Silicon-based organic-inorganic perovskite heterojunction photodetector and preparation method thereof

By introducing ITO transparent conductive layer and indium layer on the perovskite polycrystalline film, combined with specific preparation methods, the problem of decomposition of perovskite film under air conditions is solved, and high responsiveness, stability and broad-spectrum response are achieved photodetectors have expanded their application potential.

CN113921719BActive Publication Date: 2024-12-03HEBEI XIONGAN ZHONGLING ELECTRONIC TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111164584.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-30
Publication Date
2024-12-03
Estimated Expiration
2041-09-30

AI Technical Summary

Technical Problem

Perovskite polycrystalline films decompose extremely quickly under air conditions, which limits its application promotion.

Method used

Using silicon-based organic-inorganic perovskite heterojunction photodetector structure, including Si single crystal substrate, perovskite MAPbBr3 absorbing layer, ITO transparent conductive layer and indium layer, the thickness is 85-590 by specific preparation methods. The perovskite MAPbBr3 layer of nm and the ITO layer of 90-110 nm are combined with oxygen plasma treatment and magnetron sputtering technology to form a stable photodetector.

Benefits of technology

The responsiveness, signal strength and stability of the photodetector are significantly improved, the response time is shortened, the drop time is shortened, the photocurrent is reduced by 27% after 15 days, and the detection range is expanded to 400-1100 nm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113921719B_ABST
    Figure CN113921719B_ABST
Patent Text Reader

Abstract

The present invention provides a silicon-based organic-inorganic perovskite heterojunction photodetector and a preparation method thereof, wherein the photodetector comprises, from bottom to top, a bottom electrode layer, a substrate, a perovskite MAPbBr3 light-absorbing layer, a transparent conductive layer, and a top electrode layer. The present invention greatly enhances the response signal, greatly shortens the response time, and greatly improves the device stability by adding an ITO transparent conductive layer. At the same time, it is creatively proposed to change the thickness of the perovskite MAPbBr3 film to improve the device performance, and a good effect has been achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photoelectric detectors, and in particular to a silicon-based organic-inorganic perovskite heterojunction photoelectric detector and a preparation method thereof. Background Art

[0002] Under the action of light, electrons in the valence band of the semiconductor material absorb photon energy, overcome the band gap width of the semiconductor and jump to the conduction band to generate electron-hole pairs. Under the action of the built-in electric field, holes and electrons move to the two ends of the heterojunction respectively to generate current, which realizes the conversion of light signals into electrical signals.

[0003] Perovskite-based photodetectors have many unique advantages: (1) Perovskite has a direct bandgap structure and has strong absorption in the ultraviolet and visible light ranges; (2) The bandgap of perovskite can be adjusted by doping with different halogen ions; (3) The carrier mobility in perovskite materials is high and the lifetime is long, which makes the detector collection efficiency high. However, perovskite-based photodetectors also have a major disadvantage, that is, perovskite polycrystalline films decompose very quickly under air conditions. This phenomenon greatly limits the application of such detectors. Summary of the invention

[0004] The purpose of the present invention is to provide a silicon-based organic-inorganic perovskite heterojunction photodetector and a preparation method thereof, so as to solve the problem that the existing perovskite polycrystalline film decomposes very quickly under air conditions and is difficult to promote and apply.

[0005] The technical solution of the present invention is: a silicon-based organic-inorganic perovskite heterojunction photodetector, which includes a bottom electrode layer, a substrate, a perovskite MAPbBr3 light-absorbing layer, a transparent conductive layer and a top electrode layer from bottom to top.

[0006] The substrate is a Si single crystal substrate, the transparent conductive layer is an ITO conductive layer, and the bottom electrode layer and the top electrode layer are indium layers.

[0007] The thickness of the perovskite MAPbBr3 light-absorbing layer is 85-590 nm, and the thickness of the transparent conductive layer is 90-110 nm.

[0008] The bottom electrode layer and the top electrode layer are both circular or square in shape, with a diameter or side length not exceeding 2 mm; the thickness of the bottom electrode layer and the top electrode layer is 0.1-0.2 mm.

