A method for preparing porous biological filter material for aerated biological filter
By using iron tailings and other materials to prepare porous biological filter materials with melting holes on the surface, the problems of easy clogging and high flow resistance of biological filter filter materials are solved, achieving efficient water treatment and resource reuse, and reducing costs. energy consumption and environmental pollution.
Patent Information
- Application Number
- CN202110958071.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-20
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-08-20
AI Technical Summary
Existing biofilter filter materials have problems such as difficulty in backwashing, easy clogging, and large flow resistance during use. Moreover, the energy consumption per unit product is high, and industrial solid waste iron tailings cannot be effectively utilized, resulting in resource waste and environmental pollution. .
Using iron tailings as the matrix, attapulgite as the binder, activated carbon powder as the pore-forming agent, magnesium carbonate as the cosolvent, and paraffin as the meltable skeleton, a porous biological filter material with melting holes on the surface is prepared through sintering. Used in aerated biological filters to increase microbial load area and mobility.
The prepared porous biological filter material has greater water absorption, apparent porosity and specific surface area, reduces the difficulty of backwashing and flow resistance, achieves the purpose of treating waste with waste, is suitable for industrial water treatment, and has good development prospects. .
Smart Images

Figure CN113860908B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramsite filter materials, and in particular relates to a method for preparing a porous biological filter material for an aerated biological filter tank. Background Art
[0002] Industrial organic wastewater is often treated by electrolysis, adsorption, photocoagulation, biochemical method and other methods. Among them, the electrolysis method uses wastewater to undergo electrochemical and redox reactions in an electrolytic cell to decompose organic matter, and this process consumes a lot of energy. The adsorption method uses substances with high adsorption to adsorb organic matter in wastewater, but the cost of the adsorption method is relatively high, and the adsorption capacity of the adsorption material is limited, and regular desorption is required. The photocoagulation method uses ultraviolet rays to polymerize small molecular organic matter in complex wastewater to form large molecular suspended matter, and then uses a sedimentation tank to remove the suspended matter, but this method is only for some high-concentration organic wastewater. The biochemical method uses the degradation of microorganisms to treat organic wastewater. This method is low-cost and has no secondary pollution. Iron tailings are waste after ore dressing. According to statistics, 2.5-3.0 tons of tailings are discharged for every ton of iron concentrate extracted, so iron tailings are the main component of industrial solid waste. The stacking of tailings occupies a lot of land, and causes waste of resources and pollution of the human living environment. The large-scale mining and utilization of mineral resources has reduced resources, so the reuse of tailings has attracted people's attention. In industrial wastewater treatment, tailings or waste rocks are often used as the main raw materials for advanced aerated biological filter media.
[0003] At present, there has been extensive research on fillers for biofilters in China, and various forms of granular filter media have been developed. For example, three-dimensional corrugated fillers and various types of irregular fillers. These filter materials have many shortcomings during use, such as difficulty in backwashing, easy clogging, and large flow resistance. In addition, many filter materials also have the problem of high energy consumption per unit product during the actual preparation process. To this end, we propose a method of using iron tailings as the main raw material to prepare a new type of porous biological filter material that can load microorganisms, and apply it to BAF aerated biological filters to invent an industrial water treatment functional material to achieve the purpose of treating waste with waste. By developing the preparation technology of mineral porous biological filter materials, a new method for preparing water treatment degradation materials with good development prospects is provided. Summary of the invention
[0004] The purpose of the present invention is to solve the shortcomings of the prior art mentioned in the above background technology, and to propose a method for preparing a porous biological filter material for an aerated biological filter and a preparation method thereof. The purpose of treating waste with waste is achieved. By developing the preparation technology of mineral porous biological filter material, a new method for preparing water treatment degradable materials with good development prospects is provided.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for preparing a porous biological filter material for an aerated biological filter is designed. The porous biological filter material is sintered to form a ceramsite filter material with melt holes on the surface, using iron tailings as a matrix, attapulgite as a binder, activated carbon powder as a pore-forming agent, magnesium carbonate as a co-solvent, and paraffin as a fusible skeleton.
