A method for determining phase content of carbon structural steel and its application

The three-dimensional morphology image is obtained by laser confocal microscopy and divided into ferrite and pearlite phases, which solves the problem of inaccurate determination of the phase content of medium and low carbon structural steel by optical grayscale method, and realizes the phase content of carbon structural steel. accurate measurement and strength assessment.

CN113884491BActive Publication Date: 2024-10-18SGIS SONGSHAN CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111385876.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-22
Publication Date
2024-10-18
Estimated Expiration
2041-11-22

AI Technical Summary

Technical Problem

When the existing optical grayscale method is used to measure the phase content of medium and low carbon structural steel, there is a problem of inaccurate determination of the pearlite and ferrite phase content, resulting in the inability to accurately evaluate the phase content of structural steel.

Method used

A laser confocal microscope is used to obtain a three-dimensional topography of the steel sample surface, and the ferrite and pearlite phases are divided by the height standard deviation of the leveling and cross-sectional profile curves to avoid the error of the grayscale method and improve the accuracy of phase content determination. .

Benefits of technology

It achieves the accurate determination of the phase content of carbon structural steel, improves the accuracy of carbon content and strength assessment of steel, and avoids the error of the optical grayscale method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113884491B_ABST
    Figure CN113884491B_ABST
Patent Text Reader

Abstract

The present invention adopts a laser confocal microscope to obtain the three-dimensional morphology of the area to be measured, and selects three points of the same circle in the ferrite area, adopts a three-point leveling method to level the three-dimensional morphology image, uses the leveling plane as the height reference of the three-dimensional stereoscopic morphology image, intercepts the three-dimensional stereoscopic morphology image of the area to be measured, obtains a limited number of cross sections and cross-sectional contour curves, and divides the cross-sectional contour curve into ferrite phase and pearlite phase according to whether the height standard deviation of a continuous preset number of points is less than or equal to a preset value and whether the calculated height of a continuous preset number of points is less than 0, respectively adds the ferrite phase and pearlite phase of each cross section, obtains the phase content of the area to be measured, and improves the accuracy of phase content determination.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel phase content determination, and specifically relates to a method for determining the phase content of carbon structural steel. Background Art

[0002] Optical microscope and scanning electron microscope can be used to observe the metallographic structure of steel. Optical microscope is a two-dimensional morphological tool with low effective resolution and small depth of field. It cannot observe the three-dimensional morphology in the longitudinal direction. The scanning electron microscope is more complicated in sample preparation and sometimes causes sample damage. It has limitations on the scanning area and the surface height of the material. At the same time, it cannot measure information such as surface area, volume, and depth. Laser confocal microscopy can be used to observe the three-dimensional morphology and topography of the sample surface at the submicron level, and can also measure a variety of tiny dimensions, such as volume, area, grain, film thickness, depth, length and width, line roughness, surface roughness, etc. Compared with other detection methods, laser confocal has its unique advantages, which improves the clarity of the picture, has a good depth of field, and improves the resolution. It has certain advantages in metallographic structure observation.

[0003] Medium and low carbon structural steel (carbon content is 15% to 50%), the normal metallographic structure is ferrite and pearlite, the pearlite phase content has a certain correlation with its mechanical properties, and the calculation of its pearlite phase content is of great significance to the estimation of its carbon content and strength level. The existing technology mostly uses the optical grayscale method. Pearlite is a lamellar mixed structure of ferrite + cementite. The grayscale method will mechanically classify the ferrite lamellar structure as ferrite instead of pearlite. At the same time, some contamination on the inspection surface will also increase its grayscale, classifying ferrite as pearlite, thereby affecting the accuracy of phase content determination. Summary of the invention

[0004] The purpose of the present invention is to overcome the defect that when the existing optical grayscale method is used to determine the phase content of medium and low carbon carbon structural steel, the grayscale calculation is inaccurate and has errors in determining the pearlite and ferrite phase contents, resulting in the inability to accurately evaluate the relative content of the structural steel phases. A method for determining the phase content of carbon structural steel is provided, which does not estimate the phase content by grayscale, thereby improving the accuracy of the phase content determination.

[0005] In order to achieve the above object, the present invention provides a method for determining the phase content of carbon structural steel in a first aspect.

[0006] The method comprises: grinding and corroding the inspection surface of the steel sample, and then using a laser confocal microscope to measure the phase content, wherein the phase content measurement comprises:

[0007] (1) using a laser confocal microscope to obtain a three-dimensional topographic image of the surface area of ​​the sample;

[0008] (2) leveling the three-dimensional topography image, wherein the leveling plane serves as a height reference plane of the three-dimensional topography image;

[0009] (3) intercepting the three-dimensional topography image in a direction parallel to the X-axis or the Y-axis to obtain a finite number of cross sections and cross-sectional profile curves;

[0010] (4) dividing the cross section where the cross section profile curve is located into a ferrite phase and a pearlite phase according to whether the standard deviation of the heights of a preset number of consecutive points of the cross section profile curve is less than or equal to a preset value, and the area less than or equal to the preset value is the ferrite phase;

[0011] (5) The ferrite phase and the pearlite phase of each cross section are added up respectively to obtain the phase content of the area to be measured.

[0012] Preferably, the resolution of the three-dimensional topography is above 0.125 μm, the spacing between the finite number of cross sections is below 0.125 μm, and the horizontal coordinates or vertical coordinates of adjacent points in the cross-sectional contour curve are spaced below 0.125 μm.

[0013] Preferably, the preset number is greater than 5.

[0014] Preferably, the preset value is 0.025-0.035 μm.