[0009] The method for preparing the above-mentioned photoelectric detector comprises the following steps:

[0010] (a) ultrasonically cleaning the substrate with acetone, ethanol and deionized water in sequence, and drying the substrate for later use;

[0011] (b) PbBr2 and CH3NH3Br are mixed in a molar ratio of 1:1 and dissolved in a mixed solution of N,N-dimethylformamide and dimethyl sulfoxide, and the prepared solution is magnetically stirred at room temperature to obtain a perovskite precursor solution with a concentration of 0.4-1.5 mol / L;

[0012] (c) The perovskite precursor solution is dripped onto the substrate surface by spin coating. During the spin coating, toluene is used as an anti-solvent and dripped onto the film surface to form a uniform and dense CH3NH3PbBr3 film. After the spin coating is completed, the film is allowed to stand at room temperature and then annealed on a heating table preheated to 85-95 °C for 5-15 min to obtain a perovskite MAPbBr3 light-absorbing layer with a thickness of 85-590 nm.

[0013] (d) placing the sample obtained in step (c) in a magnetron sputtering chamber and evacuating the chamber; then introducing argon gas to maintain the pressure in the chamber at 0.3-0.5 Pa; then magnetron sputtering a transparent conductive layer using ITO as a target material at a sputtering power of 35-45 W to obtain a transparent conductive layer with a thickness of 90-110 nm;

[0014] (e) A bottom electrode layer and a top electrode layer are respectively formed on the back side of the substrate and the surface of the transparent conductive layer by using an indium pressing method, thereby obtaining the photodetector.

[0015] The substrate is an n-type Si single crystal substrate. After being cleaned and dried, the substrate is placed in an oxygen plasma cleaning instrument, evacuated to below 0 Pa, O2 is introduced and the air inlet valve is adjusted to keep its pressure at 15-25 Pa. After ignition, the oxygen plasma treatment is maintained for 40-80 minutes.

[0016] The volume ratio of the N,N-dimethylformamide to dimethyl sulfoxide is 3-5:1.

[0017] The spin coating was divided into two stages: low speed and high speed. The low speed was 1000 r / min, lasting for 6 s, and the high speed was 4000 r / min, lasting for 60 s. At the 26th s after the start of spin coating, 50-70 μL of toluene was taken as an anti-solvent and quickly dripped onto the film surface.

[0018] During magnetron sputtering, pre-sputter for 3-8 minutes, then remove the substrate baffle and start formal sputtering for 10-25 minutes.

[0019] The bottom electrode layer and the top electrode layer are both circular or square in shape, with a diameter or side length not exceeding 2 mm; the thickness of the bottom electrode layer and the top electrode layer is 0.1-0.2 mm.

[0020] The photoelectric detector of the present invention can achieve wide-band rapid response, ultra-high signal and high stability. It has the following advantages:

[0021] 1. The present invention utilizes ITO transparent conductive material, which unexpectedly makes the photodetector have the characteristics of ultra-high signal, ultra-fast response time and high stability. After adding the ITO transparent conductive layer, the device responsiveness is increased by nearly 350 times, the rise time is shortened by 16.7 times, and the fall time is shortened by 2 times compared with the device without ITO transparent conductive layer. In an environment with a humidity of about 40% and a temperature of about 25°C, the photocurrent is only reduced by 27% after 15 days.

[0022] 2. In the present invention, the perovskite MAPbBr3 is combined with Si to form a pn junction, so that the detection range is expanded to 400 nm-1100 nm.

[0023] 3. The photoelectric detector of the present invention has high responsiveness and high detection degree.

[0024] 4. The setting of the thickness of the perovskite MAPbBr3 layer is crucial. The thickness of the perovskite MAPbBr3 layer is creatively adjusted. When the thickness is 215 nm, the response signal of the perovskite MAPbBr3 layer is increased by 2.1 times and 14.3 times compared with the perovskite MAPbBr3 layer with a thickness of 85 nm and 590 nm, respectively, obtaining an ultra-high signal and better response.

