Preparation method of environmentally friendly modified polyurethane vinyl carbon fiber sizing agent
Through the preparation of modified polyurethane vinyl sizing agent, the problems of fluffing and breakage of carbon fiber during processing are solved, the bonding effect with vinyl resin is improved, the mechanical properties and stability of composite materials are significantly improved, and environmental protection is achieved Preparation of aqueous polymer emulsions.
Patent Information
- Application Number
- CN202111168553.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-09-30
AI Technical Summary
Carbon fiber is prone to fluffing and breaking during production and processing, which affects its mechanical properties. The combination with different types of resins is not effective, resulting in insufficient toughness and chemical stability of the composite material.
The preparation method of modified polyurethane vinyl sizing agent is adopted, through the reaction of polyethylene glycol and isocyanate monomer, graft polymerization and adding of epoxy resin and acrylate compound containing carbon-carbon double bonds to form an unsaturated carbon-carbon double bond. Bonded sizing agent, and an environmentally friendly water-based polymer emulsion is prepared through inverse emulsification technology for carbon fiber surface treatment.
It improves the wear resistance and bundling of carbon fiber, enhances the interface force between carbon fiber and vinyl resin, significantly improves the comprehensive mechanical and mechanical properties of carbon fiber reinforced vinyl composite materials, and achieves small average particle size and stable dilution. Water-based polymer emulsion with good properties.
Smart Images

Figure BDA0003290732240000081
Abstract
Description
Technical Field
[0001] The invention relates to a preparation technology of a modified polyurethane vinyl sizing agent aqueous polymer emulsion, which is mainly suitable for the application of carbon fiber reinforced vinyl resin composite materials. Background Art
[0002] Carbon fiber is an inorganic fiber material with a carbon content of more than 90%. It has the advantages of high strength, high specific modulus, light weight, good chemical stability, and low thermal expansion coefficient. It is widely used in aerospace, wind power generation, rail transportation, ships, automobiles and other fields. However, carbon fiber is a brittle material, which is prone to fluffing and breaking during the production and processing process. Reducing the mechanical properties of carbon fiber products will also bring greater risks to production. Therefore, in order to solve the above problems, one of the most commonly used methods is to sizing the surface of the carbon fiber, wrapping a layer of high molecular polymer on the surface of the carbon fiber to reduce the fluffing and breaking of the carbon fiber, and improve the wear resistance and bundling of the carbon fiber. At the same time, the sizing agent after sizing, as a binder, can better infiltrate and bond with the matrix resin to improve the overall mechanical properties of the composite material.
[0003] Commonly used resin matrices in composite materials include epoxy resin, unsaturated polyester resin, vinyl resin, etc. Epoxy resin has excellent heat resistance and stability, but due to its special molecular structure, the toughness of the composite material is poor. Vinyl resin is a thermosetting resin prepared by unsaturated carboxylic acid and epoxy resin in styrene. Vinyl resin not only has the outstanding mechanical properties of epoxy resin but also has the good mechanical processing properties of unsaturated polyester resin, has excellent chemical stability and good water resistance, and is one of the resins with broad application prospects. Since carbon fiber must be combined with different types of resins to prepare composite materials, according to the principle of like dissolves like, different resin matrices must select corresponding sizing agents. In order to have a strong connection between carbon fiber and vinyl resin, the present invention prepares a modified polyurethane vinyl carbon fiber sizing agent that has a strong connection with vinyl resin. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a modified polyurethane vinyl carbon fiber sizing agent to obtain an environmentally friendly aqueous polymer emulsion with a small average particle size and good dilution stability. The method is characterized in that the modified polyurethane vinyl carbon fiber sizing agent is prepared from two parts, the first part is a main sizing material of a synthetic modified polyurethane vinyl carbon fiber sizing agent, and the second part is a modified polyurethane vinyl carbon fiber sizing agent prepared by inverse emulsification.
