Replacement of phosphorus element by lithium-tin-metal-sulfide compound solves the problem of reaction between sulfide solid electrolyte and moisture, achieves high ionic conductivity and improved safety, and is suitable for all-solid-state batteries.
Patent Information
- Application Number
- CN202111048936.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2016-01-12
- Filing Date
- 2017-01-12
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2037-01-12
AI Technical Summary
Since sulfide solid electrolytes contain phosphorus, they easily react with moisture in the atmosphere, leading to performance degradation and the generation of toxic gases, which pose safety and stability issues.
Lithium-tin-metal-sulfide compound (LiaSnbMcSd) is used as the solid electrolyte. By replacing the phosphorus element, metals from the 4th to 6th periods of the periodic table of elements are used, such as zirconium, niobium, hafnium, gallium, indium, etc., to form lithium -Tin-metal-sulfide, prepared by heat treatment to maintain high ionic conductivity and improve safety and stability.
Improved reactivity to moisture, prevents the generation of toxic gases, improves safety and stability, maintains high ionic conductivity, and is easy to store and handle.
Smart Images

Figure CN113937350B_ABST
Abstract
Description
[0001] This invention patent application is a divisional application based on a Chinese patent application with an application date of January 12, 2017, an invention name of “Sulfide-type solid electrolyte and all-solid-state battery using the same” and an application number of 201780003777.5. Technical Field
[0002] This application claims priority based on Korean Patent Application No. 10-2016-0003514 filed on January 12, 2016 and Korean Patent Application No. 10-2017-0005605 filed on January 12, 2017, which are hereby incorporated by reference in their entirety.
[0003] The present invention relates to a solid electrolyte containing a sulfide-type compound and an all-solid-state battery using the solid electrolyte. Background Art
[0004] Various batteries that can overcome the limitations of lithium secondary batteries are currently being studied from the viewpoints of battery capacity, safety, power output, upsizing, downsizing, and the like.
[0005] Representatively, academia and industry are continuously researching the following batteries: in terms of capacity, metal-air batteries are being studied, which have a theoretical capacity comparable to that of lithium secondary batteries; in terms of safety, all-solid-state batteries are being studied without the risk of explosion; in terms of power output, supercapacitors are being studied; in terms of large-scale development, NaS batteries or RFBs (redox flow batteries); in terms of miniaturization, thin-film batteries are being studied; and so on.
[0006] Among them, the all-solid-state battery is a battery that replaces the liquid electrolyte used in conventional lithium secondary batteries with a solid electrolyte, and since no flammable solvent is used in the battery, the all-solid-state battery can significantly improve safety, and therefore will not catch fire or explode due to the decomposition reaction of the conventional electrolyte solution. In addition, there are the following advantages: since Li metal or Li alloy can be used as the negative electrode material, the energy density related to the mass and volume of the battery can be significantly improved.
[0007] Specifically, the inorganic solid electrolytes used in all-solid-state batteries can be divided into sulfide-type electrolytes and oxide-type electrolytes. At present, the most advanced solid electrolyte is the sulfide-type solid electrolyte, and the ionic conductivity of this solid electrolyte has developed to a level close to that of organic electrolyte solutions.
[0008] However, it is generally known that sulfide-type solid electrolytes contain phosphorus (P) and react with moisture and oxygen in the atmosphere, resulting in rapid performance degradation. Therefore, since the storage stability in the atmosphere is low, it is difficult to handle, and as shown in the following reaction formula (1), toxic gases such as hydrogen sulfide (H2S) are generated by reacting with water, thereby causing problems in safety and stability:
[0009] [Reaction 1]
[0010] Summary of the invention
[0011]
Technical issues
[0012] As mentioned above, most sulfide-based solid electrolytes contain phosphorus (P) and show 10 -3 S / cm to 10 -5 S / cm, but there is a problem of reaction with moisture in the atmosphere.
