Chloroprene copolymer latex and method for producing the same

By adjusting the ratio and polymerization conditions of 2-methyl-1,3-butadiene monomer in the chloroprene copolymer latex, the problem of high temperature and length of neoprene rubber vulcanization is solved, and preparation is achieved under mild conditions chloroprene copolymer rubber with good flexibility and heat resistance is suitable for medical gloves and other applications.

CN113906064BActive Publication Date: 2024-11-05RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080039256.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-25
Filing Date
2020-10-23
Publication Date
2024-11-05
Estimated Expiration
2040-10-23

AI Technical Summary

Technical Problem

The existing neoprene rubber needs to be processed at high temperature for a long time during vulcanization, resulting in low production efficiency and insufficient softness and heat resistance of the molded product, and great changes over time, affecting its application.

Method used

By adjusting the proportion of 2-methyl-1,3-butadiene monomer units and the content of tetrahydrofuran insoluble in chloroprene copolymer latex, combined with appropriate polymerization conversion and emulsifier use, the temperature is achieved The chloroprene copolymer rubber with excellent flexibility and time-stability was prepared by vulcanizing treatment under conditions.

Benefits of technology

The chloroprene copolymer rubber that has vulcanized under mild conditions has excellent softness and heat resistance, and is suitable for impregnated products such as disposable gloves for medical purposes, improving production efficiency and stability of molded products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003376495360000181
    Figure BDA0003376495360000181
Patent Text Reader

Abstract

One embodiment of the present invention relates to a chloroprene copolymer latex, a method for producing a chloroprene copolymer latex, a chloroprene copolymer latex composition, and a chloroprene copolymer rubber molded product or a dipped product. The chloroprene copolymer latex contains monomer units derived from 2-chloro-1,3-butadiene (chloroprene) and monomer units derived from 2-methyl-1,3-butadiene, wherein the content of components insoluble in tetrahydrofuran in the chloroprene copolymer is 20% by mass or less, and the proportion of monomer units derived from 2-methyl-1,3-butadiene in the chloroprene copolymer is 10 to 27 mol%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a latex containing a copolymer of 2-chloro-1,3-butadiene (chloroprene) and 2-methyl-1,3-butadiene as a main component, a method for producing the same, and a molded product, particularly a dipped product, using the latex. Background Art

[0002] Isoprene rubber (IR) and chloroprene rubber (CR) are synthetic rubbers with the same softness as natural rubber. Therefore, in recent years, as a measure to deal with allergies, isoprene rubber or chloroprene rubber is used to replace natural rubber in the raw materials of dip molding composition products (dip products), especially surgical gloves. Isoprene rubber has the characteristics of high softness and excellent touch of medical staff, but the price is high, so it cannot fully meet the needs of the market. On the other hand, chloroprene rubber is cheaper than isoprene rubber, but its softness is lower than that of isoprene rubber, so there is a problem of poor touch, and in order to obtain the target strength, it is necessary to vulcanize for a long time at high temperature, so there is a problem of low production efficiency.

[0003] In addition, the above synthetic rubbers have problems in that their physical properties change significantly with the passage of time after molding, that is, they soften and deteriorate with the passage of time in isoprene rubber and they cure and deteriorate with the passage of time in chloroprene rubber.

[0004] For example, regarding chloroprene rubber, a technology for improving flexibility is disclosed in Patent Documents 1 and 2, but a high temperature and long-time vulcanization process is required. In addition, a technology related to reducing the temperature and processing time in the vulcanization process is disclosed in Patent Document 3, but there is a problem in flexibility.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2007-106994

[0008] Patent Document 2: Japanese Patent Application Publication No. 2019-143002

[0009] Patent Document 3: Japanese Patent Application Publication No. 2019-044116 Summary of the invention

[0010] Problems to be solved by the invention

[0011] The present invention aims to solve the above-mentioned problems of the prior art and to provide a chloroprene copolymer latex at low cost, which can be vulcanized under milder conditions than before and can obtain a molded product having excellent flexibility.

[0012] Means used to solve problems

[0013] The present inventors have conducted intensive studies to solve the above-mentioned problems and, as a result, have found that, in a latex of a chloroprene copolymer containing monomer units derived from chloroprene and monomer units derived from 2-methyl-1,3-butadiene, the above-mentioned problems can be solved by setting the ratio of monomer units derived from 2-methyl-1,3-butadiene contained in the chloroprene copolymer to a specific range and by setting the content of tetrahydrofuran-insoluble components in the chloroprene copolymer to a predetermined value or less, thereby completing the present invention.

[0014] That is, the present invention relates to the following [1] to

[12] , a chloroprene copolymer latex, a method for producing the same, a latex composition thereof, a rubber composition obtained by curing the composition, and a dipped product.

[0015] [1] A chloroprene copolymer latex, the chloroprene copolymer containing monomer units derived from 2-chloro-1,3-butadiene (chloroprene) and monomer units derived from 2-methyl-1,3-butadiene, characterized in that the content of components insoluble in tetrahydrofuran in the chloroprene copolymer is 20% by mass or less, and the proportion of monomer units derived from 2-methyl-1,3-butadiene in the chloroprene copolymer is 10 to 27 mol%.

[0016] [2] The chloroprene copolymer latex according to [1], wherein the weight average molecular weight of the tetrahydrofuran-soluble component in the chloroprene copolymer is 400,000 or more.

[0017] [3] The chloroprene copolymer latex according to [1] or [2], wherein the chloroprene copolymer further contains 0.01 to 10 mol % of a third monomer unit.

[0018] [4] The chloroprene copolymer latex according to [3], wherein the third monomer unit is a monomer unit derived from 2,3-dichloro-1,3-butadiene.

[0019] [5] A method for producing a chloroprene copolymer latex, comprising the step of emulsifying and copolymerizing a monomer component containing 2-chloro-1,3-butadiene (chloroprene) and 2-methyl-1,3-butadiene, wherein the proportion of 2-methyl-1,3-butadiene in the total monomer component is 2 to 40 mol %, and the polymerization conversion rate of the total monomer is 61 to 90 mass %.

[0020] [6] The method for producing a chloroprene copolymer latex according to [5], wherein an alkyl mercaptan is used as a chain transfer agent.