[0015] Preferably, three points on the same circle are selected in the ferrite region, and the three-point leveling method is adopted to level the three-dimensional topography image;

[0016] After obtaining the cross-sectional contour curve, the basis for dividing the cross-sectional area where the cross-sectional contour curve is located into ferrite phase and pearlite phase also includes calculating the average height of each point on the cross-sectional contour curve, and the calculated height of each point is obtained by subtracting the average height from the original height of each point on the cross-sectional contour curve. The area where the calculated height of a preset number of points is less than 0 is ferrite.

[0017] Preferably, the corrosion liquid is 4% nitric acid alcohol, and the corrosion time is 3-6s.

[0018] Preferably, the grinding includes a coarse grinding process, a fine grinding process, a 3 μm polishing process and a 1 μm polishing process.

[0019] Preferably, the time of the coarse grinding process is 50-70s, the force is 90-110Nm, and the rotation speed is 90-100 rpm; the time of the fine grinding process is 11-13min, the force is 145-155Nm, and the rotation speed is 300-320 rpm.

[0020] Preferably, the rotation speed of the 3μm polishing process is 140-160 rpm, the force is 145-155Nm, the spray frequency is 25-30s / time, and the polishing time is 3-4min. The rotation speed of the 1μm polishing process is 140-160 rpm, the force is 85-95N / m, the spray frequency is 25-30s / time, and the polishing time is 2-3min.

[0021] The second aspect of the present application provides the application of the carbon structural steel phase content determination method of the first aspect of the present application in the detection of carbon structural steel phase content.

[0022] The beneficial effects of this application include:

[0023] The present invention adopts a laser confocal microscope to obtain a three-dimensional morphology image of the sample after corrosion, and intercepts the three-dimensional morphology image after leveling to obtain a cross section and a cross-sectional contour curve. According to whether the height standard deviation of a preset number of points of the cross-sectional contour curve is less than or equal to a preset value, the cross section where the cross-sectional contour curve is located is divided into ferrite and pearlite, thereby avoiding the shortcomings of the optical grayscale method for determining the phase content, being able to accurately distinguish pearlite and ferrite, thereby obtaining an accurate phase content, and estimating the carbon content and strength of the steel.

[0024] By leveling, it is avoided that the height of the adjacent ferrite in the cross section is stepped, thereby affecting the distinction between ferrite and pearlite according to the standard deviation of the height of a continuous preset number of points of the cross-sectional profile curve.

[0025] By grinding, the scratches on the sample surface can be reduced. The corrosion effect of scratches is different from that of non-scratched areas. Scratches will affect the corrosion effect of the sample and increase the complexity of the corrosion effect. Usually after corrosion, the height of the scratches in the three-dimensional topography is lower, which will also affect the height of the midpoint of the cross-sectional profile curve, thereby affecting the accurate distinction between ferrite and pearlite.

[0026] Grinding can also reduce the deformation layer on the surface of the sample. If there is a deformation layer, the complexity of corrosion will increase. In addition, the ferrite will have poor flatness after corrosion and will have a concave-convex structure, which will affect the height of the midpoint of the cross-sectional profile curve, thereby affecting the accurate distinction between ferrite and pearlite. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 The present invention is a flow chart of the method for determining the phase content of carbon structural steel.

[0029] Figure 2 In Example 1, a laser confocal microscope is used to obtain a three-dimensional morphology image of the area to be tested on the surface of the sample.

[0030] Figure 3 This is a schematic diagram of the leveling process of this application.

[0031] FIG4 is a schematic diagram of the intercept length of the characteristic tissue profile of Example 1 and a cross-sectional profile curve of the illustrated cross section, Figure 4a This is a schematic diagram of the intercept length of the characteristic tissue contour. Figure 4b for Figure 4a The cross-sectional profile curve of the cross section shown. Figure 4a The dashed line in the figure represents a cross section, and only a part of the cross section is shown. Figure 4a The changes in brightness of the image represent different phases, where the two ends of the dotted line are in the ferrite phase and the middle spans the pearlite phase. Figure 4b The horizontal axis corresponds to the X-axis, the vertical axis corresponds to the Z-axis, and the vertical axis represents the calculated height obtained by subtracting the average height from the original height.

[0032] FIG5 is a schematic diagram of the intercept length of the characteristic tissue profile of Example 2 and a cross-sectional profile curve of the illustrated cross section, Figure 5a This is a schematic diagram of the intercept length of the characteristic tissue contour. Figure 5b for Figure 5a Section profile curve for the cross section shown.

[0033] FIG6 is a schematic diagram of the intercept length of the characteristic tissue profile of Example 3 and a cross-sectional profile curve of the illustrated cross section, Figure 6a This is a schematic diagram of the intercept length of the characteristic tissue contour. Figure 6b for Figure 6a Section profile curve for the cross section shown.

[0034] FIG7 is a schematic diagram of the cut length of the characteristic structure profile of the ferrite scratch area in Example 4 and a cross-sectional profile curve of the illustrated cross section, Figure 7a This is a schematic diagram of the intercept length of the characteristic tissue contour. Figure 7b for Figure 7a Section profile curve for the cross section shown.

[0035] FIG8 is a schematic diagram of the intercept length of the characteristic structure profile of the pearlite scratch area in Example 4 and a cross-sectional profile curve of the illustrated cross section, Figure 8a This is a schematic diagram of the intercept length of the characteristic tissue contour. Figure 8b for Figure 8a Section profile curve for the cross section shown.

[0036] FIG9 is a three-dimensional topographic image of the sample surface area to be measured obtained by using a laser confocal microscope in Example 5, a schematic diagram of the intercept length of the characteristic tissue contour, and a cross-sectional profile curve of the illustrated cross section, Figure 9a is a three-dimensional topographic image of the area to be tested on the surface of the sample, Figure 9b This is a schematic diagram of the intercept length of the characteristic tissue contour. Fig.9c for Figure 9b Section profile curve for the cross section shown.

