A method for suppressing the shuttle effect of lithium-sulfur batteries by using cerium dioxide-doped porous carbon rods
By using ceria doped porous carbon rod material in lithium sulfur batteries, the insulation, electrode expansion and shuttle effects of sulfur in lithium sulfur batteries are solved, the battery performance and life are improved, and the capacity retention rate is achieved and cycle stability.
Patent Information
- Application Number
- CN202111120410.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-24
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-09-24
AI Technical Summary
The insulation of sulfur in lithium-sulfur batteries, electrode volume expansion during charging and discharge, and shuttle effect problems lead to poor battery performance and short service life.
Using ceria doped porous carbon rod material, soy protein isolate is used as a carbon source, and carbonization and hydrothermal reaction are carried out by combining potassium hydroxide and ammonium acetate to form a carbon rod with high conductivity and porous structure, which is used to fix sulfur and Inhibit the shuttle effect of polysulfides.
It significantly improves the conductivity and battery life of lithium-sulfur batteries, suppresses the shuttle effect, and is better than the capacity retention and cycling performance of existing similar materials.
Smart Images

Figure CN113964319B_ABST
Abstract
Description
Technical Field
[0001] The present invention discloses a method for suppressing the shuttle effect of lithium-sulfur batteries by using cerium dioxide-doped porous carbon rods, and belongs to the field of lithium-ion batteries, and specifically belongs to the field of design and regulation of positive electrode materials for lithium-sulfur batteries. Background Art
[0002] In recent years, lithium-ion batteries have developed rapidly. Lithium-sulfur batteries were first proposed in the 1960s. Lithium-sulfur batteries, which introduce sulfur into lithium battery systems as positive electrode materials, are a new type of secondary battery with high energy density, high cost performance and development potential. 1675mAh g -1 ) and metallic lithium ( 3861mAh g -1 ) complete reaction, the energy density of lithium-sulfur batteries (2500Wh kg -1 ) is much higher than the existing lithium-ion batteries. Although lithium-sulfur batteries have many advantages, there are still many challenges in their commercialization process. First, the inherent electronic and ionic insulation of S / Li2S hinders the charge and discharge behavior of the battery. The utilization rate of sulfur is low, and some sulfur remains after the cycle without electrochemical reaction. Electronic / ionic insulation leads to slow kinetics. The voltage platform curve of the lithium-sulfur battery is more polarized at the lower discharge platform, which further reduces the actual energy density of the lithium-sulfur battery. Secondly, the density of S8 (2.07g cm -3 ) is higher than the density of Li2S (1.66 g cm -3 ), resulting in a large volume expansion (80%) after discharge. Severe volume expansion leads to weak electrical contact between the conductive substrate and the collector, and significant capacity decay during the cycle. Unlike the embedding process of traditional lithium-ion batteries, lithium-sulfur batteries also produce a shuttle effect due to the dissolution of polysulfides in organic electrolytes. Long-chain polysulfides (Li2S n,4≤n≤8) are easily soluble in organic solvents. Due to the concentration gradient, polysulfides pass through the diaphragm and deposit on the lithium anode, causing the soluble polysulfides to be reduced to insoluble Li2S. The insoluble Li2S on the surface of lithium metal forms a barrier layer, which hinders the conduction of lithium ions. Therefore, it is necessary to design a well-structured lithium-sulfur battery positive electrode material. Generally speaking, porous conductive carbon materials are often used as positive electrode materials for lithium-sulfur batteries. The conductivity of the carrier carbon solves the sulfur insulation problem, and the porous structure reduces the volume expansion of the electrode. Most non-polar carbon materials cannot chemically adsorb polar polysulfides, and can only physically embed polysulfides. In addition to confining sulfur to porous carbon materials, materials such as conductive polymers, polar metal oxides / sulfides and carbides are also widely used as cathodes for lithium-sulfur batteries. Among them, metal oxides have polar metal oxygen bonds and hydrophilicity. For example, titanium dioxide, manganese dioxide and rare earth metal oxides are all effective polysulfide adsorbents. Unlike non-polar carbon materials, polar metal oxides and sulfur form MS n Compound (M x+ The metal cation has a strong chemical bond, which effectively prevents the shuttling of polysulfides. Summary of the invention
[0003] The purpose of the present invention is to solve the problems of sulfur insulation, electrode volume expansion during charging and discharging, and shuttle effect in lithium-sulfur batteries, and to provide a cerium dioxide doped porous carbon rod. The carrier conductive carbon solves the problem of poor sulfur conductivity, the porous structure provides reaction sites for sulfur, and the pore volume of a certain size is conducive to alleviating the electrode volume expansion, and the doped cerium dioxide nanocrystals fix polysulfides through chemical adsorption to inhibit the shuttle effect.
