Method for evaluating the aging resistance of whole composite insulators improved by electron irradiation

By preparing and processing mixed silicone rubber with different vulcanizing agent contents, and combining electronic irradiation and accelerated aging tests, the vulcanizing agent content and irradiation dose of the composite insulator were designed, which solved the improvement of the anti-aging performance of the entire composite insulator. Problem, extending its service life and improving operational safety.

CN114018968BActive Publication Date: 2024-12-06STATE GRID HUNAN ELECTRIC POWER COMPANY LIMITED +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111512737.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-11
Publication Date
2024-12-06
Estimated Expiration
2041-12-11

AI Technical Summary

Technical Problem

The prior art has failed to effectively improve the anti-aging performance of the entire composite insulator, especially the lack of key parameter design methods in the electronic radiation processing of silicone rubber umbrella skirts, resulting in the aging of composite insulators in harsh environments, affecting operational safety and life.

Method used

By preparing mixed silicone rubber with different vulcanizing agent content, high-temperature pre-vulcanization and electronic irradiation processing, the cross-linking density is tested using a variable temperature nuclear magnetic resonance analyzer, combined with an accelerated aging test chamber to evaluate the aging performance, the silicone rubber vulcanizing agent content and radiation are designed. Optimize the anti-aging properties of composite insulators according to the dose.

Benefits of technology

The evaluation and design of the electronic radiation of the entire composite insulator improves the anti-aging performance, extends its service life, improves the operational safety of on-site applications, and is suitable for composite insulators with AC and DC series voltage levels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114018968B_ABST
    Figure CN114018968B_ABST
Patent Text Reader

Abstract

The invention provides a method for evaluating the anti-aging performance of a whole composite insulator improved by electron irradiation, comprising: preparing mixed silicone rubber with different vulcanizer contents; completing high-temperature pre-vulcanization of a whole composite insulator shed of the mixed silicone rubber; completing electron irradiation processing of the whole composite insulator under different irradiation dose conditions; testing the crosslinking density of the silicone rubber shed of the composite insulator after electron irradiation with different vulcanizer contents and different irradiation doses, and obtaining the composite insulator and the vulcanizer content and irradiation dose corresponding to the maximum crosslinking density; carrying out an accelerated aging test for a given time on the composite insulator with the maximum crosslinking density and the unirradiated composite insulator; taking out the composite insulator at predetermined intervals, and measuring the aging performance parameters of the silicone rubber shed of the composite insulator; and comparing the performance parameters with those of the unirradiated high-temperature vulcanized composite insulator, so as to complete the evaluation of the anti-aging performance of the whole composite insulator improved by electron irradiation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of status assessment of power transmission and transformation equipment, and in particular relates to a method for assessing the anti-aging performance of an entire composite insulator improved by electron irradiation. Background Art

[0002] Composite insulators have been widely used in my country's high-voltage transmission lines in recent years due to their light weight, strong anti-pollution flashover capability and easy on-site installation. However, composite insulators operate outdoors for a long time, and their composite silicone rubber shed materials not only need to withstand the effects of electric fields and various stresses, but are also subject to the combined effects of a series of severe weather and environmental erosion such as light, rain, dust, high and low temperatures, freezing, and dirt, resulting in reduced electrochemical properties and thermal stability and accelerated aging. Severely aged composite insulators may even experience external insulation flashover, string drop and other serious faults under operating voltage. According to surveys by domestic and foreign power research institutions, the proportion of composite insulators with aging failures such as powdering, cracking and corrosion on the shed surface after more than 10 years of operation is as high as 57%, and aging failure is also one of the main causes of composite insulator failure in my country.

[0003] In order to effectively improve the anti-aging performance of silicone rubber materials for composite insulators and extend the service life of composite insulators, currently, special anti-aging additives (such as fluoropolysiloxane, nanosilicate, etc.) are added to the silicone rubber material formula to improve the mechanical and thermal properties of composite silicone rubber sheds. However, the above additives have poor compatibility with silicone rubber, which will increase the complexity of the silicone rubber vulcanization process. In addition, the preparation process of the additives themselves is complex and costly, which is not suitable for large-scale production and application. Electron irradiation processing is a new processing method that uses ionizing radiation to act on substances to produce chemical changes, phase changes or microstructural changes to achieve material modification. When applied to composite insulators, it mainly bombards silicone rubber polymer materials through high-energy electron beams, so that the original chain molecular structure of the material becomes a three-dimensional network structure, which can improve the material's heat and weather resistance, and thus improve the anti-aging performance and life. It is a new and effective means to solve the anti-aging performance of composite insulators. However, the research on the performance of composite insulators modified by electron irradiation in the prior art mainly focuses on the silicone rubber material itself and a certain parameter thereof, and does not involve the improvement of the anti-aging performance of the entire composite insulator, and does not provide a design method for key parameters such as the content of vulcanizing agent and irradiation dose of silicone rubber sheds during irradiation processing. In summary, due to the differences in structural shape between the entire composite insulator and the single-piece silicone rubber shed, the existing electron irradiation processing technology and performance parameter change law of silicone rubber sheds cannot be applied to the entire composite insulator.

[0004] Therefore, in view of the problems and defects of the existing methods for improving the anti-aging performance of composite insulators, it is urgent to propose an electron irradiation anti-aging performance improvement and evaluation method that is applicable to the entire composite insulator and takes into account key parameters such as the silicone rubber vulcanizer content and irradiation dose, so as to provide technical support for improving the operating safety and aging life of composite insulators after field application. Summary of the invention

[0005] The purpose of the present invention is to provide a method for evaluating the anti-aging performance of an entire composite insulator improved by electron irradiation. This method can be used to design key parameters such as the silicone rubber vulcanizer content and irradiation dose in the process of improving the anti-aging performance of the entire composite insulator by electron irradiation, and at the same time, the anti-aging performance evaluation of the composite insulator can be completed, thereby improving the operating safety and aging life after field application.

[0006] To achieve the above purpose, an embodiment of the present invention provides a method for evaluating the effect of electron irradiation on the anti-aging performance of a composite insulator, comprising:

[0007] Step S1: preparing mixed silicone rubber with different vulcanizing agent contents;

[0008] Step S2: completing high temperature pre-vulcanization of the entire composite insulator shed made of the mixed silicone rubber on an injection molding machine;

[0009] Step S3: Arranging an electron irradiation processing platform for the entire composite insulator to complete electron irradiation processing of the entire composite insulator under different irradiation dose conditions;

[0010] Step S4: using a variable temperature nuclear magnetic resonance analyzer, testing the crosslink density of the silicone rubber shed of the composite insulator after electron irradiation with different vulcanizing agent contents and different irradiation doses in step S3, and obtaining the composite insulator, vulcanizing agent content, and irradiation dose corresponding to the maximum crosslinking density;

[0011] Step S5: conducting an accelerated aging test for a given time on the composite insulator with the maximum cross-linking density and the non-irradiated composite insulator in an accelerated aging test chamber.