[0021] [7] The method for producing a chloroprene copolymer latex according to [5] or [6], wherein a potassium salt of rosin acid is used as an emulsifier.

[0022] [8] A chloroprene copolymer latex composition, characterized in that it contains:

[0023] 100 parts by mass of the solid content of the chloroprene copolymer latex according to any one of [1] to [4],

[0024] Metal oxide (B) 0.1 to 20.0 parts by mass,

[0025] Vulcanization accelerator (C) 0.1 to 10.0 parts by mass,

[0026] Sulfur (D) 0.1 to 10.0 parts by mass, and

[0027] Antioxidant (E) 0.1 to 10.0 parts by mass

[0028] [9] A chloroprene copolymer rubber molded product obtained by curing the chloroprene copolymer latex composition described in [8].

[0029]

[10] A dipped product obtained by molding the chloroprene copolymer latex composition described in [8] by a dipping method and curing the resulting product.

[0030]

[11] The dipped product according to

[10] , which is a glove.

[0031]

[12] The dipped product according to

[11] , which is a disposable medical glove.

[0032] Effects of the Invention

[0033] The chloroprene copolymer latex composition of the present invention is vulcanized under mild conditions to obtain a molded product (chloroprene copolymer rubber molded product) having excellent flexibility. In addition, the molded product of the present invention has temporal stability (resistance to thermal degradation) and can be suitably used for dipped products, particularly disposable gloves for medical use. DETAILED DESCRIPTION

[0034] The embodiments of the present invention are described in detail below, but the present invention is not limited to the structures of the embodiments described below. In addition, in the description of this specification including the claims, "to" that specifies a numerical range means above the lower limit value and below the upper limit value.

[0035] The chloroprene copolymer latex (A) of the present embodiment is a latex in which microparticles of the chloroprene copolymer are dispersed in a solvent such as water. The chloroprene copolymer contained in the chloroprene copolymer latex (A) contains at least a structure derived from 2-chloro-1,3-butadiene (chloroprene) (A-1) and a structure (monomer unit) derived from 2-methyl-1,3-butadiene (A-2). The monomer units constituting the chloroprene copolymer may also be only 2-chloro-1,3-butadiene (A-1) and 2-methyl-1,3-butadiene (A-2).

[0036] Specifically, when all monomer units constituting the chloroprene copolymer are taken as 100 mol %, the proportion of 2-methyl-1,3-butadiene (A-2) is 10 to 27 mol %, preferably 10 to 25 mol %, and more preferably 11 to 15 mol %.

[0037] When the proportion of 2-methyl-1,3-butadiene (A-2) monomer units in the chloroprene copolymer is less than 10 mol%, the tensile strength of the molded product obtained by vulcanization at 100°C becomes low. When the proportion of 2-methyl-1,3-butadiene (A-2) monomer units in the copolymer exceeds 27 mol%, the strength of the molded product also becomes low. That is, if the proportion of 2-methyl-1,3-butadiene (A-2) monomer units is 10 to 27 mol%, when the chloroprene copolymer is vulcanized at 100°C, the molded product after vulcanization can show good strength.

[0038] The above-mentioned chloroprene copolymer may contain a monomer unit derived from a monomer (A-3) in addition to a structure (monomer unit) derived from 2-chloro-1,3-butadiene (A-1) and a monomer unit derived from 2-methyl-1,3-butadiene (A-2) within a range not affecting the purpose of the present invention. Here, the monomer (A-3) is a monomer other than 2-chloro-1,3-butadiene (A-1) and 2-methyl-1,3-butadiene (A-2), and is a monomer that can be copolymerized with at least one of 2-chloro-1,3-butadiene (A-1) and 2-methyl-1,3-butadiene (A-2). The monomer (A-3) may also be a monomer that can be copolymerized with both 2-chloro-1,3-butadiene (A-1) and 2-methyl-1,3-butadiene (A-2). Examples of the monomer (A-3) include butadiene, 2,3-dichloro-1,3-butadiene, styrene, acrylonitrile, acrylic acid and its esters, methacrylic acid and its esters, and the like. The chloroprene copolymer may contain structures derived from two or more monomers as the structure derived from the monomer (A-3) as required. When the chloroprene copolymer contains a structure derived from the monomer (A-3) unit, the proportion (upper limit) of the monomer (A-3) in all the monomer components constituting the chloroprene polymer is preferably 10.0 mol% or less, more preferably 8.0 mol% or less, and further preferably 5.0 mol% or less. In addition, when the chloroprene copolymer contains a structure derived from the monomer (A-3) unit, the proportion (lower limit) of the monomer (A-3) in all the monomer components constituting the chloroprene polymer is preferably 0.01 mol% or more, more preferably 0.5 mol% or more, and further preferably 1.0 mol% or more. When the ratio of the structure derived from the monomer (A-3) is 10.0 mol % or less, the tensile strength and elongation of the molded product are good, and the stability over time of the flexibility of the molded product is good.

[0039] In the chloroprene copolymer of the present embodiment, the amount of components insoluble in tetrahydrofuran (THF) at 25° C. is 20% by mass or less, preferably 10% by mass or less, and more preferably 5% by mass or less. The components insoluble in tetrahydrofuran are components in which the polymer chains in the chloroprene copolymer particles are gelled by three-dimensional crosslinking. The amount of the components insoluble in tetrahydrofuran can be measured by the method used in the examples described below.

[0040] When the amount of the components insoluble in tetrahydrofuran at 25° C. in the chloroprene copolymer is 20% by mass or less, the softness and tensile strength of the molded product are good. The amount of the components insoluble in tetrahydrofuran in the chloroprene copolymer of the present invention is preferably 0% by mass or more, more preferably 0.1% by mass or more, and further preferably 1.5% by mass or more. The amount of the components insoluble in tetrahydrofuran in the chloroprene copolymer can be controlled by adjusting the polymerization conversion rate and the amount of the chain transfer agent when the chloroprene copolymer is produced.

[0041] For example, when the polymerization conversion rate is increased, the amount of the components insoluble in tetrahydrofuran in the chloroprene copolymer tends to become larger. In addition, the polymerization conversion rate is controlled according to the polymerization time and polymerization temperature of the chloroprene copolymer. The longer the polymerization time, the greater the polymerization conversion rate tends to be. In addition, the higher the polymerization temperature, the greater the polymerization conversion rate tends to be. On the other hand, when the amount of the chain transfer agent is increased, the amount of the components insoluble in tetrahydrofuran in the chloroprene copolymer tends to decrease.

