Preparation method of HA material for HA soluble microneedles and its application

By combining HA with 2-hydroxymethyl-β-cyclodextrin, a stable hydrogen bond structure is formed, which solves the problems of poor moldability and weak drug loading capacity of HA microneedles, and improves the mechanical strength and drug loading of microneedles. quantity, shortening drying time, reducing production and storage costs, and adapting to large-scale production needs.

CN113995951BActive Publication Date: 2024-10-11HANGZHOU MODA FRONTIER BIOTECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111320592.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-09
Publication Date
2024-10-11
Estimated Expiration
2041-11-09

AI Technical Summary

Technical Problem

HA microneedles have poor formability, weak drug loading capacity, and long drying time, resulting in high production costs and high storage pressure, making it difficult to meet market demand.

Method used

Mix HA with a molecular weight of 103kDa and 2-hydroxymethyl-β-cyclodextrin to form high-concentration and low-concentration polymer preparation gels, enhance the stability and drug-loading capacity of HA through hydrogen bonds, and centrifuge and dry Technology shortens microneedle drying time.

Benefits of technology

The mechanical strength and drug loading capacity of the microneedles are improved, the drying time is shortened, and the production and storage costs are reduced, making the HA soluble microneedles more suitable for large-scale production and application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113995951B_ABST
    Figure CN113995951B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing HA material for HA soluble microneedles and its application. The method comprises the following steps: preparing a HA material having a molecular weight of 10 3 kDa HA was mixed with 2-hydroxymethyl-β-cyclodextrin and stirred in purified water until dissolved; the mixed solution obtained by the solution was freeze-dried and the dried white powder was collected; the white powder was added with purified water to prepare a high-concentration polymer pre-gel; the high-concentration polymer pre-gel solution was placed on a four-dimensional rotator and rotated to mix until a needle-tip polymer gel was obtained; a molecular weight of 2×10 2 kDa HA is added with water to form a low-concentration polymer pre-gel, and the low-concentration polymer pre-gel is used as a backing polymer gel, wherein the concentration of the low-concentration polymer is lower than that of the high-concentration polymer pre-gel. And a microneedle patch prepared by the application method. The application can significantly improve the mechanical strength of the microneedle, can adapt to a variety of molds, and can achieve a higher drug loading and drug delivery efficiency for both lipophilic and hydrophilic drugs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of pharmaceutical preparations, and in particular to a method for preparing HA materials for HA soluble microneedles and applications thereof. Background Art

[0002] Microneedles are a new type of transdermal drug delivery method developed in the past 30 years. They are safe, efficient and painless. Microneedles pierce the stratum corneum, the largest barrier to transdermal drug penetration, in a minimally invasive manner, creating short-lived reversible micropores, which allow the drug to pass through the skin through the micropores and enter the human body to achieve a therapeutic effect. The length of the microneedles and the size of the array can be designed according to the site of action and the drug loading. Usually, microneedles are transdermal drug delivery devices with a length range of less than 2 mm, which can achieve painless, minimally invasive, and efficient drug delivery, and treat chronic diseases over time. Since the concept of "microneedles" was proposed in the 1970s, after years of research accumulation, microneedles have gradually become a relatively safe, accurate and efficient transdermal drug delivery method. It has also made breakthroughs in the field of clinical research and has gradually been put into market application, among which hyaluronic acid microneedles are the most widely used.

[0003] Hyaluronic acid (HA) is most suitable for making soluble microneedles because HA can be used to prepare biodegradable carriers with enhanced drug loading capacity, avoiding sharp waste with biological hazards and improving economic benefits. However, HA also has defects as the main material for microneedle preparation. Its strong water absorption and moisture retention makes the drying time of the microneedle array prepared by it long, basically not less than 72 hours, which greatly increases the production and storage costs and product backlog pressure, and it is difficult to quickly supply the huge market demand. Therefore, HA soluble microneedles still have a large room for improvement, and further research and improvement are needed to promote its development in the microneedle medical and beauty markets. However, at present, centrifugal injection molding, natural sedimentation or vacuum casting are mostly used for the preparation of HA microneedles in China. The microneedle formability, hardness and solubility of pure HA as a microneedle molding material cannot meet the requirements of production or medicinal use. Therefore, pure HA materials can no longer meet the needs of production and technological development. Further material mixing or physical and chemical modification is required to meet the requirements of production technology research and development and application. Moreover, there are technical problems such as the hardness of the needle tip of the soluble drug-loaded microneedle prepared from HA material does not meet the standard, the drug loading amount is small, and the drying cycle of the finished product is long. Summary of the invention

[0004] The purpose of the present invention is to address the above-mentioned problems existing in the prior art and to provide a method for preparing HA materials for HA soluble microneedles.