[0004] The object of the present invention can be achieved by the following method: A method for suppressing the shuttle effect of lithium-sulfur batteries by doping cerium dioxide with porous carbon rods, characterized in that the specific steps are:
[0005] 1. Preparation of carbon rod precursor
[0006] Soy protein isolate is used as a carbon source, sodium citrate as a complexing agent is added in a mass ratio of 3:1 to 1:1 and dissolved in deionized water, heated in a water bath, and then transferred to a tubular furnace for carbonization at 700°C to 900°C under nitrogen protection for 1 to 3 hours to obtain a black powder carbon rod precursor;
[0007] 2. Preparation of porous carbon rods
[0008] The carbon rod precursor in step 1 and potassium hydroxide are stirred in a mass ratio of 1:1 to 1:3, mixed evenly and dried in a vacuum drying oven, and then transferred to a tube furnace at 700°C to 900°C under nitrogen protection for 1 to 2 hours to obtain a porous carbon rod powder;
[0009] 3. Preparation of Ceria-doped Porous Carbon Rods
[0010] Stir ammonium acetate and cerium nitrate in anhydrous ethanol until the solution is transparent, add the porous carbon rod powder obtained in step 2 and ultrasonically disperse for 30 minutes, wherein the mass ratio of ammonium acetate, cerium nitrate and porous carbon rod powder is 1:1:3-1:1:5, then transfer to a high-pressure reactor and react at 120°C-180°C for 4-12 hours, cool to room temperature and centrifuge and dry to obtain a gray powder, transfer the gray powder to a tubular furnace and react at 800°C under nitrogen protection for 3 hours to obtain a black cerium dioxide-doped porous carbon rod material;
[0011] 4. Preparation of Carbon-Sulfur Composite Materials
[0012] The cerium dioxide-doped porous carbon rod material obtained in step 3 and elemental sulfur are ball-milled at a mass ratio of 1:4 for 1 to 3 hours, and melt-diffused at 155° C. for 3 to 5 hours under closed conditions to obtain a carbon-sulfur composite material;
[0013] 5. Preparation of positive electrode and battery assembly
[0014] The obtained carbon-sulfur composite material, conductive agent acetylene black and binder polyvinylidene fluoride are dispersed in nitrogen-methylpyrrolidone in a mass ratio of 8:1:1, stirred evenly and then coated on a clean aluminum foil and dried. After cooling to room temperature, sliced with a slicer for standby use, and assembled in a glove box filled with argon in the order of negative electrode shell, separator, lithium sheet, organic electrolyte and positive electrode shell to obtain the lithium-sulfur battery.
[0015] Furthermore, the mass ratio of the soy protein isolate and sodium citrate described in step 1 is 3:1 to 1:1. The soy protein isolate is carbonized under the action of the sodium citrate complexing agent to obtain a rod-shaped conductive carbon material. This morphology is conducive to shortening the electron transfer path and accelerating the redox reaction kinetics. Too low a sodium citrate content will cause the obtained carbon material to be irregular and more amorphous, while an excessive amount of sodium citrate will cause the obtained carbon rod material to accumulate and agglomerate, which is not conducive to use in the positive electrode carrier material of a lithium-sulfur battery;
[0016] Furthermore, the method for suppressing the shuttle effect of lithium-sulfur batteries by using a cerium dioxide-doped porous carbon rod is characterized in that the carbonization temperature of the tubular furnace in step 1 is 700° C. to 900° C., and carbonization for 3 hours at this temperature obtains a carbon rod material with a high degree of graphitization, which has good electrical conductivity and provides a good medium for the combination of electrons and active substances;
[0017] Furthermore, the mass ratio of the carbon rod precursor to potassium hydroxide described in step 2 is 1:1 to 1:3, and the porous material is obtained by alkaline etching. Under high temperature conditions, a certain amount of potassium hydroxide and the carbon rod material in situ form substances such as potassium carbonate and potassium bicarbonate, and the porous carbon rod material is obtained by acid washing to remove potassium carbonate and potassium bicarbonate. Excessive potassium hydroxide will destroy the original morphology of the carbon rod, and insufficient potassium hydroxide content will result in a smaller specific surface area of the material;
[0018] Furthermore, the method for suppressing the shuttle effect of lithium-sulfur batteries by using a cerium dioxide-doped porous carbon rod is characterized in that the carbonization temperature of the tubular furnace in step 2 is 700° C. to 900° C. Under this temperature and corresponding carbonization time conditions, a carbon rod material with a uniform porous structure can be obtained, and a larger specific surface area is conducive to providing good reaction sites for sulfur;
[0019] Furthermore, the mass ratio of ammonium acetate, cerium nitrate and porous carbon rod powder in step 3 is 1:1:3 to 1:1:5, and the OH generated by hydrolysis of ammonium acetate - The cerium hydroxide is combined with cerium nitrate cations and attached to the surface of the porous carbon rod. After hydrothermal reaction and heat treatment, the cerium dioxide doped porous carbon rod is obtained. When the content of the porous carbon rod is too high, the load is uneven and the catalytic performance of the material is attenuated. When the content of the porous carbon rod is too low, the cerium dioxide covers the surface of the carbon rod, which affects the conductivity of the material.
