optical fiber

By using the inorganic oxide particle resin layer structure in the coating resin layer of the optical fiber and adjusting the Young's modulus and linear expansion coefficient, the problem of increased transmission loss of the optical fiber during lateral pressure is solved, and excellent lateral pressure characteristics and low temperature characteristics are achieved. , ensuring the performance stability of optical fiber at low temperatures.

CN113939755BActive Publication Date: 2024-10-01SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080042591.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-06-19
Filing Date
2020-06-10
Publication Date
2024-10-01
Estimated Expiration
2040-06-10

AI Technical Summary

Technical Problem

Existing optical fibers are prone to micro-bends during lateral pressure, resulting in increased transmission loss, and the transmission loss is large at low temperatures, making it difficult to meet excellent lateral pressure characteristics and loss control at low temperatures.

Method used

Using a resin layer structure containing inorganic oxide particles, through the combination of primary resin layer and secondary resin layer, the Young's modulus and linear expansion coefficient are adjusted to improve the lateral pressure characteristics of the optical fiber and reduce transmission loss at low temperatures. Specific measures include using a resin composition containing inorganic oxide particles such as hydrophobic silica in the coating resin layer of the optical fiber, and adjusting its dispersion and thickness in the resin layer to form excellent side pressure characteristics and low temperature characteristics.

Benefits of technology

It achieves a small increase in low-temperature transmission loss of the optical fiber under lateral pressure conditions, improves the lateral pressure characteristics and low-temperature characteristics of the optical fiber, and ensures the performance stability of the optical fiber after the thermal cycle test.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113939755B_ABST
    Figure CN113939755B_ABST
Patent Text Reader

Abstract

An optical fiber comprises: a glass fiber including a core and a cladding; a coating resin layer, the coating resin layer having a primary resin layer in contact with the glass fiber and coating the glass fiber; and a secondary resin layer coating the primary resin layer, the primary resin layer and the secondary resin layer being resin layers containing inorganic oxide particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an optical fiber.

[0002] This application claims the priority based on Japanese Patent Application No. 2019-114005 filed on June 19, 2019, and cites all the contents described in the Japanese Patent Application. Background Art

[0003] Generally, an optical fiber has a coating resin layer for protecting a glass fiber as a light transmission body. In order to reduce the increase in transmission loss caused by minute bending that occurs when a lateral pressure is applied to the optical fiber, the optical fiber is required to have excellent lateral pressure characteristics.

[0004] The coating resin layer can be formed by using an ultraviolet curable resin composition containing oligomers, monomers, photopolymerization initiators, etc. For example, in Patent Document 1, it is studied to improve the lateral pressure characteristics of the optical fiber by forming a resin layer using an ultraviolet curable resin composition containing a filler made of synthetic quartz as a raw material.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2014-219550 Summary of the invention

[0008] An optical fiber involved in one embodiment of the present disclosure comprises: a glass fiber including a core and a cladding; and a coating resin layer, the coating resin layer having: a primary resin layer in contact with the glass fiber and coating the glass fiber; and a secondary resin layer coating the primary resin layer, the primary resin layer and the secondary resin layer being resin layers containing inorganic oxide particles. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] [ Figure 1 ] Figure 1 This is a schematic cross-sectional view showing an example of the optical fiber according to the present embodiment. DETAILED DESCRIPTION

[0010] [Problems to be Solved by the Present Disclosure]

[0011] The coating resin layer usually includes a primary resin layer and a secondary resin layer. It is believed that the large difference in linear expansion coefficient between the resin composition forming the primary resin layer and the resin composition forming the secondary resin layer is one of the reasons for the generation of voids in the optical fiber. When the Young's modulus of the secondary resin layer is increased in order to improve the lateral pressure characteristics of the optical fiber, if the Young's modulus of the primary resin layer is low, voids are easily generated during a thermal cycle test. If voids are generated, the transmission loss of the optical fiber at low temperatures tends to increase.

[0012] An object of the present disclosure is to provide an optical fiber that is excellent in lateral pressure characteristics and has a small increase in transmission loss at low temperatures.

[0013] [Effects of the present disclosure]

[0014] According to the present disclosure, it is possible to provide an optical fiber that is excellent in lateral pressure characteristics and has a small increase in transmission loss at low temperatures.