[0005] In order to achieve the above-mentioned invention object, the present invention adopts the following technical scheme: The method for preparing HA material for HA soluble microneedles comprises the following steps:

[0006] S100, molecular weight 10 3 kDa HA was mixed with 2-hydroxymethyl-β-cyclodextrin and stirred in purified water until dissolved;

[0007] S110, freeze-drying the dissolved mixed solution, and collecting the dried white powder;

[0008] S120, adding purified water to the white powder to prepare a high-concentration polymer pre-gel of 1% to 50% w / v;

[0009] S121, placing the high-concentration polymer pre-gel solution on a four-dimensional rotator and rotating and mixing until a needle tip polymer gel is obtained;

[0010] S130, take molecular weight 2×10 2 kDa HA is added with water to prepare a 1% to 50% w / v low-concentration polymer pre-gel, which is used as a backing polymer gel, wherein the concentration of the low-concentration polymer is lower than that of the high-concentration polymer pre-gel.

[0011] Working principle and beneficial effects: 1. Compared with the prior art, this application adopts a method of 3 kDa HA is mixed with 2-hydroxymethyl-β-cyclodextrin, which completely solves the problems of poor formability and weak drug loading capacity of pure HA materials, so that the hydroxyl group of HA and the carboxyl group of cyclodextrin in the system form a relatively stable and strong hydrogen bond, which greatly increases the stability, hardness and toughness of HA. After the carboxyl group and the hydroxyl group form a hydrogen bond, HA and 2-hydroxymethyl-β-cyclodextrin can be combined into a relatively stable ring structure, further increasing the drug loading capacity and formability of HA. At the same time, due to the presence of 2-hydroxymethyl-β-cyclodextrin, the water absorption and moisture retention of HA materials are weakened to a certain extent, which can greatly shorten the drying time of the subsequent finished microneedle array.

[0012] 2. Therefore, the high-concentration polymer preparatory gel and backing polymer gel prepared by this method are used for the preparation of existing HA soluble microneedles, which are transformed from the original HA gel of a certain concentration into a composite material formed by HA and 2-hydroxymethyl-β-cyclodextrin through hydrogen bonding, which greatly increases the mechanical strength of the microneedles, shortens the drying time of the microneedles, enhances the quality of the microneedles and saves production costs. It can adapt to the casting and molding of various molds, and can achieve higher drug loading and drug delivery efficiency for both lipophilic and hydrophilic drugs, enabling it to have the ability to further develop in the medical field.

[0013] 3. At the same time, the modification of 2-hydroxymethyl-β-cyclodextrin also inhibits the water absorption and moisture retention of HA to a certain extent, shortens the drying time of the finished microneedles, improves the overall production efficiency of microneedles, saves microneedle production costs and storage costs, and makes HA soluble microneedle products a better choice for large-scale production.

[0014] Furthermore, in step S100, the mass ratio of HA to 2-hydroxymethyl-β-cyclodextrin is 1-100:1-100.

[0015] Further, in step S100, the molecular weight of 10 3 kDa HA and 2-hydroxymethyl-β-cyclodextrin were mixed at a mass ratio of 1:5 and stirred in 10 mL of purified water until dissolved. This data is the preferred solution with the best effect.

[0016] Further, in step S120, the white powder is added with purified water to prepare a 15% w / v high concentration polymer pre-gel; in step S130, a 2×10 2 kDa HA, add water to prepare a low concentration polymer pre-gel of 10% w / v. This data is the preferred solution and has the best effect.

[0017] The method for preparing HA soluble microneedles comprises the following steps:

[0018] S000, slowly inserting the microneedle positive mold into a six-well plate filled with mixed dimethylsiloxane that has been allowed to stand to remove bubbles, evacuating the plate until tiny bubbles visible to the naked eye are completely removed, placing the six-well plate in a forced air drying oven to dry, and then removing the microneedle positive mold after cooling to room temperature to obtain a microneedle negative mold;

[0019] S100, preparing a needle tip polymer gel and a backing polymer gel using the above-mentioned HA material preparation method for HA soluble microneedles;

[0020] S200, placing the needle tip polymer gel in the microneedle negative mold and centrifuging until the position of the needle tip polymer gel is fixed, then increasing the centrifugal speed until the needle tip polymer gel completely enters the array of the microneedle negative mold, adding the backing polymer gel and centrifuging again until the surface of the backing polymer gel is completely horizontal, drying the microneedle negative mold, and obtaining a complete blank microneedle patch after drying.