[0005] The object of the present invention is to provide a method for preparing a modified polyurethane vinyl carbon fiber sizing agent, which is characterized in that the modified polyurethane vinyl carbon fiber sizing agent is prepared from two parts: the first part is a main sizing material of a synthetic modified polyurethane vinyl sizing agent; and the second part is a modified polyurethane vinyl carbon fiber sizing agent prepared by inverse emulsification.
[0006] Preferably, the modified polyurethane vinyl main slurry synthesis steps are as follows:
[0007] Step 1: In a system containing an organic solvent, firstly, at a relatively low temperature (40-55° C.), polyethylene glycol reacts with an isocyanate monomer for 1-3 hours;
[0008] Step 2: Add epoxy resin and raise the temperature to a higher temperature (70-95°C) to further carry out graft polymerization reaction for 1.5-4 hours;
[0009] Step 3: Add an acrylic acid ester compound containing a carbon-carbon double bond at a relatively high temperature (70-95° C.) and continue the graft polymerization reaction for 1-2.5 hours;
[0010] Step 4: adding the end-capped compound allyl polyether to carry out end-capping termination polymerization reaction, the reaction time is 1-2 hours;
[0011] Step 5: collecting the organic solvent by distillation under reduced pressure to obtain a main slurry of a modified polyurethane vinyl sizing agent.
[0012] Preferably, the organic solvent is selected from one or more ketone organic solvents selected from acetone, butanone, cyclohexanone and isophorone.
[0013] Preferably, the molecular weight of the polyethylene glycol includes but is not limited to 400, 800, 1000, 2000, 3000, 4000, and 6000.
[0014] Preferably, the isocyanate monomers include but are not limited to diphenylmethane diisocyanate, toluene diisocyanate, phenyl diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, lysine diisocyanate, dicyclohexylmethane diisocyanate, and isocyanate trimers.
[0015] Preferably, the epoxy resin includes but is not limited to bisphenol A epoxy resin, bisphenol F epoxy resin, and hydrogenated bisphenol A epoxy resin.
[0016] Preferably, the acrylic acid ester compound containing a carbon-carbon double bond includes, but is not limited to, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, and hydroxymethyl acrylamide.
[0017] Preferably, in the allyl polyether, the molecular weight of the allyl polyether includes but is not limited to 400, 1000, 2400, 3000, and 4000.
[0018] Preferably, the steps of obtaining the modified polyurethane vinyl carbon fiber sizing agent by inverse emulsification are as follows:
[0019] Step 6: Prepare the raw materials according to the following components: 2-3 parts by weight of epoxy resin (epoxy resin includes but is not limited to bisphenol A epoxy resin, bisphenol F epoxy resin, hydrogenated bisphenol A epoxy resin, etc.), 3-5 parts by weight of the modified polyurethane vinyl sizing agent main slurry, and 5-20 parts by weight of deionized water;
[0020] Step 7: Melt the epoxy resin and sizing agent main slurry in step 6 in an oven, and then mix and stir evenly;
[0021] Step 8: preheat the deionized water in step 6 to 60°C in advance;
[0022] Step nine: disperse the mixed material in step seven by a high-speed shear disperser at a shear stirring rate of 1500-6000 rpm, slowly drop the preheated water prepared in step eight into the high-speed dispersed material, perform phase transition emulsification for 2-3 hours, then cool to room temperature, cool and filter the material to obtain a modified polyurethane vinyl carbon fiber sizing agent.
[0023] In the present invention, the method for preparing the modified polyurethane vinyl carbon fiber sizing agent is provided, and the prepared carbon fiber sizing agent is an environmentally friendly water-soluble polymer emulsion, which is conducive to the carbon fiber sizing process operation; and the molecular structure of the sizing agent contains a large number of unsaturated carbon-carbon double bonds, which can participate in the curing reaction of the vinyl resin, and can significantly improve the interfacial force between the carbon fiber and the vinyl resin, realize the strong chemical connection of the interface layer, and is conducive to improving the comprehensive mechanical properties of the carbon fiber reinforced vinyl composite material. Through the present invention, an environmentally friendly water-based polymer emulsion with a small average particle size and good dilution stability is obtained. DETAILED DESCRIPTION
[0024] The present invention is specifically described below through examples. It is necessary to point out that the following examples cannot be understood as limiting the scope of protection of the present invention. If a person skilled in the art makes some non-essential improvements and adjustments to the present invention based on the above invention content, they still fall within the scope of the present invention.