[0013] Therefore, an object of the present invention is to provide a sulfide-type solid electrolyte which improves safety and stability while maintaining high ion conductivity by replacing phosphorus element (P) with another element.
[0014]
Technical solution
[0015] In order to achieve the above object, the present invention provides a sulfide-type solid electrolyte, characterized in that it contains a lithium-tin-metal-sulfide (LTMS) type compound represented by the following general formula 1:
[0016] [General formula 1]
[0017] Li a Sn b M c S d
[0018] wherein M and a, b, c and d are defined herein.
[0019] In addition, the present invention provides a method for preparing the sulfide-type solid electrolyte, which comprises:
[0020] i) mixing lithium sulfide, tin sulfide and a sulfide containing M (wherein M is at least one metal selected from elements belonging to Group 4, Group 5, Group 13, Group 14 and Group 15 (excluding Sn) among elements belonging to Periods 4 to 6 of the Periodic Table (IUPAC); and
[0021] ii) subjecting the mixture to a heat treatment.
[0022] In addition, the present invention provides an all-solid-state battery including the sulfide-type solid electrolyte.
[0023]
Beneficial Effects
[0024] According to the sulfide-type solid electrolyte and the all-solid-state battery using the same of the present invention, the reactivity to moisture is improved, the generation of toxic gases such as hydrogen sulfide (H2S) is prevented, the safety and stability are improved, and the ionic conductivity does not decrease even after being placed in the air, and the solid electrolyte is easy to handle and store due to its improved storage stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is the Li of the present invention. a Sn b M c S d Periodic table of elements (M) (except Sn) available in.
[0026] Figure 2 By comparing the Li a Sn b M c S d The data are obtained by analyzing the formation energy of each element (M).
[0027] Figure 3 By comparing the Li a Sn b M c S d The data are obtained by calculating the lattice volume of each element (M) in the graph.
[0028] Figure 4 By comparing the Li a Sn b M c S d The data are obtained by measuring the band gap energy of each element (M) in the graphene.
[0029] Figure 5 Li prepared in Example 1 of the present invention 13 Sn2InS 12 XRD results of . DETAILED DESCRIPTION
[0030] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily implement the present invention. However, the present invention can be implemented in many different forms and is not limited thereto.
[0031] Lithium-tin-metal-sulfide type compounds
[0032] Generally, the sulfide-based solid electrolytes used in the art are composed of Li-P-S or Li-P-X-S (where X is a metal element other than P), and thus contain phosphorus element (P). However, due to safety and stability problems such as the generation of toxic gases caused by the phosphorus element (P), the present invention aims to provide a new lithium-tin-metal-sulfide (LTMS: lithium-tin-metal-sulfide) as a solid electrolyte, which must contain lithium (Li) and sulfur (S) but does not contain phosphorus element (P).
[0033] LTMS has a structure in which the metal M partially replaces the basic crystal structure of lithium-tin-sulfide (LTS), and is preferably represented by the following general formula 1:
[0034] [General formula 1]
[0035] Li a Sn b M c S d
[0036] Wherein M is at least one metal selected from the elements of Group 4, Group 5, Group 13, Group 14 and Group 15 (excluding Sn) of the 4th to 6th periods of the Periodic Table (IUPAC), and 0 < a ≤ 20, 0 < b ≤ 5, 0 < c ≤ 5 and 0 < d ≤ 20.
[0037] M described in the general formula 1 can be confirmed by Figure 1 the Periodic Table (IUPAC). More specifically, the element M can be at least one selected from the group consisting of the following elements: transition metals such as zirconium (Zr), niobium (Nb), hafnium (Hf) and tantalum (Ta), post-transition metals such as gallium (Ga), indium (In), thallium (Tl), lead (Pb) and bismuth (Bi), and metalloids such as germanium (Ge), arsenic (As) and antimony (Sb).
[0038] For example, these elements M have 3 to 5 valence electrons, so they can form a form (M-S) by bonding with sulfur element (S), and this form (M-S) forms an anion and thus forms an electrochemical bond with metal cations such as lithium (Li + (M-S) - ). These compounds allow the migration of lithium cations (Li + ).