[0021] The complete blank microneedle patch prepared by the above method has high mechanical strength and can achieve a high drug loading capacity and drug delivery efficiency for both lipophilic and hydrophilic drugs, which enables it to have the advantage of further development in the medical field.

[0022] Furthermore, in step S200, the rotation speed range of all centrifugal operations is 100 to 5000 rpm.

[0023] Furthermore, in step S200, the needle tip polymer gel is placed in the microneedle negative mold, centrifuged at 4°C, 1500rpm for 5 minutes until the position of the needle tip polymer gel is fixed, and centrifuged at 4°C, 3000rpm for 20 minutes to allow the needle tip polymer gel to completely enter the negative mold array; after centrifugation, the excess needle tip polymer gel is removed, and the low-concentration polymer gel is added, and the centrifugation is performed at 4°C at 2000rpm, 1500rpm, 1000rpm, and 500rpm for 5 minutes each, until the surface of the low-concentration polymer gel is completely horizontal.

[0024] The complete blank microneedle patch prepared using the above data has better effect.

[0025] Furthermore, in step S200, the microneedle negative mold is placed in a constant temperature and humidity chamber at a temperature of 20° C. and a humidity of 30% for drying for 48 hours. After drying, a complete drug-containing microneedle patch is obtained using tweezers.

[0026] Further, the following steps are included:

[0027] S201, taking the remaining white powder in step S100, mixing the indocyanine green model drug and the white powder at a ratio of 2:1 v / w, adding purified water to prepare a 15% m / v high-concentration polymer drug-containing gel, placing the high-concentration polymer drug-containing gel in the microneedle negative mold and centrifuging until the position of the high-concentration polymer drug-containing gel is fixed, then increasing the centrifugal speed until the high-concentration polymer drug-containing gel completely enters the array of the microneedle negative mold, adding the backing polymer gel and centrifuging again until the surface of the backing polymer gel is completely horizontal, drying the microneedle negative mold, and obtaining a complete drug-containing microneedle patch after drying.

[0028] This step discloses the preparation scheme of a complete drug-containing microneedle patch, which can be obtained by making simple changes directly on the basis of a complete blank microneedle patch, by changing the needle tip polymer gel to a high-concentration polymer drug-containing gel.

[0029] Furthermore, in step S000, the microneedle positive mold is a conical metal microneedle with an array number of 15×15, a single needle base diameter of 130μm, a tip diameter of 12μm, and a needle length of 800μm. Due to the increase in the strength of the raw materials, the present invention has made improvements to the array number and needle type design of the microneedles, so that the total number of microneedle arrays is increased to 15*15, and the needle length can reach 800μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is a schematic diagram of a flow chart of Embodiment 1 of the present invention;

[0031] Figure 2 is a schematic diagram of a flow chart of Embodiment 2 of the present invention;

[0032] Figure 3 It is a schematic diagram of the flow chart of Example 3 of the present invention. DETAILED DESCRIPTION

[0033] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.

[0034] The current prior art HA microneedle preparation mostly adopts centrifugal injection molding, natural sedimentation or vacuum casting. The microneedle formability, hardness and solubility of pure HA as a microneedle molding material cannot meet the requirements of production or medicinal use. Therefore, pure HA materials can no longer meet the needs of production and technological development. Further material mixing or physical and chemical modification is required to meet the requirements of production technology research and development and application. Moreover, the drug loading capacity of HA soluble microneedles has always limited its further development in the field of medicine. Due to the limited hardness and toughness of the material, the single needle length of pure HA microneedles is difficult to exceed 800μm, and the spacing between single microneedles is difficult to be less than 300μm, which greatly limits the maximum number of arrays that can be achieved by microneedle patches per unit area. Because the drug loading capacity of soluble microneedles depends on the ductility of the material, the drug loading capacity and the number of microneedles, therefore, when the microneedle material is determined, the number of microneedle arrays and the needle length greatly affect the drug loading capacity of the microneedles, making the existing microneedle preparation scheme extremely low in drug loading, and it is difficult to achieve an effective blood drug concentration in the body. The microneedle array prepared by HA has a long drying time, basically not less than 72 hours, due to the strong water absorption and moisturizing properties of HA itself. This defect prolongs the production cycle of microneedle finished products, greatly increases the production and storage costs of the products, and causes a certain amount of product backlog, making it difficult to quickly supply the huge market demand.