[0025] In the present invention, the main slurry synthesis steps of the modified polyurethane vinyl sizing agent are as follows:
[0026] Step 1: In a system containing an organic solvent (the organic solvent includes but is not limited to ketone organic solvents such as acetone, butanone, cyclohexanone, isophorone, etc.), first at a relatively low temperature (40-55° C.), polyethylene glycol (molecular weight includes but is not limited to 400, 800, 1000, 2000, 3000, 4000, 6000, etc.) and an isocyanate monomer (isocyanate monomer includes but is not limited to diphenylmethane diisocyanate, toluene diisocyanate, phenyl diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, lysine diisocyanate, dicyclohexylmethane diisocyanate, isocyanate trimer, etc.) reacts for 1-3 hours;
[0027] Step 2: Then, add epoxy resin (epoxy resin includes but is not limited to bisphenol A epoxy resin, bisphenol F epoxy resin, hydrogenated bisphenol A epoxy resin, etc.), increase the temperature to a higher temperature (70-95° C.), and further carry out graft polymerization reaction for 1.5-4 hours;
[0028] Step 3: Then, at a relatively high temperature (70-95° C.), add an acrylic acid ester compound containing a carbon-carbon double bond (acrylic acid ester compounds include but are not limited to hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxymethyl acrylamide, etc.), and continue the graft polymerization reaction for 1-2.5 hours;
[0029] Step 4: Then, add the end-capped compound allyl polyether (the molecular weight of allyl polyether includes but is not limited to 400, 1000, 2400, 3000, 4000, etc.) to carry out end-capping termination polymerization reaction, and the reaction time is 1-2 hours;
[0030] Step 5: Finally, the organic solvent is collected by reduced pressure distillation to obtain a main slurry of a modified polyurethane vinyl sizing agent.
[0031] In the present invention, the steps of obtaining the modified polyurethane vinyl carbon fiber sizing agent by inversion emulsification are as follows:
[0032] Step 6: Prepare the raw materials according to the following components: 2-3 parts by weight of epoxy resin (epoxy resin includes but is not limited to bisphenol A epoxy resin, bisphenol F epoxy resin, hydrogenated bisphenol A epoxy resin, etc.), 3-5 parts by weight of the modified polyurethane vinyl sizing agent main slurry synthesized according to claim 2, and 5-20 parts by weight of deionized water;
[0033] Step 7: Melt the epoxy resin and sizing agent main slurry in step 6 in an oven, and then mix and stir evenly;
[0034] Step 8: preheat the deionized water in step 6 to 60°C in advance;
[0035] Step nine: disperse the mixed material in step seven by a high-speed shear disperser at a shear stirring rate of 1500-6000 rpm, slowly drop the preheated water prepared in step eight into the high-speed dispersed material, perform phase transition emulsification for 2-3 hours, then cool to room temperature, cool and filter the material to obtain a modified polyurethane vinyl carbon fiber sizing agent.
[0036] Example 1
[0037] 1. Synthesis of main sizing material of modified polyurethane vinyl sizing agent
[0038] Step 1: Place 200.00 g (0.0333 mol) of melted polyethylene glycol 6000 in an oil bath, add 200.00 g of butanone solvent, heat the oil bath to 50°C, build a reaction device with a stirrer, a serpentine condenser, and a thermometer, and dilute the polyethylene glycol 6000 at a speed of 180-200 rpm; wait for the temperature of the reaction system to stabilize;
[0039] Step 2: Add 16.69 g (0.0667 mol) of diphenylmethane diisocyanate, rotate at 200-220 rpm, and react for 2 hours;
[0040] Step 3: Add 37.45 g (0.0333 mol) of epoxy resin E44, rotate at 200-220 rpm, raise the reaction temperature to 85°C, and further react with isocyanate monomer for 3 hours;
[0041] Step 4: Then add 80.00 g (0.0333 mol) of allyl polyethylene glycol 2400, rotate at 200-220 rpm, and continue the reaction for 2 hours;
[0042] Step 5: After the reaction is completed, remove the butanone solvent by distillation under reduced pressure; pour it into a tray covered with aluminum foil while it is hot, and cool it to room temperature to obtain the main slurry of the modified polyurethane vinyl sizing agent.