[0037] Fig.10a This is a schematic diagram of the intercept length of the characteristic tissue contour of Example 6. Fig.10b for Fig.10a Section profile curve for the cross section shown. DETAILED DESCRIPTION

[0038] The embodiments of the present application will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present application and should not be considered to limit the scope of the present application. If the specific conditions are not specified in the examples, they are carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. If the detection method used is not particularly specified, it is carried out according to the national standard or conventional detection method.

[0039] Since pearlite is a lamellar mixed structure of ferrite + cementite, in order to overcome the existing practice of using a laser confocal microscope to determine the phase content of medium and low carbon carbon structural steels using an optical grayscale method, in which the ferrite lamellar structure is classified as ferrite instead of pearlite, thereby affecting the accuracy of phase content determination and further affecting the accuracy of carbon content and strength assessment, the present application provides a method for determining the phase content of carbon structural steel.

[0040] In order to facilitate understanding of the specific implementation process of the above-mentioned determination method, the method for determining the phase content of carbon structural steel in the present invention is described below.

[0041] Flow chart reference for the determination method of phase content in carbon structural steel Figure 1 .

[0042] A method for determining phase content of carbon structural steel, the method comprising: grinding and corroding the inspection surface of the steel sample, and then using a laser confocal microscope to determine the phase content, wherein the phase content determination comprises:

[0043] (1) using a laser confocal microscope to obtain a three-dimensional topography image of the surface area of ​​the sample;

[0044] (2) leveling the three-dimensional topography image, wherein the leveling plane serves as a height reference plane of the three-dimensional topography image;

[0045] (3) intercepting the three-dimensional topography image in a direction parallel to the X-axis or the Y-axis to obtain a finite number of cross sections and cross-sectional profile curves;

[0046] (4) dividing the cross section where the cross section profile curve is located into a ferrite phase and a pearlite phase according to whether the standard deviation of the heights of a preset number of consecutive points of the cross section profile curve is less than or equal to a preset value, and the area less than or equal to the preset value is the ferrite phase;

[0047] (5) The ferrite phase and the pearlite phase of each cross section are added up respectively to obtain the phase content of the area to be measured.

[0048] In the present invention, it should be understood that the working mode of the laser confocal microscope is the normal temperature mode. The laser confocal microscope selects Zeiss LSM800 / Imager.Z2m. The sample is ground by ATM fully automatic metallographic grinding and polishing machine. The software uses Zeiss ZEN2.6 (metallographic image observation and laser 3D mapping) and ConfoMap ST (data processing of laser 3D mapping, with functions such as leveling, noise reduction, 3D composition, and extraction of morphological contours).

[0049] The measuring method of the present invention can be applied to the determination of the phase content of carbon structural steel (including low alloy) whose rolled metallographic phase is ferrite+pearlite, such as 20, 30, 40Cr, 45, 50, etc.

[0050] The three-dimensional morphology of the test area on the surface of the sample is obtained by using a laser confocal microscope. It can be obtained in the following way: place the test area of ​​the sample to be tested after grinding and corrosion on the stage of the laser confocal microscope, and rotate the stage so that the length direction of the test area is parallel to the X-axis, and the width direction is parallel to the Y-axis. Focus on the test area in the visible light mode so that the image appears clearly in the image display area, and switch the visible light mode to the laser mode. In the channel bar of the operation interface, select 405nm laser intensity of 5%, and select 1AU for the pinhole to ensure the highest resolution. Focus on the highest point and the lowest point of the inspection field respectively, set the scanning height range, and adjust the gain value during preview to eliminate the red dots (noise) that appear when the image is scanned from the highest point to the lowest point, and then scan layer by layer to obtain the three-dimensional morphology data of the test area. The three-dimensional physical morphology of the test area is as follows. Figure 2 shown.

[0051] Preferably, the laser intensity can be adjusted to obtain a clear signal without white spots appearing during drawing.

[0052] Optionally, leveling the three-dimensional topography image can be achieved in the following way: since the ferrite is uniformly corroded, the corrosion degree is close, and the ferrite area is relatively flat, three points on the same circle are selected on the adjacent and distant ferrite, and the three-point leveling method is used to level the three-dimensional topography image, and the leveling plane is used as the height reference plane of the three-dimensional topography image. The leveling process can be referred to Figure 3 , the three points are located on the ferrite.

[0053] In a direction parallel to the X-axis or the Y-axis, intercepting the three-dimensional stereoscopic morphology image to obtain a limited number of cross sections and cross-sectional profile curves can be achieved in the following manner: switching to a laser confocal three-dimensional measurement mode, in a direction parallel to the X-axis or the Y-axis, sequentially intercepting the three-dimensional stereoscopic morphology image of the area to be measured with a certain resolution, completing the interception of the entire three-dimensional stereoscopic morphology image, and obtaining a cross section and a cross-sectional profile curve each time the interception is performed, and the shape of the cross-sectional profile curve represents the surface morphology of the sample at the cross-sectional position.