[0012] Step S6: taking out the composite insulator at predetermined intervals (e.g., 500h-1000h) and measuring the aging performance parameters of the silicone rubber shed of the composite insulator;

[0013] Step S7: comparing the performance parameters of the high-temperature (eg, 160° C.-200° C.) vulcanized composite insulators without irradiation to complete the evaluation of the electron irradiation-enhanced anti-aging performance of the entire composite insulator.

[0014] In the embodiment of the present invention, the step S1 includes:

[0015] Step S11: prepare raw materials according to the formula components of 90-100 parts by mass of methyl vinyl silicone rubber, 120-130 parts of aluminum hydroxide, 25-35 parts of fumed silica, 3-4 parts of iron oxide, 4-6 parts of α-aluminum oxide, 3-5 parts of hydroxy silicone oil, 0.5-1 part of silane coupling agent, and 1.5-2.5 parts of nano zinc oxide;

[0016] Step S12: Select 1,1-di-tert-butylperoxide-3,3,5-trimethylcyclohexane crosslinking agent as the silicone rubber vulcanizer, change its content by 0-1.5 parts, mix it with the raw materials, and process it in the order of raw rubber internal mixing → molding and filtering → kneading → open mixing to obtain mixed silicone rubber with different vulcanizer contents.

[0017] In this embodiment of the present invention, step S2 includes:

[0018] Step S21: turning on the working power of the injection molding machine, placing the composite insulator core rod into the shed vulcanization mold and securely fixing it, and heating the shed vulcanization mold to increase the temperature;

[0019] Step S22: when the temperature of the shed vulcanization mold rises to a set temperature T (e.g., 160° C.-200° C.), the heat preservation mode is turned on to maintain the temperature, and the mixed silicone rubber is placed in the injection barrel of the injection molding machine;

[0020] Step S23: setting the pressure P of the injection molding machine (e.g., 16MPa-20MPa), injecting the mixed silicone rubber into the heated shed vulcanization mold through the injection nozzle, and starting high-temperature pre-vulcanization under the action of the pressure P and the temperature T;

[0021] Step S24: when the vulcanization time reaches a set time H (e.g., 5 min-15 min), the mold heating power supply is turned off, and the composite insulator is taken out from the shed vulcanization mold to obtain a composite insulator pre-vulcanized product of the mixed rubber with a given vulcanizing agent content;

[0022] Step S25: repeating steps S21 to S24 until the high-temperature pre-vulcanization of the entire composite insulator shed containing the mixed rubber with the entire vulcanizing agent content is completed.

[0023] In this embodiment of the present invention, step S3 includes:

[0024] Step S31: Arrange an electron irradiation processing platform for the entire composite insulator, wherein the electron irradiation processing platform includes an electron accelerator, a beam-under-beam trolley, a conveyor belt, and air cooling equipment;

[0025] The electron accelerator is used to generate a high-energy electron beam, the entire composite insulator to be irradiated is placed on the rotating part of the under-beam trolley, the under-beam trolley is fixed on the conveyor belt, and the air cooling device is used to supply air to the beam area to maintain a constant temperature and prevent the local temperature rise caused by the electron beam bombardment from affecting the irradiation processing effect;

[0026] Step S32: Turn on the working power of the electron irradiation processing platform, turn on the power of the air cooling device and set the air outlet temperature, set the rotation speed of the rotating parts of the under-beam trolley and the transmission speed v of the conveyor belt, and when the under-beam trolley is transmitted to the electron beam flow area of ​​the electron accelerator, the electron beam bombards the composite insulator shed silicone rubber material to complete the electron irradiation processing, wherein the irradiation dose G of the composite insulator is calculated according to formula (1):

[0027]

[0028] Among them, U is the accelerator output voltage, I is the beam current, t is the irradiation time of the composite insulator, and M is the mass of the silicone rubber of the composite insulator;

[0029] Step S33: changing the irradiation dose of the composite insulator by adjusting the conveyor belt speed, and repeating step S32 until the electron irradiation processing of the composite insulator under all irradiation dose conditions is completed.

[0030] In the embodiment of the present invention, step S5 includes:

[0031] Step S51: constructing a composite insulator aging test platform, the aging test platform comprising a high-voltage test transformer, a wall bushing, an aging test chamber, a composite insulator sample, a bracket, a temperature and humidity control system, a salt spray generation system, an ultraviolet light generation system, and a rainfall spray system; wherein the composite insulator sample is suspended on a special bracket on the top of the aging test chamber, the high-voltage test transformer is used to apply an operating voltage to the composite insulator, and the temperature and humidity control system, the salt spray generation system, the ultraviolet light generation system, and the rainfall spray system are used to provide the composite insulator sample with adjustable temperature and humidity, rainfall, fog vapor concentration, and light intensity, respectively;

[0032] Step S52: Turn on the working power of the aging test box, set the temperature and humidity, rainfall, fog vapor concentration, and light intensity of the artificial climate room through the temperature and humidity control system, salt fog generating system, ultraviolet light generating system, and rainfall spraying system, apply operating voltage to the composite insulator through the test transformer, set the aging test time T (for example, 2000h-5000h), and start the accelerated aging test of the composite insulator.

[0033] In this embodiment of the present invention, step S6 includes:

[0034] Step S61: taking out a number of irradiated and non-irradiated composite insulators at a preset time t (e.g., 500 h) from the start of the aging test;

[0035] Step S62: Cut a piece of silicone rubber shed from the upper, middle and lower parts of each composite insulator, clean the stains and residues on the surface of the silicone rubber shed with ultrapure water in an ultrasonic cleaner, and reserve them as performance test samples after drying;

[0036] Step S63: Cut a portion of each silicone rubber shed sample in step S62 to form a standard dumbbell-shaped sample and record the sample width b and thickness d. Use an electronic universal testing machine to test the tensile force p of the sample and use formula (2) to calculate the tensile strength σ of the sample. t The average tensile strength of the samples at different positions of the upper, middle and lower parts is taken as the tensile strength of the entire composite insulator shed.

[0037]

[0038] Step S64: intercept a portion of each silicone rubber shed sample in step S62, and use a variable temperature nuclear magnetic resonance analyzer to test the crosslinking density ρ of the portion, and take the average crosslinking density of the silicone rubber shed at different positions of the upper, middle and lower parts as the crosslinking density of the shed of the entire composite insulator;

[0039] Step S65: intercept a portion of each silicone rubber shed sample in step S62, use a contact angle tester to test the contact angle between a water droplet and the surface of the silicone rubber material, and take the average value of the contact angles of the silicone rubber shed surface at different positions of the upper, middle and lower parts as the contact angle of the shed of the entire composite insulator;

[0040] Step S66: intercept a portion of each silicone rubber shed sample in step S62, cut it into a long rectangular sample and record the sample thickness d, use a plate breakdown voltage tester to test the breakdown voltage V of the long rectangular sample, use formula (3) to calculate the breakdown field strength E, and use the average breakdown field strength of the silicone rubber shed at different positions of the upper, middle and lower parts as the breakdown field strength of the entire composite insulator shed.

[0041]

[0042] In the embodiment of the present invention, t=T / N, where N is the total number of times the composite insulator is taken out.

