Bulk GaN crystal, c-plane GaN wafer, and method for manufacturing bulk GaN crystal
By controlling the peak angle difference of the XRD sway curve on the specific main surface of the block GaN crystal, and fixing the c-side GaN wafer with halogen compounds and metal wires in the ammonia thermal method, the problems of c-side bending and declination change are solved. Improves the performance consistency and quality uniformity of c-side GaN wafers.
Patent Information
- Application Number
- CN202080047247.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-07-01
- Filing Date
- 2020-06-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-06-30
AI Technical Summary
In the prior art, it is difficult to manufacture a c-plane GaN chip with a narrow range of deflection angle variation in the main plane, and the c-plane of the block GaN crystal is relatively curved, which affects the consistency of device performance and quality uniformity.
The peak angle difference of the (002) XRD sway curve is less than 0.05 degrees by measuring the (002) on the specific main surface of the block GaN crystal, and using a halogen compound as a mineralizer in the ammonia thermal method, the c-side GaN wafer is formed by fixing the c-side GaN wafer through a metal wire. The seed crystal assembly ensures the orientation of the c-axis, a-axis and m-axis consistent, and the growth of GaN crystals is carried out.
The improvement of c-side bending and the reduction of in-main deflection angle variation is achieved, and the performance consistency and quality uniformity of c-side GaN wafers are improved. It is suitable for the manufacturing of high-output laser diodes and power semiconductor devices.
Smart Images

Figure CN114026274B_ABST
Abstract
Description
Technical Field
[0001] The present invention mainly relates to a bulk GaN crystal, a c-plane GaN wafer and a method for manufacturing the bulk GaN crystal. Background Art
[0002] GaN (gallium nitride) has a wurtzite crystal structure belonging to the hexagonal system.
[0003] In recent years, GaN wafers, which are free-standing wafers formed of GaN crystals, have attracted attention as substrates for nitride semiconductor devices.
[0004] Nitride semiconductor devices are semiconductor devices that use nitride semiconductors in the main part of the device structure. Nitride semiconductors are also called nitride III-V compound semiconductors, III-nitride compound semiconductors, GaN semiconductors, etc., including GaN, and compounds in which part or all of the gallium in GaN is replaced by other elements of the boron group of the periodic table (B, Al, In, etc.).
[0005] GaN wafers with various crystal plane orientations have been reported, and among them, GaN wafers with a primary plane (large-area surface) roughly parallel to the (000±1) crystal plane, i.e., c-plane GaN wafers, are being actively researched and developed for the purpose of application in high-output laser diodes and power semiconductor devices.
[0006] The manufacturing process of c-plane GaN wafers may include a step of slicing a bulk GaN crystal grown along the c-axis direction approximately parallel to the c-plane. The variation of the off-cut angle in the main surface of the c-plane GaN wafer after slicing is related to the curvature of the c-plane of the bulk GaN crystal before slicing (Patent Document 1).
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: U.S. Patent Application Publication No. 2008 / 0029783 Summary of the invention
[0010] Problems to be solved by the invention
[0011] In order to produce a c-plane GaN wafer with a narrow variation range of off-angles in the primary plane, it is necessary to grow a bulk GaN crystal with improved c-plane curvature. In this case, the degree of reduction of curvature is referred to as improvement of curvature.
[0012] The objects of the present invention include at least: providing a bulk GaN crystal with improved c-plane curvature; providing a c-plane GaN wafer with reduced variation in off-angle within the primary plane; and providing a new method for manufacturing bulk GaN crystal.
[0013] Solutions to the problem
[0014] The embodiments of the present invention include the following aspects, but are not limited thereto.
[0015] [1] A bulk GaN crystal having a primary surface selected from a surface inclined at least 0 degrees and not more than 10 degrees relative to a (0001) crystal plane and a surface inclined at least 0 degrees and not more than 10 degrees relative to a (000-1) crystal plane, wherein the primary surface is a specific primary surface A satisfying the following conditions (i) and (ii):
[0016] (i) a first line having a length of 80 mm and extending along a first direction can be drawn on the specific principal surface A, and the difference between the maximum value and the minimum value of the peak angle of the (002) XRD rocking curve of the GaN crystal measured at 17 measurement points arranged at intervals of 5 mm on the first line with the ω axis perpendicular to the first direction is 0.05 degrees or less;
[0017] (ii) An imaginary line segment, i.e., a second line, with a length of 80 mm extending along a second direction perpendicular to the first direction can be drawn on the specific main surface A, and the difference between the maximum and minimum values of the peak angle of the (002) XRD rocking curve of the GaN crystal measured with the ω axis perpendicular to the second direction at 17 measurement points arranged on the second line at intervals of 5 mm is less than 0.05 degrees.