[0039] In the present invention, the element M replacing the phosphorus element (P) must be able to form a compound by synthesis with lithium (Li) and sulfur (S), and preferably has excellent ion conductivity and is an electrical insulator, so as to be used as a solid electrolyte for an all-solid-state battery. Therefore, in order to confirm whether the above conditions are met through virtual simulation in the following experimental example, thirteen elements that can replace the phosphorus element (P) with a temperature of 10 -5 The elements (As(III), Ga(III), In(III), Sb(III), Bi(III), Pb(IV), Zr(IV), Hf(IV), Ce(IV), As(V), Nb(V), Ta(V), Sb(V)) of the Sn site in Li4SnS4 with an ionic conductivity of 0.1 S / cm were then simulated, and the formation energy, lattice volume and band gap energy were obtained based on density functional theory (DFT (density functional theory), GGA-PBE).
[0040] Formation Energy
[0041] The structural model of the lithium-tin-metal-sulfide type compound substituted with the above 13 candidate elements was simulated, and the formation enthalpy (ΔH) of each atom was calculated. It can be said that the enthalpy (ΔH) at a temperature of 0K and a pressure of 0 is the total energy in the optimized grid model. In the present invention, the standard formation enthalpy is used to determine the relative value, but the present invention is not limited to this.
[0042] Therefore, the formation energy of compounds substituted with the above 13 elements as solid electrolyte candidates was simulated. The obtained data are shown in Figure 2 As a result, based on Li4SnS4 (LSS), which is a compound before substitution, an element species with a lower formation energy has a more stable energy level when forming a compound, and thus can substitute the Sn site. Therefore, from the aspect of computational chemistry, when the formation energy based on Li4SnS4 (LSS) has a negative value, the element is an element that can be spontaneously substituted and well synthesized. It can be determined that the elements that meet these conditions are Ga(III), In(III), Sb(III), Bi(III), Zr(IV), Hf(IV), Ce(IV), and Ta(V).
[0043] Lattice volume
[0044] Unlike in liquids, the transfer of ions in the solid phase occurs through limited paths in the crystal lattice. In general, the ionic conductivity of solid electrolytes is lower than that of liquid electrolytes. However, for some solids, it is reported that the ionic conductivity is theoretically higher than that of liquids, and measuring or predicting the ionic conductivity of solid electrolytes is important for all-solid-state secondary batteries because the ionic conductivity of the electrolyte is an important factor in determining the charge and discharge rate of the battery as well as the output rate.
[0045] The ion migration mechanism in this solid phase is mainly caused by ionic point defects or lattice defects caused by defects, as well as electrostatic attraction and repulsion. Ionic point defects can be divided into Schottky defects formed by cation / anion pairs and Frenkel defects formed by a pair of interstitial atoms at different positions.
[0046] Schottky defect is a state where an atom that should have existed in the lattice point does not exist, and this atomic vacancy is called an attack point. This means that an atom in the crystal leaves its original position and exists on the surface of the crystal. In addition, Frenkel defect is a defect caused by the insertion of another atom into the gap between the lattices of atoms constituting the crystal lattice, that is, a defect caused by the insertion of an atom that leaves the Schottky defect into the lattice.
[0047] The lattice volume refers to the space of lattice defects as described above in such a solid electrolyte, and such space forms a three-dimensional channel between the lattices, and ion conduction can be achieved by placing cations in such a channel.
[0048] As a result of substitution by each element, the overall framework structure is maintained, but the lattice volume changes. The larger the lattice volume, the more channels that are more suitable for ion migration are formed, thereby improving ion conductivity (H. Aono and E. Sugimoto, "Electrical property and sinterability of LiTi2(PO4)3 mixed with lithium salt (Li3PO4 or Li3BO3)", Solid State Ionics, 47, 257 (1991)).