[0035] In order to solve the above technical problems, the present application proposes the following embodiments:

[0036] Example 1

[0037] like Figure 1 As shown, the method for preparing HA material for HA soluble microneedles comprises the following steps:

[0038] S100, molecular weight 10 3 kDa HA is mixed with 2-hydroxymethyl-β-cyclodextrin, and stirred in purified water until dissolved; wherein the mass ratio of HA to 2-hydroxymethyl-β-cyclodextrin is 1-100:1-100.

[0039] In fact, in this step, in order to improve the poor formability and drug loading capacity of pure HA material, the molecular weight of 10 3 kDa HA and 2-hydroxymethyl-β-cyclodextrin (2-HP-β-CD) were mixed at a mass ratio of 1:5 and stirred in 10 mL of purified water until dissolved. Since HA and 2-HP-β-CD were mixed and dissolved in a certain ratio, the hydroxyl group of HA in the system formed a relatively stable and strong hydrogen bond with the carboxyl group of cyclodextrin, which greatly increased the stability, hardness and toughness of HA. After the carboxyl group and the hydroxyl group formed a hydrogen bond, HA and 2-HP-β-CD could be combined into a relatively stable ring structure, further increasing the drug loading capacity and formability of HA. At the same time, due to the presence of 2-HP-β-CD, the water absorption and moisture retention of HA materials were weakened to a certain extent, which could greatly shorten the drying time of the subsequent finished microneedle array.

[0040] S110, freeze-drying the dissolved mixed solution, and collecting the dried white powder;

[0041] In fact, in this step, the best freezing environment should be controlled at minus 80 degrees Celsius for freeze drying, and the dried white powder is collected for later use.

[0042] S120, adding purified water to the white powder to prepare a high-concentration polymer pre-gel of 1% to 50% w / v;

[0043] In this step, the white powder is added with purified water to prepare a 15% w / v high concentration polymer pre-gel for later use, such as 10, 20, 30, 40% w / v.

[0044] S121, placing the high-concentration polymer pre-gel solution on a four-dimensional rotator and rotating and mixing for 12 hours until a needle tip polymer gel is obtained;

[0045] S130, take molecular weight 2×10 2 kDa HA is added with water to prepare a low-concentration polymer pre-gel of 1% to 50% w / v, and the low-concentration polymer pre-gel is used as a backing polymer gel, such as 10, 20, 30, or 40% w / v. The concentration of the low-concentration polymer is lower than that of the high-concentration polymer pre-gel.

[0046] In this way, the needle tip polymer gel and the backing polymer gel can be obtained as the preparation material of the microneedle.

[0047] Example 2

[0048] like Figure 2 As shown, this embodiment uses the needle tip polymer gel and the backing polymer gel obtained in Example 1 to prepare a complete blank microneedle patch, including the following steps:

[0049] S000, slowly inserting the microneedle positive mold into a six-well plate filled with mixed dimethylsiloxane (PDMS) that has been allowed to stand to remove bubbles, evacuating for 3 hours to completely remove tiny bubbles visible to the naked eye, placing the six-well plate in a 70° C. forced air drying oven for 2 hours, and removing the microneedle positive mold after cooling to room temperature to obtain a microneedle negative mold;

[0050] The number of microneedle positive mold arrays in this step is 15×15 conical metal microneedles (single needle base diameter 130μm, tip diameter 12μm, needle length 800μm). The purpose is to increase the number of microneedle arrays per unit area. It is precisely because of the increased strength of the raw materials that this type of microneedle positive mold can be used. The two are closely related technical solutions.

[0051] S100, preparing a needle tip polymer gel and a backing polymer gel using the HA material preparation method for HA soluble microneedles in Example 1;

[0052] S200, placing the needle tip polymer gel in the microneedle negative mold, centrifuging at 4°C, 1500rpm for 5 minutes until the position of the needle tip polymer gel is fixed, then increasing the centrifugal speed, and continuing to centrifuge at 4°C, 3000rpm for 20 minutes to allow the needle tip polymer gel to completely enter the array of the microneedle negative mold, removing excess needle tip polymer gel, adding a small amount of backing polymer gel, and centrifuging at 2000rpm, 1500rpm, 1000rpm, and 500rpm at 4°C for 5 minutes each. If the surface of the backing polymer gel has not reached a flat state, repeat the above operation until the surface of the backing polymer gel is completely horizontal, and place the microneedle negative mold in a constant temperature and humidity chamber at a temperature of 20°C and a humidity of 30% for drying for 48 hours. After drying, use tweezers to obtain a complete blank microneedle patch.