[0018] [2] A bulk GaN crystal having a first principal surface and a second principal surface facing in opposite directions, one of the first principal surface and the second principal surface being a surface inclined at an angle of not less than 0 degrees and not more than 10 degrees relative to a (0001) crystal plane, and the other being a surface inclined at an angle of not less than 0 degrees and not more than 10 degrees relative to a (000-1) crystal plane, and the bulk GaN crystal satisfies the following conditions (i) and (ii):
[0019] (i) a first line having a length of 80 mm and extending along a first direction can be drawn on the first principal surface, and the difference between the maximum and minimum values of the peak angle of the (002) XRD rocking curve of the GaN crystal measured at 17 measurement points arranged at intervals of 5 mm on the first line with the ω axis perpendicular to the first direction is 0.05 degrees or less;
[0020] (ii) An imaginary line segment of 80 mm in length extending along a second direction perpendicular to the first direction, i.e., a second line, can be drawn on the first principal surface, and the difference between the maximum and minimum values of the peak angle of the (002) XRD rocking curve of the GaN crystal measured with the ω axis perpendicular to the second direction at 17 measurement points arranged on the second line at intervals of 5 mm is less than 0.05 degrees.
[0021] [3] The bulk GaN crystal according to [1] or [2], wherein:
[0022] The difference between the maximum value and the minimum value of the peak angle in the above condition (i) and the difference between the maximum value and the minimum value of the peak angle in the above condition (ii) are both 0.02 degrees or less.
[0023] [4] The bulk GaN crystal according to any one of [1] to [3], wherein
[0024] The 17 measurement points in the above condition (i) and the 17 measurement points in the above condition (ii) do not include a measurement point at which the peak angle differs from an adjacent measurement point by 0.01 degrees or more.
[0025] [5] The bulk GaN crystal according to any one of [1] to [4], wherein
[0026] The curvature radius of the surface along the first direction calculated from the rate of change of the peak angle in the above condition (i) and the curvature radius of the surface along the second direction calculated from the rate of change of the peak angle in the above condition (ii) are both greater than 300 m.
[0027] [6] The bulk GaN crystal according to any one of [1] and [3] to [5], wherein
[0028] In all 100 μm×100 μm virtual regions that can be arbitrarily set except for the portion that is less than 5 mm from the periphery in a plan view in the specific main surface A, the dislocation density is less than 1×10 6 cm -2 .
[0029] [7] The bulk GaN crystal according to any one of [1] and [3] to [6], wherein
[0030] In all 2 mm × 2 mm virtual regions that can be arbitrarily set in the specific main surface A except for the portion that is less than 5 mm from the outer periphery when viewed from above, the dislocation density is less than 1 × 10 5 cm -2 .
[0031] [8] The bulk GaN crystal according to any one of [2] to [5], wherein
[0032] In all 100 μm×100 μm virtual regions that can be arbitrarily set in the first main surface except for the portion that is less than 5 mm from the periphery in a plan view, the dislocation density calculated based on the number of dislocations in the region and the area of the region is less than 1×10 6 cm -2 .
[0033] [9] The bulk GaN crystal according to any one of [2] to [5] and [8], wherein
[0034] In all 2 mm × 2 mm imaginary regions that can be arbitrarily set in the first main surface except for the portion that is less than 5 mm from the periphery when viewed from above, the dislocation density calculated based on the number of dislocations in the region and the area of the region is less than 1 × 10 5 cm -2 .
[0035]
[10] The bulk GaN crystal according to any one of [1] to [9], which satisfies one or more conditions selected from the following (a) to (g):
[0036] (a) H concentration is 1×10 17 atoms / cm 3 above;
[0037] (b) O concentration is 1×10 17 atoms / cm 3 above;
[0038] (c) The concentration of at least one of Li, Na and K is less than 1×10 15 atoms / cm 3 ;
[0039] (d) The F concentration is 1×10 15 atoms / cm 3 above;
[0040] (e) The concentration of at least one of Cl, Br and I is 1×10 15 atoms / cm 3 above;
[0041] (f) I concentration is 1×10 15 atoms / cm 3 above;
[0042] (g) Si concentration is less than 2×10 15 atoms / cm 3 .