[0049] Therefore, the lattice volume of the compound substituted with the above 13 elements as a solid electrolyte candidate was simulated, and the obtained data is shown in Figure 3In the case of a compound having a higher lattice volume based on the lattice volume of Li4SnS4(LSS) (i.e., the compound before substitution), since the activation energy when Li ions diffuse tends to be lower, it can be said that the ionic conductivity is also high. Therefore, it can be expected that the ionic conductivity will be greater than 10 of Li4SnS4(LSS). -5 S / cm ion conductivity. Among the above 13 elements, when 11 elements other than Ga(III) and As(V) are substituted, the lattice volume is large. In particular, when In(III), Sb(III), Bi(III) or Ce(IV) elements are substituted, high ion conductivity can be expected.
[0050] Band Gap Energy
[0051] The band gap, also known as the energy gap, is the energy level or energy difference between the highest energy level where electrons are present and the lowest energy level where electrons are not present. The band gap of an insulator or semiconductor is usually the energy difference between the highest part of the valence band and the lowest part of the conduction band, and is expressed in electron volts (eV). This is the energy required to transfer the outer electrons around the nucleus to a free state, and as one would expect, the larger the band gap, the better the insulation.
[0052] Therefore, the band gap energy of compounds substituted with 13 elements as solid electrolyte candidates was simulated, and the obtained data are shown in Figure 4 As the band gap becomes larger, it has excellent electrical insulation, can be stably used as a solid electrolyte, and has a wide operating voltage range. Considering that the band gap of Li4SnS4 (LSS) is 2eV, it can be considered that when replaced by an element with a band gap higher than 2eV, a stable compound can be produced. It has been shown that when replaced with Ga(III), In(III), Zr(IV), Hf(IV), Nb(V), Ta(V) as elements that meet these conditions, the band gap is similar to the reference value (ie, the band gap of Li4SnS4 (LSS)), so it is determined that it has insulating properties and can be used as a solid electrolyte.
[0053] As a result of comprehensive consideration of formation energy, lattice volume and band gap energy, it is shown that the formation energy is below 0 eV and the lattice volume is The three elements In(III), Zr(IV) and Ta(V) that satisfy the above and band gap energy of 2 eV or more are excellent in synthesizability, ionic conductivity and electrical insulation. Therefore, it is determined that these elements are suitable as substitutes for phosphorus (P) in sulfide-type solid electrolytes.
[0054] These lithium-tin-metal-sulfide type compounds can be prepared to have an average particle size ranging from several nanometers to several thousand micrometers. In addition, there is no particular limitation on the morphology, but the average particle size is preferably in the range of 0.1 μm to 50 μm.
[0055] Nano-scale particle size can easily increase the contact area with common active materials, which can become a favorable condition for charging and discharging by expanding the transfer path of lithium ions, so having nano-scale particle size is advantageous.
[0056] Preparation method of lithium-tin-metal-sulfide type compound
[0057] The preparation method of the lithium-tin-metal-sulfide type compound of the general formula 1 proposed in the present invention can be prepared according to the known preparation method of the lithium-tin-metal-sulfide type compound.
[0058] Typically, the lithium-tin-metal-sulfide type compound is prepared by a method comprising the steps of: i) mixing lithium sulfide, tin sulfide, and M-containing sulfide; and ii) heat treating the mixture.
[0059] Hereinafter, each step will be described in detail.
[0060] First, lithium sulfide, tin sulfide, and M-containing sulfide in powder form are mixed to prepare a mixed powder.
[0061] The lithium sulfide is not particularly limited in the present invention, and known substances can be selected and used. Generally, it can be Li2S, Li2S2, etc., and Li2S is preferably used.
[0062] Tin sulfide is not particularly limited in the present invention, and a known material can be selected and used. Generally, it can be SnS2, SnS, etc., and SnS2 is preferably used.
[0063] As the compound containing M, various materials can be used depending on the kind of M. For example, when M is In, Zr, or Ta, In2S3, ZrS3, Ta2S3, etc. can be used.