[0020] Furthermore, the method for inhibiting the shuttle effect of lithium-sulfur batteries by doping porous carbon rods with cerium dioxide is characterized in that the reaction temperature of the high-pressure reactor described in step three is 180°C and the reaction time is 4 to 12 hours. If the hydrothermal temperature is too low or the time is too short, the conversion rate of cerium ions will be low, the cerium dioxide loading amount will be reduced, and the catalytic performance of the material will be affected. If the hydrothermal temperature is too high or the time is too long, the morphology of cerium dioxide will be destroyed and agglomeration will be caused, thereby affecting the conductive properties of the material.
[0021] For the sake of simplicity, the carbon rod (Carbon Rod) material, porous carbon rod (Porous Carbon Rod) material, and cerium dioxide doped porous carbon rod (CeO2 / Porous Carbon Rod) material are named CR, PCR, and CeO2 / PCR, respectively, and the three materials after sulfur loading are named S@CR, S@PCR, and S@CeO2 / PCR, respectively.
[0022] The present invention includes the following gain effects:
[0023] Using renewable soy protein isolate as a carbon source has the advantages of being environmentally friendly and cheap and readily available.
[0024] Through electrochemical testing, we compared it with similar materials reported so far, and the results are as followsFig.36 As shown;
[0025] Under different loading amounts and current densities, the capacity retention rate of lithium-sulfur batteries assembled with cerium dioxide-doped porous carbon rod materials after 200 cycles is better than that of similar materials reported so far (Electroanal.Chem, 2020, 876, 114545), (Nano Energy, 2021, 81, 105602), (Appl.Surf.Sci. 2020, 508, 145286), (ACSApp.Energy Mater. 2021, 4, 5713-5736), (Mater.Today Energy, 2020, 17, 100484), (Chem.Eng.J. 2021, 417, 128172);
[0026] The prepared carbon rod material has excellent conductivity, and as a carrier it solves the problem of low conductivity of sulfur at room temperature; the rod-like morphology shortens the transition distance of lithium ions during charging and discharging, accelerates the kinetics of redox reactions, and thus improves battery performance.
[0027] The porous structure provides a large number of loading sites for sulfur. A large number of micropores provide an ultra-high specific surface area, which can increase the loading capacity of the sulfur electrode. A certain number of mesopores effectively alleviate the volume expansion of the electrode during charging and discharging, thereby increasing the service life of the battery.
[0028] After the introduction of cerium dioxide nanocrystals, the rare earth metal Ce cations and electron-rich oxygen atoms capture polysulfides through strong chemical bonding, inhibiting the shuttle effect of polysulfides and alleviating the irreversible attenuation of capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Flow chart of the preparation of cerium dioxide doped porous carbon rods;
[0030] Figure 2 (a) SEM image of carbon rod (CR) material; (b) SEM image of porous carbon rod (PCR) material; (c) SEM image of cerium dioxide doped porous carbon rod (CeO2 / PCR) material; (d) TEM image of CeO2 / PCR; (e), (f) lattice fringe images of CeO2 / PCR; (g) mapping test image of CeO2 / PCR;
[0031] Figure 3 TEM images of CR materials;
[0032] Figure 4 TEM images of PCR;
[0033] Figure 5Adsorption isotherm plot of PCR material;
[0034] Figure 6 Pore size distribution curve of PCR material;
[0035] Figure 7 TEM images of the morphology and size of ceria;
[0036] Figure 8 XRD patterns of CR, PCR, and CeO2 / PCR;
[0037] Fig. 9 XPS of C element in S@CeO2 / PCR;
[0038] Fig.10 XPS of Ce element in S@CeO2 / PCR;
[0039] Fig.11 XPS of S element in S@CeO2 / PCR
[0040] Fig.12 DFT: Calculation of binding energy of CeO2 / PCR with S and Li2S8;
[0041] Fig.13 Comparison of polysulfide adsorption experiments of CR, PCR, and CeO2 / PCR;
[0042] Fig.14 XPS full spectrum of S@CeO2 / PCR;
[0043] Fig.15 Model diagram after optimization of S8, Li2S8, and CeO2;
[0044] Fig.16 Tafel slope test (Oxidation) of batteries assembled with three materials;
[0045] Fig.17 Tafel slope test (Reduction) of batteries assembled with three materials;
[0046] Fig.18 CV test of symmetrical batteries with three electrode materials;
[0047] Fig.19 Li2S deposition experiment of CR materials;
[0048] Fig. 20 Li2S deposition experiment of PCR material;
[0049] Fig.21 Li2S deposition experiment on CeO2 / PCR material;
[0050] Fig. 22 Impedance spectra of the three materials and calculation diagram of lithium ion diffusion coefficient;