[0025] 5. The order of the photoresponsive thin film layer structure of the present invention is Si single crystal substrate, perovskite MAPbBr3 layer, and ITO layer. Perovskite MAPbBr3 and Si single crystal are light absorption layers, and the incident light is basically absorbed to generate electron-hole pairs; due to the energy level matching between the perovskite MAPbBr3 and Si interface, a built-in electric field is formed, which separates the electron-hole pairs excited by light, and the electrons move toward the Si single crystal, and the holes move toward the ITO layer; ITO is a conductive layer that allows incident light to penetrate without absorption, and has good conductive properties, collecting holes separated by tunneling. Through creative research on each structural layer, the arrangement relationship of each layer is determined, and combined with the thickness of each layer, the performance of the photodetector is improved.

[0026] 6. The thickness of the perovskite MAPbBr3 layer is set to 215 nm, which can absorb almost all incident light intensity and increase the light absorption efficiency. When the thickness of the layer is greater than 215 nm, it not only increases the economic cost, but also is not conducive to the separation and tunneling of photogenerated electron-hole pairs. This is concluded after long-term research.

[0027] 7. The maximum responsivity of the present invention reaches 0.87 A / W, the measurable wavelength range is 400-1100 nm, the rise time reaches 129 ms, and the fall time reaches 130 ms. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the experiment of Example 1.

[0029] Figure 2 It is a schematic diagram of the experiment of Example 2.

[0030] Figure 3 1 is a graph showing the responsivity and detectivity of the perovskite photodetectors obtained in Example 1 and Example 2 under a -1 V bias voltage as the wavelength changes.

[0031] Figure 4 This is a response time test graph of the perovskite photodetector obtained in Example 1 and Example 2 under a -1 V bias voltage.

[0032] Figure 5 This is a time stability test graph of the perovskite photodetector obtained in Example 1 and Example 2 under a -1 V bias voltage.

[0033] Figure 6 This is a graph showing the responsivity trend of the perovskite film photodetectors with different thicknesses obtained in Example 3 under a bias voltage of -1 V as the thickness of the perovskite film changes.

[0034] In the figure, 1. Si single crystal substrate, 2. Perovskite MAPbBr3 light-absorbing layer, 3. ITO transparent conductive layer, 4. Bottom electrode, 5. Top electrode, 6. Ammeter, 7. Laser. DETAILED DESCRIPTION

[0035] The present invention is further described below in conjunction with the examples. The processes and methods not described in detail in the following examples are conventional methods well known in the art. Unless otherwise specified, the raw materials or reagents used in the examples are commercially available and can be purchased through commercial channels.

[0036] Example 1

[0037] a. A 500 μm thick n-Si single crystal substrate was ultrasonically treated with acetone, ethanol and deionized water for 20 min each.

[0038] b. Place the clean and dry substrate face up in an oxygen plasma cleaner, evacuate to below 0 Pa, introduce O2 and adjust the inlet valve to keep the pressure at 20 Pa. After ignition, maintain oxygen plasma treatment for 60 min to allow the surface to naturally oxidize and form a SiO2 layer.

[0039] c. Mix 146.8 mg of lead bromide (PbBr2) and 44.76 mg of methyl bromide (CH3NH3Br) in a molar ratio of 1:1 and dissolve them in a mixed solution of 800 μL of N,N-dimethylformamide (DMF) and 200 μL of dimethyl sulfoxide (DMSO) (solvent volume ratio 4:1). Place the prepared solution on a magnetic stirrer and stir it at room temperature for more than 8 hours to fully dissolve it, and obtain a perovskite precursor solution with a concentration of 0.4 mol / L.