[0043]
[11] The bulk GaN crystal according to [9], having a wavelength of 3140 to 3200 cm in the infrared absorption spectrum. -1 There are peaks attributed to gallium vacancy-hydrogen complexes.
[0044]
[12] A method for manufacturing a c-plane GaN wafer, the method comprising at least:
[0045] The step of preparing the bulk GaN crystal according to any one of [1] to
[11] ; and
[0046] The step of slicing the GaN crystal.
[0047]
[13] The manufacturing method according to
[12] , wherein:
[0048] The c-plane GaN wafer has a disk shape, and the diameter of a circle constituting the disk shape is 50 mm or more.
[0049]
[14] A c-plane GaN wafer having a main surface selected from a surface inclined at 0 to 10 degrees relative to a (0001) crystal plane and a surface inclined at 0 to 10 degrees relative to a (000-1) crystal plane, wherein the main surface is a specific main surface B satisfying the following condition (iii):
[0050] (iii) The specific main surface B can draw an imaginary line segment of more than 50 mm, and the variation range of the m-axis component and the a-axis component of the deflection angle are both less than 0.05 degrees, except for the portion less than 5 mm from the periphery when viewed from above.
[0051]
[15] A c-plane GaN wafer having a third main surface and a fourth main surface facing in opposite directions, one of the third main surface and the fourth main surface being a surface inclined at a degree of not less than 0 and not more than 10 with respect to a (0001) crystal plane, and the other being a surface inclined at a degree of not less than 0 and not more than 10 with respect to a (000-1) crystal plane,
[0052] The third main surface can draw an imaginary line segment of more than 50 mm, and except for the portion less than 5 mm from the periphery when viewed from above, the variation range of the m-axis direction component and the a-axis direction component of the deflection angle are both within 0.05 degrees.
[0053]
[16] The c-plane GaN wafer according to
[14] or
[15] , wherein:
[0054] The variation range of the m-axis direction component of the above-mentioned off-angle and the variation range of the a-axis direction component are both within 0.02 degrees.
[0055]
[17] A c-plane GaN wafer according to any one of
[14] to
[16] , having a diameter selected from 50 mm to 55 mm, 75 mm to 80 mm, 100 mm to 105 mm, and 150 mm to 155 mm.
[0056]
[18] The c-plane GaN wafer according to any one of
[14] ,
[16] and
[17] , wherein:
[0057] In all 100 μm×100 μm virtual regions that can be arbitrarily set except for the portion that is less than 5 mm from the periphery in a plan view in the specific main surface B, the dislocation density is less than 1×10 6 cm -2 .
[0058]
[19] The c-plane GaN wafer according to any one of
[14] ,
[16] ,
[17] and
[18] , wherein:
[0059] In all 2 mm × 2 mm virtual regions that can be arbitrarily set except for the portion less than 5 mm from the periphery in the plan view of the specific main surface B, the dislocation density is less than 1 × 10 5 cm -2 .
[0060]
[20] The c-plane GaN wafer according to any one of
[15] to
[17] , wherein
[0061] The dislocation density is less than 1×10 6 cm -2 .
[0062]
[21] The c-plane GaN wafer according to any one of
[15] to
[17] and
[20] , wherein
[0063] The dislocation density is less than 1×10 5 cm -2 .
[0064]
[22] The c-plane GaN wafer according to any one of
[14] to
[21] , which satisfies one or more conditions selected from the following (a) to (g):
[0065] (a) H concentration is 1×10 17 atoms / cm 3 above;
[0066] (b) O concentration is 1×10 17 atoms / cm 3 above;
[0067] (c) The concentration of at least one of Li, Na and K is less than 1×10 15 atoms / cm 3 ;
[0068] (d) The F concentration is 1×10 15 atoms / cm 3 above;
[0069] (e) The concentration of at least one of Cl, Br and I is 1×10 15 atoms / cm 3 above;
[0070] (f) I concentration is 1×10 15 atoms / cm 3 above;
[0071] (g) Si concentration is less than 2×10 15 atoms / cm 3 .