[0043] In the embodiment of the present invention, step S7 includes:

[0044] Step S71: Analyze the functional relationship between the tensile strength, crosslinking density, contact angle, breakdown field strength and aging time t of the irradiated and unirradiated composite insulator sheds according to the data obtained in step S6, and fit the functional relationship, wherein the functions of the tensile strength, crosslinking density, contact angle, breakdown field strength and aging time t of the irradiated composite insulator shed are respectively denoted as σ 辐照 (t),ρ 辐照 (t),θ 辐照 (t), E 辐照 (t); the tensile strength, crosslinking density, contact angle, breakdown field strength of the unirradiated composite insulator shed and the aging time t are respectively denoted as σ 普通 (t),ρ 普通 (t),θ 普通 (t), E 普通 (t);

[0045] Step S72: According to the minimum allowable tensile strength value σ of the entire composite insulator shed min , minimum allowable value of crosslink density ρ min , the minimum allowable contact angle θ min , Minimum allowable value of breakdown field strength E min According to formulas (4)-(7), the tensile strength life, cross-linking density life, contact angle life and breakdown field strength life of electron irradiated insulators and ordinary insulators are calculated, where the tensile strength life, cross-linking density life, contact angle life and breakdown field strength life of electron irradiated insulators are denoted as T σ辐照 , T ρ辐照 , T θ辐照 , T E辐照 The tensile strength life, cross-linking density life, contact angle life and breakdown field strength life of ordinary insulators are denoted as T σ普通 , T ρ普通 , T θ普通 , T E普通 ,

[0046]

[0047]

[0048]

[0049]

[0050] Among them, σ -1 辐照 (σ), ρ -1 辐照 (ρ), θ -1 辐照 (θ), E -1 辐照(E), σ -1 普通 (σ), ρ -1 普通 (ρ), θ -1 普通 (θ), E -1 普通 (E) are σ 辐照 (t),ρ 辐照 (t),θ 辐照 (t), E 辐照 (t),σ 普通 (t),ρ 普通 (t),θ 普通 (t), E 普通 The inverse function of (t);

[0051] Step S73: Compare the lifespans of the corresponding parameters of the electron-irradiated composite insulator and the ordinary composite insulator according to formula (8), and take the minimum value k as the ratio of the anti-aging lifespan of the entire composite insulator that can be improved by electron irradiation:

[0052]

[0053] In an embodiment of the present invention, the aging performance parameter includes at least one of the following:

[0054] Tensile strength, cross-link density, hydrophobic angle, breakdown field strength.

[0055] Through the above technical scheme, (1) the entire composite insulator silicone rubber shed can be subjected to electron irradiation and anti-aging performance evaluation, providing technical support for improving the aging life of the entire composite insulator; (2) the key parameters such as the silicone rubber vulcanizer content and irradiation dose in the electron irradiation processing to improve the anti-aging performance of the composite insulator can be designed to improve the operating safety and aging life after field application; (3) the test and aging performance evaluation methods are easy to implement and highly operational, providing a new, complete and reliable design scheme for improving the anti-aging performance and operating life of composite insulators in harsh environments; (4) it is suitable for electron irradiation processing and evaluation of composite insulators of AC and DC series voltage levels to improve anti-aging performance.

[0056] Other features and advantages of the embodiments of the present invention will be described in detail in the subsequent detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] The accompanying drawings are used to provide a further understanding of the embodiments of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the embodiments of the present invention, but do not constitute a limitation on the embodiments of the present invention. In the accompanying drawings:

[0058] Figure 1A flow chart of a method for evaluating the improvement of the anti-aging performance of a whole composite insulator by electron irradiation according to an embodiment of the present invention is schematically shown;

[0059] Figure 2 A schematic diagram of an electron irradiation processing platform for a whole composite insulator according to an embodiment of the present invention is shown;

[0060] Figure 3 A schematic structural diagram of a composite insulator aging test platform according to an embodiment of the present invention is shown schematically. DETAILED DESCRIPTION

[0061] The specific implementation of the embodiment of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the embodiment of the present invention, and is not used to limit the embodiment of the present invention.

[0062] In the embodiment of the present invention, the common composite insulator may refer to a composite insulator that has not been electron irradiated.

[0063] Figure 1 The flowchart of the method for evaluating the electron irradiation to improve the anti-aging performance of the whole composite insulator according to an embodiment of the present invention is schematically shown. Figure 1 As shown, in an embodiment of the present invention, the method for evaluating the anti-aging performance of the entire composite insulator improved by electron irradiation may include the following steps:

[0064] Step S1: preparing mixed silicone rubber with different vulcanizing agent contents;

[0065] Step S2: completing high temperature pre-vulcanization of the entire composite insulator shed made of the mixed silicone rubber on an injection molding machine;

[0066] Step S3: Arranging an electron irradiation processing platform for the entire composite insulator to complete electron irradiation processing of the entire composite insulator under different irradiation dose conditions;

[0067] Step S4: using a variable temperature nuclear magnetic resonance analyzer, testing the crosslink density of the silicone rubber shed of the composite insulator after electron irradiation with different vulcanizing agent contents and different irradiation doses in step S3, and obtaining the composite insulator, vulcanizing agent content, and irradiation dose corresponding to the maximum crosslinking density;

[0068] Step S5: conducting an accelerated aging test for a given time on the composite insulator with the maximum cross-linking density and the unirradiated composite insulator in an accelerated aging test chamber;

[0069] Step S6: taking out the composite insulator at predetermined intervals (e.g., 500h-1000h) and measuring the aging performance parameters of the silicone rubber shed of the composite insulator;

[0070] Step S7: comparing the performance parameters of the high-temperature (eg, 160° C.-200° C.) vulcanized composite insulators without irradiation to complete the evaluation of the electron irradiation-enhanced anti-aging performance of the entire composite insulator.

[0071] In the embodiment of the present invention, the step S1 includes:

[0072] Step S11: prepare raw materials according to the formula components of 90-100 parts by mass of methyl vinyl silicone rubber, 120-130 parts of aluminum hydroxide, 25-35 parts of fumed silica, 3-4 parts of iron oxide, 4-6 parts of α-aluminum oxide, 3-5 parts of hydroxy silicone oil, 0.5-1 part of silane coupling agent, and 1.5-2.5 parts of nano zinc oxide;

[0073] Step S12: Select 1,1-di-tert-butylperoxide-3,3,5-trimethylcyclohexane crosslinking agent as the silicone rubber vulcanizer, change its content by 0-1.5 parts, mix it with the raw materials, and process it in the order of raw rubber internal mixing → molding and filtering → kneading → open mixing to obtain mixed silicone rubber with different vulcanizer contents.