[0051] Fig.23 CV curve of S@CeO2 / PCR material;
[0052] Fig.24 Rate test diagram of lithium-sulfur batteries assembled with three materials;
[0053] Fig.25 The charge and discharge curves of S@CeO2 / PCR assembled lithium-sulfur batteries at different current densities;
[0054] Fig.26 Comparison of charge and discharge of lithium-sulfur batteries assembled with three materials under high load;
[0055] Fig. 27 Thermogravimetric curve of S@CeO2 / PCR;
[0056] Fig.28 The charge and discharge curves of S@CR material at different current densities;
[0057] Fig.29 The charge and discharge curves of S@PCR material at different current densities;
[0058] Fig.30 Capacity-voltage curve of S@CR material;
[0059] Fig.31 Capacity-voltage curve of S@PCR material;
[0060] Fig.32 Capacity-voltage curve of S@CeO2 / PCR material;
[0061] Fig.33 SEM image of the electrode surface of CeO2 / PCR material after charge and discharge cycles;
[0062] Fig.34 Capacity-voltage curves of S@CeO2 / PCR material at different cycle times;
[0063] Fig.35 CV curves of CR and PCR materials.
[0064] Fig.36 Electrochemical comparison with similar materials reported so far. DETAILED DESCRIPTION
[0065] The above contents of the present invention are further described in detail below through embodiments, but the subject matter of the present invention is not limited to the following embodiments, and all technologies realized based on the above contents of the present invention belong to the scope of the present invention.
[0066] Experimental drugs
[0067]
[0068] Instrument Name model factory Analytical Balance FC-204 Shanghai Jingke Balance Magnetic stirrer CL-200 Gongyi Yuhua Instrument Co., Ltd. Vacuum drying oven ZK-82BB Shanghai Experimental Instrument Factory Co., Ltd. Button battery sealing machine MSK-110 Shenzhen Kejing Zhida Technology Co., Ltd. Pole punching machine MSK-T10 Shenzhen Kejing Zhida Technology Co., Ltd. LAND Battery Testing System CT2001A Wuhan Jinnuo Electronics Co., Ltd. X-ray diffractometer X'Pert PRO PANalytical Electrochemical workstation CHI760E Shanghai Chenhua Instrument Co., Ltd. Scanning electron microscopy FEI sirion200 FEI Vacuum glove box ZKX Nanjing University Instrument Factory Thermogravimetric Analyzer TGA / SDTA851e Mettler Toledo
[0069] Example 1
[0070] 1. Preparation of carbon rod precursor
[0071] Soy protein isolate is used as a carbon source, sodium citrate as a complexing agent is added in a mass ratio of 3:1 to 1:1 and dissolved in deionized water, heated in a water bath, and then transferred to a tubular furnace for carbonization at 700°C to 900°C under nitrogen protection for 1 to 3 hours to obtain a black powder carbon rod precursor;
[0072] 2. Preparation of porous carbon rods
[0073] The carbon rod precursor in step 1 and potassium hydroxide are stirred in a mass ratio of 1:1 to 1:3, mixed evenly and dried in a vacuum drying oven, and then transferred to a tube furnace at 700°C to 900°C under nitrogen protection for 1 to 2 hours to obtain a porous carbon rod powder;
[0074] 3. Preparation of Ceria-doped Porous Carbon Rods
[0075] Stir ammonium acetate and cerium nitrate in anhydrous ethanol until the solution is transparent, add the porous carbon rod powder obtained in step 2 and ultrasonically disperse for 30 minutes, wherein the mass ratio of ammonium acetate, cerium nitrate and porous carbon rod powder is 1:1:3-1:1:5, then transfer to a high-pressure reactor and react at 120°C-180°C for 4-12 hours, cool to room temperature and centrifuge and dry to obtain a gray powder, transfer the gray powder to a tubular furnace and react at 800°C under nitrogen protection for 3 hours to obtain a black cerium dioxide-doped porous carbon rod material;
[0076] 4. Preparation of Carbon-Sulfur Composite Materials
[0077] The cerium dioxide-doped porous carbon rod material obtained in step 3 and elemental sulfur are ball-milled at a mass ratio of 1:4 for 1 to 3 hours, and melt-diffused at 155° C. for 3 to 5 hours under closed conditions to obtain a carbon-sulfur composite material;
[0078] 5. Preparation of positive electrode and battery assembly
[0079] The obtained carbon-sulfur composite material, conductive agent acetylene black and binder polyvinylidene fluoride are dispersed in nitrogen-methylpyrrolidone in a mass ratio of 8:1:1, stirred evenly and then coated on a clean aluminum foil and dried. After cooling to room temperature, sliced with a slicer for standby use, and assembled in a glove box filled with argon in the order of negative electrode shell, separator, lithium sheet, organic electrolyte and positive electrode shell to obtain the lithium-sulfur battery.