[0042] The weight average molecular weight of the component soluble in tetrahydrofuran at 25°C in the above-mentioned chloroprene copolymer, measured according to the method or conditions adopted in the examples described later, is preferably 400,000 or more, more preferably 500,000 or more, and further preferably 550,000 or more. If the weight average molecular weight of the component soluble in tetrahydrofuran at 25°C in the chloroprene copolymer is 400,000 or more, a molded product with good mechanical properties can be obtained. The weight average molecular weight of the component soluble in tetrahydrofuran at 25°C in the chloroprene copolymer is preferably 3 million or less, more preferably 2 million or less, and further preferably 900,000 or less. If the weight average molecular weight of the component soluble in tetrahydrofuran at 25°C in the chloroprene copolymer is 3 million or less, a molded product with good softness and tensile strength can be obtained.

[0043] [Method for producing chloroprene copolymer latex (A)]

[0044] As a method for producing the chloroprene copolymer latex (A), a method of radically polymerizing monomers in an aqueous emulsion is simple and the most industrially advantageous method.

[0045] By using an emulsifier to emulsify and polymerize 2-chloro-1,3-butadiene (A-1) and 2-methyl-1,3-butadiene (A-2), or 2-chloro-1,3-butadiene (A-1), 2-methyl-1,3-butadiene (A-2), and a monomer (A-3), a copolymer latex (A) in which particles of a chloroprene copolymer are dispersed in water is obtained. The polymerization temperature during the emulsion polymerization is preferably 20 to 35° C., and the polymerization time is preferably 5 to 8 hours. When the polymerization temperature and polymerization time during the emulsion polymerization are within the above range, the desired polymerization conversion rate is achieved, so it is preferred.

[0046] The 2-methyl-1,3-butadiene content in the chloroprene copolymer of the present invention can be adjusted by the charging ratio of 2-chloro-1,3-butadiene (A-1) and 2-methyl-1,3-butadiene (A-2) during polymerization, the polymerization conversion rate, and the like.

[0047] The higher the proportion of 2-methyl-1,3-butadiene (A-2) in all monomers when charged in the polymerization, the higher the content of monomer units derived from 2-methyl-1,3-butadiene (A-2) in the chloroprene copolymer can be. However, 2-methyl-1,3-butadiene (A-2) has lower reactivity at the start of emulsion polymerization than 2-chloro-1,3-butadiene (A-1). Therefore, when the proportion of 2-methyl-1,3-butadiene (A-2) charged is high, the polymerization progresses slowly and the reaction time tends to be longer.

[0048] 2-methyl-1,3-butadiene (A-2) becomes easily copolymerized into the polymer as the polymerization of the chloroprene copolymer proceeds. Therefore, by increasing the polymerization conversion rate during the polymerization of the chloroprene copolymer, the content of the monomer units derived from 2-methyl-1,3-butadiene in the chloroprene copolymer can be increased. On the other hand, when the polymerization conversion rate is low, the amount of residual monomers increases, and it takes time to remove the residual monomers, and the mechanical properties of the molded product are reduced.

[0049] As described above, in order to effectively obtain the chloroprene copolymer of the present invention, it is preferred that the 2-methyl-1,3-butadiene (A-2) in all the monomer components used is set to 2 to 40 mol%, more preferably 10 to 30 mol%, and more preferably 15 to 25 mol%. In addition, the polymerization conversion rate of all monomers is preferably set to 61 to 90 mass%, more preferably 75 to 87 mass%, and more preferably 75 to 86 mass%. If the polymerization conversion rate of all monomers is 90 mass% or less, the quality of the chloroprene copolymer obtained by polymerization is good, and the physical properties of the molded product obtained from the chloroprene copolymer latex (A) are also good.

[0050] As an emulsifier for emulsion polymerization, an anionic surfactant is preferred. Examples of anionic surfactants include rosin acid soap, sodium salt of naphthalenesulfonic acid condensate, sodium salt of dodecylbenzenesulfonic acid, sodium salt of dodecylsulfuric acid, etc. From the perspective of convenience of coagulation operation, ordinary rosin acid soap can be used. In particular, from the perspective of coloring stability, sodium salt and / or potassium salt of disproportionated rosin acid can be used, and from the perspective of polymerization rate, potassium salt of disproportionated rosin acid is more preferred.

[0051] When the total amount of all monomers of 2-chloro-1,3-butadiene (A-1), 2-methyl-1,3-butadiene (A-2), and monomer (A-3) is set to 100 parts by mass, the amount of the emulsifier used is preferably 0.5 to 20.0 parts by mass, more preferably 1.0 to 10.0 parts by mass, and further preferably 1.5 to 5.0 parts by mass. If the amount of the emulsifier used is 0.5 parts by mass or more, poor emulsification is less likely to occur, and the heat generated by polymerization can be controlled. In addition, if the amount of the emulsifier used is 0.5 parts by mass or more, problems such as the formation of agglomerates and poor product appearance will not occur. On the other hand, if the amount of the emulsifier used is 20.0 parts by mass or less, emulsifiers such as rosin acid will not remain in the chloroprene copolymer, and therefore, adhesion is less likely to occur in the chloroprene copolymer. Therefore, when the amount of the emulsifier used is 20.0 parts by mass or less, there will be no problems with processability and handling due to adhesion of the chloroprene copolymer latex composition to a mold (form) during molding or adhesion of the molded product during use, and there will be no deterioration in the color tone of the molded product.

[0052] As the polymerization initiator, a common free radical polymerization initiator can be used. In the case of emulsion polymerization, for example, an organic or inorganic peroxide such as benzoyl peroxide, potassium persulfate, ammonium persulfate, cumene hydroperoxide, tert-butyl hydroperoxide, or an azo compound such as azobisisobutyronitrile can be used. The polymerization initiator can be used alone or in combination of two or more.

[0053] In the polymerization of the chloroprene copolymer of the present embodiment, in order to adjust the amount of the component insoluble in tetrahydrofuran, a chain transfer agent is preferably used. When the total amount of all monomers of 2-chloro-1,3-butadiene (A-1), 2-methyl-1,3-butadiene (A-2), and monomer (A-3) is 100 parts by mass, the amount of the chain transfer agent used is preferably 0.01 to 15.0 parts by mass, more preferably 0.05 to 10.0 parts by mass, and even more preferably 0.1 to 1.0 parts by mass.