[0074] In this embodiment of the present invention, step S2 includes:

[0075] Step S21: turning on the working power of the injection molding machine, placing the composite insulator core rod into the shed vulcanization mold and securely fixing it, and heating the shed vulcanization mold to increase the temperature;

[0076] Step S22: when the temperature of the shed vulcanization mold rises to a set temperature T (e.g., 160° C.-200° C.), the heat preservation mode is turned on to maintain the temperature, and the mixed silicone rubber is placed in the injection barrel of the injection molding machine;

[0077] Step S23: setting the pressure P of the injection molding machine (e.g., 16MPa-20MPa), injecting the mixed silicone rubber into the heated shed vulcanization mold through the injection nozzle, and starting high-temperature pre-vulcanization under the action of the pressure P and the temperature T;

[0078] Step S24: when the vulcanization time reaches a set time H (e.g., 5 min-15 min), the mold heating power supply is turned off, and the composite insulator is taken out from the shed vulcanization mold to obtain a composite insulator pre-vulcanized product of the mixed rubber with a given vulcanizing agent content;

[0079] Step S25: repeating steps S21 to S24 until the high-temperature pre-vulcanization of the entire composite insulator shed containing the mixed rubber with the entire vulcanizing agent content is completed.

[0080] In this embodiment of the present invention, step S3 includes:

[0081] Step S31: Arrange an electron irradiation processing platform for the entire composite insulator, wherein the electron irradiation processing platform includes an electron accelerator, a beam-under-beam trolley, a conveyor belt, and air cooling equipment;

[0082] The electron accelerator is used to generate a high-energy electron beam, the entire composite insulator to be irradiated is placed on the rotating part of the under-beam trolley, the under-beam trolley is fixed on the conveyor belt, and the air cooling device is used to supply air to the beam area to maintain a constant temperature and prevent the local temperature rise caused by the electron beam bombardment from affecting the irradiation processing effect;

[0083] Step S32: Turn on the working power of the electron irradiation processing platform, turn on the power of the air cooling device and set the air outlet temperature, set the rotation speed of the rotating parts of the under-beam trolley and the transmission speed v of the conveyor belt, and when the under-beam trolley is transmitted to the electron beam flow area of ​​the electron accelerator, the electron beam bombards the composite insulator shed silicone rubber material to complete the electron irradiation processing, wherein the irradiation dose G of the composite insulator is calculated according to formula (1):

[0084]

[0085] Among them, U is the accelerator output voltage, I is the beam current, t is the irradiation time of the composite insulator, and M is the mass of the silicone rubber of the composite insulator;

[0086] Step S33: changing the irradiation dose of the composite insulator by adjusting the conveyor belt speed, and repeating step S32 until the electron irradiation processing of the composite insulator under all irradiation dose conditions is completed.

[0087] In the embodiment of the present invention, step S5 includes:

[0088] Step S51: constructing a composite insulator aging test platform, the aging test platform comprising a high-voltage test transformer, a wall bushing, an aging test chamber, a composite insulator sample, a bracket, a temperature and humidity control system, a salt spray generation system, an ultraviolet light generation system, and a rainfall spray system; wherein the composite insulator sample is suspended on a special bracket on the top of the aging test chamber, the high-voltage test transformer is used to apply an operating voltage to the composite insulator, and the temperature and humidity control system, the salt spray generation system, the ultraviolet light generation system, and the rainfall spray system are used to provide the composite insulator sample with adjustable temperature and humidity, rainfall, fog vapor concentration, and light intensity, respectively;

[0089] Step S52: Turn on the working power of the aging test box, set the temperature and humidity, rainfall, fog vapor concentration, and light intensity of the artificial climate room through the temperature and humidity control system, salt fog generating system, ultraviolet light generating system, and rainfall spraying system, apply operating voltage to the composite insulator through the test transformer, set the aging test time T (for example, 2000h-5000h), and start the accelerated aging test of the composite insulator.

[0090] In this embodiment of the present invention, step S6 includes:

[0091] Step S61: taking out a number of irradiated and non-irradiated composite insulators at a preset time t (e.g., 500 h) from the start of the aging test;

[0092] Step S62: Cut a piece of silicone rubber shed from the upper, middle and lower parts of each composite insulator, clean the stains and residues on the surface of the silicone rubber shed with ultrapure water in an ultrasonic cleaner, and reserve them as performance test samples after drying;

[0093] Step S63: Cut a portion of each silicone rubber shed sample in step S62 to form a standard dumbbell-shaped sample and record the sample width b and thickness d. Use an electronic universal testing machine to test the tensile force p of the sample and use formula (2) to calculate the tensile strength σ of the sample. t The average tensile strength of the samples at different positions of the upper, middle and lower parts is taken as the tensile strength of the entire composite insulator shed.

[0094]

[0095] Step S64: intercept a portion of each silicone rubber shed sample in step S62, and use a variable temperature nuclear magnetic resonance analyzer to test the crosslinking density ρ of the portion, and take the average crosslinking density of the silicone rubber shed at different positions of the upper, middle and lower parts as the crosslinking density of the shed of the entire composite insulator;

[0096] Step S65: intercept a portion of each silicone rubber shed sample in step S62, use a contact angle tester to test the contact angle between a water droplet and the surface of the silicone rubber material, and take the average value of the contact angles of the silicone rubber shed surface at different positions of the upper, middle and lower parts as the contact angle of the shed of the entire composite insulator;

[0097] Step S66: intercept a portion of each silicone rubber shed sample in step S62, cut it into a long rectangular sample and record the sample thickness d, use a plate breakdown voltage tester to test the breakdown voltage V of the long rectangular sample, use formula (3) to calculate the breakdown field strength E, and use the average breakdown field strength of the silicone rubber shed at different positions of the upper, middle and lower parts as the breakdown field strength of the entire composite insulator shed.

[0098]

[0099] In the embodiment of the present invention, t=T / N, where N is the total number of times the composite insulator is taken out.

[0100] In the embodiment of the present invention, step S7 includes:

[0101] Step S71: Analyze the functional relationship between the tensile strength, crosslinking density, contact angle, breakdown field strength and aging time t of the irradiated and unirradiated composite insulator sheds according to the data obtained in step S6, and fit the functional relationship, wherein the functions of the tensile strength, crosslinking density, contact angle, breakdown field strength and aging time t of the irradiated composite insulator shed are respectively denoted as σ 辐照 (t),ρ 辐照 (t),θ 辐照 (t), E 辐照 (t); the tensile strength, crosslinking density, contact angle, breakdown field strength of the unirradiated composite insulator shed and the aging time t are respectively denoted as σ 普通 (t),ρ 普通 (t),θ 普通 (t), E 普通 (t);

[0102] Step S72: According to the minimum allowable tensile strength value σ of the entire composite insulator shed min , minimum allowable value of crosslink density ρ min , the minimum allowable contact angle θ min , Minimum allowable value of breakdown field strength E min According to formulas (4)-(7), the tensile strength life, cross-linking density life, contact angle life and breakdown field strength life of electron irradiated insulators and ordinary insulators are calculated, where the tensile strength life, cross-linking density life, contact angle life and breakdown field strength life of electron irradiated insulators are denoted as T σ辐照 , T ρ辐照 , T θ辐照 , T E辐照 The tensile strength life, cross-linking density life, contact angle life and breakdown field strength life of ordinary insulators are denoted as T σ普通 , T ρ普通 , T θ普通 , T E普通 ,

[0103]

[0104]

[0105]

[0106]

[0107] Among them, σ -1 辐照 (σ), ρ -1 辐照 (ρ), θ -1 辐照 (θ), E -1 辐照(E), σ -1 普通 (σ), ρ -1 普通 (ρ), θ -1 普通 (θ), E -1 普通 (E) are σ 辐照 (t),ρ 辐照 (t),θ 辐照 (t), E 辐照 (t),σ 普通 (t),ρ 普通 (t),θ 普通 (t), E 普通 The inverse function of (t);

[0108] Step S73: Compare the lifespans of the corresponding parameters of the electron-irradiated composite insulator and the ordinary composite insulator according to formula (8), and take the minimum value k as the ratio of the anti-aging lifespan of the entire composite insulator that can be improved by electron irradiation:

[0109]

[0110] In an embodiment of the present invention, the aging performance parameter includes at least one of the following:

[0111] Tensile strength, cross-link density, hydrophobic angle, breakdown field strength.