[0072]
[23] The c-plane GaN wafer according to
[22] has a wavelength of 3140 to 3200 cm in the infrared absorption spectrum. -1 There are peaks attributed to gallium vacancy-hydrogen complexes.
[0073]
[24] An epitaxial wafer comprising:
[0074] The c-plane GaN wafer according to any one of
[14] to
[23] , and
[0075] One or more nitride semiconductor layers are epitaxially grown on the c-plane GaN wafer.
[0076]
[25] A method for manufacturing an epitaxial wafer, the method comprising:
[0077] The step of preparing the c-plane GaN wafer according to any one of
[14] to
[23] ; and
[0078] A step of epitaxially growing one or more nitride semiconductor layers on the c-plane GaN wafer.
[0079]
[26] A method for manufacturing a nitride semiconductor device, the method comprising:
[0080] The step of preparing the c-plane GaN wafer according to any one of
[14] to
[23] ; and
[0081] A step of epitaxially growing one or more nitride semiconductor layers on the c-plane GaN wafer.
[0082]
[27] A method for manufacturing a bulk GaN crystal, the method comprising:
[0083] The step of preparing the c-plane GaN wafer according to any one of
[14] to
[23] ; and
[0084] A step of epitaxially growing GaN crystal from a gas phase on the c-plane GaN wafer.
[0085]
[28] A method for manufacturing a bulk GaN crystal, the method comprising:
[0086] The step of growing GaN crystal on a seed assembly by an ammonothermal method,
[0087] The seed crystal assembly includes a plurality of c-plane GaN wafers, and the plurality of c-plane GaN wafers are fixed to each other using metal wires.
[0088]
[29] The method for manufacturing a bulk GaN crystal according to
[28] , wherein:
[0089] The directions of the c-axis, a-axis, and m-axis of all the c-plane GaN wafers constituting the seed crystal assembly are consistent.
[0090]
[30] The method for manufacturing a bulk GaN crystal according to
[29] , wherein:
[0091] When the direction of the N-polarity side of the main surface of the c-plane GaN chip constituting the above-mentioned seed crystal component is set as the surface direction, the seed crystal component has two or more c-plane GaN chips each having a rectangular or substantially rectangular main surface arranged adjacently and side by side on the surface direction side of the above-mentioned seed crystal component, and a c-plane GaN chip is arranged on the opposite direction side of the surface direction of the above-mentioned seed crystal component.
[0092]
[31] The method for producing a bulk GaN crystal according to any one of
[28] to
[30] , wherein:
[0093] In the step of growing the GaN crystal by the ammonothermal method, a mineralizer containing a halogen-containing compound is used, and at least one metal wire selected from a Pt wire and an Au wire is used as the metal wire.
[0094] Effects of the Invention
[0095] In one embodiment, a bulk GaN crystal with improved c-plane curvature can be provided. In another embodiment, a c-plane GaN wafer with reduced variation in off-angle within the main surface can be provided. In yet another embodiment, a new method for manufacturing bulk GaN crystal can be provided.
[0096] If the c-plane GaN wafer has reduced variation in off-angle within the main surface, the performance difference between individual device chips manufactured from the GaN wafer can be reduced, and the quality between batches can be made uniform. BRIEF DESCRIPTION OF THE DRAWINGS
[0097] Figure 1 An example of bulk GaN crystal according to a preferred embodiment is shown. Figure 1 (a) is a stereogram, Figure 1 (b) is a top view.
[0098] Figure 2 (a) is a cross-sectional view of a GaN crystal in which the c-plane is bent over a long distance along the direction of the measurement line. Figure 2 (b) is Figure 2 (a) is a graph obtained by measuring an XRD rocking curve with the c-plane as a reflection plane on a measurement line of a GaN crystal, and plotting the peak angle against the position of the measurement point.
[0099] Figure 3 (a) is a cross-sectional view of a GaN crystal in which the c-plane is strongly bent locally along the direction of the measurement line but is not bent over a long distance. Figure 3 (b) is Figure 3 (a) is a graph obtained by measuring an XRD rocking curve with the c-plane as a reflection plane on a measurement line of a GaN crystal, and plotting the peak angle against the position of the measurement point.
[0100] Figure 4 This is a perspective view showing an example of a c-plane GaN wafer according to the embodiment.
[0101] Figure 5 This is a diagram for explaining that the off angle of a c-plane GaN wafer can be decomposed into an m-axis direction component and an a-axis direction component.