[0040] d. The Si substrate was placed in a glove box filled with N2 and fixed to the suction cup of the coating machine. 50 μL of the perovskite precursor solution was slowly dripped onto the surface of the Si substrate. The spin coating was divided into two stages: low speed and high speed. The low speed was 1000 r / min, the duration was 6 s, and the high speed was 4000 r / min, the duration was 60 s. At the 26th second of the start of spin coating, 60 μL of toluene was quickly dripped onto the film surface as an anti-solvent to form a more uniform and dense CH3NH3PbBr3 film. After the spin coating was completed, it was left to stand at room temperature for 10 min, and then placed on a heating table preheated to 90 °C for annealing for 10 min to obtain a perovskite MAPbBr3 polycrystalline film with a thickness of 85 nm.

[0041] e. Two In electrodes are vertically pressed on the back of the Si single crystal substrate and on both sides of the upper surface of the perovskite MAPbBr3 light-absorbing layer, that is, the circular top and bottom electrodes with a diameter of 1 mm and a thickness of 0.15 mm are made by pressing indium to obtain a perovskite photodetector. The bottom and top electrodes are led out with wires and connected to an ammeter.

[0042] Turn on the power supply, the voltage is -1 V, the bottom electrode is connected to the positive electrode, and the top electrode is connected to the negative electrode. Irradiate the focused point light source on the surface of the thin film photoresponse layer, and irradiate the 532 nm laser spot near the top electrode. Use an ammeter to record the change of photocurrent. Change the laser wavelength, and the detector responsivity changes, such as Figure 3 shown.

[0043] The focused point light source is irradiated on the surface of the thin film photoresponse layer, and the 532 nm laser spot is irradiated near the top electrode. The interval between the shutter switch is 5 s. The change of photocurrent is recorded by an ammeter. After data processing and analysis, the response time of the detector is obtained, such as Figure 4 The photocurrent was tested at 25°C and 40% humidity for 0 h, 24 h and 48 h, and the stability of the detector was recorded. Figure 5 shown.

[0044] Example 2

[0045] a. A 500 μm thick n-Si single crystal substrate was ultrasonically treated with acetone, ethanol and deionized water for 20 min each.

[0046] b. Place the clean and dry substrate face up in an oxygen plasma cleaner, evacuate to below 0 Pa, introduce O2 and adjust the inlet valve to keep the pressure at 20 Pa. After ignition, maintain oxygen plasma treatment for 60 min to allow the surface to naturally oxidize and form a SiO2 layer.

[0047] c. Mix 146.8 mg of lead bromide (PbBr2) and 44.76 mg of methyl bromide (CH3NH3Br) at a molar ratio of 1:1 and dissolve them in a mixed solution of 800 μL of N,N-dimethylformamide (DMF) and 200 μL of dimethyl sulfoxide (DMSO) (solvent volume ratio 4:1). Place the prepared solution on a magnetic stirrer and stir it at room temperature for more than 8 hours to fully dissolve it, and obtain a perovskite precursor solution with a concentration of 0.4 mol / L.

[0048] d. The Si substrate was placed in a glove box filled with N2 and fixed to the suction cup of the coating machine. 50 μL of the perovskite precursor solution was slowly dripped onto the surface of the Si substrate. The spin coating was divided into two stages: low speed and high speed. The low speed was 1000 r / min, the duration was 6 s, and the high speed was 4000 r / min, the duration was 60 s. At the 26th second of the start of spin coating, 60 μL of toluene was quickly dripped onto the film surface as an anti-solvent to form a more uniform and dense CH3NH3PbBr3 film. After the spin coating was completed, it was left to stand at room temperature for 10 min, and then placed on a heating table preheated to 90 °C for annealing for 10 min to obtain a perovskite MAPbBr3 polycrystalline film with a thickness of 85 nm.

