesive layer 1;
[0096] S9: Lamination: The blue light protection prism structure layer 3 and the second substrate layer 4 are aligned and laminated, and the peak of the prism 31 penetrates the adhesive layer 6, and the layers are cured by a high-pressure mercury lamp or LED lamp through a roller lamination method, and the curing energy is 2500mj / cm 3, and finally rolled up to obtain a blue light-proof and high-brightness microlens composite film.
[0097] Preferably, in step S6, the adhesive further comprises nano cerium oxide B and nano zinc oxide B, and the weight ratio of the UV adhesive, nano cerium oxide B and nano zinc oxide B is 2.5:1.5:1.5.
[0098] Preferably, in step S8, the adhesive coating further comprises nano cerium oxide C and nano zinc oxide C, and the weight ratio of the acrylic resin B, nano cerium oxide C and nano zinc oxide C is 4:3.5:3.5.
[0099] Preferably, in step S9, a laser marking device is used to perform marking and pressing, and the prism 31 and the octagonal base 53 are coaxially arranged.
[0100] Example 3
[0101] A blue light protection high-brightness microlens composite film comprises, from bottom to top, a back glue layer 1, a first substrate layer 2, an anti-blue light prism structure layer 3, an adhesive layer 6, and a second substrate layer 4 which are stacked in sequence, and also comprises a microlens structure layer 5 stacked on the second substrate layer 4, wherein the microlens structure layer 5 is arrayed with a quadrangular pyramid structure 51 and an octagonal protrusion structure, and four adjacent octagonal protrusion structures are surrounded to form a rhombus area, wherein the quadrangular pyramid structure 51 is filled in the rhombus area, and the octagonal protrusion structure comprises a coaxially stacked octagonal base 53 and a microlens 52, wherein the blue light protection prism structure layer 3 is arrayed with prisms 31, wherein the height of the prisms 31 is cyclically arranged in a period of one high and N low in both the horizontal and vertical directions, and N≥0, the spacing between adjacent prisms 31 is 60 μm, and blue light absorbing particles with a particle size of 50 nm are uniformly distributed in the prisms 31.
[0102] Preferably, the bottom surface contour of the microlens 52 coincides with the inscribed circle of the octagonal base 53, the inscribed circle diameter of the octagonal base 53 is 120 μm, the height of the microlens 52 is cyclically arranged in a period of high and low in both the horizontal and vertical directions, and M ≥ 0, and the height of the octagonal protrusion structure is 12 μm.
[0103] Preferably, the side lengths of the quadrangular pyramid structure 51 and the octagonal base 53 are equal, and the height of the quadrangular pyramid structure 51 is 10 μm.
[0104] Preferably, when M≥1, the microlenses 52 are arranged cyclically in a period of high M and low, the octagonal base 53 is stacked with microlenses 52 of two heights to form a high octagonal convex structure 531 and a low octagonal convex structure 532 accordingly, and the low octagonal convex structure 532 is equal to the height of the quadrangular pyramid structure 51.
[0105] Preferably, when N≥1, the prisms 31 are arranged in a cyclical manner with a period of high and low, the vertex angle of the prisms 31 is not less than 90°, and the spacing between the high prisms 31 and the low prisms 31 is 60 μm.
[0106] Preferably, the vertex of the tall prism 31 corresponds to the center of the octagonal base 53 .