[0102] Figure 6 FIG. 1 is a schematic diagram of a crystal growth apparatus that can be preferably used in the growth of GaN crystals based on the ammonothermal method.
[0103] Figure 7 is a process diagram showing the steps performed in a fabrication experiment of a large-area bulk GaN crystal.
[0104] Figure 8 (a) is a top view of a temporary seed crystal assembly, Figure 8 (b) Yes Figure 8 (a) is a side view of a temporary seed assembly shown.
[0105] Fig. 9 It is a top view of a temporary seed crystal assembly having a plurality of through holes formed therein.
[0106] Fig.10 It is a cross-sectional view showing a state in which one end and the other end of a Pt wire pass through one and the other through holes in an I-type through hole pair from the surface side of a permanent seed crystal component and then meet on the back side.
[0107] Fig.11 is a top view of the permanent seed assembly.
[0108] Fig.12 FIG. 4 is a photograph (substituting for the photograph of the drawing) showing the appearance of a large-area bulk GaN crystal as viewed from the N-polar side.
[0109] Fig.13 (a) and (b) are graphs showing the results of measuring the peak angles of the (002) XRD rocking curve of a large-area bulk GaN crystal every 5 mm along the first line and the second line over a length of 80 mm, respectively.
[0110] Explanation of symbols
[0111] 10 Block crystals
[0112] 11. First main surface
[0113] 12 Second main surface
[0114] 100 c-plane wafer
[0115] 101 Third main surface
[0116] 102 Fourth Main Surface DETAILED DESCRIPTION
[0117] In GaN crystals, the (0001) crystal plane and the (000-1) crystal plane are collectively referred to as the c-plane, the {10-10} crystal plane is referred to as the m-plane, and the {11-20} crystal plane is referred to as the a-plane. The crystal axis perpendicular to the c-plane is referred to as the c-axis, the crystal axis perpendicular to the m-plane is referred to as the m-axis, and the crystal axis perpendicular to the a-plane is referred to as the a-axis.
[0118] In this specification, when a crystal axis, a crystal plane, a crystal direction, etc. are mentioned, unless otherwise specified, they refer to the crystal axis, crystal plane, crystal direction, etc. of GaN crystal.
[0119] The Miller index (hkil) of the hexagonal crystal has the relationship of h+k=i, and therefore, it may be expressed as a three-digit number (hkl). For example, if (0002) is expressed as a three-digit number, it is (002).
[0120] In this specification, for convenience, the (0001) crystal plane and the (000-1) crystal plane are sometimes combined and expressed as the (000±1) crystal plane. In addition, in the drawings, the
[0001] direction is represented as the +c direction, and the [000-1] direction is represented as the -c direction.
[0121] Hereinafter, an embodiment of the present invention will be described with reference to the drawings as appropriate. The description described below is an example (representative example) of the embodiment of the present invention, and the present invention is not limited to these contents unless it exceeds the gist of the invention.
[0122] In the present specification, when expressed as "X to Y" (X and Y are arbitrary numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", and also includes the meaning of "preferably greater than X" and "preferably less than Y".
[0123] In addition, in this specification, when the word “independent” is used to describe two or more objects together, it means that the two or more objects may be the same or different.
[0124] 1. Bulk GaN crystal
[0125] One embodiment of the present invention relates to a bulk GaN crystal.
[0126] A first mode of a bulk GaN crystal as an embodiment of the present invention relates to a bulk GaN crystal having a principal surface selected from a surface inclined at least 0 degrees and least 10 degrees relative to a (0001) crystal plane, and a surface inclined at least 0 degrees and least 10 degrees relative to a (000-1) crystal plane, wherein the principal surface is a specific principal surface A that satisfies the following conditions (i) and (ii).
[0127] (i) a first line having a length of 80 mm and extending along a first direction can be drawn on the specific principal surface A, and the difference between the maximum value and the minimum value of the peak angle of the (002) XRD rocking curve of the GaN crystal measured at 17 measurement points arranged at intervals of 5 mm on the first line with the ω axis perpendicular to the first direction is 0.05 degrees or less;
[0128] (ii) An imaginary line segment, i.e., a second line, with a length of 80 mm extending along a second direction perpendicular to the first direction can be drawn on the specific main surface A, and the difference between the maximum and minimum values of the peak angle of the (002) XRD rocking curve of the GaN crystal measured with the ω axis perpendicular to the second direction at 17 measurement points arranged on the second line at intervals of 5 mm is less than 0.05 degrees.