[0049] e. After the sample is placed in the magnetron sputtering chamber, a mechanical pump is used to evacuate the chamber. When the vacuum degree reaches below 10Pa, a molecular pump is used to evacuate the chamber. Wait until the vacuum degree in the sputtering chamber reaches 1×10 -5 Pa. Fill the sputtering chamber with argon gas at a certain flow rate through the inlet valve, and then adjust the molecular pump gate valve to maintain the pressure in the sputtering chamber at 0.4Pa, and adjust the sputtering power to 40 W. After adjusting the film growth conditions, pre-sputter for five or six minutes to ensure that the glow in the chamber is stable, the film is deposited at a certain rate, and the obtained film is dense and uniform. After the glow is stable, remove the substrate baffle and start formal sputtering. When the time reaches 15 minutes, a 100 nm thick ITO conductive layer is obtained. Close the baffle; after the growth is completed, turn off the vacuum system, close the gate valve and the solenoid valve, fill with nitrogen so that the pressure in the chamber is atmospheric pressure, open the chamber door and take out the sample.

[0050] f. Two In electrodes are vertically pressed on the back of the Si single crystal substrate and on both sides of the upper surface of the ITO conductive layer, that is, the circular top and bottom electrodes with a diameter of 1 mm and a thickness of 0.15 mm are made by pressing indium to obtain a perovskite photodetector. The bottom and top electrodes are led out with wires and connected to the ammeter.

[0051] Turn on the power supply, the voltage is -1 V, the bottom electrode is connected to the positive electrode, and the top electrode is connected to the negative electrode. Irradiate the focused point light source on the surface of the thin film photoresponse layer, and irradiate the 532 nm laser spot near the top electrode. Use an ammeter to record the change of photocurrent. Change the laser wavelength, and the detector responsivity changes, such as Figure 3 shown.

[0052] The focused point light source is irradiated on the surface of the thin film photoresponse layer, and the 532 nm laser spot is irradiated near the top electrode. The interval between the shutter switch is 5 s. The change of photocurrent is recorded by an ammeter. After data processing and analysis, the response time of the detector is obtained, such as Figure 4 As shown. Under the conditions of temperature of 25 ℃ and humidity of 40%, the photocurrent was tested at time intervals of 0 h, 24 h, 48 h, 72 h, 96 h, 120 h, 168 h, 216 h, 264 h and 360 h to record the stability of the detector, as shown in Figure 5 shown.

[0053] pass Figure 3 It can be seen that due to the introduction of the ITO transparent conductive layer, the power consumption at 532nm wavelength is 6.36mW / cm 2 Under power density laser irradiation, the responsivity of the photodetector increased from 0.394mA / W to 0.135A / W.

[0054] pass Figure 4 It can be seen that due to the introduction of the ITO transparent conductive layer, the power consumption at 532 nm is 6.36 mW / cm 2 Under high-power-density laser irradiation, the rise time of the photodetector is shortened from 2176 ms to 130 ms, and the fall time is shortened from 257 ms to 125 ms.

[0055] pass Figure 5 It can be seen that due to the introduction of the ITO transparent conductive layer, the power consumption at 532 nm is 6.36 mW / cm 2 Under high-power laser irradiation, after about 15 days of testing, the photocurrent decreased by only 27% compared to the original device. However, after about 15 days of testing, the photocurrent of the device without the ITO transparent conductive layer decreased by 93% compared to the original device.

[0056] Example 3

[0057] A photodetector was prepared according to the method of Example 2, except that the concentrations of the perovskite precursor solution were 0.4 mol / L, 0.6 mol / L, 0.8 mol / L, 1 mol / L, 1.2 mol / L and 1.5 mol / L, respectively, and the thicknesses of the corresponding perovskite MAPbBr3 polycrystalline films were 85 nm, 160 nm, 215 nm, 380 nm, 440 nm and 590 nm, respectively, and were numbered 1, 2, 3, 4, 5, and 6, respectively, and the thickness of the ITO transparent conductive layer was 100 nm.

[0058] The focused light source is irradiated on the surface of the ITO transparent conductive layer, and the 671 nm laser spot is irradiated near the upper electrode. The change of photocurrent is recorded by an ammeter. When the test sample is changed, the detector responsivity changes. The perovskite MAPbBr3 polycrystalline samples with different thicknesses are tested, such as Figure 6 shown.