[0054] It can be understood that the corrosion process adopts chemical corrosion, and for carbon structural steel, it is mainly an electrochemical dissolution process. The main structures of carbon structural steel are ferrite and pearlite. Pearlite is a lamellar mixed structure of ferrite and cementite. The potential of ferrite is -0.5V to -0.4V, and cementite is slightly lower than +0.37V. During the corrosion process, ferrite is the anode and cementite is the cathode. During the electrochemical dissolution process, ferrite is evenly dissolved by one layer, and cementite is basically insoluble. However, due to the large potential difference and fast etching speed at the phase boundary, the amount of dissolution at the phase boundary is large, forming a deeper groove. Therefore, for the ferrite and pearlite of carbon structural steel, the ferrite corrosion is more uniform, and the surface morphology of the three-dimensional stereoscopic morphology diagram presents a highly close area, while the pearlite corrosion is uneven, presenting a highly oscillating area. Therefore, the ferrite phase and the pearlite phase can be distinguished according to the surface morphology changes. The surface morphology changes can be characterized by the changes in the height standard deviation of the continuous points of the cross-sectional profile curve. However, the ferrite lamellae in pearlite are uniformly dissolved, and the surface morphology of the ferrite lamellae in pearlite is uniform. The height standard deviation of the continuous points corresponding to the ferrite lamellae in the cross-sectional profile curve is similar to the height standard deviation of the continuous points corresponding to the ferrite phase. However, the thickness of the ferrite lamellae in the equilibrium pearlite is about 0.25μm to 0.5μm, and the number of continuous points corresponding to the ferrite lamellae in the cross-sectional profile curve is limited, that is, when calculating the height standard deviation of the continuous points, when the number of points involved in the calculation is large and exceeds a certain value, the height standard deviation of the continuous points corresponding to the pearlite phase in the cross-sectional profile curve will be different from the height standard deviation of the ferrite phase. Therefore, the ferrite phase and the pearlite phase can be distinguished according to the height standard deviation of the continuous preset number of points of the cross-sectional profile curve. When the height standard deviation is less than or equal to the preset value, the cross section where the cross-sectional profile curve is located is the ferrite phase. When the height standard deviation is greater than the preset value, the cross section where the interface profile curve is located is the pearlite phase.

[0055] It can be understood that the process of adding the ferrite phase and pearlite phase of each cross section to obtain the phase content of the area to be tested is to obtain the amount of ferrite and pearlite phase of each cross section according to whether the height standard deviation of a continuous preset number of points of the cross-sectional contour curve is less than or equal to the preset value, and by successively intercepting the three-dimensional morphology image of the area to be tested, a finite number of cross sections have been obtained, and the ferrite of each cross section is added to obtain the ferrite amount of the area to be tested, and the pearlite of each cross section is added to obtain the pearlite amount of the area to be tested, thereby obtaining the phase content of the area to be tested.

[0056] Pearlite is a lamellar mixed structure of ferrite + cementite. The grayscale method will mechanically classify the ferrite lamellar structure as ferrite instead of pearlite. At the same time, certain pollution on the inspection surface will also increase its grayscale. Classifying ferrite as pearlite for calculation will affect the determination of phase content. The present invention does not use the optical grayscale method to estimate the phase content. A laser confocal microscope is used to obtain the three-dimensional morphology of the area to be measured, and the three-dimensional stereoscopic morphology of the area to be measured is intercepted in turn to obtain a limited number of cross sections and cross-sectional contour curves. According to whether the height standard deviation of the continuous preset number of points of the cross-sectional contour curve is less than or equal to the preset value, the cross section where the cross-sectional contour curve is located is divided into ferrite phase and pearlite phase, thereby improving the accuracy of phase content determination. Since the phase content is determined based on the height standard deviation, the accurate quantification of the height affects the accuracy of the measurement result. At the same time, the difference in the height standard deviation of the continuous preset number of points in the cross-sectional contour curve will be caused by the difference in the corrosion effect of pearlite and ferrite, and the corrosion effect will affect the accuracy of the result. Therefore, it is necessary to ensure accurate quantification of height and the difference in corrosion effects between pearlite and ferrite, as well as to accurately reflect the difference in corrosion effects between pearlite and ferrite. By leveling, the leveling plane is used as the height reference plane of the three-dimensional topography, which can ensure that the height measurement reference of the area to be measured is consistent, and the height can be accurately quantified. In addition, it can avoid the height of the adjacent ferrite in the cross section from being stepped, thereby affecting the reflection of the difference in corrosion effects between pearlite and ferrite. By grinding, scratches on the surface of the sample can be reduced. The corrosion effects of scratches and non-scratched areas are different. Scratches will affect the corrosion effects of ferrite and pearlite, and increase the complexity of the corrosion effect. Usually after corrosion, the height of the scratches in the three-dimensional topography is lower, which will affect the height of the midpoint of the cross-sectional profile curve, thereby affecting the accurate distinction between ferrite and pearlite based on the difference in corrosion effects between pearlite and ferrite. Grinding can also reduce the deformation layer on the surface of the sample. If there is a deformation layer, the complexity of corrosion will increase. In addition, the ferrite will have poor flatness after corrosion and will have a concave-convex structure, which will affect the height of the midpoint of the cross-sectional profile curve and will also affect the accurate distinction between ferrite and pearlite based on the difference in corrosion effects of pearlite and ferrite.

[0057] In a preferred embodiment of the present invention, the resolution of the three-dimensional topography is above 0.125 μm, the spacing between the finite number of sections is below 0.125 μm, and the horizontal or vertical coordinates of adjacent points in the cross-sectional contour curve are spaced below 0.125 μm.

[0058] The resolution of the three-dimensional morphology is reflected in the three-dimensional coordinate spacing of adjacent points in the three-dimensional morphology grid map. The three-dimensional morphology map is intercepted according to the coordinate spacing of adjacent points. The spacing of a finite number of sections is equal to the value of the resolution, and the horizontal or vertical coordinate spacing of adjacent points in the cross-sectional contour curve is equal to the value of the resolution. The higher the resolution of the three-dimensional morphology, the smaller the spacing of the finite number of sections and the horizontal or vertical coordinate spacing of adjacent points, and the higher the accuracy of the phase content calculation. When the resolution of the three-dimensional morphology is above 0.125μm, the spacing of the finite number of sections and the horizontal or vertical coordinate spacing of adjacent points are below 0.125μm, the phase content calculation has a higher accuracy. The thickness of the ferrite lamellae in pearlite is 0.25μm to 0.5μm. When the interval between adjacent points in the cross-sectional profile curve is determined, the number of continuous points corresponding to the ferrite lamellae in the cross-sectional profile curve can be determined. When distinguishing pearlite from ferrite, the value of the continuous preset number can be determined. For example, when the interval between adjacent points in the cross-sectional profile curve is 0.125μm, the number of continuous points corresponding to the ferrite lamellae in the cross-sectional profile curve is 2-4 points. When distinguishing pearlite from ferrite, the value of the continuous preset number is greater than or equal to 5.