[0129] In addition, a second mode of a bulk GaN crystal as an embodiment of the present invention relates to a bulk GaN crystal having a first principal surface and a second principal surface facing in opposite directions to each other, one of the first principal surface and the second principal surface is a surface inclined at 0 degrees or more and 10 degrees or less relative to a (0001) crystal plane, and the other surface is a surface inclined at 0 degrees or more and 10 degrees or less relative to a (000-1) crystal plane, and the bulk GaN crystal satisfies the following conditions (i) and (ii):
[0130] (i) a first line having a length of 80 mm and extending along a first direction can be drawn on the first principal surface, and the difference between the maximum and minimum values of the peak angle of the (002) XRD rocking curve of the GaN crystal measured at 17 measurement points arranged at intervals of 5 mm on the first line with the ω axis perpendicular to the first direction is 0.05 degrees or less;
[0131] (ii) An imaginary line segment of 80 mm in length extending along a second direction perpendicular to the first direction, i.e., a second line, can be drawn on the first principal surface, and the difference between the maximum and minimum values of the peak angle of the (002) XRD rocking curve of the GaN crystal measured with the ω axis perpendicular to the second direction at 17 measurement points arranged on the second line at intervals of 5 mm is less than 0.05 degrees.
[0132] In the first mode described above, from the viewpoint of being able to obtain the effect of the present invention, as long as the main surface is selected from a surface inclined at least 0 degrees and not more than 10 degrees relative to the (0001) crystal plane, and a surface inclined at least 0 degrees and not more than 10 degrees relative to the (000-1) crystal plane, there is no particular restriction on the form of other surfaces constituting the bulk GaN crystal, and they may be flat or have projections and depressions.
[0133] In the bulk GaN crystal in the first embodiment, when one of the faces inclined at 0 degrees or more and 10 degrees or less relative to the (0001) crystal plane and the faces inclined at 0 degrees or more and 10 degrees or less relative to the (000-1) crystal plane is a specific principal face A, and there is a principal face on the opposite side of the specific principal face A, and the principal face on the opposite side is a face not selected as the specific principal face A of the above two faces, the bulk GaN crystal becomes the same as the bulk GaN crystal in the second embodiment. In this case, the specific principal face A in the first embodiment is the first principal face in the second embodiment.
[0134] Below, the specific method of the bulk GaN crystal in the second method (also referred to as "bulk GaN crystal") is described, but the composition, characteristics, uses, etc. of each element of the bulk GaN crystal including the methods of conditions (i) and (ii) can also be similarly applied to the bulk GaN crystal in the first method.
[0135] Figure 1 An example of a bulk GaN crystal according to a preferred embodiment is shown. Figure 1 (a) is a stereogram, Figure 1 (b) is a top view.
[0136] Reference Figure 1 The bulk crystal 10 is a plate formed only of GaN crystals, and has two main faces (large surface areas) facing opposite directions, namely, a first main face 11 and a second main face 12. One side of the first main face 11 and the second main face 12 is Ga polarity, and the other side is N polarity. The first main face 11 and the second main face 12 are parallel to each other, but are not required to be strictly parallel.
[0137] When the first principal surface 11 is Ga polarity and the second principal surface 12 is N polarity, the first principal surface is tilted relative to the (0001) crystal plane by more than 0 degrees and less than 10 degrees. In other words, the tilt of the first principal surface relative to the (0001) crystal plane refers to the angle formed by the
[0001] direction of the bulk crystal 10 and the normal vector of the first principal surface.
[0138] When the first primary surface 11 is of N polarity and the second primary surface 12 is of Ga polarity, the first primary surface is inclined at 0 degrees or more and 10 degrees or less with respect to the (000-1) crystal plane.
[0139] The first main surface 11 and the second main surface 12 may be in a state of being crystal-grown (as-grown), or may be surfaces that have been flattened by processing.
[0140] The first main face 11 of the block crystal 10 can be roughly rectangular, two of the sides forming the roughly rectangular shape are roughly parallel to the orthographic projection of the m-axis on the first main face 11, and the other two sides are roughly parallel to the orthographic projection of the a-axis on the first main face 11. The shape and size of the second main face 12 are roughly the same as those of the first main face 11.