[0080] Performance characterization of the above embodiments
[0081] (1) XRD test: The phase compositions of CeO2 / PCR, PCR and CR materials at room temperature were tested by X′Pertpro X-ray diffraction with Cu Kα radiation, and the 2θ range was 10°~90°.
[0082] (2) SEM test. Scanning electron microscopy (SEM, FEI-Sirion200) was used to characterize the morphology of CR, PCR and CeO2 / PCR materials.
[0083] (3) TEM test. Transmission electron microscopy (TEM, JEM-2100) was used to further observe the structures of CR, PCR and CeO2 / PCR materials.
[0084] (4) XPS test: The chemical states of C, Ce and S elements were determined by X-ray photoelectron spectroscopy (XPS, PHI5700, Physical Electronics, USA).
[0085] (5) Charge and discharge test: The Land-CT2001A battery measures the constant current charge and discharge performance of lithium-sulfur batteries in the voltage range of 1.7V to 2.8V at room temperature.
[0086] (6) CV test. The voltage scan range was 1.5-3 V and the scan rate was 0.1 mV s -1 Cyclic voltammetry (CV) curves.
[0087] (8) EIS test. 5 Electrochemical impedance spectroscopy (EIS) analysis was carried out on a CHI760E electrochemical station at room temperature and 6 Hz.
[0088] (9) Tafel slope test. The Tafel slope was tested on CHI760E with a voltage range of 2.4 V to 2.0 V and a scan rate of 5 mV s -1 .
[0089] (10) Li2S deposition experiment. A mixed solution of lithium sulfide (Li2S) and sulfur powder was rapidly stirred in tetraethylene glycol dimethyl ether at a molar ratio of 1:7 to prepare 0.4 mol L -1 Li2S8 solution. CR, PCR and CeO2 / PCR were used as nucleation substrates to assemble the battery, and lithium foil was used as the anode. During the battery assembly process, 25 μL of Li2S8 (0.4 mol L -1 ) was dripped on the cathode side, and then 25 μL of electrolyte without Li2S8 was dripped on the lithium anode side. The battery was discharged at a constant current of 0.112 mA to 2.06 V, and then discharged at a constant voltage of 2.05 V until the current dropped to 10 -5 mA or less.
[0090] (11) CV test of symmetrical battery. Prepare 1:1 (v / v) DOL / DME, and quickly stir lithium sulfide (Li2S) and sulfur powder in a molar ratio of 1:5 in the prepared solution to prepare 0.2 mol L -1 Li2S6 solution. CR, PCR and CeO2 / PCR were used as working electrode and counter electrode respectively. A total of 40 μL of the prepared electrolyte was dropped on both sides of the diaphragm. The voltage range was -0.7 V and 0.7 V at 10 mV s -1 The CV of the symmetric cell was measured at a scan rate of .
[0091] (12) Binding energy calculation. The calculation is based on density functional theory (DFT) and implemented in the CASTEP module. The generalized gradient approximation of the Perdew-Burke-Ernzerhof (GGA-PBE) functional was selected as the exchange-correlation functional. Equation (1) is the energy calculation formula;
[0092] E Binding Energy =E Total -(E1+E2)
[0093] Figure 1 The flow chart of the preparation of cerium dioxide doped porous carbon rods. Soy protein isolate is used as the carbon source, and the carbon rod (CR) is obtained by carbonization under the action of a complexing agent. Soy protein isolate has the advantages of being environmentally friendly, cheap, and easy to obtain. After alkali etching, a porous carbon rod (PCR) is obtained. CeO2 nanocrystals are doped in the porous carbon rods to prepare CeO2 / PCR materials.