[0064] In this case, the content ratio of lithium sulfide, tin sulfide and M-containing sulfide may be controlled in various ways according to the molar ratio of the final lithium-tin-metal-sulfide type compound, and is not particularly limited in the present invention.
[0065] The mixing may be performed by a dry or wet mixing method and is not particularly limited in the present invention.
[0066] Mixing is performed by the method for conventional mixed powder production, and mechanical grinding can be performed to perform uniform particle mixing. For mechanical grinding, for example, a roller mill, ball mill or jet mill can be used. Mixing can be performed for 1 hour to 8 hours, preferably 1 hour to 6 hours.
[0067] Next, the mixed powder obtained in the above step is heat-treated to produce a lithium-tin-metal-sulfide type compound.
[0068] The heat treatment in this step is preferably performed at a temperature range of 400° C. to 850° C. for about 1 minute to about 60 minutes, specifically 1 minute to 30 minutes, more specifically 1 minute to 10 minutes.
[0069] The heat treatment may be performed at least once and may be performed in two steps including a first heat treatment and a second heat treatment, and in this case, when the second heat treatment is performed at a higher temperature than that in the first heat treatment, particle formation and manufacture of the lithium-tin-sulfide type compound are facilitated.
[0070] In this case, if the temperature of the heat treatment is lower than the above range, the preparation of the lithium-tin-metal-sulfide type compound itself may become difficult. On the contrary, if the temperature of the heat treatment exceeds the above range, the particles of the lithium-tin-metal-sulfide type compound become larger, whereby the ion conductivity may decrease, or it may become difficult to produce particles of uniform size.
[0071] All-solid-state battery
[0072] The above-mentioned lithium-tin-metal-sulfide type compound of the present invention can be preferably used as a solid electrolyte of an all-solid-state battery.
[0073] The all-solid-state battery comprises a positive electrode, a negative electrode and a solid electrolyte disposed therebetween.
[0074] The lithium-tin-metal-sulfide type compound of the present invention has high ion conductivity and simultaneously does not generate toxic gas, thereby ensuring the same or higher physical properties as other conventional sulfide type solid electrolytes.
[0075] The thickness of the solid electrolyte layer formed of the lithium-tin-metal-sulfide type compound varies greatly depending on the structure of the all-solid-state battery. However, for example, it is preferably 0.1 μm or more and 1 mm or less, and more preferably 1 μm or more and 100 μm or less. The solid electrolyte preferably has high lithium ion conductivity, and for example, the lithium ion conductivity at room temperature is preferably 1×10 -4 S / cm or more.
[0076] In this case, the solid electrolyte may include a solid electrolyte generally used in an all-solid-state battery in addition to a lithium-tin-metal-sulfide type compound. For example, an inorganic solid electrolyte or an organic solid electrolyte may be used.
[0077] In the case of an inorganic solid electrolyte, a ceramic material, a crystalline material, or an amorphous material can be used, and an inorganic solid electrolyte such as sulfo-LISICON (Li 3.25 Ge 0.25 P 0.75 S4), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-P2S5, Li3PS4, Li7P3S 11 , Li2O-B2O3, Li2O-B2O3-P2O5, Li2O-V2O5-SiO2, Li2O-B2O3, Li3PO4, Li2O-Li2WO4-B2O3, LiPON, LiBON, Li2O-SiO2, LiI, Li3N, Li5La3Ta2O 12 、Li7La3Zr2O 12 、Li6BaLa2Ta2O 12 、Li3PO (4-3 / 2w) Nw (where w is w<1) and Li 3.6 Si 0.6 P 0.4 O4.
[0078] In addition, examples of organic solid electrolytes include those prepared by mixing lithium salts with polymer materials such as polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyalginate lysine, polyester sulfide, polyvinyl alcohol, and polyvinylidene fluoride. In this case, these may be used alone or in combination of at least one.