[0053] The high-concentration polymer preparatory gel and backing polymer gel prepared by the method are used for the preparation of existing HA soluble microneedles, which are transformed from the original HA gel of a certain concentration into a composite material formed by HA and 2-hydroxymethyl-β-cyclodextrin through hydrogen bonding, which greatly increases the mechanical strength of the microneedles, shortens the drying time of the microneedles, enhances the quality of the microneedles and saves production costs. The microneedles can be adapted to the casting and molding of various molds, and can achieve a higher drug loading amount and drug delivery efficiency for both lipophilic and hydrophilic drugs, enabling them to have the ability to be further developed in the medical field.

[0054] Example 3

[0055] like Figure 3 As shown, based on Example 1 and Example 2, the preparation of drug-loaded microneedles, that is, the preparation of a complete drug-containing microneedle patch, includes the following steps:

[0056] S000, slowly inserting the microneedle positive mold into a six-well plate filled with mixed dimethylsiloxane (PDMS) that has been allowed to stand to remove bubbles, evacuating for 3 hours to completely remove tiny bubbles visible to the naked eye, placing the six-well plate in a 70° C. forced air drying oven for 2 hours, and removing the microneedle positive mold after cooling to room temperature to obtain a microneedle negative mold;

[0057] S100, preparing a backing polymer gel and a white powder by using the HA material preparation method for HA soluble microneedles in Example 1;

[0058] S201, take the remaining white powder in step S100, mix the indocyanine green model drug and the white powder at a ratio of 2:1 v / w, add purified water to prepare a 15% m / v high-concentration polymer drug-containing gel, place the high-concentration polymer drug-containing gel in the microneedle negative mold, centrifuge at 4°C and 1500 rpm for 5 min until the high-concentration polymer drug-containing gel is fixed, then increase the centrifugal speed, and continue centrifuging at 4°C and 3000 rpm for 20 min to allow the high-concentration polymer drug-containing gel to completely enter the microneedle negative mold. In the array of the microneedle negative mold, remove excess high-concentration polymer drug-containing gel, add a small amount of backing polymer gel, and centrifuge at 2000rpm, 1500rpm, 1000rpm, and 500rpm at 4°C for 5 minutes each. If the surface of the backing polymer gel has not reached a flat state, repeat the above operation until the surface of the backing polymer gel is completely horizontal. Place the microneedle negative mold in a constant temperature and humidity chamber at a temperature of 20°C and a humidity of 30% and dry it for 48 hours. After drying, use tweezers to obtain the complete drug-containing microneedle patch.

[0059] In the above-mentioned embodiment, due to the further material improvement of the HA material, the hydroxyl and carboxyl groups between HA and 2-HP-β-CD form intermolecular hydrogen bonds, and the mechanical strength of the finished microneedles finally prepared is significantly improved, which can adapt to the casting and molding of various molds, and can achieve a higher drug loading and drug delivery efficiency for both lipophilic and hydrophilic drugs, so that it has the ability to be further developed in the medical field; at the same time, the modification of 2-HP-β-CD also inhibits the water absorption and moisture retention of HA to a certain extent, shortens the drying time of the finished microneedles, improves the overall production efficiency of the microneedles, saves the production cost and storage cost of the microneedles, and makes the HA soluble microneedle products a better choice for large-scale production.

[0060] The parts not described in detail in the present invention are prior art, so the present invention does not describe them in detail.

[0061] It is to be understood that the term "one" should be understood as "at least one" or "one or more", that is, in one embodiment, the number of an element may be one, while in another embodiment, the number of the element may be multiple, and the term "one" should not be understood as a limitation on the quantity.

[0062] Although more professional terms are used in this article, the possibility of using other terms is not excluded. These terms are used only to more conveniently describe and explain the essence of the present invention; interpreting them as any additional restrictions is contrary to the spirit of the present invention.

[0063] The present invention is not limited to the above-mentioned optimal implementation mode. Anyone can derive other various forms of products under the inspiration of the present invention. However, no matter what changes are made in the shape or structure, all technical solutions that are the same or similar to those of the present application fall within the protection scope of the present invention.