[0059] In a preferred embodiment of the present invention, the preset number is greater than 5.

[0060] When the resolution is 0.125 μm, the spacing between the finite cross sections is 0.125 μm, the points in the cross section profile curve, the horizontal coordinates or vertical coordinates of adjacent points are 0.125 μm apart, and when distinguishing pearlite from ferrite, the value of the continuous preset number is greater than or equal to 5. When the resolution is higher, the spacing between the finite cross sections and the horizontal coordinates or vertical coordinates of the points in the cross section profile curve are smaller, and the minimum value of the preset number is the minimum integer greater than the ratio of the thickness of the ferrite lamella in the pearlite (0.25 μm to 0.5 μm) to the horizontal coordinate or vertical coordinate spacing, and the minimum integer is greater than or equal to 5.

[0061] In a preferred embodiment of the present invention, the preset value is 0.025-0.035 μm.

[0062] When the resolution of the three-dimensional morphology is 0.125μm, the spacing of a finite number of cross sections is 0.125μm, and the interval of the horizontal coordinate or vertical coordinate of the points in the cross-sectional profile curve is 0.125μm, the ferrite phase and pearlite phase of the cross-sectional profile curve can be more accurately divided according to whether the height standard deviation of 5 consecutive points of the cross-sectional profile curve is less than or equal to 0.025-0.035μm, and the phase content calculation has a higher accuracy. When the resolution of the three-dimensional morphology is greater than 0.125μm, when calculating the height standard deviation, the calculation range, that is, the total horizontal coordinate or vertical coordinate difference of the consecutive preset number of points, is consistent with the calculation range of the resolution of 0.125μm and the preset number of 5, the preset value is also 0.025-0.035μm.

[0063] In a preferred embodiment of the present invention, three points on the same circle are selected in the ferrite region, and the three-point leveling method is adopted to level the three-dimensional morphology image; after obtaining the cross-sectional contour curve, the basis for dividing the cross-sectional contour curve into ferrite phase and pearlite phase also includes calculating the average height of each point on the cross-sectional contour curve, and the original height of each point on the cross-sectional contour curve is subtracted from the average height to obtain the calculated height of each point, and the region where the calculated height of a preset number of points is less than 0 is ferrite.

[0064] The main structures of carbon structural steel are ferrite and pearlite. Pearlite is a lamellar mixed structure of ferrite and cementite. The potential of ferrite is -0.5V to -0.4V, and cementite is slightly lower than +0.37V. During the corrosion process, ferrite is the anode and cementite is the cathode. During the electrochemical dissolution process, ferrite is evenly dissolved and cementite is basically insoluble. For ferrite and pearlite of carbon structural steel, ferrite corrodes more evenly, and the surface morphology of the three-dimensional morphology diagram shows a highly close area, while pearlite corrodes unevenly, showing a highly oscillating area. In addition, since ferrite is easily corroded, a relatively low-height area is presented in the surface morphology of the three-dimensional topography. On the basis of distinguishing ferrite and pearlite phases according to whether the height standard deviation of a continuous preset number of points is less than or equal to the preset value, the ferrite and pearlite phases can be further distinguished according to the height of a continuous preset number of points on the cross-sectional profile curve. Regarding the provisions of the continuous preset number, since pearlite contains ferrite lamellae and a large amount of dissolved at the phase boundary, a deeper groove is formed. When the height of multiple consecutive points is relatively low, it is distinguished as ferrite. After defining the height reference plane, the original height of each point on the cross-sectional profile curve is obtained. The average height of each point can be obtained by averaging the original height of each point. The calculated height of each point is obtained by subtracting the average height from the original height of each point. The area where the calculated height of a continuous preset number of points is less than 0 is ferrite. This basis is a specific method for distinguishing ferrite and pearlite phases according to the height of a continuous preset number of points on the cross-sectional profile curve. Since three points on the same circle are selected in the ferrite region, the three-point leveling method is adopted to level the three-dimensional topography image, and the calibration plane is the height reference plane of the three-dimensional topography image, and the height of the height reference plane is 0, the point corresponding to the ferrite in the cross-sectional profile curve has a height close to the height of the height reference plane, that is, close to 0, and the original height of the point on the cross-sectional profile curve corresponding to the ferrite minus the average height is less than 0.

[0065] In a preferred embodiment of the present invention, the corrosion liquid is 4% nitric acid alcohol, and the corrosion time is 3-6s.

[0066] Preferably, after the corrosion is completed, the inspection surface of the steel sample is rinsed with clean water, ultrasonically cleaned for 1-2 minutes, and the inspection surface of the steel sample is rinsed and dried with alcohol.

[0067] When 4% nitric acid alcohol is used and the corrosion time is 3-6s, the corrosion effects on the pearlite phase and the ferrite phase are significantly different, and the corrosion degree of pearlite is weaker. Ferrite and pearlite can be distinguished by the difference in corrosion effects, that is, the cross-section where the cross-sectional contour curve is located can be divided into ferrite phase and pearlite phase by whether the height standard deviation of a continuous preset number of points is less than or equal to a preset value and whether the calculated height of a continuous preset number of points is less than 0.

[0068] Optionally, the corrosion time can be 3s, 4s, 5s, or 6s.

[0069] In a preferred embodiment of the present invention, the grinding includes a coarse grinding process, a fine grinding process, a 3 μm polishing process and a 1 μm polishing process.