[0015] [Description of Embodiments of the Present Disclosure]

[0016] First, the contents of the embodiments of the present disclosure are listed and described. One embodiment of the present disclosure relates to an optical fiber comprising: a glass fiber including a core and a cladding; and a coating resin layer, the coating resin layer comprising: a primary resin layer in contact with the glass fiber and coating the glass fiber; and a secondary resin layer coating the primary resin layer, the primary resin layer and the secondary resin layer being resin layers containing inorganic oxide particles.

[0017] By making the primary resin layer and the secondary resin layer contain inorganic oxide particles, the lateral pressure characteristics of the optical fiber can be improved and the increase in transmission loss at low temperature after a heat cycle test can be reduced.

[0018] The inorganic oxide particles may be at least one selected from the group consisting of silicon dioxide, zirconium dioxide, aluminum oxide, magnesium oxide, titanium oxide, tin oxide, and zinc oxide, from the viewpoint of facilitating adjustment of the Young's modulus of the coating resin layer.

[0019] The inorganic oxide particles are silicon dioxide, and the amount of silicon atoms contained in the coating resin layer may be 3 mass % or more and 22 mass % or less, because the inorganic oxide particles are excellent in dispersibility in the resin layer and the generation of voids is easily suppressed.

[0020] From the viewpoint of further reducing the increase in transmission loss at low temperatures, the Young's modulus of the primary resin layer may be 0.03 MPa or more and 0.7 MPa or less at 23°C.

[0021] From the viewpoint of further improving the lateral pressure characteristics of the optical fiber, the Young's modulus of the secondary resin layer at 23° C. may be greater than or equal to 1300 MPa and less than or equal to 2750 MPa.

[0022] [Details of the embodiments of the present disclosure]

[0023] Specific examples of the resin composition and optical fiber involved in the embodiments of the present disclosure are described with reference to the accompanying drawings as needed. It should be noted that the present invention is not limited to these examples, but is represented by the claims, and is intended to include all changes within the meaning and scope equivalent to the claims. In the following description, the same elements in the description of the drawings are marked with the same symbols, and repeated descriptions are omitted.

[0024] <Optical fiber>

[0025] Figure 1 The optical fiber 10 is a schematic cross-sectional view showing an example of the optical fiber according to the present embodiment. The optical fiber 10 includes a glass fiber 13 including a core 11 and a cladding 12 , and a coating resin layer 16 including a primary resin layer 14 and a secondary resin layer 15 provided on the outer periphery of the glass fiber 13 .

[0026] The cladding 12 surrounds the core 11. The core 11 and the cladding 12 mainly include glass such as quartz glass. For example, the core 11 can use quartz glass doped with germanium or pure quartz glass, and the cladding 12 can use pure quartz glass or quartz glass doped with fluorine.

[0027] exist Figure 1 For example, the outer diameter (D2) of the glass fiber 13 is about 100 μm to 125 μm, and the diameter (D1) of the core 11 constituting the glass fiber 13 is about 7 μm to 15 μm. The thickness of the coating resin layer 16 is generally about 22 μm to 70 μm. The thickness of each layer of the primary resin layer 14 and the secondary resin layer 15 can be about 5 μm to 50 μm.

[0028] When the outer diameter (D2) of the glass fiber 13 is about 125 μm and the thickness of the coating resin layer 16 is 60 μm to 70 μm, the thickness of each layer of the primary resin layer 14 and the secondary resin layer 15 can be about 10 μm to 50 μm, for example, the thickness of the primary resin layer 14 can be 35 μm, and the thickness of the secondary resin layer 15 can be 25 μm. The outer diameter of the optical fiber 10 can be about 245 μm to 265 μm.

[0029] When the outer diameter (D2) of the glass fiber 13 is about 125 μm and the thickness of the coating resin layer 16 is 27 μm to 48 μm, the thickness of each layer of the primary resin layer 14 and the secondary resin layer 15 can be about 10 μm to 38 μm, for example, the thickness of the primary resin layer 14 can be 25 μm, and the thickness of the secondary resin layer 15 can be 10 μm. The outer diameter of the optical fiber 10 can be about 179 μm to 221 μm.