[0141] In a modified example, the first main surface 11 may have a shape other than a rectangle, for example, a shape obtained by cutting off part or all of the four corners of a rectangle, a hexagon, a circle, or an irregular shape.
[0142] The first major surface 11 of the bulk crystal 10 has a size such that at least two imaginary line segments perpendicular to each other and each having a length of 80 mm can be drawn thereon.
[0143] When the first principal surface 11 of the bulk crystal 10 is circular, it is preferably sized to allow a virtual circle with a diameter of preferably 85 mm, more preferably 110 mm to be drawn thereon, or may be sized to allow a virtual circle with a diameter of 160 mm to be drawn thereon.
[0144] The thickness of the bulk crystal 10 , that is, the dimension in the direction perpendicular to the first main surface 11 and the second main surface 12 , is preferably 1 mm or more, more preferably 2 mm or more, and preferably 30 mm or less, more preferably 20 mm or less.
[0145] The curvature of the c-plane of a GaN crystal having a primary surface with c-axis orientation can be evaluated by measuring the (002) XRD rocking curve with the c-plane as the reflection plane at regular intervals along a measurement line extending on the primary surface and examining changes in its peak angle.
[0146] In the XRD rocking curve measurement at each measurement point, the ω axis is made perpendicular to the measurement line. This makes it possible to know whether the inclination of the c-axis along the measurement line changes, that is, the bending state of the c-plane in the measurement line direction.
[0147] The ω axis is the rotation axis of the sample when measuring the XRD rocking curve. Another name for XRD rocking curve measurement is also called ω scan.
[0148] For example, Figure 2 As shown in (a), for a GaN crystal whose c-plane is bent over a long distance along the direction of the measurement line, when the XRD rocking curve with the c-plane as the reflection plane is measured on the measurement line and its peak angle ω is plotted against the position of the measurement point, the following is obtained: Figure 2 (b) The stronger the curvature, the greater the rate of change of ω.
[0149] On the other hand, Figure 3 In the example shown in (a), the c-plane is strongly bent locally along the direction of the measurement line, but the direction of the bend changes alternately up and down along the measurement line, and no bending is observed over a long distance. For such a GaN crystal, when the XRD rocking curve is similarly measured on the measurement line and its peak angle ω is plotted against the position of the measurement point, it can be obtained Figure 3 (b) Such a coordinate diagram.
[0150] according to Figure 2 and Figure 3 It can be understood that, whether due to the bending of the c-plane over a long distance or due to the local bending, the maximum and minimum values of the peak angle of the XRD rocking curve measured on the measurement line will increase.
[0151] In the bulk crystal 10 , the curvature of the c-plane is improved to such an extent that the following conditions (i) and (ii) are satisfied.
[0152] (i) An imaginary line segment of 80 mm in length extending along the first direction, i.e., the first line, can be drawn on the first principal surface 11, and the difference between the maximum and minimum values of the peak angle of the (002) XRD rocking curve of the bulk crystal 10 measured by making the ω axis perpendicular to the first direction at 17 measurement points arranged in parallel with a spacing of 5 mm on the first line is less than 0.05 degrees.
[0153] (ii) An imaginary line segment, i.e., a second line, with a length of 80 mm extending along a second direction perpendicular to the first direction can be drawn on the first principal surface 11, and the difference between the maximum and minimum values of the peak angle of the (002) XRD rocking curve of the bulk crystal 10 measured with the ω axis perpendicular to the second direction at 17 measurement points arranged in parallel at intervals of 5 mm on the second line is less than 0.05 degrees.
[0154] In conditions (i) and (ii), the first direction may be perpendicular to the a-axis, for example, but is not limited thereto.
[0155] There may be multiple lines corresponding to the first line described in condition (i), but as long as at least one such line can be found, that is, as long as on a line which is at least one imaginary line segment extending along the first direction, the ω axis is made perpendicular to the line at a distance of 5 mm over a length of 80 mm and the peak angle of the (002) XRD rocking curve of the bulk crystal 10 is measured, and the difference between the maximum and minimum values is less than 0.05 degrees, it can be evaluated that the degree of curvature of the c-plane of the bulk crystal 10 in the first direction has been sufficiently reduced.