[0070] When cutting the sample, a deformation layer and scratches will appear on the inspection surface of the steel sample. If there is a deformation layer, the complexity of the corrosion will increase, and the ferrite will have poor flatness after corrosion, and there will be a concave-convex structure, which will affect the height of the midpoint of the cross-sectional profile curve, and will affect the accurate distinction between ferrite and pearlite based on the difference in corrosion effects between pearlite and ferrite. If there are scratches, the corrosion effect at the scratched and non-scratched locations is different. Scratches will affect the corrosion effects of ferrite and pearlite, and increase the complexity of the corrosion. Usually after corrosion, the height of the scratches in the three-dimensional morphology diagram is low, which will affect the height of the midpoint of the cross-sectional profile curve, thereby affecting the accurate distinction between ferrite and pearlite based on the difference in corrosion effects between pearlite and ferrite. Scratches and deformation layers on the surface of the sample can be reduced by grinding. In the grinding process, the coarse grinding and fine grinding processes are more efficient than the polishing process in eliminating the deformation layer, but new deformation layers may be generated. The larger the abrasive grain size in the polishing liquid in the polishing process, the higher the efficiency of eliminating the deformation layer, but new deformation layers may also be generated. In order to ensure the polishing efficiency and prevent the generation of new deformation layers at the same time, the coarse grinding process, fine grinding process, 3μm polishing process and 1μm polishing process are combined for grinding. The mirror surface with no more than 3 visible scratches at 100 times is basically free of plastic deformation layer on the surface.

[0071] Optionally, the grinding process may sequentially perform coarse grinding, fine grinding, 3 μm polishing, and 1 μm polishing.

[0072] In a preferred embodiment of the present invention, the time of the coarse grinding process is 50 to 70 seconds, the force is 90 to 110 Nm, and the rotation speed is 90 to 100 rpm; the time of the fine grinding process is 11 to 13 minutes, the force is 145 to 155 Nm, and the rotation speed is 300 to 320 rpm.

[0073] Rough grinding is to use a grinding wheel to smooth the inspection surface and remove the deformation layer caused by cutting. Because the grinding wheel is coarse and the grinding is fast, the deformation layer caused to the inspection surface is large, so a short time and slightly smaller force are selected; fine grinding is to use 18um abrasive to remove the deformation layer caused by rough grinding, grinding it away layer by layer. Considering efficiency, a large force, high speed and long time are selected.

[0074] In a preferred embodiment of the present invention, the rotation speed of the 3μm polishing process is 140-160 rpm, the force is 145-155Nm, the spray frequency is 25-30s / time, and the polishing time is 3-4min. The rotation speed of the 1μm polishing process is 140-160 rpm, the force is 85-95N / m, the spray frequency is 25-30s / time, and the polishing time is 2-3min.

[0075] The abrasive size in the polishing liquid, the applied pressure and the polishing time have an impact on the polishing effect. The 1μm abrasive has a smaller degree of mechanical grinding on the inspection surface than the 3μm abrasive, which basically eliminates the deformation layer caused to the inspection surface, which is reflected in the metallographic clarity. The pressure applied with the 1um abrasive is also reduced accordingly, and the deformation layer produced by the 3um is ground away instead of adding a new deformation layer. The time is also reduced accordingly. If the time is too long, after the 3um deformation layer is ground away, another 1um deformation layer is added, and the number of scratches increases, which is not worth the loss.

[0076] The choice of polishing speed is used to balance the speed and the spray frequency. The choice of the spray frequency needs to keep the abrasive in a lubricated state and discharge the grinding products. If the spray is insufficient, the dry grinding state will produce more scratches. According to the difference in the corrosion effect of pearlite and ferrite, ferrite and pearlite can be accurately distinguished.

[0077] The second aspect of the present invention provides the application of the method for determining the phase content of carbon structural steel according to the first aspect of the present application for detecting the phase content of carbon structural steel.

[0078] The present invention does not use the optical grayscale method to estimate the phase content, but uses a laser confocal microscope to obtain the three-dimensional morphology of the area to be measured, intercepts the three-dimensional stereoscopic morphology of the area to be measured in turn, obtains a limited number of cross sections and cross-sectional profile curves, and divides the cross section where the cross-sectional profile curve is located into a ferrite phase and a pearlite phase according to whether the height standard deviation of the continuous preset number of points of the cross-sectional profile curve is less than or equal to the preset value, thereby improving the accuracy of the phase content determination. In addition, three points of the same circle are selected in the ferrite area, and the three-point leveling method is adopted to level the three-dimensional morphology map, and the leveling plane is used as the height reference of the three-dimensional morphology map. After obtaining the cross-sectional profile curve, the average height of each point of the cross-sectional profile curve is calculated, and the original height of each point on the cross-sectional profile curve is subtracted from the average height to obtain the calculated height of each point, and the ferrite and pearlite are distinguished according to whether the calculated height of the continuous preset number of points is less than 0. By combining the two distinguishing methods, it is judged whether the height standard deviation of the continuous preset number of points is less than or equal to the preset value, and whether the calculated height of the continuous preset number of points is less than 0, which can further improve the accuracy of the phase content determination. At the same time, through a specific grinding process, the deformation layer and scratches on the inspection surface of the steel sample can be reduced, the complexity of the corrosion effect can be reduced, the influence of the deformation layer and scratches on the height of the midpoint of the cross-sectional profile curve can be reduced, and the influence on accurately distinguishing ferrite and pearlite based on the difference in the corrosion effects of pearlite and ferrite can be reduced.

[0079] The following examples take the measurement of the phase content (the matrix structure is rolled ferrite + pearlite) of 50 carbon structural steel as an example.