[0094] Figure 2 (a) and Figure 3 The SEM and TEM images of the CR material are shown in Figure 2. After the complex precursor is carbonized, carbon rods of uniform size are obtained. This rod-like structure shortens the electron transfer distance and is conducive to the rapid combination of lithium ions and sulfur. The etched carbon rods show a porous structure, such as Figure 2 (b) and Figure 4 shown. Figure 5 and Figure 6 The adsorption isotherm and pore size distribution curve of PCR materials are shown respectively. PCR materials contain mesopores of 2 to 30 nm and micropores of 0.624 nm. A large number of micropores and mesoporous structures can physically capture polysulfide. The BET calculation results show that the specific surface area of PCR materials is 1378.8527 m 2 g -1 The porous structure provides sites for the redox reaction of sulfur. In addition, pores of a certain size reduce volume expansion during charge and discharge, thus improving battery life. CeO2 / PCR materials obtained by hydrothermal synthesis of porous carbon rods and cerium salts, such as Figure 2 (c) shows that a uniformly distributed CeO2 nanocrystal array grows on the surface of the CeO2 / PCR material. Figure 2 (g) EDS was used to analyze the distribution of Ce, C, and O elements in CeO2 / PCR materials. Combined with the TEM image of CeO2 / PCR materials ( Figure 2 d), uniform cerium-based oxide grows on the surface of the porous carbon rod. Compared with the PCR material before CeO2 doping, cerium grows into nanoparticles with a particle size of 20 to 50 nm ( Figure 7 ). Figure 2 (d) and Figure 2 (e) The lattice fringe results correspond to the (111) and (220) crystal planes of CeO2, respectively.
[0095] Figure 8 The XRD spectrum shows that the characteristic peaks corresponding to the (111), (200), (220) and (311) crystal planes of CeO2 are 28.4, 32.9, 47.4 and 56.3 respectively. This proves that the CeO2 / PCR material has been successfully synthesized. The XPS graph of the C element in S@CeO2 / PCR ( Fig. 9 ), XPS graph of Ce element in S@CeO2 / PCR ( Fig.10 ) and XPS of S element in S@CeO2 / PCR ( Fig.11 ) Figure 2 analyzes the chemical states of C, S and Ce in S@CeO2 / PCR. Fig.14 The full XPS spectrum of S@CeO2 / PCR. In the C1S XPS spectrum, 285.0eV, 287.9eV and 287.9eV correspond to CC / C=C bond and CS bond respectively. 882.85eV and 901.15eV are the characteristic peaks of Ce 3d 3 / 2 and Ce3d 5 / 2 (ΔE=18.3eV), indicating that the cation is Ce 4+The S 2p XPS peaks at 163.57 eV and 164.75 eV correspond to S 2p3 / 2 and S 2p1 / 2, respectively (ΔE=1.18 eV), which differ by 0.43 eV from the standard peak of sulfur (164.0 eV). The characteristic peak of S shifts negatively, while the characteristic peaks of C and Ce shift positively. This proves that in S@CeO2 / PCR, the electrons of cerium and sulfur from the C-S bond and Ce-S bond transfer to the S orbital. The porous carbon rods and CeO2 nanocrystals synergistically adsorb and store sulfur, effectively suppressing the shuttle effect. Fig.12 The binding energy between CeO2 nanocrystals and active materials was verified by theoretical simulation. Based on density functional theory (DFT), the binding energy between CeO2 and Li2S8 was calculated by first principles. Fig.15 The structure and energy of optimized CeO2, S8 and Li2S8. According to the formula, the binding energy of CeO2 nanocrystals with S8 and Li2S8 is -7.202eV and -15.399eV respectively. The CeO2 / PCR material can adsorb and store active substances, which further proves that CeO2 embedded in the porous carbon rod has a strong chemical interaction with sulfur and polysulfide. Fig.13 The adsorption performance of CR, PCR and CeO2 / PCR materials on polysulfide was compared. 50 mg of sample and 0.02 mol L -1 Li2S6 was added to 3 ml of DME / DOL mixed solvent. The CeO2 / PCR Li2S6 solution faded more obviously than other Li2S6 solutions, which is consistent with the above conclusion. At the same time, the four supernatants were detected by UV spectrophotometer. The absorption peaks of polysulfide decreased successively.