[0112] The embodiments of the present invention are further described in detail below with reference to the accompanying drawings and the "FXBW-10 / 70" type 10kV whole composite insulator electron irradiation improvement and evaluation as examples.

[0113] (1) Preparation of mixed silicone rubber with different vulcanizer contents.

[0114] (1.1) Prepare the raw materials according to the formula composition of 100 parts by mass of methyl vinyl silicone rubber, 130 parts by mass of aluminum hydroxide, 30 parts by mass of fumed silica, 3.75 parts by mass of iron oxide, 5 parts by mass of α-aluminum oxide, 4 parts by mass of hydroxy silicone oil, 0.5 parts by mass of silane coupling agent, and 1.8 parts by mass of nano zinc oxide.

[0115] (1.2) Select 1,1-di-tert-butyl peroxide-3,3,5-trimethylcyclohexane crosslinking agent as the silicone rubber vulcanizer, change its content to 0, 0.3, 0.6, and 0.9 parts, mix it with the raw materials in step (1.1), and process it in the order of raw rubber mixing → molding and filtering → kneading → open mixing to obtain mixed silicone rubber with different vulcanizer contents.

[0116] (2) High temperature pre-vulcanization of the FXBW-10 / 70 type 10kV composite insulator shed with silicone rubber having a vulcanizing agent content of 0-0.9 parts is completed on an injection molding machine:

[0117] (2.1) Select the injection molding machine of model HYZ-500B, turn on its 380V working power supply, put the 10kV composite insulator core rod into the shed vulcanization mold and fix it securely, and heat the mold to increase the temperature.

[0118] (2.2) When the mold temperature rises to the set temperature of 180°C, the insulation mode is turned on to maintain the temperature, and the mixed silicone rubber with a vulcanizer content of 0 obtained in step (1) is placed in the injection cylinder of the injection molding machine.

[0119] (2.3) The pressure of the injection molding machine is set to 18 MPa, and the mixed silicone rubber with a vulcanizer content of 0 is injected into the heated shed mold through the injection nozzle, and high-temperature pre-vulcanization is started under the above pressure and temperature.

[0120] (2.4) When the vulcanization time reaches the set value of 10 minutes, the mold heating power is turned off, and the composite insulator is taken out of the mold to obtain a 10kV composite insulator pre-vulcanized product with a vulcanizer content of 0.

[0121] (2.5) Repeat steps (2.1) to (2.4) until the high temperature pre-vulcanization of the FXBW-10 / 70 type 10 kV composite insulator shed with the vulcanizing agent content of 0.3, 0.6, and 0.9 parts of the mixed rubber is completed.

[0122] (3) Arrange the electron irradiation processing platform for the entire composite insulator to complete the electron irradiation processing of the entire composite insulator under different irradiation dose conditions.

[0123] (3.1) By attachment Figure 2 Arrange the whole composite insulator electron irradiation processing platform. The processing platform includes an electron accelerator 10, a beam trolley device 20, a conveyor belt 30, and an air cooling device 40. The electron accelerator 10 is used to generate a high-energy electron beam, and the whole composite insulator 50 to be irradiated is placed on the rotating part of the beam trolley device 20. The beam trolley device 20 is fixed on the electron irradiation processing platform conveyor belt 30. The air cooling device 40 is used to supply air to the beam area to keep the temperature constant and prevent the local temperature rise caused by the electron beam bombardment from affecting the irradiation processing effect.

[0124] (3.2) The 10 kV composite insulator with a certain vulcanizing agent content in step (2) is placed on the rotating part of the trolley device under the beam of the electron irradiation processing platform, and the 380 V working power supply of the electron irradiation processing platform is turned on. The electron accelerator is a 5 MeV DD accelerator with an average beam current of 1.5 mA, a beam scanning area size of 1350 × 1350 mm, and an energy instability of <1%. The 380 V power supply of the air cooling device is turned on and the air outlet temperature is set to 20 ° C. The speed of the rotating part of the trolley device under the beam is set to 6 r / min and the conveyor belt transmission speed is set to 3.5 m / min. When the trolley under the beam is transmitted to the electron beam area of ​​the electron accelerator, the electron beam bombards the silicone rubber material of the composite insulator shed to complete the electron irradiation processing. The irradiation dose G of the composite insulator is calculated according to the following formula.

[0125]

[0126] In formula (1), U is the accelerator output voltage, I is the beam current, t is the irradiation time of the composite insulator, and M is the mass of the silicone rubber of the composite insulator.

[0127] For the 10 kV whole composite insulator with different vulcanizing agent contents obtained in step (2), the irradiation doses are respectively 0, 30, 60, 90, and 120 kGy, so that the combinations of different vulcanizing agent contents and irradiation doses are shown in Table 1.

[0128] Table 1 Combined working conditions of 10kV composite insulators with different vulcanizing agent contents and irradiation doses

[0129]

[0130] (3.3) The irradiation dose of the composite insulator is changed by adjusting the conveyor belt speed, and step (3.2) is repeated until the electron irradiation processing of the 10 kV composite insulator under all the different irradiation doses and vulcanizing agent contents in Table 1 is completed.

[0131] (4) Using a "VTMR20-010V" variable temperature nuclear magnetic resonance analyzer, the crosslink density of the silicone rubber shed of the composite insulator after electron irradiation with different vulcanizer contents and irradiation doses in step (3) was tested, and the measurement results are shown in Table 2. As can be seen from Table 2, when the vulcanizer content is 0.6 parts and the irradiation dose is 60 kGy, the crosslink density of the silicone rubber shed of the 10 kV composite insulator after electron irradiation reaches a maximum value of 3.52 mol / cm3, and the composite insulator, vulcanizer content, and irradiation dose corresponding to the maximum crosslink density are obtained.

[0132] Table 2 Crosslink density of silicone rubber shed of 10kV composite insulator (unit: mol / cm3)

[0133]

[0134] (5) In an accelerated aging test chamber, an accelerated aging test is performed for a given time on the 10 kV composite insulator with the maximum crosslinking density in step (4) and the unirradiated 10 kV ordinary composite insulator (corresponding to a vulcanizing agent content of 0.3 parts and an irradiation dose of 0).