[0007] The raw materials of the porous biological filter material are formulated by weight as follows: 80-100 parts of iron tailings, 5-15 parts of attapulgite, 1-10 parts of activated carbon powder, and 1-15 parts of magnesium carbonate;
[0008] The method for preparing the porous biological filter material for the aerated biological filter specifically comprises the following steps:
[0009] Step 1: Grind the raw material iron tailings in a mill for 1 hour, pass through a 200-mesh sieve, and place in a drying oven for drying;
[0010] Step 2, grinding and mixing the dried iron tailings with a pore-forming agent, a binder and a flux in proportion, adding water and stirring evenly to obtain a mixture A for standby use;
[0011] Step 3, the mixed material A obtained in step 2 is wrapped on a paraffin frame by a granulator to form ceramsite with a particle size of 5-6 mm and a frame, covered with a layer of plastic wrap, and placed in a cool place for aging for 24 hours;
[0012] Step 4: Place the aged ceramsite in a constant temperature drying oven and dry for 3 hours, and collect the melted paraffin solution. After drying, ceramsite with melt holes on the surface is obtained;
[0013] Step 5, sintering the ceramsite obtained in step 4 by a staged heating method to form a ceramsite filter material;
[0014] Step 6: polish the surface of the ceramsite filter material obtained in step 5 to remove the remaining skin at the melt hole opening to obtain the ceramsite filter material with melt holes on the surface.
[0015] Furthermore, in step 1, the iron tailings are high-silicon iron tailings, wherein the SiO2 specific gravity ranges from 60-66%, and the Al2O3 ranges from 8-10%.
[0016] Furthermore, in step 3, the paraffin skeleton includes a melt core, and a plurality of melt rods are evenly distributed on the circumference of the melt core, and the maximum radius of the melt rods around the melt core is the same as the radius of the ceramsite.
[0017] Further, in step 4, the melt holes on the surface of the expanded clay are interconnected.
[0018] Furthermore, in step 5, the staged temperature-raising sintering method comprises the following steps:
[0019] A. In the first stage, the temperature is raised from room temperature to 450°C at a rate of 5°C / min;
[0020] B. In the second stage, the temperature was raised from 450°C to 530°C at a rate of 3°C / min, and kept at 530°C for 15 minutes;
[0021] C. The third stage is to heat up at a rate of 7°C / min from 530°C to a sintering temperature of 1050°C, stay at the sintering temperature of 1050°C for 60 minutes, and then cool to room temperature with the furnace.
[0022] Compared with the existing technology, the method for preparing a porous biological filter material for an aerated biological filter tank using the technical solution has the following beneficial effects:
[0023] The porous biological filter material with melt holes on the surface is sintered by using iron tailings as a matrix, attapulgite as a binder, activated carbon powder as a pore-forming agent, magnesium carbonate as a cosolvent, and paraffin as a fusible skeleton. By adjusting the preparation process, the prepared filter material has a water absorption rate of 38.95%, an apparent porosity of 48.53%, and a volume density of 1.18 parts / cm 3 , hydrochloric acid solubility is 1.2%, and the specific surface area is 6.211m 2 / portion, pore volume is 0.012cm 3 / portion, with an average pore size of 3.5nm, a larger area for microbial loading, which can reduce the difficulty of backwashing, is not easy to clog and has low flow resistance, achieving the purpose of treating waste with waste. A new method for water treatment degradation materials with good development prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0025] Figure 1 It is a schematic diagram of the cross-sectional structure of the ceramsite filter material of the present invention;
[0026] Figure 2 It is a structural schematic diagram of the paraffin skeleton of the present invention;
[0027] Figure 3 It is a flowchart of the preparation of porous biological filter material according to the present invention;
[0028] Figure 4 is a line graph of ammonia nitrogen removal rate of porous biological filter material according to the present invention;
[0029] Marked in the figure: 1, melt core; 2, melt rod; 3, melt hole. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with specific examples. These examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.