[0096] Fig.16 and Fig.17 The catalytic performance was evaluated by calculating the Tafel slope of the redox conversion rate. The slope of the redox conversion rate of CeO2 / PCR was always lower than that of PCR and CR. The results show that the catalyst has good catalytic performance and fast catalytic kinetics for polysulfide redox. Fig.18 The redox reaction kinetics of the three materials were studied for CV measurements of symmetric cells containing Li2S6 electrolyte. Compared with the original CR and PCR materials, the porous carbon rods embedded with CeO2 nanocrystals have a higher current density, indicating that the redox kinetics between liquid polysulfides have been significantly enhanced. To demonstrate the positive effect of porous carbon rods embedded with CeO2 nanocrystals on the nucleation of Li2S, Li2S nucleation experiments were carried out using CR, PCR and CeO2 / PCR as deposition substrates, Li foil as anode and Li2S8 solution as cathode. The nucleation and growth of Li2S (2.05V) are shown in the constant potential discharge process. Fig.19 , Fig. 20 and Fig.21The deposition capacity of Li2S in CeO2 / PCR is 256.54 mAh g -1 , much higher than CR (43.18 mAh g -1 ) and PCR (115.71 mAh g -1 ). The results show that the presence of CeO2 nanocrystals promotes the nucleation of Li2S and accelerates the rapid transformation of liquid polysulfide to solid Li2S.
[0097] Fig.12 (a) is the fitted EIS spectra of lithium-sulfur batteries assembled with S@CR, S@PCR, and S@CeO2 / PCR as positive electrodes after cycling. These three curves are semicircles in the high-frequency region and straight lines in the low-frequency region. The calculation formula for the lithium ion diffusion coefficient is formula (2);
[0098]
[0099] Where R is the gas constant (8.314 JK -1 mol -1 ), T is room temperature (298K), A is the electrode area (1.5386×10 - 4 m 2 ), n is the number of electrons transferred per molecule of active substance, F is the Faraday constant (96500C mol -1 ), C is the lithium ion concentration in the positive electrode material, from Z' to ω -1 / 2 The slope of the straight line is σ. The σ of S@CR, S@PCR and S@CeO2 / PCR materials are 3.1192, 0.5202 and 0.6569 respectively. C is 9.219×10 -3 mol m -3 . Li of three materials + Diffusion coefficient (D Li+ ) are 2.759×10 -12 cm 2 S -1 ,9.920×10 -11 cm 2 S -1 and 6.221×10 -11 cm 2 S -1 . High Li + The diffusion coefficient is related to the structure of the carbon rods. The interconnected uniform rods shorten the transfer path of electrons / lithium ions. The diffusion coefficient of PCR material is better than that of CR material. The porous structure increases the contact area between the electrode and the electrolyte, which promotes the diffusion of lithium ions. Li+Slightly lower than the porous carbon rod, indicating that CeO2 nanocrystals have no significant effect on the electron / ion transfer of the porous carbon rod. The CeO2 nanocrystals are uniformly embedded in the porous carbon rod to improve the cycle performance. The rate performance of Li-S batteries is shown in Figure 2. Fig.12 (c) The initial discharge capacity of S@CeO2 / PCR battery at 0.1C is 1040.4 mAh g -1 , Fig.13 Thermogravimetric test results show that the sulfur content is 73.37% and the average sulfur loading is 1.0 mg cm -2 When the current density increases to 0.2C, 0.5C and 1C, it can maintain 920mAhg -1 、719.4mAh g -1 and 538.9mAh g -1 After the current density was reversed to 1C, 0.5C and 0.2C, the specific capacity was 915.3 mAh g -1 , the capacity recovery rate of S@CeO2 / PCR is about 99.5%. The capacity recovery rates of S@CR and S@PCR batteries are 74.03% and 92.5%, respectively. Fig.12 (d) is the charge and discharge performance comparison of S@CeO2 / PCR battery at different current densities. -2 (0.58C), 1.5mA cm -2 (0.87C) and 2mA cm -2 (1.16C), the initial discharge capacity is 826.2 mAh g -1 , 681mAh g -1 and 546mAh g -1 The average Coulombic efficiencies were 99.05%, 98.54% and 98.07% respectively. Fig.14 The results of polarization voltage and lithium ion diffusion rate of the three materials at different current densities correspond to each other. The polarization rate of S@CR battery is much higher than that of S@PCR and S@CeO2 / PCR batteries. Fig.12(e) Comparison of the charge and discharge performance of lithium-sulfur batteries with three materials as positive electrodes. The diffusion ability of lithium ions in the positive electrode material is closely related to the capacity and life of the battery. The specific capacity of the CR material decreases rapidly after cycling. The porous carbon rods enhance the rapid binding between lithium ions and active substances, thereby alleviating the polarization phenomenon. Due to the shuttle effect, the CR and PCR materials have different degrees of attenuation over a long