[0043] 2. Preparation of modified polyurethane vinyl sizing agent
[0044] Step 6: 45.00 g of epoxy resin E20 and 45.00 g of epoxy resin E51 were placed in a 2 L stainless steel cylinder, and the two materials were completely melted in an oven at 80°C;
[0045] Step 7: Add 90.00g of the modified polyurethane vinyl sizing agent main slurry synthesized above, melt it completely, and stir it evenly;
[0046] Step 8: Preheat 450.00 g of deionized water in a 60°C water bath;
[0047] Step nine: Use a high-speed disperser (speed of about 1500-6000 rpm) to evenly mix the materials in step 2, slowly drop the warm water prepared in step 3) into the high-speed dispersed materials, perform phase transition emulsification for 2 hours, then cool to room temperature, cool and filter the material to obtain a milky white modified polyurethane vinyl carbon fiber sizing agent.
[0048] Step 10: Test the solid content, viscosity, pH value, particle size and dilution stability of the sizing agent.
[0049] The sizing agent prepared by Example 1 has a solid content of 49.87%, a viscosity of 375.0 cP (2#, 30 rpm), a pH value of 6.45, and an average particle size of 320 nm. The sizing agent is easily diluted by adding deionized water. The sizing solution with a solid content of 2% has good dilution stability. There is no stratification when stored at room temperature for 72 hours, and no precipitation is precipitated at the bottom.
[0050] Example 2
[0051] 1. Synthesis of main sizing material of modified polyurethane vinyl sizing agent
[0052] Step 1: Place 133.20 g (0.0333 mol) of melted polyethylene glycol 4000 in an oil bath, add 250.00 g of acetone solvent, heat the oil bath to 55°C, build a reaction device with a stirrer, a serpentine condenser, and a thermometer, dilute polyethylene glycol 4000 at a speed of 180-200 rpm, and wait for the temperature of the reaction system to stabilize;
[0053] Step 2: Add 11.61 g (0.0667 mol) of diphenylmethane diisocyanate TDI-80, the speed is 200-220 rpm, and the reaction time is 2.5 hours;
[0054] Step 3: Add 22.20 g (0.0222 mol) of epoxy resin E20, rotate at 200-220 rpm, raise the reaction temperature to 85°C, and further react with isocyanate for 2.5 hours;
[0055] Step 4: Add 2.58 g (0.0222 mol) of hydroxyethyl acrylate, rotate at 200-220 rpm, and continue the reaction for 2 hours;
[0056] Step 5: Add 53.33 g (0.0222 mol) of allyl polyethylene glycol 2400, rotate at 200-220 rpm, and continue the reaction for 2 hours;
[0057] Step 6: After the reaction is completed, the acetone solvent is removed by distillation under reduced pressure;
[0058] Step 7: Pour into a tray covered with aluminum foil while it is still hot and cool to room temperature to obtain the main slurry of modified polyurethane vinyl sizing agent.
[0059] 2. Preparation of modified polyurethane vinyl sizing agent
[0060] Step 8: 75.00 g of epoxy resin E20 and 45.00 g of epoxy resin E51 were placed in a 2L stainless steel cylinder, and the two materials were completely melted in an oven at 80°C;
[0061] Step 9: Add 120.00 g of the modified polyurethane vinyl sizing agent main slurry synthesized above, melt it completely, and stir it evenly;
[0062] Step 10: Preheat 660.29 g of deionized water in a 60°C water bath;
[0063] Step 11: Use a high-speed disperser (speed of about 1500-6000 rpm) to evenly mix the materials in step 2, slowly drop the warm water prepared in step 3) into the high-speed dispersed materials, perform phase transition emulsification for 3 hours, then cool to room temperature, cool and filter the material to obtain a milky white modified polyurethane vinyl carbon fiber sizing agent.