[0107] As a preference, the method comprises the following steps:
[0108] S1: Laser engraving: Take a roll blank A made of copper or nickel, and use an ultra-precision engraving machine to engrave a quadrangular pyramid structure 51 and an octagonal protrusion structure on the roll blank A to obtain a microlens structure mold, then take a roll blank B made of copper or nickel, and use a diamond knife engraving process to engrave a prism 31 structure on the roll blank B to obtain a prism structure mold;
[0109] S2: prepare anti-blue light coating liquid: take nano cerium oxide A, nano zinc oxide A, and solvent A in a weight ratio of 1:2:150, mix them evenly, fully disperse them, stir for 30 minutes, and set the stirring speed to 1500rpm / min, then continue to add acrylic resin A and continue stirring for 40 minutes, the weight ratio of acrylic resin A to solvent A is 1.5:1, finally add photoinitiator A and continue stirring for 10 minutes, the weight ratio of photoinitiator A to acrylic resin A is 0.1:1, and after stirring, the anti-blue light coating liquid is obtained, wherein nano cerium oxide A and nano zinc oxide A are used as blue light absorbing particles;
[0110] S3: Take the first substrate layer 2, use an ultra-precision coating machine to coat the anti-blue light coating liquid on the first substrate layer 2, and use a prism structure mold to transfer the prism 31 structure to the first substrate layer 2, and then evaporate the solvent A at a temperature of 60 to 120° C., and then obtain the anti-blue light prism structure layer 3 after light curing;
[0111] S4: preparing UV type acrylic resin: taking acrylate monomer and polyurethane acrylate oligomer, mixing and stirring until the acrylate monomer is completely dissolved, then adding photoinitiator B and continuing stirring for 10 minutes, finally adding dispersing aid and lubricant and continuing stirring for 5 minutes, to obtain a uniform and stable UV type acrylic resin, wherein the weight ratio of acrylate monomer, polyurethane acrylate oligomer, dispersing aid, photoinitiator B and lubricant is 35:60:2:6:0.5;
[0112] S5: Take the second substrate layer 4, use an ultra-precision coater to coat the UV type acrylic resin on the second substrate layer 4, and use a microlens structure mold to transfer the quadrangular pyramid structure 51 and the octagonal convex structure to the second substrate layer 4, and then perform UV light curing in a Class 100 clean room environment, wherein the wavelength of the UV lamp is 365nm, and the light curing time is 2s, to obtain a microlens structure layer 5;
[0113] S6: preparing adhesive: taking UV type adhesive, butanone A, and leveling agent in a weight ratio of 3:7:0.02, mixing and stirring, and then adding butanone B or ethyl acetate A to dilute until the solid content reaches 20%, and then continuing to stir at high speed for 30 minutes, and the speed is set to 1500rpm / min, to obtain a uniform and stable adhesive;
[0114] S7: The adhesive is coated on the other side of the second substrate layer 4 by a slit or concave coating method, the wet thickness after coating is 50 μm, and then placed in an oven at 40-70° C. for drying for 3 min, the air inlet and exhaust flow rate of the oven is set to 35,000 cubic meters per hour, and the dry thickness of the adhesive after drying is 5 μm;
[0115] S8: coating of adhesive layer 1: taking acrylic resin B, polyurethane monomer, photoinitiator C, PBMA diffusion particles, ethyl acetate B, butyl acetate, and composite auxiliary agent in a weight ratio of 4:5:0.1:0.01:2:2:0.01, mixing and stirring to prepare adhesive coating, coating on one side of the first substrate layer 2, and preparing adhesive layer 1 after light curing or heat curing;
[0116] S9: Lamination: The blue light protection prism structure layer 3 and the second substrate layer 4 are aligned and laminated, and the peak of the prism 31 penetrates the adhesive layer 6, and the layers are cured by a high-pressure mercury lamp or LED lamp through a roller lamination method, and the curing energy is 3000mj / cm 3 , and finally rolled up to obtain a blue light-proof and high-brightness microlens composite film.
[0117] Preferably, in step S6, the adhesive further comprises nano cerium oxide B and nano zinc oxide B, and the weight ratio of the UV adhesive, nano cerium oxide B and nano zinc oxide B is 3:2:2.
[0118] Preferably, in step S8, the adhesive coating further comprises nano cerium oxide C and nano zinc oxide C, and the weight ratio of the acrylic resin B, nano cerium oxide C and nano zinc oxide C is 4:4:4.
[0119] Preferably, in step S9, a laser marking device is used to perform marking and pressing, and the prism 31 and the octagonal base 53 are coaxially arranged.
[0120] Example 4
[0121] The blue light protection high brightness microlens composite film obtained in the above embodiments and the existing KMOP-2HH microlens prism composite film produced by Kangdexin Company were taken as comparative examples to conduct brightness performance tests. The test method is as follows:
[0122] (1) Brightness performance test: The above-mentioned microlens composite film is made into a universal backlight module, which is placed horizontally or vertically. After being powered on for 15 minutes, the light source of the backlight module is allowed to stabilize. The test optical instrument is placed 50±3 cm above or in front of the backlight module to test the brightness data of the backlight module. The brightness of the comparative example is used as a reference to obtain the brightness ratio of Examples 1-3 relative to the comparative example.