[0080] Example 1

[0081] Step 1: Rough grinding, fine grinding, 3μm polishing process and 1μm polishing are sequentially applied to the inspection surface of the carbon structural steel sample, wherein the time of the rough grinding process is 60s, the force is 100Nm, the speed is 90 rpm, the time of the fine grinding process is 12min, the force is 150Nm, the speed is 300 rpm, the speed of the 3μm polishing process is 150 rpm, the force is 150Nm, the spray frequency is 30s / time, the polishing time is 3min, the speed of the 1μm polishing process is 150 rpm, the force is 90N / m, the spray frequency is 30s / time, and the polishing time is 2min;

[0082] Step 2: Corrode the inspection surface of the carbon structural steel. The corrosion method is chemical corrosion, the corrosion liquid is 4% nitric acid alcohol, and the corrosion time is 4s. After the corrosion is completed, rinse the inspection surface of the steel sample with clean water, ultrasonically clean it for 1-2 minutes, and rinse and dry the inspection surface of the steel sample with alcohol.

[0083] Step 3: Place the area to be tested of the sample to be tested after grinding and corrosion on the stage of the laser confocal microscope, and rotate the stage so that the length direction of the area to be tested is parallel to the X-axis and the width direction is parallel to the Y-axis. Focus the area to be tested in the visible light mode so that the image appears clearly in the image display area, and switch the visible light mode to the laser mode. In the channel bar of the operation interface, select 405nm laser intensity as 5%, and select 1AU for the pinhole to ensure the highest resolution. Adjust the focus knob clockwise until the blue screen appears and the black basically covers the image. Click the [Set Start Point] button to determine the upper limit point, and slowly adjust the focus knob counterclockwise. When the red dot appears in the image, reduce the main gain value of the channel bar until the red dot just does not appear. This process does not stop until the blue screen appears and the black basically covers the image. Click the [Set Beam Point] button to determine the lower limit point. To obtain 3D data of the full height (the lowest and highest can be measured). Click Stop to stop the preview mode, and click the Best Optimization button to automatically set the optimized scanning step. In laser mode, the area to be tested is scanned layer by layer to obtain a two-dimensional topography map of the area to be tested. After obtaining the two-dimensional topography map, the Gaussian operator method is used to reduce noise in the image, flatten the image, remove noise peaks, and then switch the two-dimensional topography map to a three-dimensional topography map to obtain the three-dimensional physical morphology of the area to be tested. The resolution of the three-dimensional topography map is 0.125μm.

[0084] Step 4: Select three points on the same circle on the adjacent and distant ferrite, and use the three-point leveling method to level the three-dimensional topography image. The leveling plane is used as the height reference plane of the three-dimensional topography image.

[0085] Step 5: In the direction parallel to the X-axis, intercept the three-dimensional morphology image to obtain a finite number of cross sections and cross-sectional profile curves, the spacing between the finite number of cross sections is 0.125 μm, and the horizontal coordinate spacing of the points in the cross-sectional profile curve is 0.125 μm.

[0086] Step 6: Calculate the height standard deviation of five consecutive points of the cross-sectional profile curve, and determine whether the height standard deviation of the five consecutive points is less than 0.025 to 0.035 μm.

[0087] Step 7: Using the calibration plane as a reference, obtain the original height of each point on the cross-sectional profile curve. Calculate the average height of each point on the cross-sectional profile curve from the original height of each point. Subtract the average height from the original height of each point on the cross-sectional profile curve to obtain the calculated height of each point. Determine whether the calculated heights of 5 consecutive points on the cross-sectional profile curve are less than 0.

[0088] Figure 4b The calculated heights of the points corresponding to ferrite in the cross-sectional profile curve are shown. The calculated heights are all less than 0, and the height fluctuation of the cross-sectional profile curve corresponding to ferrite is small.

[0089] Table 1 shows Figure 4bThe standard deviation of the original heights of 5 consecutive points in the AB, CD and EF segments is shown in Table 1. The AB and EF segments are located in pearlite, with standard deviations ranging from 0.014 to 0.403, and the CD segment is located in ferrite, with standard deviations ranging from 0.002 to 0.029.

[0090] AB CD EF Minimum value (um) 0.014 0.002 0.014 Maximum value (um) 0.403 0.029 0.225 Average value(um) 0.108 0.006 0.074 Standard deviation(um) 0.049 0.002 0.032

[0091] Table 1

[0092] Example 2

[0093] The phase content determination method of Example 1 is followed, except that the corrosion time is <3s.

[0094] Figure 5a This is a schematic diagram of the intercept length of the characteristic tissue contour. Figure 5b for Figure 5a Section profile curve for the cross section shown.

[0095] Table 2 shows Figure 5b The standard deviation of the original heights of 5 consecutive points in segments AB, CD and EF.

[0096] Compared with Example 1, the corrosion time is insufficient, the ferrite is not corroded enough, the height is uneven, the height difference between pearlite and ferrite is narrowed, the discreteness is close, and the difference between the two phases is not obvious, which is not conducive to data analysis to determine the region.

[0097] AB CD EF Minimum value (um) 0.012 0.022 0.008 Maximum value (um) 0.128 0.160 0.100 Average value(um) 0.057 0.022 0.040 Standard deviation(um) 0.017 0.019 0.017

[0098] Table 2

[0099] Example 3

[0100] The phase content determination method of Example 1 is followed, except that the corrosion time is >6s.

[0101] Figure 6a This is a schematic diagram of the intercept length of the characteristic tissue contour. Figure 6b for Figure 6a Section profile curve for the cross section shown.

[0102] Table 3 shows Figure 6b The standard deviation of the original heights of 5 consecutive points in segments AB, CD and EF.

[0103] Compared with Example 1, as the corrosion time is long, the peaks and valleys of the pearlite region become wider, the relative maximum height decreases, and the ferrite region is over-corroded and becomes uneven, the dispersion increases, the relative average height increases, and the contrast relative to the pearlite decreases, which is not conducive to regional determination.