[0054] The chain transfer agent is not particularly limited, and known chain transfer agents such as alkyl mercaptans such as n-dodecyl mercaptan, n-decyl mercaptan, octyl mercaptan, or tert-dodecyl mercaptan, dialkyl xanthate disulfides such as diisopropyl xanthate disulfide or diethyl xanthate, and iodoform can be used. Alkyl mercaptans are more preferred, and n-dodecyl mercaptan is even more preferred.

[0055] When the polymerization conversion rate is 61 to 90% by mass and the chain transfer agent is 0.01 to 15.0 parts by mass, the amount of the tetrahydrofuran-insoluble component in the chloroprene copolymer can be adjusted to a desired range (20% by mass or less).

[0056] In the polymerization of the chloroprene copolymer, a co-catalyst may be used together with the polymerization initiator as desired. The co-catalyst that can be used together with the polymerization initiator is not particularly limited, and a common co-catalyst can be used. For example, anthraquinone sulfonate, potassium sulfite, sodium disulfite, sodium sulfite, tetraethylene pentamine, and N,N-dimethyl-p-toluidine can be mentioned. The co-catalyst may be used alone or in combination of two or more.

[0057] Generally speaking, in emulsion polymerization, in order to obtain a polymer with a desired molecular weight and molecular weight distribution, a polymerization terminator is added at the moment of reaching a specified polymerization conversion to stop the polymerization reaction. In an embodiment of the present invention, a polymerization terminator may also be used. The type of the polymerization terminator is not particularly limited, and commonly used polymerization terminators, such as phenothiazine, p-tert-butylcatechol, hydroquinone, hydroquinone monomethyl ether, diethylhydroxylamine, etc. may be used. One polymerization terminator may be used alone, or two or more may be used in combination.

[0058] Furthermore, a stabilizer such as an acid acceptor and / or an antioxidant may be blended into the chloroprene copolymer latex (A) within a range not impairing the purpose of the present invention.

[0059] [Chloroprene copolymer latex composition]

[0060] The chloroprene copolymer latex composition of one embodiment of the present invention comprises the solid content of the chloroprene copolymer latex (A) obtained by the above-mentioned polymerization method, the metal oxide (B), the vulcanization accelerator (C), the sulfur (D) and the antioxidant (E). Here, the solid content of the chloroprene copolymer latex (A) is a component obtained by drying the chloroprene copolymer latex (A) by standing it in an oven at 141° C. for 30 minutes, that is, a component obtained by removing a solvent such as water as a dispersion medium from the chloroprene copolymer latex (A). In addition, the chloroprene copolymer latex composition may also contain a solvent such as water in the chloroprene copolymer latex (A).

[0061] When the solid content in the chloroprene copolymer latex (A) is 100 parts by mass, the chloroprene copolymer latex composition may further contain 0.1 to 20.0 parts by mass of a metal oxide (B), 0.1 to 10.0 parts by mass of a vulcanization accelerator (C), 0.1 to 10.0 parts by mass of sulfur (D), and 0.1 to 10.0 parts by mass of an antioxidant (E). By vulcanizing the chloroprene copolymer latex composition prepared with this composition, a rubber molded product (e.g., a film) having improved flexibility and stability over time is obtained. Among the raw materials used for preparation, the water-insoluble component and the component that destabilizes the colloidal state of the chloroprene copolymer latex are added to the chloroprene copolymer latex after preparing an aqueous dispersion in advance.

[0062] The type of the metal oxide (B) is not particularly limited, and for example, zinc oxide, lead oxide, and lead tetraoxide can be used, and zinc oxide is particularly preferred. The metal oxide (B) may be used alone or in combination of two or more.

[0063] When the amount of solid content in the chloroprene copolymer latex (A) is set to 100 parts by mass, the amount of the metal oxide (B) contained in the chloroprene copolymer latex composition of the present embodiment is usually 0.1 to 20.0 parts by mass, preferably 0.5 to 15.0 parts by mass, and more preferably 1.0 to 10.0 parts by mass. If the amount of the metal oxide (B) is 0.1 parts by mass or more, an appropriate vulcanization rate is obtained. When the amount of the metal oxide (B) is 20.0 parts by mass or less, a cross-linked structure is well obtained by vulcanization treatment, and scorching is not easy to occur. In addition, the colloidal state of the chloroprene copolymer latex composition is stabilized, so it is not easy to cause problems such as precipitation.

[0064] The type of the vulcanization accelerator (C) is not particularly limited, and a vulcanization accelerator generally used in the vulcanization treatment of isoprene-based polymer latex or chloroprene-based polymer latex can be used. For example, thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, and thiazole-based vulcanization accelerators can be mentioned.

[0065] As thiuram-based vulcanization accelerators, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, etc. can be mentioned. As dithiocarbamate-based vulcanization accelerators, sodium dibutylthiodicarbamate, zinc dibutylthiodicarbamate, zinc diethylthiodicarbamate, etc. can be mentioned. As thiourea-based vulcanization accelerators, ethylenethiourea, diethylthiourea, trimethylthiourea, N,N'-diphenylthiourea (DPTU), etc. can be mentioned. As guanidine-based vulcanization accelerators, diphenylguanidine (DPG), di-o-tolylguanidine, etc. can be mentioned. As thiazole-based vulcanization accelerators, 2-mercaptobenzothiazole, di-2-benzothiazole disulfide, 2-mercaptobenzothiazole zinc, etc. can be mentioned. The vulcanization accelerator (C) can be used alone or in combination of two or more.

[0066] When the amount of solid content in the chloroprene copolymer latex (A) is set to 100 parts by mass, the amount of the vulcanization accelerator (C) contained in the chloroprene copolymer latex composition of the present embodiment is usually 0.1 to 10.0 parts by mass, preferably 0.3 to 5.0 parts by mass, and more preferably 0.5 to 2.5 parts by mass. If the amount of the vulcanization accelerator (C) is within this range, an appropriate vulcanization rate is obtained, and it is not easy to produce a deficiency of the cross-linked structure caused by insufficient vulcanization treatment, and it is not easy to produce scorch. In addition, the vulcanization density of the molded product obtained from the chloroprene copolymer latex composition of the present embodiment is also appropriate. Therefore, by setting the amount of the vulcanization accelerator (C) within the above range, the softness of the molded product is within an appropriate range.