[0030] When the outer diameter (D2) of the glass fiber 13 is about 100 μm and the thickness of the coating resin layer 16 is 22 μm to 37 μm, the thickness of each of the primary resin layer 14 and the secondary resin layer 15 can be about 5 μm to 32 μm, for example, the thickness of the primary resin layer 14 can be 25 μm, and the thickness of the secondary resin layer 15 can be 10 μm. The outer diameter of the optical fiber 10 can be about 144 μm to 174 μm.

[0031] (Secondary resin layer)

[0032] From the viewpoint of reducing the linear expansion coefficient of the secondary resin layer and improving the lateral pressure characteristics and low temperature characteristics of the optical fiber, the secondary resin layer 15 contains inorganic oxide particles. The secondary resin layer 15 may be formed by curing a resin composition containing a base resin and hydrophobic inorganic oxide particles, wherein the base resin contains an oligomer containing urethane (meth) acrylate, a monomer, and a photopolymerization initiator. That is, the secondary resin layer 15 may contain a cured product of a resin composition containing a base resin and hydrophobic inorganic oxide particles, wherein the base resin contains an oligomer containing urethane (meth) acrylate, a monomer, and a photopolymerization initiator.

[0033] The inorganic oxide particles involved in the present embodiment are subjected to a hydrophobic treatment on their surface. The hydrophobic treatment involved in the present embodiment refers to the introduction of a hydrophobic group on the surface of the inorganic oxide particles. The inorganic oxide particles introduced with a hydrophobic group have excellent dispersibility in the resin composition. The hydrophobic group can be a reactive group such as (meth) acryloyl, vinyl, or a non-reactive group such as an aliphatic hydrocarbon group (such as an alkyl group) or an aromatic hydrocarbon group (such as a phenyl group). When the inorganic oxide particles have a reactive group, a resin layer with a high Young's modulus is easily formed.

[0034] The inorganic oxide particles involved in the present embodiment are dispersed in a dispersion medium. By using inorganic oxide particles dispersed in a dispersion medium, the inorganic oxide particles can be uniformly dispersed in the resin composition, thereby improving the storage stability of the resin composition. As a dispersion medium, as long as it does not hinder the curing of the resin composition, it is not particularly limited. The dispersion medium can be reactive or non-reactive.

[0035] As a reactive dispersion medium, monomers such as (meth)acryloyl compounds and epoxy compounds can be used. As (meth)acryloyl compounds, for example, 1,6-hexanediol di(meth)acrylate, EO-modified bisphenol A di(meth)acrylate, polyethylene glycol di(meth)acrylate, PO-modified bisphenol A di(meth)acrylate, polypropylene glycol di(meth)acrylate, and polytetramethylene glycol di(meth)acrylate can be cited. As (meth)acryloyl compounds, compounds exemplified by the above-mentioned monomers can be used.

[0036] As a non-reactive dispersion medium, a ketone solvent such as methyl ethyl ketone (MEK), an alcohol solvent such as methanol (MeOH), or an ester solvent such as propylene glycol monomethyl ether acetate (PGMEA) can be used. When a non-reactive dispersion medium is used, the base resin and the inorganic oxide particles dispersed in the dispersion medium are mixed, and then a part of the dispersion medium is removed to prepare the resin composition.

[0037] The inorganic oxide particles dispersed in the dispersion medium also exist in a state dispersed in the resin layer after the resin composition is cured. When a reactive dispersion medium is used, the inorganic oxide particles are mixed in the resin composition together with the dispersion medium, and are incorporated into the resin layer while maintaining a dispersed state. When a non-reactive dispersion medium is used, at least a portion of the dispersion medium evaporates from the resin composition and disappears, but the inorganic oxide particles are still retained in the resin composition in a dispersed state, and also exist in a dispersed state in the cured resin layer. When the inorganic oxide particles present in the resin layer are observed using an electron microscope, they are observed in a state of primary particle dispersion.