[0135] (5.1) According to the attached Figure 3 A composite insulator aging test platform is constructed. The aging test platform includes a high-voltage test transformer 1, a wall bushing 2, an aging test chamber 3, a composite insulator sample 4, a bracket 5, a temperature and humidity control system 6, a salt spray generation system 7, an ultraviolet light generation system 8, and a rain spray system 9. The composite insulator samples 4 (6 of each 10kV composite insulators and 10kV ordinary composite insulators with maximum cross-linking density) are suspended on a special bracket 5 at the top of the aging test chamber 3, the high-voltage test transformer 1 is used to apply operating voltage to the composite insulator sample 4, and the temperature and humidity control system 6, the salt spray generation system 7, the ultraviolet light generation system 8, and the rain spray system 9 are respectively used to provide the composite insulator sample 4 with an adjustable amplitude of temperature and humidity, rainfall, fog vapor concentration, light intensity, etc., to simulate accelerated aging environment.

[0136] (5.2) Turn on the 380V working power supply of the aging test chamber, and set the parameters such as temperature and humidity, rainfall, fog vapor concentration (fog vapor particle size 5-10μm, NaCl content in salt water 5kg / m3), light intensity, etc. in the artificial climate chamber through the temperature and humidity control system, salt fog generation system, ultraviolet light generation system and rainfall spray system, as shown in Table 3; apply an operating voltage of 5.77kV (i.e., 10kV system operating voltage) to the composite insulator through the test transformer, set the aging test time T to 2000h, and start the accelerated aging test of the composite insulator.

[0137] Table 3 Parameters of simulated accelerated aging environment for 10kV composite insulators

[0138]

[0139] (6) At regular intervals, the composite insulator is taken out to measure the aging performance parameters of its silicone rubber shed, such as tensile strength, cross-linking density, hydrophobic angle, and breakdown field strength.

[0140] (6.1) Calculated from the beginning of the aging test, one irradiated and one unirradiated composite insulator is taken out every t = 500h (the total number of times taken out N = T / t = 2000 / 500 = 4).

[0141] (6.2) Cut a piece of silicone rubber shed from the upper, middle and lower parts of the removed composite insulator, use ultra-pure water to clean the stains and residues on the surface of the silicone rubber shed in a "kq2000de" ultrasonic cleaner, and keep it as a performance test sample after drying.

[0142] (6.3) Cut a portion of each silicone rubber shed sample in step (6.2) into a standard dumbbell shape and record the width b and thickness d of the sample. Use an electronic universal testing machine to test its breaking force p and calculate its tensile strength σ using formula (2): t The average tensile strength of the silicone rubber at different positions of the upper, middle and lower parts is taken as the tensile strength of the entire composite insulator shed. The test data are shown in Table 4.

[0143]

[0144] (6.4) A portion of each silicone rubber shed sample in step (6.2) is cut off, and its crosslink density ρ is tested using a "VTMR20-010V" variable temperature nuclear magnetic resonance analyzer, and the average crosslink density of the silicone rubber shed at different positions of the upper, middle and lower parts is used as the crosslink density of the entire composite insulator shed. The test data are shown in Table 5.

[0145] (6.5) A portion of each silicone rubber shed sample in step (6.2) is cut off, and the contact angle between the water droplet and the silicone rubber material surface is tested using a "Solon-20" contact angle tester. The average contact angle of the silicone rubber shed at different positions of the upper, middle and lower parts is used as the contact angle of the entire composite insulator shed. The test data are shown in Table 6.

[0146] (6.6) Cut a part of each silicone rubber shed sample in step (6.2) into a long rectangle and record its thickness b. Use a "plate breakdown voltage" tester to test its breakdown voltage V. Use formula (3) to calculate the breakdown field strength E. The average value of the breakdown field strength of the silicone rubber shed at different positions in the upper, middle and lower parts is used as the breakdown field strength of the entire composite insulator shed. The test data is shown in Table 7.

[0147]

[0148] Table 4 Sheath tensile strength of irradiated and non-irradiated 10kV composite insulators after aging (unit: MPa)

[0149]

[0150] Table 5 Sheath crosslink density of irradiated and non-irradiated 10kV composite insulators after aging (unit: mol / cm 3 )

[0151]

[0152] Table 6 Shed contact angles of irradiated and non-irradiated 10kV composite insulators after aging (unit: degree)

[0153]

[0154] Table 7 Breakdown field strength of sheds of irradiated and unirradiated 10kV composite insulators after aging (kV / mm)

[0155]

[0156] (7) Compare the aging performance parameters of the irradiated 10kV composite insulators with those of the unirradiated 10kV ordinary high-temperature vulcanized composite insulators, and complete the evaluation of the anti-aging performance of the entire composite insulator after electron irradiation.

[0157] (7.1) According to the data in Tables 4 to 7, the functional relationship between the tensile strength, crosslinking density, contact angle, breakdown field strength and aging time t of the irradiated and unirradiated composite insulator sheds is analyzed, and the functional relationship is fitted, which is denoted as σ 辐照 (t),ρ 辐照 (t),θ 辐照 (t), E 辐照 (t) and σ 普通 (t),ρ 普通 (t),θ 普通 (t), E 普通 (t).

[0158] σ 辐照 (t) = 4.68 + 6.80 × 10 -4 t-8.0×10 -7 t 2 (4)

[0159] ρ 辐照 (t) = 3.55 + 1.46 × 10 -4 t-5.43×10 -7 t 2 (5)

[0160] θ 辐照 (t) = 110.11-4.57×10 -4 t-4.57×10 -6 t 2 (6)

[0161] E 辐照 (t) = 22.91-2.40 × 10 -3 t-8.29×10 -7 t 2 (7)

[0162] σ 普通 (t) = 4.20 + 7.89 × 10 -4 t-9.14×10 -7 t 2 (8)

[0163] ρ普通 (t) = 3.16 + 3.68 × 10 -4 t-7.14×10 -7 t 2 (9)

[0164] θ 普通 (t) = 108.8-1.80×10 -3 t-6.00×10 -6 t 2 (10)

[0165] E 普通 (t) = 21.74-1.17 × 10 -3 t-1.29×10 -6 t 2 (11)

[0166] (7.2) According to the minimum allowable value of the tensile strength, cross-linking density, contact angle and breakdown field strength of the entire composite insulator shed (σ min =0.15MPa, ρ min =0.25mol / cm 3 ,θ min =45°, E min =2.0kV / mm), calculate the tensile strength life, cross-linking density life, contact angle life and breakdown field strength life of electron irradiated insulators and ordinary insulators.

[0167]

[0168]

[0169]

[0170]

[0171] In formulas (12)-(15), σ -1 辐照 (σ), ρ -1 辐照 (ρ), θ -1 辐照 (θ), E -1 辐照 (E), σ -1 普通 (σ), ρ -1 普通 (ρ), θ -1 普通 (θ), E -1 普通 (E) are σ 辐照 (t),ρ 辐照 (t),θ辐照 (t), E 辐照 (t),σ 普通 (t),ρ 普通 (t),θ 普通 (t), E 普通 The inverse function of (t).