[0123] The performance parameters of the blue light protection high brightness micro-lens composite and comparative examples obtained in various embodiments of the present invention are shown in Table 1:
[0124] Table 1
[0125] sample Brightness percentage Example 1 103% Example 2 104% Example 3 105% Comparative Example 100%
[0126] In conclusion, the above is only a preferred embodiment of the present invention, and all equivalent changes and modifications made within the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A blue light blocking high brightness microlens composite film, comprising, from bottom to top, a back adhesive layer (1), a first substrate layer (2), a blue light blocking prism structure layer (3), an adhesive layer (6), and a second substrate layer (4), characterized in that: The invention also comprises a microlens structure layer (5) stacked on the second substrate layer (4), wherein the microlens structure layer (5) is provided with a quadrangular pyramid structure (51) and an octagonal protrusion structure in an array, wherein four adjacent octagonal protrusion structures surround and form a rhombus region, wherein the quadrangular pyramid structure (51) is filled in the rhombus region, wherein the octagonal protrusion structure comprises a coaxially stacked octagonal base (53) and a microlens (52), wherein the anti-blue light prism structure layer (3) is provided with a prism (31) in an array, wherein the height of the prism (31) is arranged in a cyclic manner in the horizontal and vertical directions with a period of one high and N low, and N≥0, wherein the spacing between adjacent prisms (31) is 50 to 60 μm, and wherein blue light absorbing particles with a particle size of 10 to 50 nm are uniformly distributed in the prism (31).
2. The blue light-proof high-brightness microlens composite film according to claim 1, characterized in that: The bottom surface profile of the microlens (52) coincides with the inscribed circle of the octagonal base (53), the inscribed circle diameter of the octagonal base (53) is 100-120 μm, the height of the microlens (52) is arranged in a cyclic manner in both the horizontal and vertical directions with a period of high and low, and M≥0, and the height of the octagonal protrusion structure is 6-12 μm.
3. The blue light-proof high-brightness microlens composite film according to claim 2, characterized in that: The side lengths of the quadrangular pyramid structure (51) and the octagonal base (53) are equal, and the height of the quadrangular pyramid structure (51) is 6 to 10 μm.
4. The blue light-proof high-brightness microlens composite film according to claim 3, characterized in that: When M≥1, the microlenses (52) are arranged cyclically in a period of high M and low M, the octagonal base (53) is stacked with microlenses (52) of two heights and correspondingly forms a high octagonal convex structure (531) and a low octagonal convex structure (532), and the low octagonal convex structure (532) has the same height as the quadrangular pyramid structure (51).
5. The blue light-proof high-brightness microlens composite film according to claim 4, characterized in that: When N≥1, the prisms (31) are arranged cyclically in a period of high N low, the vertex angle of the prisms (31) is not less than 90°, and the spacing between the high prism (31) and the low prism (31) is 50-60 μm.
6. The blue light-proof high-brightness microlens composite film according to claim 5, characterized in that: The vertex of the tall prism (31) corresponds to the center of the octagonal base (53).