[0038] The inorganic oxide particles are preferably at least one selected from the group consisting of silica, zirconium dioxide, alumina, magnesium oxide, titanium oxide, tin oxide, and zinc oxide, because they are excellent in dispersibility in the resin layer and can easily form a tough resin layer. Hydrophobic silica particles are more preferably used as the inorganic oxide particles involved in this embodiment because they are low in price, easy to surface treat, have ultraviolet transmittance, and can easily impart a moderate hardness to the resin layer.

[0039] From the viewpoint of improving the Young's modulus of the resin layer, the average primary particle size of the inorganic oxide particles is preferably 5nm or more and 800nm, more preferably 10nm or more and 700nm or less, and more preferably 10nm or more and 650nm or less. The average primary particle size (for example) can be measured by image analysis of electron microscope photographs, light scattering method, BET method, etc. When the particle size of the primary particle is relatively small, the dispersion medium of the primary particles of the inorganic oxide appears to be transparent under visual observation. When the particle size of the primary particle is relatively large (more than 40nm), the dispersion medium of the primary particles appears to be turbid, but no precipitate is observed.

[0040] Based on the total amount of the resin composition, the content of the inorganic oxide particles is preferably 1% by mass or more and 65% by mass or less, more preferably 10% by mass or more and 60% by mass or less, and further preferably 15% by mass or more and 60% by mass or less. If the content of the inorganic oxide particles is 1% by mass or more, it is easy to form a resin layer with excellent lateral pressure characteristics. If the content of the inorganic oxide particles is 65% by mass or less, it is easy to improve the coating properties of the resin composition.

[0041] The average primary particle size of the inorganic oxide particles contained in the secondary resin layer may be 5 nm to 200 nm, 8 nm to 100 nm, 9 nm to 50 nm, or 10 nm to 30 nm. The content of the inorganic oxide particles contained in the secondary resin layer may be 1 mass % to 65 mass %, 10 mass % to 60 mass %, or 15 mass % to 60 mass %, based on the total amount of the secondary resin layer.

[0042] As the urethane (meth)acrylate, an oligomer obtained by reacting a polyol compound, a polyisocyanate compound, and a hydroxyl group-containing (meth)acrylate compound can be used.

[0043] As the polyol compound, for example, polytetramethylene glycol, polypropylene glycol, and bisphenol A-ethylene oxide addition diol can be listed. The number average molecular weight of the polyol compound can be 400 to 4000, 400 to 2000, or 400 to 1000. As the polyisocyanate compound, for example, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, isophorone diisocyanate and dicyclohexylmethane 4,4'-diisocyanate can be listed. As the hydroxyl-containing (meth) acrylate compound, for example, 2-hydroxyethyl (meth) acrylate, 2-hydroxybutyl (meth) acrylate, 1,6-hexanediol mono (meth) acrylate, pentaerythritol tri (meth) acrylate, 2-hydroxypropyl (meth) acrylate and tripropylene glycol mono (meth) acrylate can be listed.

[0044] As a catalyst for synthesizing urethane (meth) acrylate, an organic tin compound is generally used. Examples of the organic tin compound include dibutyltin dilaurate, dibutyltin diacetate, dibutyltin maleate, dibutyltin bis(2-ethylhexyl thioglycolate), dibutyltin bis(isooctyl thioglycolate), and dibutyltin oxide. From the perspective of availability or catalyst performance, dibutyltin dilaurate or dibutyltin diacetate is preferably used as the catalyst.

[0045] When synthesizing urethane (meth)acrylate, a lower alcohol having a carbon number of 5 or less may be used. Examples of the lower alcohol include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-2-propanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 3-methyl-1-butanol, 2-methyl-2-butanol, 3-methyl-2-butanol, and 2,2-dimethyl-1-propanol.

[0046] The oligomer may further contain epoxy (meth)acrylate. As epoxy (meth)acrylate, an oligomer obtained by reacting a compound having a (meth)acryloyl group with an epoxy resin having two or more glycidyl groups can be used.

[0047] As the monomer, at least one selected from the group consisting of a monofunctional monomer having one polymerizable group and a polyfunctional monomer having two or more polymerizable groups can be used. Two or more monomers may be used in combination.