[0172] (7.3) Compare the life of corresponding parameters of electron-irradiated composite insulators and ordinary composite insulators, and take the minimum value k as the proportion of the anti-aging life of the entire composite insulator that can be improved by electron irradiation.

[0173]

[0174] From formula (16), it can be seen that the use of electron irradiation to process the silicone rubber shed of the composite insulator can at least increase the anti-aging life of the entire composite insulator by 8.46%.

[0175] The beneficial effects of the embodiments of the present invention may include:

[0176] (1) The entire composite insulator silicone rubber shed can be subjected to electron irradiation and anti-aging performance evaluation, providing technical support for improving the aging life of the entire composite insulator;

[0177] (2) Key parameters such as the content of silicone rubber vulcanizer and irradiation dose used in electron irradiation to improve the anti-aging performance of composite insulators can be designed to improve operational safety and aging life after field application;

[0178] (3) The test and aging performance evaluation methods are easy to implement and highly operational, providing a new, complete and reliable design solution for improving the anti-aging performance and service life of composite insulators in harsh environments;

[0179] (4) It is suitable for the electron irradiation processing and evaluation of composite insulators of AC and DC voltage levels to enhance their anti-aging performance.

[0180] Those skilled in the art will appreciate that the embodiments of the present application may be provided as methods, systems, or computer program products. Therefore, the present application may adopt the form of a complete hardware embodiment, a complete software embodiment, or an embodiment in combination with software and hardware. Moreover, the present application may adopt the form of a computer program product implemented in one or more computer-usable storage media (including but not limited to disk storage, CD-ROM, optical storage, etc.) that include computer-usable program code.

[0181] The present application is described with reference to the flowcharts and / or block diagrams of the methods, devices (systems), and computer program products according to the embodiments of the present application. It should be understood that each process and / or box in the flowchart and / or block diagram, as well as the combination of the processes and / or boxes in the flowchart and / or block diagram, can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, a special-purpose computer, an embedded processor, or other programmable data processing device to generate a machine, so that the instructions executed by the processor of the computer or other programmable data processing device generate instructions for implementing the processes in the flowchart and / or block diagram. Figure 1 A process or multiple processes and / or boxes Figure 1 A device that provides the functions specified in a block or multiple blocks.

[0182] These computer program instructions may also be stored in a computer-readable memory capable of directing a computer or other programmable data processing device to operate in a specific manner, so that the instructions stored in the computer-readable memory produce an article of manufacture comprising an instruction device, which implements the process Figure 1 A process or multiple processes and / or boxes Figure 1 A function specified in one or more boxes.

[0183] These computer program instructions can also be loaded onto a computer or other programmable data processing device so that a series of operating steps are executed on the computer or other programmable device to produce a computer-implemented process, thereby providing instructions for implementing the process. Figure 1 A process or multiple processes and / or boxes Figure 1 The steps for the functions specified in one or more boxes.

[0184] In a typical configuration, a computing device includes one or more processors (CPU), input / output interfaces, network interfaces, and memory.

[0185] The memory may include non-permanent memory in a computer-readable medium, random access memory (RAM) and / or non-volatile memory in the form of read-only memory (ROM) or flash RAM. The memory is an example of a computer-readable medium.

[0186] Computer readable media include permanent and non-permanent, removable and non-removable media that can be implemented by any method or technology to store information. Information can be computer readable instructions, data structures, program modules or other data. Examples of computer storage media include, but are not limited to, phase change memory (PRAM), static random access memory (SRAM), dynamic random access memory (DRAM), other types of random access memory (RAM), read-only memory (ROM), electrically erasable programmable read-only memory (EEPROM), flash memory or other memory technology, compact disk read-only memory (CD-ROM), digital versatile disk (DVD) or other optical storage, magnetic cassettes, magnetic tape magnetic disk storage or other magnetic storage devices or any other non-transmission media that can be used to store information that can be accessed by a computing device. As defined herein, computer readable media does not include temporary computer readable media (transitory media), such as modulated data signals and carrier waves.

[0187] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, commodity or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, commodity or device. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the process, method, commodity or device including the elements.

[0188] The above are only embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included within the scope of the claims of the present application.