7. The method for preparing a blue light-proof high-brightness microlens composite film according to claim 6, characterized in that: The steps include: S1: Laser engraving: Take a roll blank A made of copper or nickel, and use an ultra-precision engraving machine to engrave a quadrangular pyramid structure (51) and an octagonal protrusion structure on the roll blank A to obtain a microlens structure mold, then take a roll blank B made of copper or nickel, and use a diamond knife engraving process to engrave a prism (31) structure on the roll blank B to obtain a prism structure mold; S2: preparing an anti-blue light coating liquid: taking nano cerium oxide A, nano zinc oxide A, and solvent A in a weight ratio of 1:1:100 to 1:2:150, uniformly mixing and fully dispersing, stirring for 20 to 30 minutes, and setting the stirring speed to 1500rpm / min, then continuing to add acrylic resin A and continuing to stir for 40 minutes, the weight ratio of acrylic resin A to solvent A is 1.2:1 to 1.5:1, and finally adding photoinitiator A and continuing to stir for 10 minutes, the weight ratio of photoinitiator A to acrylic resin A is 0.07:1 to 0.1:1, and after stirring, an anti-blue light coating liquid is obtained, wherein nano cerium oxide A and nano zinc oxide A are used as blue light absorbing particles; S3: taking the first substrate layer (2), coating the anti-blue light coating liquid on the first substrate layer (2) using an ultra-precision coating machine, and transferring the prism (31) structure onto the first substrate layer (2) using a prism structure mold, and then first volatilizing the solvent A at a temperature of 60 to 120° C., and then photocuring to obtain the anti-blue light prism structure layer (3); S4: preparing UV type acrylic resin: taking acrylate monomer and polyurethane acrylate oligomer, mixing and stirring until the acrylate monomer is completely dissolved, then adding photoinitiator B and continuing stirring for 10 minutes, finally adding dispersing aid and lubricant and continuing stirring for 5 minutes, to obtain a uniform and stable UV type acrylic resin, wherein the weight ratio of acrylate monomer, polyurethane acrylate oligomer, dispersing aid, photoinitiator B and lubricant is 40:55:2:5:0.5 to 35:60:2:6:0.5; S5: taking the second substrate layer (4), coating the second substrate layer (4) with a UV acrylic resin using an ultra-precision coating machine, and transferring the quadrangular pyramid structure (51) and the octagonal protrusion structure onto the second substrate layer (4) using a microlens structure mold, and then performing UV light curing in a Class 100 clean room environment, wherein the wavelength of the UV lamp is 365 nm and the light curing time is 1 to 2 seconds, to obtain a microlens structure layer (5); S6: preparing adhesive: taking UV type adhesive, butanone A, and leveling agent in a weight ratio of 2:8:0.01 to 3:7:0.02, mixing and stirring, and then adding butanone B or ethyl acetate A to dilute until the solid content reaches 10-20%, and then continuing to stir at high speed for 30 minutes, and the speed is set to 1500 rpm / min, to obtain a uniform and stable adhesive; S7: using a slit or concave coating method, the adhesive is coated on the other side of the second substrate layer (4), the wet thickness after coating is 30-50 μm, and then placed in an oven at 40-70° C. for drying for 2-3 minutes, the air inlet and exhaust flow rate of the oven is set to 30,000-35,000 cubic meters per hour, and the dry thickness of the adhesive after drying is 2-5 μm; S8: coating of adhesive layer (1): acrylic resin B, polyurethane monomer, photoinitiator C, PBMA diffusion particles, ethyl acetate B, butyl acetate, and composite auxiliary agent are mixed and stirred in a weight ratio of 4:5:0.1:0.01:1:1:0.01 to 4:5:0.1:0.01:2:2:0.01 to obtain an adhesive coating, which is coated on one side of the first substrate layer (2), and then cured by light or heat to obtain an adhesive layer (1); S9: Lamination: The blue light protection prism structure layer (3) and the second substrate layer (4) are aligned and laminated, and the peak of the prism (31) penetrates the adhesive layer (6). The layers are laminated by roller pressing and cured by a high-pressure mercury lamp or LED lamp. The curing energy is 2000-3000 mj / cm 3 , and finally rolled up to obtain a blue light-proof and high-brightness microlens composite film.
8. The method for preparing a blue light-proof high-brightness microlens composite film according to claim 7, characterized in that: In step S6, the adhesive further includes nano cerium oxide B and nano zinc oxide B, and the weight ratio of the UV adhesive, nano cerium oxide B, and nano zinc oxide B is 2:1:1 to 3:2:
2.
9. The method for preparing a blue light-proof high-brightness microlens composite film according to claim 8, characterized in that: In step S8, the adhesive coating further includes nano cerium oxide C and nano zinc oxide C, and the weight ratio of the acrylic resin B, nano cerium oxide C and nano zinc oxide C is 4:3:3 to 4:4:
4.
10. The method for preparing a blue light-proof high-brightness microlens composite film according to claim 7, characterized in that: In step S9, a laser marking device is used to perform marking and pressing, and the prism (31) and the octagonal base (53) are coaxially arranged.
Citation Information
Patent Citations
Anti-blue-light high-brightness micro-lens composite film
CN216083157U