[0048] Examples of the monofunctional monomer include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, isopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, 3-octyl (meth)acrylate, 1,2-dole-3-nitropropene ... -phenoxybenzyl ester, phenoxydiethylene glycol acrylate, phenoxypolyethylene glycol acrylate, 4-tert-butylcyclohexanol acrylate, tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentyl (meth)acrylate, nonylphenol polyethylene glycol (meth)acrylate, nonylphenoxypolyethylene glycol (meth)acrylate, isobornyl (meth)acrylate and other (meth)acrylate monomers; (meth)acrylic acid, (meth)acrylic acid dimer, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, ω-carboxy-polycaprolactone (meth) carboxyl-containing monomers such as N-(meth)acryloylmorpholine, N-vinylpyrrolidone, N-vinylcaprolactam, N-acryloylpiperidine, N-methacryloylpiperidine, N-(meth)acryloylpyrrolidine, 3-(3-pyridyl)propyl(meth)acrylate, cyclotrimethylolpropaneformalacrylate, etc.; maleimide monomers such as maleimide, N-cyclohexylmaleimide, and N-phenylmaleimide; (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-methyl(meth)acrylamide Amide monomers such as acrylamide, N-butyl (meth)acrylamide, N-butyl (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, and N-methylolpropane (meth)acrylamide; aminoalkyl (meth)acrylate monomers such as aminoethyl (meth)acrylate, aminopropyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and tert-butylaminoethyl (meth)acrylate; succinimide monomers such as N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyoctamethylenesuccinimide.

[0049] Examples of the polyfunctional monomer include ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, di(meth)acrylate of an alkylene oxide adduct of bisphenol A, tetraethylene glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, and 1,4-butanediol di(meth)acrylate. 、1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, 1,14-tetradecanediol di(meth)acrylate, 1,16-hexadecanediol di(meth)acrylate, 1,20-eicosandiol di(meth)acrylate, isoprene diol di(meth)acrylate, 3-ethyl-1,8-octanediol di(meth)acrylate, E of bisphenol A Monomers having two polymerizable groups, such as O addition di(meth)acrylate; and monomers having three or more polymerizable groups, such as trimethylolpropane tri(meth)acrylate, trimethyloloctane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, trimethylolpropane polypropoxy tri(meth)acrylate, trimethylolpropane polyethoxy polypropoxy tri(meth)acrylate, tri[(meth)acryloyloxyethyl]isocyanurate, pentaerythritol tri(meth)acrylate, pentaerythritol polyethoxy tetra(meth)acrylate, pentaerythritol polypropoxy tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate and caprolactone-modified tri[(meth)acryloyloxyethyl]isocyanurate.

[0050] From the viewpoint of increasing the Young's modulus of the resin layer, the monomer preferably contains a polyfunctional monomer, and more preferably contains a monomer having two polymerizable groups.

[0051] As a photopolymerization initiator, it can be appropriately selected from known free radical photopolymerization initiators and used. As a photopolymerization initiator, for example, 1-hydroxycyclohexyl phenyl ketone (Omnirad 184, manufactured by IGM Resins), 2,2-dimethoxy-2-phenylacetophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropane-1-one, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinyl-propane-1-one (Omnirad 907, manufactured by IGM Resins), 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Omnirad TPO, manufactured by IGM Resins) and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, manufactured by IGM Resins).

[0052] The resin composition may further contain a silane coupling agent, a leveling agent, a defoaming agent, an antioxidant, a sensitizer, and the like.

[0053] The silane coupling agent is not particularly limited as long as it does not hinder the curing of the resin composition. Examples of the silane coupling agent include tetramethyl silicate, tetraethyl silicate, mercaptopropyl trimethoxysilane, vinyl trichlorosilane, vinyl triethoxysilane, vinyl tri(β-methoxy-ethoxy)silane, β-(3,4-epoxycyclohexyl)-ethyl trimethoxysilane, dimethoxydimethylsilane, diethoxydimethylsilane, 3-acryloxypropyl trimethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-glycidoxypropyl methyl diethoxysilane, γ-methacryloxypropyl trimethoxysilane, N-(β-aminoethyl)silane, and the like.