[0031] The present invention will now be further described with reference to the accompanying drawings.
[0032] The invention discloses a method for preparing a porous biological filter material for an aerated biological filter. The porous biological filter material uses iron tailings as a matrix, attapulgite as a binder, activated carbon powder as a pore-forming agent, magnesium carbonate as a cosolvent, paraffin as a fusible skeleton, and is sintered to form a ceramsite filter material with melt holes on the surface.
[0033] Raw material selection: The selection of iron tailings, high silicon iron tailings in Anhui area are selected. The chemical composition of iron tailings: SiO2 content reaches 60.5%-62.5%, which is high silicon iron tailings. The content of Fe2O3 is 13.5%, and other components are: Al2O3, CaO, MgO, K2O, Na2O, TiO2, P2O5, MnO2, etc.
[0034] The attapulgite is selected from the attapulgite unique to the Xuyi area of Jiangsu Province. Its spatial configuration is layered chain-like and has good bonding and adsorption properties. In the process of preparing porous biological ceramsite filter material, attapulgite is used as a binder to increase the plasticity of the ceramsite filter material. The chemical composition of the attapulgite: the content of SiO2 is 60.5%, the content of Al2O3, Fe2O3, and MgO is 8.5%, 4.7%, and 0.8%, while the content of K2O, CaO, TiO2, and P2O5 are all less than 1%. The main component MgO can be used as a flux to reduce the sintering temperature, and the presence of Al2O3 can increase the strength of the filter material and reduce the expansion coefficient.
[0035] As a pore-forming agent, activated carbon powder is selected. When the activated carbon powder burns, an oxidation reaction occurs to generate CO and CO2 gases, which can form pores in the biofilter material when volatilized.
[0036] Solvent, magnesium carbonate is selected as flux. At high temperature, SiO2 and Al2O3 in the filter material can react chemically. The melting points of SiO2 and Al2O3 are extremely high. The higher the content of the two, the higher the sintering temperature, and the more difficult it is to sinter into ceramsite. Therefore, a small amount of flux should be added to reduce the liquid phase generation temperature. During the sintering process, the magnesium oxide decomposed by magnesium carbonate plays a fluxing role. At the same time, the decomposition of magnesium carbonate will produce CO2 gas, which plays a pore-forming role.
[0037] Meltable skeleton, paraffin skeleton made of paraffin (see Figure 2), comprising a melting core 1, a plurality of melting rods 2 are evenly distributed on the circumference of the melting core 1, the maximum radius of the melting rods 2 around the melting core 1 is the same as the radius of the ceramsite, during the drying process of the ceramsite, the paraffin skeleton melts, a cavity is formed inside the ceramsite, and a melting hole 3 is formed on the surface of the ceramsite, thereby increasing the specific surface area of the ceramsite.
[0038] Example 1
[0039] Take the above iron tailings as raw materials, take 80 parts of raw materials, grind them in a mill for 1 hour, pass through a 200 mesh sieve, and place them in a drying oven for drying. After grinding and mixing the iron tailings, pore-forming agent, binder and flux in proportion, add an appropriate amount of water, and mix them in a granulator and wrap them on a paraffin skeleton to make ceramsite with a particle size of 5-6mm and a skeleton, cover it with a layer of plastic wrap, and place it in a cool place to age for 24 hours. The aged ceramsite is placed in a constant temperature drying oven to dry for 3 hours, and the melted paraffin solution is collected. After drying, ceramsite with melt holes 3 on the surface is obtained. The ceramsite is sintered in a staged heating method to be fired into ceramsite filter material, and the surface of the ceramsite filter material is polished to remove the skin remaining at the mouth of part of the melt hole 3 to obtain a ceramsite filter material with a melt hole on the surface.
[0040] The amount of the binder attapulgite added is 5 parts;
[0041] The pore-forming agent is active C powder, and the addition amount is 1 part;
[0042] The co-solvent is magnesium carbonate, which is added in an amount of 1 part;
[0043] The calcination process of stage heating is as follows: heating rate of 5℃ / min, from room temperature to 450℃; heating rate of 3℃ / min, from 450℃ to 530℃, keeping at 530℃ for 15min; heating rate of 7℃ / min, from 530℃ to sintering temperature of 1050℃, staying at sintering temperature for 60min, and then cooling to room temperature with the furnace.