[0067] The type of sulfur (D) is not particularly limited. In addition to powdered sulfur, precipitated sulfur, colloidal sulfur, surface-treated sulfur, and insoluble sulfur, sulfur-containing compounds such as polysulfides and polymer polysulfides (except the above-mentioned vulcanization accelerators) can also be used. Sulfur (D) can be used alone or in combination of two or more. When the amount of solid components in the chloroprene copolymer latex (A) is set to 100 parts by mass, the amount of sulfur (D) contained in the chloroprene copolymer latex composition of the present embodiment is usually 0.1 to 10.0 parts by mass, preferably 0.2 to 7.0 parts by mass, and more preferably 0.45 to 2.0 parts by mass. If the amount of sulfur (D) is within this range, an appropriate vulcanization speed is obtained, and it is not easy to produce insufficient cross-linked structure caused by insufficient vulcanization treatment, and it is not easy to produce scorch. In addition, the colloidal state of the chloroprene copolymer latex composition is stabilized, so it is not easy to produce problems such as precipitation.

[0068] The type of antioxidant (E) is not particularly limited. When the molded product is desired to have high heat resistance, it is preferred to use an antioxidant that prevents thermal deterioration and an antioxidant that prevents ozone deterioration in combination.

[0069] Examples of antioxidants for preventing thermal aging include diphenylamine-based antioxidants such as octylated diphenylamine, p-(p-toluene-sulfonamide) diphenylamine, and 4,4'-bis(α,α-dimethylbenzyl) diphenylamine. When such antioxidants are added, the molded article tends to have heat resistance and further has stain resistance (discoloration suppression, etc.).

[0070] Examples of antioxidants for preventing deterioration caused by ozone include N,N′-diphenyl-p-phenylenediamine (DPPD) and N-isopropyl-N′-phenyl-p-phenylenediamine (IPPD).

[0071] When the chloroprene copolymer rubber molded product of the present embodiment is used as a disposable medical glove, emphasis is placed on appearance (particularly color tone) and sanitation, and therefore, a hindered phenol antioxidant is preferably used as the antioxidant (E). Examples of the hindered phenol antioxidant include 2,2'-methylenebis-(4-ethyl-6-tert-butylphenol) and 4,4'-methylenebis-(2,6-di-tert-butylphenol).

[0072] The amount of the antioxidant (E) contained in the chloroprene copolymer latex composition of the present embodiment is usually 0.1 to 10.0 parts by mass, preferably 0.5 to 5.5 parts by mass, and more preferably 2.0 to 4.8 parts by mass, based on 100 parts by mass of the solid content in the chloroprene copolymer latex (A). When the amount of the antioxidant (E) is within this range, a sufficient antioxidant effect is obtained, and the vulcanization treatment is not inhibited, and the deterioration of the color tone is not likely to occur.

[0073] Furthermore, the chloroprene copolymer latex composition of the present embodiment may further contain other additives as desired in addition to the chloroprene copolymer latex (A), the metal oxide (B), the vulcanization accelerator (C), the sulfur (D), and the antioxidant (E) as long as the purpose of the present invention is not impaired. Examples of the additives that may be contained include a pH adjuster, a filler, a pigment, a colorant, a defoamer, a thickener, and the like.

[0074] [Chloroprene copolymer rubber molded product]

[0075] The chloroprene copolymer latex composition of the present embodiment is molded and cured to obtain a molded product. For example, the chloroprene copolymer latex composition of the embodiment is molded by a dipping method to obtain a dipped product.

[0076] Before the dipping process, the chloroprene copolymer latex composition of the present embodiment may be aged under predetermined conditions. The temperature conditions for the aging are 15 to 40° C., and the aging time is 15 to 72 hours. For example, the aging condition of 20° C. for 24 hours may be adopted. The starting point of the aging is the time when the chloroprene copolymer latex (A) and the metal oxide (B), the vulcanization accelerator (C), the sulfur (D), and the antioxidant (E) are all mixed.

[0077] By sequentially carrying out the steps of aging, immersion and coagulation, drying, and vulcanization (curing), a film-shaped molded product is obtained.

[0078] The immersion and coagulation treatment can be carried out by immersing a plate or mold coated with a coagulant in the chloroprene copolymer latex composition for a predetermined period of time, so that the solid components in the chloroprene copolymer latex composition such as the chloroprene copolymer are deposited on the surface of the plate or mold. As the coagulant, a metal salt can be used, for example, a nitrate can be used.

[0079] In order to avoid problems with the appearance of the molded product, such as the formation of bubbles and pinholes, a drying step (rough drying step) may be performed at a relatively low temperature of 70° C. to 100° C. before the vulcanization step.

[0080] The vulcanization temperature in the vulcanization step can be set to 100° C. in air, for example. The vulcanization time at the vulcanization temperature can be set to 20 minutes to 60 minutes, for example. However, it is preferred that the vulcanization treatment be performed sufficiently within a range in which the tensile strength and tensile elongation of the molded product are not deteriorated.

[0081] By vulcanizing the composition deposited on the surface of the plate or the mold under the above conditions, a chloroprene copolymer rubber molded product can be obtained. The chloroprene copolymer rubber molded product preferably has a 100% elastic modulus of 0.6MPa or more and 0.65MPa or less, a 500% elastic modulus of 0.5MPa or more and 1.6MPa or less, a tensile strength of 17MPa or more and 35MPa or less, and a tensile elongation of 800% or more and 1500% or less. The 100% elastic modulus is used as an index of flexibility, indicating that the smaller the value of the 100% elastic modulus, the higher the flexibility. The chloroprene copolymer latex rubber molded product of this embodiment has excellent flexibility. In addition, the physical property changes before and after the thermal degradation treatment are small, and the changes over time are excellent.

[0082] [Disposable gloves for medical use]

[0083] The chloroprene copolymer rubber molded product can be particularly suitably used as disposable gloves for medical use.