[0079] Meanwhile, the positive electrode and the negative electrode used for the all-solid-state battery of the present invention are not particularly limited, and known positive electrodes and negative electrodes may be used.
[0080] The all-solid-state battery proposed in the present invention defines the constitution of the solid electrolyte as described above, and other elements constituting the battery, ie, the positive electrode and the negative electrode, are not particularly limited in the present invention and follow the following description.
[0081] The negative electrode for all-solid-state batteries is lithium metal alone, or the negative electrode active material can be laminated on the negative electrode current collector.
[0082] In this case, the negative electrode current collector is not particularly limited as long as it is conductive and does not cause any chemical change in the all-solid-state battery, and for example, copper, stainless steel, aluminum, nickel, titanium, sintered carbon, copper or stainless steel whose surface is treated with carbon, nickel, titanium, silver, etc., or an aluminum-cadmium alloy, etc. can be used. In addition, similar to the positive electrode current collector, the negative electrode current collector can also include various forms, such as a film, sheet, foil, mesh, porous body, foam body, and non-woven fabric having fine irregularities formed on its surface.
[0083] The negative electrode active material can be any one selected from the group consisting of lithium metal, lithium alloy, lithium metal composite oxide, lithium-containing titanium composite oxide (LTO), and combinations thereof. In this case, the lithium alloy can be an alloy of lithium and at least one metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Ba, Ra, Al, and Sn. In addition, the lithium metal composite oxide is an oxide (MeO x ) of lithium and any one metal (Me) selected from the group consisting of Si, Sn, Zn, Mg, Cd, Ce, Ni, and Fe, and for example, it can be LixFe2O3 (0 < x ≤ 1) or LixWO2 (0 < x ≤ 1).
[0084] In addition, the negative electrode active material can be a metal composite oxide, such as Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of Groups 1, 2, and 3 of the periodic table, halogens; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8); oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, and Bi2O5, and carbon-based negative electrode active materials such as crystalline carbon, amorphous carbon, or carbon composites, and the negative electrode active materials can be used alone or in combination of two or more.
[0085] The positive electrode for the all-solid-state battery of the present invention is not particularly limited and can be a material for a known all-solid-state battery.
[0086] The positive electrode current collector is not particularly limited as long as it has high conductivity and does not cause chemical change in the relevant battery, and for example, stainless steel, aluminum, nickel, titanium, sintered carbon, or aluminum or stainless steel whose surface is treated with carbon, nickel, titanium, silver, etc. can be used.
[0087] The positive electrode active material can be changed according to the use of the lithium secondary battery, and lithium metal oxides such as LiNi 0.8-x Co0.2 AlxO2、LiCo x Mn y O2、LiNi x Co y O2、LiNi x Mn y O2、LiNi x Co y Mn z O2, LiCoO2, LiNiO2, LiMnO2, LiFePO4, LiCoPO4, LiMnPO4 and Li4Ti5O 12 ; Sulfur compounds such as Cu2Mo6S8, FeS, CoS and NiS, as well as oxides, sulfides or halides of scandium, ruthenium, titanium, vanadium, molybdenum, chromium, manganese, iron, cobalt, nickel, copper, zinc, and more specifically TiS2, ZrS2, RuO2, Co3O4, Mo6S8, V2O5, etc. can be used, but the present invention is not limited to this.
[0088] The shape of the positive electrode active material is not particularly limited, and may be a particle shape, such as spherical, elliptical, rectangular, etc. The average particle size of the positive electrode active material may be (but not limited to) in the range of 1 μm to 50 μm. The average particle size of the positive electrode active material may be obtained, for example, by measuring the particle size of the active material using a scanning electron microscope and calculating its average value.
[0089] The binder contained in the positive electrode is not particularly limited, and a fluorine-containing binder such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE) may be used.
[0090] The content of the binder is not particularly limited as long as it can fix the positive electrode active material, and may be in the range of 0 wt % to 10 wt % based on the entire positive electrode.