[0044] Example 2
[0045] Take the above iron tailings as raw materials, take 90 parts of raw materials, grind them in a mill for 1 hour, pass through a 200 mesh sieve, and place them in a drying oven for drying. After grinding and mixing the iron tailings, pore-forming agent, binder and flux in proportion, add an appropriate amount of water, and mix them in a granulator and wrap them on a paraffin skeleton to make ceramsite with a particle size of 5-6mm and a skeleton, cover it with a layer of plastic wrap, and place it in a cool place to age for 24 hours. The aged ceramsite is placed in a constant temperature drying oven to dry for 3 hours, and the melted paraffin solution is collected. After drying, ceramsite with melt holes 3 on the surface is obtained. The ceramsite is sintered in a staged heating method to be fired into ceramsite filter material, and the surface of the ceramsite filter material is polished to remove the skin remaining at the mouth of part of the melt hole 3 to obtain a ceramsite filter material with a melt hole on the surface.
[0046] The amount of the binder attapulgite added is 10 parts;
[0047] The pore-forming agent is active C powder, and the addition amount is 5 parts;
[0048] The cosolvent is magnesium carbonate, which is added in an amount of 7.5 parts;
[0049] The calcination process of stage heating is as follows: heating rate of 5℃ / min, from room temperature to 450℃; heating rate of 3℃ / min, from 450℃ to 530℃, keeping at 530℃ for 15min; heating rate of 7℃ / min, from 530℃ to sintering temperature of 1050℃, staying at sintering temperature for 60min, and then cooling to room temperature with the furnace.
[0050] Example 3
[0051] Take the above iron tailings as raw materials, take 100 parts of raw materials, grind them in a mill for 1 hour, pass through a 200 mesh sieve, and place them in a drying oven for drying. After grinding and mixing the iron tailings, pore-forming agent, binder and flux in proportion, add an appropriate amount of water, and mix them in a granulator and wrap them on a paraffin skeleton to make ceramsite with a particle size of 5-6mm and a skeleton, cover it with a layer of plastic wrap, and place it in a cool place to age for 24 hours. The aged ceramsite is placed in a constant temperature drying oven to dry for 3 hours, and the melted paraffin solution is collected. After drying, ceramsite with melt holes 3 on the surface is obtained. The ceramsite is sintered in a staged heating method to be fired into ceramsite filter material, and the surface of the ceramsite filter material is polished to remove the skin remaining at the mouth of part of the melt hole 3 to obtain a ceramsite filter material with a melt hole on the surface.
[0052] The amount of the binder attapulgite added is 15 parts;
[0053] The pore-forming agent is active C powder, and the addition amount is 10 parts;
[0054] The cosolvent is magnesium carbonate, which is added in an amount of 15 parts;
[0055] The calcination process of stage heating is as follows: heating rate of 5℃ / min, from room temperature to 450℃; heating rate of 3℃ / min, from 450℃ to 530℃, keeping at 530℃ for 15min; heating rate of 7℃ / min, from 530℃ to sintering temperature of 1050℃, staying at sintering temperature for 60min, and then cooling to room temperature with the furnace.
[0056] Example 4
[0057] The ceramsite filter material obtained in Example 2 was used as the optimal embodiment for experimental testing. The sintering temperature of the porous biological filter material in this embodiment was 1050°C. At this temperature, the water absorption rate of the filter material was 38.95%, the apparent porosity was 48.53%, the volume density was 1.18 g / cm3, the hydrochloric acid solubility was 1.2%, and the specific surface area was 6.211 m 2 / g, pore volume is 0.012cm 3 / g, and the average pore size is 3.5nm.