[0084] If the 100% elastic modulus of the chloroprene copolymer rubber molded product is 0.65 MPa or less, flexibility can be obtained in the disposable medical gloves, which is preferred. The lower limit of the 100% elastic modulus of the chloroprene copolymer rubber molded product may be, for example, 0.6 MPa or more.

[0085] When the 500% elastic modulus of the chloroprene copolymer rubber molded product is 0.5 MPa or more, the disposable medical gloves feel soft and are less prone to fatigue even when used for a long time. When the 500% elastic modulus of the chloroprene copolymer rubber molded product is 1.6 MPa or less, the force required to return the fingers when bending the disposable medical gloves is appropriate, which is preferred.

[0086] If the tensile strength of the chloroprene copolymer rubber molded product is 17 MPa or more, it is preferred because the medical disposable gloves are less likely to break. The upper limit of the tensile strength of the chloroprene copolymer rubber molded product may be, for example, 35 MPa or less.

[0087] If the tensile elongation of the chloroprene copolymer rubber molded product is 800% or more, the disposable medical gloves are less likely to break, which is preferred. The upper limit of the tensile elongation of the chloroprene copolymer rubber molded product may be, for example, 1500% or less.

[0088] Example

[0089] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples.

[0090] Embodiment 1:

[0091] (1) Preparation of chloroprene copolymer latex (A)

[0092] Into a reactor having an internal capacity of 5 L, 1200 g of 2-chloro-1,3-butadiene (A-1), 300 g of 2-methyl-1,3-butadiene (A-2), 1290 g of purified water, 65 g of disproportionated rosin acid (R-600 manufactured by Arakawa Chemical Industries, Ltd.), 17.1 g of potassium hydroxide, 3.9 g of sodium hydroxide, 3.3 g of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate, and 1.65 g of n-dodecyl mercaptan were added. The starting materials added to the reactor were emulsified to convert the rosin acid into rosin acid soap.

[0093] It should be noted that 2-chloro-1,3-butadiene (A-1) and 2-methyl-1,3-butadiene (A-2) were blended as raw material monomers, and purified water was blended as a dispersion medium for emulsion polymerization. In addition, rosin acid, potassium hydroxide, and sodium hydroxide were blended as raw materials for emulsifiers, and sodium salt of β-naphthalenesulfonic acid formaldehyde condensate was blended as an emulsifier.

[0094] To the emulsion obtained by emulsifying the starting materials, 4 g of potassium persulfate as a polymerization initiator was added, and emulsion polymerization was carried out at 30° C. in a nitrogen atmosphere. When the polymerization conversion rate of all monomers reached 84% by mass, the polymerization was terminated. Subsequently, unreacted 2-chloro-1,3-butadiene (A-1) and 2-methyl-1,3-butadiene (A-2) were removed by steam distillation to obtain a chloroprene copolymer latex (A).

[0095] The polymerization conversion rate is calculated as follows. That is, the emulsion after the start of polymerization is collected and allowed to stand in an oven at 141°C for 30 minutes to dry it to obtain a dried solid. The obtained dried solid contains a polymer and solid components other than the polymer. Therefore, the components that do not volatilize from the various components used in the emulsion polymerization at 141°C are calculated based on the amount of polymerization raw materials input, and are set as the mass of the solid components other than the polymer. In addition, the value obtained by subtracting the mass of the solid components other than the polymer from the mass of the dried solid obtained by drying the emulsion after the start of polymerization is set as the "amount of chloroprene copolymer produced", and the polymerization conversion rate is calculated by formula (1). The calculated polymerization conversion rate is shown in Table 1.

[0096] Polymerization conversion rate [mass %] = [(production amount of chloroprene copolymer) / (total input mass of all monomers)] × 100 (1)

[0097] In addition, the "mass of all monomers charged" in the formula (1) is the amount of all monomers charged contained in the emulsion collected in order to obtain a dry solidified product.

[0098] In addition, various physical properties of the obtained chloroprene copolymer latex (A) were evaluated.

[0099] (i) Components insoluble in tetrahydrofuran in the chloroprene copolymer:

[0100] The content of the components insoluble in tetrahydrofuran in the chloroprene copolymer is determined as follows. That is, 1 g of the chloroprene copolymer latex (A) is added to 100 mL of tetrahydrofuran at 25°C and shaken for 10 hours using a shaker (SA300) manufactured by Yamato Science Co., Ltd. The mixture of the chloroprene copolymer latex (A) and tetrahydrofuran after the shaking treatment is centrifuged and separated using a centrifugal sedimentation separator (manufactured by Kokusan Co., Ltd., H-9R) to obtain a dissolved phase of the supernatant. The obtained dissolved phase is heated to 100°C, tetrahydrofuran is evaporated for 1 hour, and the mass of the dried solid is measured. Thus, the mass of the dissolved components in the chloroprene copolymer and dissolved in the dissolved phase is obtained.

[0101] By substituting the mass of the chloroprene copolymer in 1 g of the chloroprene copolymer latex (A) and the mass of the above-mentioned soluble component into formula (2), the content of the tetrahydrofuran-insoluble component in the chloroprene copolymer that is not dissolved in tetrahydrofuran at 25° C. is calculated. The measured content of the tetrahydrofuran-insoluble component is shown in Table 1.

[0102] Content of tetrahydrofuran-insoluble components (mass %)

[0103] ={1-[(mass of dissolved component) / (mass of chloroprene copolymer in 1 g of chloroprene copolymer latex (A))]}×100···(2)

[0104] In formula (2), the mass of the chloroprene copolymer in 1 g of the chloroprene copolymer latex (A) is regarded as the mass of the solid content obtained by drying and solidifying 1 g of the chloroprene copolymer latex (A). Here, when drying and solidifying the chloroprene copolymer latex (A), it is left to stand in an oven at 141° C. for 30 minutes.

[0105] (ii) Weight average molecular weight (Mw):

[0106] Hereinafter, an example of a method for obtaining the weight average molecular weight (Mw) of the tetrahydrofuran-soluble component in the chloroprene copolymer at 25° C. is described. The sample is prepared by preparing a dissolved phase of the supernatant after centrifugal precipitation and separation in the same manner as in the preparation of the sample for measuring the amount of the above-mentioned tetrahydrofuran-insoluble component, and diluting it with tetrahydrofuran. The obtained sample is subjected to polystyrene-equivalent molecular weight measurement by GPC (gel permeation chromatography) to measure the weight average molecular weight (Mw).