[0047] The invention also includes the following:

[0048] N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethyldimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-chloropropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, bis-[3-(triethoxysilyl)propyl]tetrasulfide, bis-[3-(triethoxysilyl)propyl]disulfide, γ-trimethoxysilylpropyldimethylthiocarbamoyltetrasulfide and γ-trimethoxysilylpropylbenzothiazolyltetrasulfide.

[0054] The Young's modulus of the secondary resin layer is preferably 1300 MPa to 2750 MPa at 23° C., more preferably 1400 MPa to 2700 MPa, and further preferably 1500 MPa to 2700 MPa. If the Young's modulus of the secondary resin layer is 1300 MPa or more, the lateral pressure characteristics are easily improved, and if it is 2750 MPa or less, appropriate toughness can be imparted to the secondary resin layer, thereby easily improving the low-temperature characteristics.

[0055] (Primary resin layer)

[0056] From the viewpoint of reducing the linear expansion coefficient of the primary resin layer, improving the lateral pressure characteristics and low temperature characteristics of the optical fiber, the primary resin layer 14 contains inorganic oxide particles. The primary resin layer 14 can be formed by curing a resin composition containing a base resin and inorganic oxide particles, wherein the base resin contains an oligomer containing carbamate (meth) acrylate, a monomer, a photopolymerization initiator, and a silane coupling agent. As carbamate (meth) acrylate, monomer, photopolymerization initiator, silane coupling agent, and inorganic oxide particles, it can be appropriately selected from the compounds exemplified in the secondary resin layer. However, the resin composition forming the primary resin layer has a different composition from the base resin forming the secondary resin layer.

[0057] Based on the total amount of the resin composition, the content of the inorganic oxide particles is preferably 1% by mass or more and 45% by mass or less, more preferably 2% by mass or more and 40% by mass or less, and further preferably 3% by mass or more and 30% by mass or less. If the content of the inorganic oxide particles is 1% by mass or more, a tough resin layer is easily formed. If the content of the inorganic oxide particles is 45% by mass or less, a resin layer with a low Young's modulus can be formed.

[0058] The average primary particle size of the inorganic oxide particles contained in the primary resin layer may be 5 nm to 200 nm, 10 nm to 100 nm, 15 nm to 80 nm, or 20 nm to 70 nm. Based on the total amount of the primary resin layer, the content of the inorganic oxide particles contained in the primary resin layer may be 1 mass % to 45 mass %, 2 mass % to 40 mass %, or 3 mass % to 30 mass %.

[0059] From the viewpoint of suppressing the generation of voids in the optical fiber, the Young's modulus of the primary resin layer at 23°C±2°C is preferably 0.03 MPa to 0.7 MPa, more preferably 0.04 MPa to 0.65 MPa, and even more preferably 0.05 MPa to 0.6 MPa.

[0060] The inorganic oxide particles contained in the primary resin layer and the secondary resin layer are preferably hydrophobic silica particles because they are excellent in dispersibility in the resin layer and are easy to suppress the occurrence of pores. Based on the total amount of the coating resin layer, the amount of silicon atoms (Si) contained in the coating resin layer is preferably 3% by mass or more and 22% by mass or less, more preferably 4% by mass or more and 20% by mass or less, and further preferably 4% by mass or more and 19% by mass or less. If the amount of Si is 3% by mass or more, it is easy to improve the lateral pressure characteristics of the optical fiber. If the amount of Si is 22% by mass or less, it is easy to improve the low-temperature characteristics of the optical fiber. The amount of Si can be measured by ICP-AES.

[0061] Example

[0062] Hereinafter, evaluation test results using examples and comparative examples according to the present disclosure are shown, and the present disclosure is described in more detail. It should be noted that the present invention is not limited to these examples.

[0063] [Resin composition for primary resin layer]

[0064] (Oligomer)

[0065] As oligomers, urethane acrylates a1, a2, and a3 obtained by reacting polypropylene glycol having a molecular weight of 4000, isophorone diisocyanate, hydroxyethyl acrylate, and methanol were prepared. In the urethane acrylates a1, a2, and a3, the ratio of the oligomer having acryloyl groups at both ends to the oligomer having acryloyl groups at one end was adjusted by changing the mixing ratio of hydroxyethyl acrylate and methanol.