[0064] Step 12: Test the solid content, viscosity, pH value, particle size and dilution stability of the sizing agent.
[0065] The sizing agent prepared by Example 2 has a solid content of 36.76%, a viscosity of 173.5 cP (2#, 60 rpm), a pH value of 6.19, and an average particle size of 346 nm. The sizing agent is easily diluted by adding deionized water. The sizing solution with a solid content of 2% has good dilution stability. There is no stratification when stored at room temperature for 72 hours, and no precipitation is precipitated at the bottom.
[0066] Example 3
[0067] 1. Synthesis of main sizing material of modified polyurethane vinyl sizing agent
[0068] Step 1: Place 200.00 g (0.1000 mol) of molten polyethylene glycol PEG2000 in an oil bath, add 200.00 g of butanone solvent, heat the oil bath to 50°C, build a reaction device with a stirrer, a serpentine condenser, and a thermometer, dilute PEG2000 at a speed of 180-200 rpm, and keep the temperature of the reaction system stable;
[0069] Step 2: Add 34.84 g (0.2000 mol) of toluene diisocyanate TDI-80, rotate at 200-220 rpm, and react for 3 hours;
[0070] Step 3: Add 74.90 g (0.0667 mol) of epoxy resin E44, rotate at 200-220 rpm, raise the reaction temperature to 80°C, and further react with isocyanate for 2.5 hours;
[0071] Step 4: Add 7.74 g (0.0667 mol) of hydroxypropyl acrylate, rotate at 200-220 rpm, and continue the reaction for 2.5 hours;
[0072] Step 5: At a higher temperature (70-85°C), 66.67 g (0.0667 mol) of allyl polyethylene glycol APEG1000 was added at a speed of 200-220 rpm, and the reaction was continued for 2 hours;
[0073] Step 6: After the reaction is completed, the butanone solvent is removed by distillation under reduced pressure;
[0074] Step 7: Pour into a tray covered with aluminum foil while it is still hot and cool to room temperature to obtain the main slurry of modified polyurethane vinyl sizing agent.
[0075] 2. Preparation of modified polyurethane vinyl sizing agent
[0076] Step 8: 75.00 g of epoxy resin E20 and 45.00 g of epoxy resin E51 were placed in a 2 L stainless steel cylinder, and the two materials were completely melted in an oven at 80°C;
[0077] Step 9: Add 60.00g of the modified polyurethane vinyl sizing agent main slurry synthesized above, melt it completely, and stir it evenly;
[0078] Step 10: Preheat 334.29 g of deionized water in a 60°C water bath;
[0079] Step 11: Use a high-speed disperser (speed of about 1500-6000 rpm) to evenly mix the materials in step 2, slowly drop the warm water prepared in step 3) into the high-speed dispersed materials, perform phase transition emulsification for 3 hours, then cool to room temperature, cool and filter the material to obtain a milky white modified polyurethane vinyl carbon fiber sizing agent.
[0080] Step 12: Test the solid content, viscosity, pH value, particle size and dilution stability of the sizing agent.
[0081] The sizing agent prepared by Example 3 has a solid content of 36.04%, a viscosity of 246.0 cP (2#, 60 rpm), a pH value of 5.98, and an average particle size of 369 nm. The sizing agent is easily diluted by adding deionized water. The sizing solution with a solid content of 2% has good dilution stability. There is no stratification when stored at room temperature for 72 hours, and no precipitation is precipitated at the bottom.
[0082] The comparative example used a vinyl sizing agent used by a carbon fiber manufacturer.
[0083] The sizing agents prepared in Examples 1-3 of the present invention or the sizing agents of the comparative examples were diluted with deionized water to a solid content of 1.3%, and the diluted sizing agents were uniformly coated on the surface of the unsizing carbon fiber precursor by a sizing device, and sizing carbon fibers were obtained after drying. The properties of the carbon fibers treated with the sizing agents of Examples 1-3 of the present invention and the comparative examples were tested, and the results are shown in Table 1.