Claims

1. A method for preparing HA material for HA soluble microneedles, characterized in that: The following steps are involved: S100, molecular weight 10 3 kDa HA was mixed with 2-hydroxymethyl-β-cyclodextrin and stirred in purified water until dissolved; Wherein, the mass ratio of HA to 2-hydroxymethyl-β-cyclodextrin is 1~100:1~100; S110, freeze-drying the dissolved mixed solution, and collecting the dried white powder; S120, adding purified water to the white powder to prepare a high-concentration polymer pre-gel of 1% to 50% w / v; S121, placing the high-concentration polymer pre-gel solution on a four-dimensional rotator and rotating and mixing until a needle tip polymer gel is obtained; S130, take molecular weight 2×10 2 kDa HA is added with water to prepare a 1% to 50% w / v low-concentration polymer pre-gel, which is used as a backing polymer gel, wherein the concentration of the low-concentration polymer is lower than that of the high-concentration polymer pre-gel.

2. The method for preparing HA material for HA soluble microneedles according to claim 1, characterized in that: In step S100, the molecular weight of 10 3 kDa HA was mixed with 2-hydroxymethyl-β-cyclodextrin at a mass ratio of 1:5 and stirred in 10 mL of purified water until dissolved.

3. The method for preparing HA material for HA soluble microneedles according to claim 1, characterized in that: In step S120, the white powder is added with purified water to prepare a 15% w / v high concentration polymer pre-gel; in step S130, a 2×10 2 kDa HA was prepared by adding water to a 10% w / v low concentration polymer pre-gel.

4. A method for preparing HA soluble microneedles, characterized in that: The following steps are involved: S000, slowly inserting the microneedle positive mold into a six-well plate filled with mixed dimethylsiloxane that has been allowed to stand to remove bubbles, evacuating the plate until tiny bubbles visible to the naked eye are completely removed, placing the six-well plate in a forced air drying oven to dry, and then removing the microneedle positive mold after cooling to room temperature to obtain a microneedle negative mold; S100, preparing a needle tip polymer gel and a backing polymer gel by using the HA material preparation method for HA soluble microneedles according to any one of claims 1 to 3; S200, placing the needle tip polymer gel in the microneedle negative mold and centrifuging until the position of the needle tip polymer gel is fixed, then increasing the centrifugal speed until the needle tip polymer gel completely enters the array of the microneedle negative mold, adding the backing polymer gel and centrifuging again until the surface of the backing polymer gel is completely horizontal, drying the microneedle negative mold, and obtaining a complete blank microneedle patch after drying.

5. The method for preparing HA soluble microneedles according to claim 4, characterized in that: In step S200, the rotation speed range of all centrifugal operations is 100-5000 rpm.

6. The method for preparing HA soluble microneedles according to claim 5, characterized in that: In step S200, the needle tip polymer gel is placed in the microneedle negative mold, and centrifuged at 4°C and 1500 rpm for 5 min until the position of the needle tip polymer gel is fixed, and centrifuged at 4°C and 3000 rpm for 20 min to allow the needle tip polymer gel to completely enter the negative mold array; after centrifugation, the excess needle tip polymer gel is removed, and the low-concentration polymer gel is added, and the centrifugation is performed at 4°C at 2000 rpm, 1500 rpm, 1000 rpm, and 500 rpm for 5 min each, until the surface of the low-concentration polymer gel is completely horizontal.

7. The method for preparing HA soluble microneedles according to claim 6, characterized in that: In step S200, the microneedle negative mold is placed in a constant temperature and humidity chamber at a temperature of 20°C and a humidity of 30% for drying for 48 hours. After drying, a complete blank microneedle patch is obtained with tweezers.

8. The method for preparing HA soluble microneedles according to claim 4, characterized in that: The following steps are involved: S201, taking the remaining white powder in step S100, mixing the indocyanine green model drug and the white powder at a ratio of 2:1 v / w, adding purified water to prepare a 15% m / v high-concentration polymer drug-containing gel, placing the high-concentration polymer drug-containing gel in the microneedle negative mold and centrifuging until the position of the high-concentration polymer drug-containing gel is fixed, then increasing the centrifugal speed until the high-concentration polymer drug-containing gel completely enters the array of the microneedle negative mold, adding the backing polymer gel and centrifuging again until the surface of the backing polymer gel is completely horizontal, drying the microneedle negative mold, and obtaining a complete drug-containing microneedle patch after drying.

9. The method for preparing HA soluble microneedles according to any one of claims 4 to 8, characterized in that: In step S000, the microneedle positive mold is a conical metal microneedle array with an array number of 15×15, a single needle base diameter of 130 μm, a tip diameter of 12 μm, and a needle length of 800 μm.