[0066] (Inorganic oxide particles)

[0067] As the inorganic oxide particles, hydrophobic silica particles having a methacryloyl group and an average primary particle size of 20 to 60 nm were prepared and dispersed in MEK.

[0068] (Resin composition)

[0069] A base resin was prepared by mixing 75 parts by mass of urethane acrylate a1, a2 or a3, 12 parts by mass of nonylphenoxy polyethylene glycol acrylate, 6 parts by mass of N-vinyl caprolactam, 2 parts by mass of 1,6-hexanediol diacrylate, 1 part by mass of 2,4,6-trimethylbenzoyldiphenylphosphine oxide and 1 part by mass of 3-mercaptopropyltrimethoxysilane. Next, after mixing the base resin with silica particles, most of MEK as a dispersion medium was removed under reduced pressure to prepare a resin composition for a primary resin layer.

[0070] [Resin composition for secondary resin layer]

[0071] (Oligomer)

[0072] As oligomers, urethane acrylate (UA) and epoxy acrylate (EA) obtained by reacting polypropylene glycol having a molecular weight of 600, 2,4-toluene diisocyanate, and hydroxyethyl acrylate were prepared.

[0073] (Inorganic oxide particles)

[0074] As inorganic oxide particles, a silica sol containing hydrophobic silica particles having a methacryloyl group and having an average primary particle size of 10 to 20 nm dispersed in MEK was prepared.

[0075] (Resin composition)

[0076] First, 20 parts by mass of UA, 20 parts by mass of EA, 25 parts by mass of isobornyl acrylate, 20 parts by mass of 2-phenoxyethyl acrylate, 15 parts by mass of tripropylene glycol diacrylate, 0.5 parts by mass of 1-hydroxycyclohexyl phenyl ketone, and 0.5 parts by mass of 2,4,6-trimethylbenzoyldiphenylphosphine oxide were mixed to prepare a base resin. Next, after mixing the base resin with silica sol, most of MEK as a dispersion medium was removed under reduced pressure to prepare resin compositions for the secondary resin layers.

[0077] In Table 1 and Table 2, the numerical value of the silica particles is the content based on the total amount of the resin composition. It should be noted that the total amount of the resin composition can be considered to be the same as the total amount of the cured product of the resin composition.

[0078] [Production of optical fiber]

[0079] An optical fiber was produced by forming a primary resin layer with a thickness of 35 μm on the outer periphery of a glass fiber having a core and a cladding and having a diameter of 125 μm using a resin composition for a primary resin layer, and further forming a secondary resin layer with a thickness of 25 μm on the outer periphery using a resin composition for a secondary resin layer. The line speed was set to 1500 m / min.

[0080] (Young's modulus of primary resin layer)

[0081] The Young's modulus of the primary resin layer is measured by the Pullout Modulus (POM) method at 23°C. Two locations of the optical fiber are fixed by two chuck devices, and the coating resin layer (primary resin layer and secondary resin layer) portion between the two chuck devices is removed. Then, one chuck device is fixed, and the other chuck device is slowly moved in the opposite direction of the fixed chuck device. If the length of the portion of the optical fiber clamped by the moving chuck device is set to L, the movement amount of the chuck is set to Z, the outer diameter of the primary resin layer is set to Dp, the outer diameter of the glass fiber is set to Df, the Poisson's ratio of the primary resin layer is set to n, and the load when the chuck device is moved is set to W, the Young's modulus of the primary resin layer is calculated by the following formula.

[0082] Young's modulus (MPa) = ((1+n)W / πLZ) × ln(Dp / Df)

[0083] (Young's modulus of secondary resin layer)

[0084] The Young's modulus of the secondary resin layer is determined from the 2.5% secant value by conducting a tensile test (distance between marking lines: 25 mm) at 23±2°C and 50±10% RH using a tubular coating resin layer (length: 50 mm or more) obtained by extracting a glass fiber from an optical fiber.

[0085] (Si content of coating resin layer)

[0086] By using ICP-AES, the amount of silicon atoms (Si) contained in the coating resin layer was calculated according to the following procedure. As a pretreatment method for quantitative analysis of Si, an alkali fusion method was used.