Claims

1. A method for evaluating the effect of electron irradiation on the aging resistance of a composite insulator, characterized in that: include: Step S1: preparing mixed silicone rubber with different vulcanizing agent contents; Step S2: completing high temperature pre-vulcanization of the entire composite insulator shed made of the mixed silicone rubber on an injection molding machine; Step S3: Arranging an electron irradiation processing platform for the entire composite insulator to complete electron irradiation processing of the entire composite insulator under different irradiation dose conditions; Step S4: using a variable temperature nuclear magnetic resonance analyzer, testing the crosslink density of the silicone rubber shed of the composite insulator after electron irradiation with different vulcanizing agent contents and different irradiation doses in step S3, and obtaining the composite insulator, vulcanizing agent content, and irradiation dose corresponding to the maximum crosslinking density; Step S5: conducting an accelerated aging test for a given time on the composite insulator with the maximum cross-linking density and the unirradiated composite insulator in an accelerated aging test chamber; Step S6: taking out the composite insulator at predetermined intervals and measuring the aging performance parameters of the silicone rubber shed of the composite insulator; Step S7: comparing the performance parameters with those of the un-irradiated high-temperature vulcanized composite insulator to complete the evaluation of the anti-aging performance of the whole composite insulator after electron irradiation; Wherein, the step S1 comprises: Step S11: prepare raw materials according to the formula components of 90-100 parts by mass of methyl vinyl silicone rubber, 120-130 parts of aluminum hydroxide, 25-35 parts of fumed silica, 3-4 parts of iron oxide, 4-6 parts of α-aluminum oxide, 3-5 parts of hydroxy silicone oil, 0.5-1 part of silane coupling agent, and 1.5-2.5 parts of nano zinc oxide; Step S12: selecting 1,1-di-tert-butylperoxide-3,3,5-trimethylcyclohexane crosslinking agent as a silicone rubber vulcanizing agent, changing its content by 0-1.5 parts, mixing with the raw materials, and processing in the order of raw rubber internal mixing → molding and filtering → kneading → open mixing to obtain mixed silicone rubber with different vulcanizing agent contents; Wherein, the step S2 comprises: Step S21: turning on the working power of the injection molding machine, placing the composite insulator core rod into the shed vulcanization mold and securely fixing it, and heating the shed vulcanization mold to increase the temperature; Step S22: when the temperature of the shed vulcanization mold rises to the set temperature T, the heat preservation mode is turned on to maintain the temperature, and the mixed silicone rubber is placed in the injection cylinder of the injection molding machine; Step S23: setting the pressure P of the injection molding machine, injecting the mixed silicone rubber into the heated shed vulcanization mold through the injection nozzle, and starting high-temperature pre-vulcanization under the action of the pressure P and the temperature T; Step S24: when the vulcanization time reaches the set time H, the mold heating power supply is turned off, and the composite insulator is taken out from the shed vulcanization mold to obtain a composite insulator pre-vulcanized product of the mixed rubber with a given vulcanizing agent content; Step S25: repeating steps S21 to S24 until the high-temperature pre-vulcanization of the entire composite insulator shed with the mixed rubber containing all the vulcanizing agent content is completed; Wherein, the step S3 comprises: Step S31: Arrange an electron irradiation processing platform for the entire composite insulator, wherein the electron irradiation processing platform includes an electron accelerator, a beam-under-beam trolley, a conveyor belt, and air cooling equipment; The electron accelerator is used to generate a high-energy electron beam, the entire composite insulator to be irradiated is placed on the rotating part of the under-beam trolley, the under-beam trolley is fixed on the conveyor belt, and the air cooling device is used to supply air to the beam area to maintain a constant temperature and prevent the local temperature rise caused by the electron beam bombardment from affecting the irradiation processing effect; Step S32: Turn on the working power of the electron irradiation processing platform, turn on the power of the air cooling device and set the air outlet temperature, set the rotation speed of the rotating parts of the under-beam trolley and the transmission speed v of the conveyor belt, and when the under-beam trolley is transmitted to the electron beam flow area of ​​the electron accelerator, the electron beam bombards the composite insulator shed silicone rubber material to complete the electron irradiation processing, wherein the irradiation dose G of the composite insulator is calculated according to formula (1): Among them, U is the accelerator output voltage, I is the beam current, t is the irradiation time of the composite insulator, and M is the mass of the silicone rubber of the composite insulator; Step S33: changing the irradiation dose of the composite insulator by adjusting the conveyor belt speed, and repeating step S32 until the electron irradiation processing of the composite insulator under all irradiation dose conditions is completed; Wherein, the step S5 comprises: Step S51: constructing a composite insulator aging test platform, the aging test platform comprising a high-voltage test transformer, a wall bushing, an aging test chamber, a composite insulator sample, a bracket, a temperature and humidity control system, a salt spray generation system, an ultraviolet light generation system, and a rainfall spray system; wherein the composite insulator sample is suspended on a special bracket on the top of the aging test chamber, the high-voltage test transformer is used to apply an operating voltage to the composite insulator, and the temperature and humidity control system, the salt spray generation system, the ultraviolet light generation system, and the rainfall spray system are used to provide the composite insulator sample with adjustable temperature and humidity, rainfall, fog vapor concentration, and light intensity, respectively; Step S52: Turn on the working power of the aging test box, set the temperature and humidity, rainfall, fog steam concentration, and light intensity of the artificial climate chamber through the temperature and humidity control system, the salt fog generation system, the ultraviolet light generation system, and the rainfall spray system, apply the operating voltage to the composite insulator through the test transformer, set the aging test time T, and start the accelerated aging test of the composite insulator; Wherein, the step S6 comprises: Step S61: taking out a number of irradiated and non-irradiated composite insulators at a preset time interval t starting from the start of the aging test; Step S62: Cut a piece of silicone rubber shed from the upper, middle and lower parts of each composite insulator, clean the stains and residues on the surface of the silicone rubber shed with ultrapure water in an ultrasonic cleaner, and reserve them as performance test samples after drying; Step S63: Cut a portion of each silicone rubber shed sample in step S62 to form a standard dumbbell-shaped sample and record the sample width b and thickness d. Use an electronic universal testing machine to test the tensile force p of the sample and use formula (2) to calculate the tensile strength σ of the sample. t The average tensile strength of the samples at different positions of the upper, middle and lower parts is taken as the tensile strength of the entire composite insulator shed. Step S64: intercept a portion of each silicone rubber shed sample in step S62, and use a variable temperature nuclear magnetic resonance analyzer to test the crosslinking density ρ of the portion, and take the average crosslinking density of the silicone rubber shed at different positions of the upper, middle and lower parts as the crosslinking density of the shed of the entire composite insulator; Step S65: intercept a portion of each silicone rubber shed sample in step S62, use a contact angle tester to test the contact angle between a water droplet and the surface of the silicone rubber material, and take the average value of the contact angles of the silicone rubber shed surface at different positions of the upper, middle and lower parts as the contact angle of the shed of the entire composite insulator; Step S66: intercept a portion of each silicone rubber shed sample in step S62, cut it into a long rectangular sample and record the sample thickness d, use a plate breakdown voltage tester to test the breakdown voltage V of the long rectangular sample, use formula (3) to calculate the breakdown field strength E, and use the average breakdown field strength of the silicone rubber shed at different positions of the upper, middle and lower parts as the breakdown field strength of the entire composite insulator shed. Wherein, the step S7 comprises: Step S71: Analyze the functional relationship between the tensile strength, crosslinking density, contact angle, breakdown field strength and aging time t of the irradiated and unirradiated composite insulator sheds according to the data obtained in step S6, and fit the functional relationship, wherein the functions of the tensile strength, crosslinking density, contact angle, breakdown field strength and aging time t of the irradiated composite insulator shed are respectively denoted as σ 辐照 (t),ρ 辐照 (t),θ 辐照 (t), E 辐照 (t); the tensile strength, crosslinking density, contact angle, breakdown field strength of the unirradiated composite insulator shed and the aging time t are respectively denoted as σ 普通 (t),ρ 普通 (t),θ 普通 (t), E 普通 (t); Step S72: According to the minimum allowable tensile strength value σ of the entire composite insulator shed min , minimum allowable value of crosslink density ρ min , the minimum allowable contact angle θ min , Minimum allowable value of breakdown field strength E min According to formulas (4)-(7), the tensile strength life, cross-linking density life, contact angle life and breakdown field strength life of electron irradiated insulators and ordinary insulators are calculated, where the tensile strength life, cross-linking density life, contact angle life and breakdown field strength life of electron irradiated insulators are denoted as T σ辐照 , T ρ辐照 , T θ辐照 , T E辐照 The tensile strength life, cross-linking density life, contact angle life and breakdown field strength life of ordinary insulators are denoted as T σ普通 , T ρ普通 , T θ普通 , T E普通 , Among them, σ -1 辐照 (σ), ρ -1 辐照 (ρ), θ -1 辐照 (θ), E -1 辐照 (E), σ -1 普通 (σ), ρ -1 普通 (ρ), θ -1 普通 (θ), E -1 普通 (E) are the inverse functions of σ 辐照 (t), ρ 辐照 (t), θ 辐照 (t), E 辐照 (t), σ 普通 (t), ρ 普通 (t), θ 普通 (t), E 普通 (t); Step S73: Compare the lifespans of the corresponding parameters of the electron-irradiated composite insulator and the ordinary composite insulator according to formula (8), and take the minimum value k as the ratio of the anti-aging lifespan of the entire composite insulator that can be improved by electron irradiation:

2. The method according to claim 1, characterized in that t = T / N, N is the total number of times the composite insulator is removed.

3. The method according to claim 1, characterized in that The aging performance parameter includes at least one of the following: Tensile strength, cross-link density, hydrophobic angle, breakdown field strength.