[0084] Table 1
[0085]
[0086] Note: × represents poor, ○ represents average, ◎ represents
[0087] In the table shown in Table 1, the larger the stiffness value, the better the stiffness; the better the fiber wettability, the better the compatibility of the carbon fiber and the matrix resin; the larger the composite interlayer shear strength value, the better the compatibility of the carbon fiber and the matrix resin. It can be seen from Table 1 that the performance of the sizing agent prepared by the preparation method of the present invention is better than the vinyl sizing agent in the comparative example.
[0088] The method for preparing the modified polyurethane vinyl carbon fiber sizing agent of the present invention is that the prepared carbon fiber sizing agent is an environmentally friendly water-soluble polymer emulsion, which is beneficial to the carbon fiber sizing process operation; and the sizing agent molecular structure contains a large number of unsaturated carbon-carbon double bonds, which can participate in the curing reaction of the vinyl resin, can significantly improve the interfacial force between the carbon fiber and the vinyl resin, realize the strong chemical connection of the interface layer, and is beneficial to improve the comprehensive mechanical properties of the carbon fiber reinforced vinyl composite material.
Claims
1. A method for preparing an environmentally friendly modified polyurethane vinyl carbon fiber sizing agent, characterized in that: The modified polyurethane vinyl carbon fiber sizing agent is made from two parts: The synthesis steps of the modified polyurethane vinyl sizing agent main slurry as the first part include: Step 1: Place 200.00g of melted polyethylene glycol 6000 in an oil bath, add 200.00g of butanone solvent, heat the oil bath to 50°C, build a reaction device with a stirrer, a serpentine condenser, and a thermometer, dilute polyethylene glycol 6000 at a speed of 180-200rpm, and wait for the temperature of the reaction system to stabilize; Step 2: Add 16.69 g of diphenylmethane diisocyanate, rotate at 200-220 rpm, and react for 2 hours; Step 3: Add 37.45g of epoxy resin E44, rotate at 200-220rpm, raise the reaction temperature to 85°C, and further react with isocyanate monomer for 3 hours; Step 4: Then add 80.00g of allyl polyethylene glycol 2400, rotate at 200-220rpm, and continue the reaction for 2 hours; Step 5: After the reaction is completed, the butanone solvent is removed by distillation under reduced pressure, and the mixture is poured into a tray covered with aluminum foil while hot, and cooled at room temperature to obtain a main slurry of a modified polyurethane vinyl sizing agent; The steps of preparing the modified polyurethane vinyl carbon fiber sizing agent by inverse emulsification as the second part include: Step 6: 45.00 g of epoxy resin E20 and 45.00 g of epoxy resin E51 were placed in a 2 L stainless steel cylinder, and the two materials were completely melted in an oven at 80°C; Step 7: Add 90.00g of the modified polyurethane vinyl sizing agent main slurry synthesized above, melt it completely, and stir it evenly; Step 8: Preheat 450.00 g of deionized water in a 60°C water bath; Step nine: In a high-speed disperser, at a speed of 1500-6000 rpm, first mix the materials in step seven evenly, slowly drop the warm water prepared in step eight into the high-speed dispersed materials, perform phase transition emulsification for 2 hours, then cool to room temperature, cool and filter the material to obtain a milky white modified polyurethane vinyl carbon fiber sizing agent.