[0104] AB CD EF Minimum value (um) 0.022 0.001 0.017 Maximum value (um) 0.219 0.177 0.297 Average value(um) 0.085 0.011 0.102 Standard deviation(um) 0.036 0.008 0.044

[0105] Table 3

[0106] Example 4

[0107] According to the phase content determination method of Example 1, different grinding processes are coarse grinding, fine grinding, 3μm polishing process and 1μm polishing, which act on the inspection surface of the carbon structural steel sample in sequence, wherein the time of the coarse grinding process is 60s, the force is 130Nm, and the rotation speed is 90 rev / min, the time of the fine grinding process is 10min, the force is 160Nm, and the rotation speed is 300 rev / min, the polishing process is that the rotation speed of the 3μm polishing process is 140 rev / min, the force is 130Nm, the spray frequency is 30s / time, and the polishing time is 3min, and the rotation speed of the 1μm polishing process is 170 rev / min, the force is 80N / m, the spray frequency is 30s / time, and the polishing time is 3min.

[0108] Figure 7a As can be seen, scratches appear in the ferrite area. Figure 7b It can be seen that the curve in the ferrite region has valleys, which increases the dispersion. Figure 8a It can be seen that scratches appear in the pearlite area. Figure 8b It can be seen that there are valleys in the pearlite region curve, which lowers the mean and increases the dispersion. If the width exceeds 5 points, it will lead to misjudgment.

[0109] Example 5

[0110] According to the phase content determination method of Example 1, different grinding processes are coarse grinding, fine grinding, 3μm polishing process and 1μm polishing, which act on the inspection surface of the carbon structural steel sample in sequence, wherein the time of the coarse grinding process is 60s, the force is 100Nm, and the rotation speed is 90 rev / min, the time of the fine grinding process is 12min, the force is 150Nm, and the rotation speed is 300 rev / min, the polishing process is that the rotation speed of the 3μm polishing process is 140 rev / min, the force is 170Nm, the spray frequency is 30s / time, and the polishing time is 2min, the rotation speed of the 1μm polishing process is 170 rev / min, the force is 100N / m, the spray frequency is 30s / time, and the polishing time is 1min.

[0111] As can be seen from FIG9 , when the polishing is poor, the structure is not clear, and the 3D image shows that the ferrite area is rough and the contour line is also very rough. Compared with Example 1, the effect is very poor.

[0112] Example 6

[0113] The phase content determination method of Example 1 is used, except that the type of carbon structural steel is different, and the carbon structural steel is SWRCH22A steel.

[0114] Table 4 shows Fig.10bThe standard deviation of the original heights of 5 consecutive points in segments AB, CD and EF.

[0115] It can be seen from Table 4 that the method of Example 1 has good adaptability to different steel grades.

[0116] AB CD EF Minimum value (um) 0.007 0.001 0.011 Maximum value (um) 0.123 0.020 0.109 Average value(um) 0.034 0.004 0.048 Standard deviation(um) 0.025 0.002 0.022

[0117] Table 4.

Claims

1. A method for determining phase content of carbon structural steel, the method comprising: After the inspection surface of the steel sample is ground and corroded, the phase content is measured using a laser confocal microscope, wherein the phase content measurement includes: (1) using a laser confocal microscope to obtain a three-dimensional topographic image of the surface area of ​​the sample; (2) leveling the three-dimensional topography image, wherein the leveling plane serves as a height reference plane of the three-dimensional topography image; (3) intercepting the three-dimensional topography image in a direction parallel to the X-axis or the Y-axis to obtain a finite number of cross sections and cross-sectional profile curves; (4) dividing the cross section where the cross section profile curve is located into a ferrite phase and a pearlite phase according to whether the standard deviation of the heights of a preset number of consecutive points of the cross section profile curve is less than or equal to a preset value, and the area less than or equal to the preset value is the ferrite phase; (5) The ferrite phase and the pearlite phase of each cross section are added up respectively to obtain the phase content of the area to be measured.

2. The measuring method according to claim 1, characterized in that The resolution of the three-dimensional morphology is above 0.125 μm, the spacing between the finite number of cross sections is below 0.125 μm, and the horizontal coordinates or vertical coordinates of adjacent points in the cross-sectional contour curve are spaced below 0.125 μm.

3. The measuring method according to claim 2, characterized in that The preset number is greater than 5.

4. The measuring method according to claim 3, characterized in that The preset value is 0.025-0.035 μm.

5. The measuring method according to claim 1, characterized in that Select three points on the same circle in the ferrite area and use the three-point leveling method to level the three-dimensional topography; After obtaining the cross-sectional contour curve, the basis for dividing the cross-sectional area where the cross-sectional contour curve is located into ferrite phase and pearlite phase also includes calculating the average height of each point on the cross-sectional contour curve, and the calculated height of each point is obtained by subtracting the average height from the original height of each point on the cross-sectional contour curve. The area where the calculated height of a preset number of points is less than 0 is ferrite.

6. The measuring method according to claim 1, characterized in that The corrosion liquid is 4% nitric acid alcohol, and the corrosion time is 3-6s.

7. The measuring method according to claim 1, characterized in that The grinding includes a coarse grinding process, a fine grinding process, a 3 μm polishing process and a 1 μm polishing process.

8. The measuring method according to claim 7, characterized in that The time of the coarse grinding process is 50 to 70 seconds, the force is 90 to 110 Nm, and the rotation speed is 90 to 100 rpm. The time of the fine grinding process is 11 to 13 minutes, the force is 145 to 155 Nm, and the rotation speed is 300 to 320 rpm.

9. The measuring method according to claim 7, characterized in that The rotation speed of the 3μm polishing process is 140-160 rpm, the force is 145-155Nm, the spray frequency is 25-30s / time, and the polishing time is 3-4min. The rotation speed of the 1μm polishing process is 140-160 rpm, the force is 85-95N / m, the spray frequency is 25-30s / time, and the polishing time is 2-3min.

Citation Information

Patent Citations