period of time. Although the porous structure can physically adsorb polysulfide, it cannot fundamentally solve the shuttle effect. CeO2 / PCR material has strong polarity and can chemically restrict the shuttling of polysulfide on the basis of physical adsorption. The content ratio of electrolyte (μL) / sulfur (mg) is about 10.67μL / mg. When the S loading is 2.5mg cm -2 The first discharge capacity is 657.4 mAh g -1 After 100 cycles, the capacity remains at 629.2 mAh g -1 , the current density is 1 mA cm -2 (0.31C). After 100 cycles, the capacity retention rate of S@CeO2 / PCR was 95.71%, and the average Coulomb efficiency was 99.23%. After 100 cycles, the capacity retention rate of S@CR was only 8.12%, and the capacity retention rate of S@PCR was 88.7%. Fig.15 The cathode SEM images of CeO2 / PCR materials after 100 cycles were tested, where (c), (d), (e), and (f) are C, O, S, and Ce elements, respectively. The results show that the S@CeO2 / PCR material basically maintains its original morphology after charge and discharge cycles. Fig.16 The capacity-voltage curve of the material corresponds to the typical charging and discharging platform of a lithium-sulfur battery. 2.31V is the charging platform, and 2.28V / 2.03V are the two discharge platforms of the lithium-sulfur battery. Fig.12 (b) and Fig.17 CV curves of S@CeO2 / PCR and S@PCR materials. At 2.61V, Li2S2 / Li2S is converted into elemental sulfur (S8); at 2.18V and 1.93V, elemental sulfur is converted into lithium polysulfide and then into Li2S2 / Li2S. Compared with the CV curve of S@CR material, the CV curves of S@CeO2 / PCR and S@PCR materials have stronger cycle stability at different cycles. Due to the synergistic effect of porous carbon rod material and CeO2 nanocrystals, the CV curves of S@CeO2 / PCR and S@PCR materials remain basically unchanged during the cycle. The porous carbon rod structure enhances the diffusion of lithium ions in the cathode and the rapid combination with active materials, and provides sulfur reaction sites. The strong polarity of CeO2 nanocrystals combined with polysulfides suppresses the shuttle effect.
Claims
1. A method for inhibiting the shuttle effect of lithium-sulfur batteries by using cerium dioxide-doped porous carbon rods, characterized in that The specific steps are:
1. Preparation of carbon rod precursor Soy protein isolate was used as the carbon source, sodium citrate as a complexing agent was added in a mass ratio of 3:1 to 1:1 and dissolved in deionized water, heated in a water bath, and then transferred to a tubular furnace for carbonization at 700°C to 900°C under nitrogen protection for 1 to 3 hours to obtain a black powder carbon rod precursor; 2. Preparation of porous carbon rods The carbon rod precursor in step 1 and potassium hydroxide are stirred in a mass ratio of 1:1 to 1:3, mixed evenly, dried in a vacuum drying oven, and then transferred to a tube furnace at 700° C. to 900° C. under nitrogen protection for 1 to 2 hours to obtain a porous carbon rod powder; 3. Preparation of Ceria-doped Porous Carbon Rods Stir ammonium acetate and cerium nitrate in anhydrous ethanol until the solution is transparent, add the porous carbon rod powder obtained in step 2 and ultrasonically disperse for 30 minutes, wherein the mass ratio of ammonium acetate, cerium nitrate and porous carbon rod powder is 1:1:3-1:1:5, then transfer to a high-pressure reactor and react at 120°C-180°C for 4-12 hours, cool to room temperature and centrifuge and dry to obtain a gray powder, transfer the gray powder to a tubular furnace and react at 800°C under nitrogen protection for 3 hours to obtain a black cerium dioxide-doped porous carbon rod material; 4. Preparation of Carbon-Sulfur Composite Materials The cerium dioxide-doped porous carbon rod material obtained in step 3 and elemental sulfur are ball-milled at a mass ratio of 1:4 for 1 to 3 hours, and melt-diffused at 155° C. for 3 to 5 hours under closed conditions to obtain a carbon-sulfur composite material; 5. Preparation of positive electrode and battery assembly The obtained carbon-sulfur composite material, conductive agent acetylene black and binder polyvinylidene fluoride are dispersed in nitrogen-methylpyrrolidone in a mass ratio of 8:1:1, stirred evenly and then coated on a clean aluminum foil and dried. After cooling to room temperature, sliced with a slicer for standby use, and assembled in a glove box filled with argon in the order of negative electrode shell, lithium sheet, diaphragm, organic electrolyte, positive electrode and positive electrode shell to obtain the lithium-sulfur battery.
Citation Information
Patent Citations
Cathode material of lithium-sulfur battery and preparation method thereof
CN109473647A
Preparation method of soybean protein isolate-based high-rate lithium-sulfur battery cathode carbon material
CN110148748A