[0058] The above filter material was selected for biofilm formation experiment, and the porous mineral biofilter material prepared in the experiment was placed in the reactor. During the biofilm formation process, another important indicator for measuring the success of biofilm formation of the filter material is the removal rate of ammonia nitrogen. When the removal rate of ammonia nitrogen exceeds 60%, the biofilm formation is successful.
[0059] See also Figure 4 It can be seen that the ammonia nitrogen removal rate of the filter material has a trend of gradual increase. When the experiment was carried out for 15 days, the ammonia nitrogen removal rate reached a maximum of 92.00%. The ammonia nitrogen removal rate did not change much in the early stage of startup. This is because the microorganisms in the reactor have not fully adapted to the water environment, and the nitrification of organic matter in the water is not obvious. At the same time, the heterotrophic bacteria in the water compete with nitrifying bacteria. From the 8th day, the ammonia nitrogen removal rate increased significantly, reaching 70.12%, and the biofilm was successful. This is because nitrifying bacteria gradually attached and grew on the filter material, which increased the ammonia nitrogen removal rate. From the 15th day to the 20th day, the ammonia nitrogen removal rate was relatively stable, reaching a maximum of 95.00%. This shows that the nitrifying bacteria in the reactor have matured in biofilm growth. Therefore, the porous filter material prepared by this method is suitable as a filter material for aerated biological filters.
[0060] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a porous biological filter material for an aerated biological filter, characterized in that: The porous biological filter material is made of iron tailings as a matrix, attapulgite as a binder, activated carbon powder as a pore-forming agent, magnesium carbonate as a flux, and paraffin as a fusible skeleton, and is sintered to form a ceramsite filter material with melt holes on the surface; The raw materials of the porous biological filter material are formulated by weight as follows: 80-100 parts of iron tailings, 5-15 parts of attapulgite, 1-10 parts of activated carbon powder, and 1-15 parts of magnesium carbonate; The method for preparing the porous biological filter material for the aerated biological filter specifically comprises the following steps: Step 1: Grind the raw material iron tailings in a mill for 1 hour, pass through a 200-mesh sieve, and place in a drying oven for drying; Step 2, grinding and mixing the dried iron tailings with a pore-forming agent, a binder and a flux in proportion, adding water and stirring evenly to obtain a mixture A for standby use; Step 3, the mixed material A obtained in step 2 is wrapped on a paraffin frame by a granulator to form ceramsite with a particle size of 5-6 mm and a frame, covered with a layer of plastic wrap, and placed in a cool place for aging for 24 hours; Step 4, placing the aged ceramsite in a constant temperature drying oven and drying for 3 hours, and collecting the melted paraffin solution. After drying, ceramsite with melt holes (3) on the surface is obtained; Step 5, sintering the ceramsite obtained in step 4 by a staged heating method to form a ceramsite filter material; Step 6, grinding the surface of the ceramsite filter material obtained in step 5 to remove the remaining skin at the opening of part of the melt hole (3), so as to obtain a ceramsite filter material with a melt hole on the surface; In step 3, the paraffin skeleton comprises a melting core (1), a plurality of melting rods (2) are evenly distributed in the circumferential direction of the melting core (1), the maximum radius of the melting rods (2) around the melting core (1) is the same as the radius of the expanded clay, and the melting holes on the surface of the expanded clay are interconnected.
2. The method for preparing a porous biological filter material for an aerated biological filter according to claim 1, characterized in that: In step 1, the iron tailings are high-silicon iron tailings, wherein the SiO2 specific gravity ranges from 60-66%, and the Al2O3 ranges from 8-10%.
3. The method for preparing a porous biological filter material for an aerated biological filter according to claim 1, characterized in that: In step 5, the staged temperature-raising sintering method comprises the following steps: A. In the first stage, the temperature is raised from room temperature to 450°C at a rate of 5°C / min; B. In the second stage, the temperature was raised from 450°C to 530°C at a rate of 3°C / min, and kept at 530°C for 15 minutes; C. The third stage is to heat up from 530°C to 1050°C at a heating rate of 7°C / min, stay at 1050°C for 60 minutes, and then cool to room temperature with the furnace.