[0087] About 0.1 to 0.2 g of the coated resin layer was heat treated at 800 ° C for 60 minutes to ash it. 3 g of sodium carbonate and 0.5 g of boric acid were added to 0.1 g of ash, alkali-melted at 1000 ° C for 30 minutes, and then 10 mL of concentrated hydrochloric acid was added, and ultrapure water was further added to obtain a sample solution fixed to 100 mL. The sample solution was diluted 10 times with ultrapure water, and the amount of Si was measured at a wavelength of 212.412 nm using Thermo Fisher SCIENTIFIC (model: Icap 6500 Duo).

[0088] (Thermal cycle test)

[0089] For the optical fiber heated between -40°C and 23°C (maintained at each temperature for 1 hour, transition time of 60 minutes) for 50 cycles, the transmission characteristics of the signal light of wavelength 1550nm were measured under the temperature conditions of 23°C and -40°C, and the transmission losses at 23°C and -40°C were obtained. The case where the difference in transmission loss obtained by subtracting the transmission loss at 23°C from the transmission loss at -40°C was less than 0dB / km (the transmission loss at -40°C was small) was evaluated as "A", the case where it was greater than 0dB / km and less than 0.01dB / km was evaluated as "B", and the case where it was greater than 0.01dB / km was evaluated as "C".

[0090] (Side pressure characteristics)

[0091] The transmission loss of light with a wavelength of 1550 nm when the optical fiber is wound in a single layer on a winding reel with a diameter of 280 mm and a surface covered with sandpaper is measured by the OTDR (Optical Time Domain Reflectometer) method. In addition, the transmission loss of light with a wavelength of 1550 nm when the optical fiber is wound in a single layer on a winding reel with a diameter of 280 mm without sandpaper is measured by the OTDR method. The measured transmission loss difference is calculated, and the case where the transmission loss difference is less than 0.6 dB / km is evaluated as the lateral pressure characteristic "A", and the case where the transmission loss difference exceeds 0.6 dB / km is evaluated as the lateral pressure characteristic "B".

[0092] [Table 1]

[0093]

[0094] [Table 2]

[0095] Comparative Example 1 2 3 4 Primary resin layer Oligomer a2 a2 a2 a2 Silica particles (mass %) - 50 - - Young's modulus (MPa) 0.2 0.8 0.2 0.2 Secondary resin layer Silica particles (mass %) 20 - 65 - Young's modulus (MPa) 1800 1600 2800 1100 Si content (mass %) 5.1 12.8 16.7 <![CDATA[<0.05 * ]]> Thermal Cycle Test C A C A Lateral pressure resistance A B B B

[0096] *Below detection limit

[0097] Explanation of symbols

[0098] 10. Fiber Optics

[0099] 11 Core

[0100] 12 Cladding

[0101] 13 Fiberglass

[0102] 14 Primary resin layer

[0103] 15 Secondary resin layer

[0104] 16 Coating resin layer

Claims

1. An optical fiber, comprising: A glass fiber comprising a core and a cladding; and a coating resin layer, The coating resin layer comprises: a primary resin layer in contact with the glass fiber and coating the glass fiber; and a secondary resin layer coating the primary resin layer. The primary resin layer and the secondary resin layer are resin layers containing inorganic oxide particles, The average primary particle size of the inorganic oxide particles contained in the primary resin layer is 20 nm or more and 70 nm or less, The average primary particle size of the inorganic oxide particles contained in the secondary resin layer is 10 nm or more and 30 nm or less.

2. The optical fiber according to claim 1, wherein The inorganic oxide particles are at least one selected from the group consisting of silicon dioxide, zirconium dioxide, aluminum oxide, magnesium oxide, titanium oxide, tin oxide, and zinc oxide.

3. The optical fiber according to claim 2, wherein: The inorganic oxide particles are silicon dioxide, and the amount of silicon atoms contained in the coating resin layer is 3 mass % or more and 22 mass % or less.

4. The optical fiber according to any one of claims 1 to 3, wherein The Young's modulus of the primary resin layer is 0.03 MPa or more and 0.7 MPa or less at 23°C.

5. The optical fiber according to any one of claims 1 to 3, wherein The Young's modulus of the secondary resin layer at 23° C. is 1300 MPa to 2750 MPa.