[0091] The positive electrode may further include a conductive material. The conductive materials are not particularly limited as long as they can improve the conductivity of the positive electrode, and examples thereof may include nickel powder, cobalt oxide, titanium oxide, and carbon. Examples of carbon may include any one or more selected from the group consisting of Ketjen black, acetylene black, furnace black, graphite, carbon fiber, and fullerene.
[0092] In this case, the content of the conductive material may be selected in consideration of other conditions of the battery such as the type of the conductive material, and may be, for example, in the range of 1 wt % to 10 wt % with respect to the entire positive electrode.
[0093] The preparation of the all-solid-state battery having the configuration described above is not particularly limited in the present invention, but can be performed by a known method.
[0094] For example, a solid electrolyte is placed between a positive electrode and a negative electrode, followed by compression molding to assemble a battery.
[0095] The assembled battery is placed in a case and sealed by heat pressing, etc. Laminated packaging made of aluminum, stainless steel, etc., and cylindrical or square metal containers are very suitable as outer packaging materials.
[0096] The battery of the present invention contains the lithium-tin-metal-sulfide type solid electrolyte proposed in the present invention as a component, thereby having excellent charge and discharge characteristics. Although the all-solid-state battery composed only of solid can prevent safety accidents such as explosion, it is the ultimate battery form with excellent safety However, all-solid-state batteries have not yet been widely used because they have not yet achieved high capacity and high power. The main reason for this is the material properties of the electrolyte.
[0097] By including the lithium-tin-metal-sulfide type compound proposed in the present invention as a component of the solid electrolyte, excellent battery characteristics can be ensured.
[0098] Hereinafter, preferred embodiments of the present invention and comparative examples are described. However, the following embodiments are merely preferred embodiments of the present invention, and the present invention is not limited to the following embodiments.
[0099] Example 1: Li 13 Sn2InS 12 Synthesis
[0100] In order to synthesize the Li 13 Sn2InS 12 (i.e. Li where M is In 4-x Sn 1-x M x S4 compound), Li2S, SnS2 and In2S3 were mixed in a molar ratio of 5:2:1. In this case, SnS2 was prepared by mixing Sn and S in a molar ratio of 1:2 and heat-treating at 400°C. A total of 5 g of the sample was sampled, and pellets were prepared by using CIP, and then the sample was sealed in a quartz tube while maintaining a vacuum, and fully heat-treated at 600°C for more than 20 hours to obtain Li 13 Sn2InS 12 .
[0101] Experimental Example 1: XRD Results
[0102] The solid electrolyte prepared in Example 1 was subjected to X-ray diffraction analysis (XRD) to confirm its crystallinity. The results are shown in Figure 5 middle.
[0103] like Figure 5As shown, it is determined that the solid electrolyte particles of Example 1 have a crystal structure similar to that of Li4SnS4, and part of the peaks are shifted due to indium (In) substitution.
[0104] Therefore, the all-solid-state battery of the present invention is safer and has a high energy density, and thus can be preferably used as a substitute for renewable energy or electric vehicle power sources.
Claims
1. A sulfide-type solid electrolyte, characterized in that: The sulfide-based solid electrolyte comprises Li 13 Sn2InS 12 A lithium-tin-metal-sulfide (LTMS) type compound represented by The sulfide-type solid electrolyte is used to form a solid electrolyte layer of an all-solid-state battery.
2. A method for preparing the sulfide-type solid electrolyte according to claim 1, characterized in that: The method comprises the following steps: i) mixing lithium sulfide, tin sulfide and a sulfide containing M, wherein M is In; and ii) subjecting the mixture to a heat treatment.
3. The method for preparing a sulfide-type solid electrolyte according to claim 2, characterized in that: The heat treatment is performed at 400° C. to 850° C. one or more times.
4. An all-solid-state battery comprising a positive electrode (cathode); a negative electrode (anode); and a solid electrolyte disposed therebetween, It is characterized in that The solid electrolyte is the sulfide-type solid electrolyte according to claim 1.