[0107] As for the measurement conditions of GPC, LC-20AD manufactured by Shimadzu Corporation was used as the GPC measurement apparatus, RID-10A (differential refractive index detector) manufactured by Shimadzu Corporation was used as the detector, the type of column was set to PLgel 10μm MiniMIX-B manufactured by Agilent Technologies, Inc., the eluent was tetrahydrofuran (Kanto Chemical, for HPLC), the column temperature was 40°C, and the elution rate was 0.4 ml / min.

[0108] (iii) Monomer unit content in chloroprene copolymer:

[0109] The content of the component derived from 2-methyl-1,3-butadiene (A-2) in the chloroprene copolymer is determined by 1 The obtained chloroprene copolymer latex was coagulated with methanol, dried, and then heavy chloroform was added to the obtained coagulated material. After filtering out the substances insoluble in heavy chloroform, the obtained solution was subjected to 1 H-NMR analysis. 1 In the H-NMR analysis, JNM-AL400 manufactured by JEOL Ltd. was used as a measuring apparatus, and tetramethylsilane was used as a standard for chemical shift.

[0110] according to 1The content of the component derived from 2-methyl-1,3-butadiene (A-2) was calculated by formula (3) from the peak areas of the peak derived from 2-chloro-1,3-butadiene (A-1) (5.4 ppm) and the peak derived from 2-methyl-1,3-butadiene (A-2) (5.1 ppm) in the H-NMR spectrum.

[0111] Content of components derived from 2-methyl-1,3-butadiene (A-2) (%)

[0112] =(peak area of ​​5.1 ppm) / (peak area of ​​5.1 ppm+peak area of ​​5.4 ppm)×100···(3)

[0113] In addition, even when the monomer (A-3) is contained, when the monomer (A-3) does not have a peak overlapping with the peak of 5.1 ppm and the peak of 5.4 ppm, in order to obtain the proportion of 2-methyl-1,3-butadiene (A-2) in the total of 2-chloro-1,3-butadiene (A-1) and 2-methyl-1,3-butadiene (A-2), formula (3) can also be used. When obtaining the proportion of monomer (A-3), the peak area of ​​the peak derived from the monomer (A-3) that does not overlap with any peak of 2-chloro-1,3-butadiene (A-1) and 2-methyl-1,3-butadiene (A-2) is used, and the proportion of monomer (A-3) in the total of 2-chloro-1,3-butadiene (A-1) and monomer (A-3) is calculated according to the same formula as formula (3). Similarly, the proportion of monomer (A-3) in all monomer components constituting the chloroprene polymer can also be obtained.

[0114] When the monomer (A-3) has a peak overlapping with the peak at 5.1 ppm and the peak at 5.4 ppm, the monomer (A-3) is used. 1 H- 1 The peaks derived from 2-chloro-1,3-butadiene (A-1), 2-methyl-1,3-butadiene (A-2), and monomer (A-3) were identified from the results of multidimensional NMR measurement such as HCOSY (COrrelation Spectroscopy), and the ratio of each substance was determined by performing the same calculation using the peak areas.

[0115] (2) Preparation of Chloroprene Copolymer Latex Composition

[0116] 100 parts by mass of the chloroprene copolymer latex (A) obtained in (1) above, 3.7 parts by mass of zinc oxide (AZ-SW manufactured by Osaki Kogyo Co., Ltd.), 1.0 parts by mass of zinc dibutylthiodicarbamate (Nocceler (registered trademark) BZ manufactured by Ouchi Shinko Chemical Co., Ltd.) as a vulcanization accelerator, 1.0 parts by mass of zinc 2-mercaptobenzothiazole (Nocceler (registered trademark) MZ manufactured by Ouchi Shinko Chemical Co., Ltd.), 0.5 parts by mass of diphenylguanidine (Nocceler (registered trademark) D manufactured by Ouchi Shinko Chemical Co., Ltd.), 0.45 parts by mass of sulfur (S-50 manufactured by Nippon Color Industries Co., Ltd.), and 2.0 parts by mass of a phenolic antioxidant (K-840 manufactured by Chukyo Yushi Co., Ltd.) were placed in a container equipped with a stirring device. The mixture was stirred for 20 minutes to uniformly mix, thereby obtaining a chloroprene copolymer latex composition. The chloroprene copolymer latex composition after the stirring was matured by being left to stand at 20° C. for 24 hours.

[0117] In addition, zinc oxide AZ-SW, sulfur S-50 and phenolic antioxidant K-840 are in the form of a dispersion in which zinc oxide (B), sulfur (D) and antioxidant (E) as active ingredients are dispersed in a liquid medium. Therefore, the amount of zinc oxide AZ-SW, sulfur S-50 and phenolic antioxidant K-840 added is the amount of only the active ingredients in the zinc oxide AZ-SW, sulfur S-50 and K-840 added.

[0118] (3) Film production

[0119] Using the chloroprene copolymer latex composition obtained in the above (2), a film of the chloroprene copolymer is formed by a dipping method.

[0120] A ceramic plate of 200 mm in length, 100 mm in width and 5 mm in thickness was prepared as a mold for the film of the chloroprene copolymer. The mold was dipped in a 30% by mass calcium nitrate aqueous solution, pulled up, and dried in an oven at 40° C. for 10 minutes, thereby allowing calcium nitrate as a coagulant to adhere to the surface of the mold.

[0121] Then, the dried mold was immersed in the chloroprene copolymer latex composition obtained in (2) above to deposit the solid content of the chloroprene copolymer latex composition on the surface of the mold. After the mold was pulled up from the chloroprene copolymer latex composition, it was dried in an oven at 70°C for 30 minutes.

[0122] Next, the mold with the solid components deposited on the surface was heated in an oven at 100° C. for 20 minutes to vulcanize the solid components of the chloroprene copolymer latex composition deposited on the mold surface, thereby solidifying it. After cooling in the atmosphere, the solidified molded product on the mold surface was cut into a desired shape and size, thereby obtaining a vulcanized film as a chloroprene copolymer rubber molded product.