[0059] pass Figure 6 It can be seen that the responsivity of the detector increases first and then decreases with the thickness of the perovskite MAPbBr3 polycrystalline film. When the thickness of the perovskite MAPbBr3 polycrystalline film is 215 nm, the photodetector has the best performance and a responsivity of 0.87 A / W.

Claims

1. A silicon-based organic-inorganic perovskite heterojunction photodetector, characterized in that: The photodetector includes, from bottom to top, a bottom electrode layer, a substrate, a perovskite MAPbBr3 light-absorbing layer, a transparent conductive layer and a top electrode layer; the substrate is a Si single crystal substrate, the transparent conductive layer is an ITO conductive layer, the bottom electrode layer and the top electrode layer are indium layers, wherein the transparent conductive layer completely covers the perovskite MAPbBr3 light-absorbing layer.

2. The photodetector according to claim 1, characterized in that: The thickness of the perovskite MAPbBr3 light-absorbing layer is 215 nm, and the thickness of the transparent conductive layer is 90-110 nm.

3. The photodetector according to claim 1, characterized in that: The bottom electrode layer and the top electrode layer are both circular or square in shape, with a diameter or side length not exceeding 2 mm; the thickness of the bottom electrode layer and the top electrode layer is 0.1-0.2 mm.

4. A method for preparing a photoelectric detector according to any one of claims 1 to 3, characterized in that: The following steps are involved: (a) ultrasonically cleaning the substrate with acetone, ethanol and deionized water in sequence, and drying the substrate for later use; (b) PbBr2 and CH3NH3Br are mixed in a molar ratio of 1:1 and dissolved in a mixed solution of N,N-dimethylformamide and dimethyl sulfoxide, and the prepared solution is magnetically stirred at room temperature to obtain a perovskite precursor solution with a concentration of 0.4-1.5 mol / L; (c) The perovskite precursor solution is dripped onto the substrate surface by spin coating. During the spin coating, toluene is used as an anti-solvent and dripped onto the film surface to form a uniform and dense CH3NH3PbBr3 film. After the spin coating is completed, the film is allowed to stand at room temperature and then annealed on a heating table preheated to 85-95 °C for 5-15 min to obtain a perovskite MAPbBr3 light-absorbing layer with a thickness of 85-590 nm. (d) placing the sample obtained in step (c) in a magnetron sputtering chamber and evacuating the chamber; then introducing argon gas to maintain the pressure in the chamber at 0.3-0.5 Pa; then magnetron sputtering a transparent conductive layer using ITO as a target material at a sputtering power of 35-45 W to obtain a transparent conductive layer with a thickness of 90-110 nm; (e) A bottom electrode layer and a top electrode layer are respectively formed on the back side of the substrate and the surface of the transparent conductive layer by using an indium pressing method, thereby obtaining the photodetector.

5. The preparation method according to claim 4, characterized in that: The substrate is an n-type Si single crystal substrate. After being cleaned and dried, the substrate is placed in an oxygen plasma cleaning instrument, evacuated to below 0 Pa, O2 is introduced and the air inlet valve is adjusted to keep its pressure at 15-25 Pa. After ignition, the oxygen plasma treatment is maintained for 40-80 minutes.

6. The preparation method according to claim 4, characterized in that: The volume ratio of the N,N-dimethylformamide to dimethyl sulfoxide is 3-5:

1.

7. The preparation method according to claim 4, characterized in that: The spin coating was divided into two stages: low speed and high speed. The low speed was 1000 r / min, lasting for 6 s, and the high speed was 4000 r / min, lasting for 60 s. At the 26th s after the start of spin coating, 50-70 μL of toluene was taken as an anti-solvent and quickly dripped onto the film surface.

8. The preparation method according to claim 4, characterized in that: During magnetron sputtering, pre-sputter for 3-8 minutes, then remove the substrate baffle and start formal sputtering for 10-25 minutes.

9. The preparation method according to claim 4, characterized in that: The bottom electrode layer and the top electrode layer are both circular or square in shape, with a diameter or side length not exceeding 2 mm; the thickness of the bottom electrode layer and the top electrode layer is 0.1-0.2 mm.