2. A method for preparing an environmentally friendly modified polyurethane vinyl carbon fiber sizing agent, characterized in that: The modified polyurethane vinyl carbon fiber sizing agent is made from two parts: The synthesis steps of the modified polyurethane vinyl sizing agent main slurry as the first part include: Step 1: Place 133.20 g of melted polyethylene glycol 4000 in an oil bath, add 250.00 g of acetone solvent, heat the oil bath to 55°C, build a reaction device with a stirrer, a serpentine condenser, and a thermometer, dilute polyethylene glycol 4000 at a speed of 180-200 rpm, and wait for the temperature of the reaction system to stabilize; Step 2: Add 11.61g of diphenylmethane diisocyanate TDI-80, the speed is 200-220rpm, and the reaction time is 2.5 hours; Step 3: Add 22.20 g of epoxy resin E20, rotate at 200-220 rpm, raise the reaction temperature to 85°C, and further react with isocyanate for 2.5 hours; Step 4: Add 2.58 g of hydroxyethyl acrylate, rotate at 200-220 rpm, and continue the reaction for 2 hours; Step 5: Add 53.33 g of allyl polyethylene glycol 2400, rotate at 200-220 rpm, and continue the reaction for 2 hours; Step 6: After the reaction is completed, the acetone solvent is removed by distillation under reduced pressure; Step 7: Pour the mixture into a tray covered with aluminum foil while it is still hot, and cool it to room temperature to obtain the main slurry of the modified polyurethane vinyl sizing agent; The steps of preparing the modified polyurethane vinyl carbon fiber sizing agent by inverse emulsification as the second part include: Step 8: 75.00 g of epoxy resin E20 and 45.00 g of epoxy resin E51 were placed in a 2L stainless steel cylinder, and the two materials were completely melted in an oven at 80°C; Step 9: Add 120.00 g of the modified polyurethane vinyl sizing agent main slurry synthesized above, melt it completely, and stir it evenly; Step 10: Preheat 660.29 g of deionized water in a 60°C water bath; Step 11: In a high-speed disperser, at a speed of 1500-6000 rpm, first mix the materials in step 9 evenly, slowly drop the warm water prepared in step 10 into the high-speed dispersed materials, perform phase transition emulsification for 3 hours, then cool to room temperature, cool and filter the material to obtain a milky white modified polyurethane vinyl carbon fiber sizing agent.
3. A method for preparing an environmentally friendly modified polyurethane vinyl carbon fiber sizing agent, characterized in that: The modified polyurethane vinyl carbon fiber sizing agent is made from two parts: The synthesis steps of the modified polyurethane vinyl sizing agent main slurry as the first part include: Step 1: Place 200.00g of molten polyethylene glycol PEG2000 in an oil bath, add 200.00g of butanone solvent, heat the oil bath to 50°C, build a reaction device with a stirrer, a serpentine condenser, and a thermometer, dilute PEG2000 at a speed of 180-200rpm, and keep the temperature of the reaction system stable; Step 2: Add 34.84g toluene diisocyanate TDI-80, the speed is 200-220rpm, and the reaction time is 3 hours; Step 3: Add 74.90g of epoxy resin E44, rotate at 200-220rpm, raise the reaction temperature to 80°C, and further react with isocyanate for 2.5 hours; Step 4: Add 7.74 g of hydroxypropyl acrylate, rotate at 200-220 rpm, and continue the reaction for 2.5 hours; Step 5: Add 66.67 g of allyl polyethylene glycol APEG1000 at 70-85°C, rotate at 200-220 rpm, and continue the reaction for 2 hours; Step 6: After the reaction is completed, the butanone solvent is removed by distillation under reduced pressure; Step 7: Pour the mixture into a tray covered with aluminum foil while it is still hot, and cool it to room temperature to obtain the main slurry of the modified polyurethane vinyl sizing agent; The steps of preparing the modified polyurethane vinyl carbon fiber sizing agent by inverse emulsification as the second part include: Step 8: 75.00 g of epoxy resin E20 and 45.00 g of epoxy resin E51 were placed in a 2 L stainless steel cylinder, and the two materials were completely melted in an oven at 80°C; Step 9: Add 60.00g of the modified polyurethane vinyl sizing agent main slurry synthesized above, melt it completely, and stir it evenly; Step 10: Preheat 334.29 g of deionized water in a 60°C water bath; Step 11: In a high-speed disperser, at a speed of 1500-6000 rpm, first mix the materials in step 9 evenly, slowly add the warm water prepared in step 10 to the high-speed dispersed materials, perform phase transition emulsification for 3 hours, then cool to room temperature, cool and filter the material to obtain a milky white modified polyurethane vinyl carbon fiber sizing agent.