[0123] The film was cut into a dumbbell-shaped specimen equivalent to No. 6 specified in JIS K6251-2017 to obtain a test piece. The thickness of the test piece was 0.15 to 0.25 mm. Then, the test piece was heated at 100°C for 22 hours in air, thereby performing a thermal degradation treatment. For each of the test pieces before and after the thermal degradation treatment, a tensile test was performed at 23°C by the method according to JIS K6251-2017 to measure the tensile strength, tensile elongation, and elastic modulus at 100% elongation (100% elastic modulus), and elastic modulus at 500% elongation (500% elastic modulus). The various physical properties of the film measured in the above manner are collectively shown in Table 1. In addition, in Table 1, the "weight average molecular weight (Mw)" in the column of latex properties is the weight average molecular weight of the tetrahydrofuran-soluble component in the chloroprene copolymer at 25°C.

[0124] Embodiment 2:

[0125] The copolymer latex composition, film, and test piece were prepared by the same method as in Example 1 except that the charged amounts of 2-chloro-1,3-butadiene and 2-methyl-1,3-butadiene were changed as shown in Table 1 and the polymerization conversion rate at the end of the reaction was 76% by mass to prepare a chloroprene copolymer latex (A), and various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0126] Embodiment 3:

[0127] A copolymer latex composition, a film, and a test piece were prepared by the same method as in Example 1 except that the polymerization conversion rate at the end of the reaction was 64 mass % to prepare the chloroprene copolymer latex (A), and various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0128] Embodiment 4:

[0129] The amount of 2-chloro-1,3-butadiene, 2-methyl-1,3-butadiene and 2,3-dichloro-1,3-butadiene charged was changed as shown in Table 1, and the polymerization conversion rate at the end of the reaction was set to 83% by mass to prepare a chloroprene copolymer latex (A). A copolymer latex composition, a film and a test piece were prepared by the same method as in Example 1, and various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0130] Comparative Example 1:

[0131] The copolymer latex composition, film, and test piece were prepared by the same method as in Example 1, and various evaluations were performed in the same manner as in Example 1, except that the charged amounts of 2-chloro-1,3-butadiene, 2-methyl-1,3-butadiene, and n-dodecyl mercaptan were changed as shown in Table 1, and the polymerization conversion rate at the end of the reaction was set to 90% by mass to prepare the chloroprene copolymer latex (A). The results are shown in Table 1.

[0132] Comparative Example 2:

[0133] The copolymer latex composition, film, and test piece were prepared by the same method as in Example 1 except that the charged amounts of 2-chloro-1,3-butadiene and 2-methyl-1,3-butadiene were changed as shown in Table 1 and the polymerization conversion rate at the end of the reaction was set to 82% by mass to prepare the chloroprene copolymer latex (A). Various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0134] Comparative Example 3:

[0135] The copolymer latex composition, film, and test piece were prepared by the same method as in Example 1 except that the charged amounts of 2-chloro-1,3-butadiene and 2-methyl-1,3-butadiene were changed as shown in Table 1 and the polymerization conversion rate at the end of the reaction was set to 67% by mass to prepare the chloroprene copolymer latex (A). Various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0136] Comparative Example 4:

[0137] A copolymer latex composition, a film, and a test piece were prepared by the same method as in Example 1 except that the polymerization conversion rate at the end of the reaction was 60 mass % to prepare the chloroprene copolymer latex (A), and various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0138] Comparative Example 5:

[0139] The copolymer latex composition, film, and test piece were prepared by the same method as in Example 1 except that the amount of n-dodecyl mercaptan charged was changed as shown in Table 1 to set the polymerization conversion rate at the end of the reaction to 82 mass % to prepare the chloroprene copolymer latex (A), and various evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0140] [Table 1]

[0141]

[0142] In Examples 1 to 4, in which the chloroprene copolymer in the latex contained a monomer unit derived from 2-methyl-1,3-butadiene, a large amount of crosslinked structures were formed by vulcanization treatment at 100°C, compared with Comparative Example 1 in which the polymer in the latex did not contain a monomer unit derived from 2-methyl-1,3-butadiene, and a film having high flexibility and strength was obtained. In Comparative Example 1, the film could not be peeled off from the mold after the vulcanization treatment and could not be evaluated. The tensile strength (before heat degradation treatment) of the molded products obtained in Comparative Examples 2 to 5 was insufficient for surgical gloves.

[0143] Comparison of Examples 1 to 4 and Comparative Examples 2 to 4 shows that when the ratio of the monomer unit derived from 2-methyl-1,3-butadiene contained in the chloroprene copolymer in the latex is 10 mol% or less, the strength is low, and when the ratio increases, the strength is improved, but when it exceeds 27 mol%, the strength is reduced.

[0144] In Comparative Example 5, the content of the tetrahydrofuran-insoluble component was large, the flexibility was reduced, and the elongation and tensile strength of the film were reduced.

Claims

1. A chloroprene copolymer latex, wherein the chloroprene copolymer contains monomer units derived from 2-chloro-1,3-butadiene (chloroprene) and monomer units derived from 2-methyl-1,3-butadiene, It is characterized in that The content of the tetrahydrofuran-insoluble component in the chloroprene copolymer is 20% by mass or less, the proportion of the monomer unit derived from 2-methyl-1,3-butadiene in the chloroprene copolymer is 10 to 27 mol%, and the chloroprene copolymer further contains 0.01 to 10 mol% of a third monomer unit. The weight average molecular weight of the tetrahydrofuran-soluble component in the chloroprene copolymer is 550,000 or more and 900,000 or less, The third monomer unit is a monomer unit derived from 2,3-dichloro-1,3-butadiene.

2. A chloroprene copolymer latex composition, It is characterized in that contain: 100 parts by mass of the solid content of the chloroprene copolymer latex according to claim 1, Metal oxide (B) 0.1 to 20.0 parts by mass, Vulcanization accelerator (C) 0.1 to 10.0 parts by mass, Sulfur (D) 0.1 to 10.0 parts by mass, and Antioxidant (E) 0.1 to 10.0 parts by mass 3. A chloroprene copolymer rubber molded product obtained by curing the chloroprene copolymer latex composition according to claim 2.

4. A dipped product, which is obtained by molding the chloroprene copolymer latex composition according to claim 2 by a dipping method and curing the same.

5. The dipped article according to claim 4, which is a glove.

6. The dipped product according to claim 5, which is a disposable glove for medical use.