[0156] The same applies to condition (ii). As long as the difference between the maximum and minimum values of the peak angle of the (002) XRD rocking curve of the bulk crystal 10 measured on a line serving as at least one imaginary line segment along the second direction with the ω axis perpendicular to the line at a distance of 5 mm over a length of 80 mm is less than 0.05 degrees, it can be evaluated that the degree of curvature of the c-plane of the bulk crystal 10 in the second direction has been sufficiently reduced.
[0157] The difference between the maximum and minimum values of the peak angle of the rocking curve between the 17 measurement points described in condition (i) and the difference between the maximum and minimum values of the peak angle of the rocking curve between the 17 measurement points described in condition (ii) are independently preferably 0.04 degrees or less, more preferably 0.03 degrees or less, and even more preferably 0.02 degrees or less. This preferred range may satisfy only one of condition (i) and condition (ii), but preferably all conditions are satisfied.
[0158] For example, although it is an extreme assumption, the curvature in the first direction of the c-plane of the bulk crystal 10 is as follows Figure 2In the case where only the long-distance bending occurs and the peak angle of the rocking curve changes monotonically along the first line as in the example shown, the difference between the maximum and minimum values of the peak angle between the 17 measurement points described in condition (i) is equal to the difference between the peak angle between the two measurement points at both ends 80 mm apart. In such a case, as the difference between the maximum and minimum values decreases by 0.05 degrees, 0.04 degrees, 0.03 degrees, and 0.02 degrees, the curvature radius of the c-plane along the first direction increases to about 92m, about 115m, about 153m, and about 229m.
[0159] Preferably, the 17 measurement points described in condition (i) and the 17 measurement points described in condition (ii) independently do not include measurement points where the peak angle of the rocking curve differs from the adjacent measurement points by more than 0.01 degrees. In other words, whether on the first line or the second line, in the respective 80 mm intervals containing the 17 measurement points, the inclination of the c-axis does not change by more than 0.01 degrees within every 5 mm. This means that there is no locally strongly bent portion on the c-plane of the bulk crystal 10. The above preferred range may also satisfy only one of the conditions (i) and (ii), but preferably all conditions are satisfied.
[0160] In a preferred example, the radius of curvature of the c-plane along the first direction calculated from the rate of change of the peak angle of the rocking curve between the 17 measurement points described in condition (i) and the radius of curvature of the c-plane along the second direction calculated from the rate of change of the peak angle of the rocking curve between the 17 measurement points described in condition (ii) are independently 300 μm or more. This preferred range may satisfy only one of condition (i) and condition (ii), but preferably all conditions are satisfied.
[0161] In the calculation of the curvature radius described here, a value obtained by linear fitting using the least square method was used as the rate of change of the peak angle of the rocking curve between 17 measurement points.
[0162] In the bulk crystal 10, except for the portion less than 5 mm from the periphery when viewed from above, in any 100 μm×100 μm region on the first main surface 11, the dislocation density calculated based on the number of dislocations in the region and the area of the region can be less than 1×10 6 cm -2 This can also be expressed as follows: in all 100 μm × 100 μm hypothetical regions that can be arbitrarily set in the first main surface except for the portion that is less than 5 mm from the periphery when viewed from above, the dislocation density calculated based on the number of dislocations in the region and the area of the region is less than 1×10 6 cm -2This change in expression also applies to the following description.
[0163] In addition, in the bulk crystal 10, except for the portion less than 5 mm from the periphery when viewed from above, in any 2 mm×2 mm region on the first main surface 11, the dislocation density calculated based on the number of dislocations in the region and the area of the region can be less than 1×10 5 cm -2 .
[0164] The dislocation density of the first main surface 11 can be examined by observing the cathode luminescence (CL) image or the photoluminescence (PL) image. However, it should be noted that since the bulk crystal 10 is grown by the ammonothermal method, in the CL image and the PL image, due to the influence of the strong yellow band luminescence, the dislocation does not appear in the form of dark spots accompanied by sharp contrast. Therefore, in order to facilitate visual identification of the dislocation, a GaN film can be formed on the first main surface 11 by a vapor phase method and the surface CL image and the surface PL image of the GaN film can be observed.
[0165] When the first main surface 11 is Ga polarity, the etch scar density can be regarded as the dislocation density. If necessary, after being flattened by CMP (chemical mechanical polishing), etching can be performed for 1 hour using 89% sulfuric acid heated to 270°C, thereby forming etch scars corresponding to the dislocations on the first main surface.
[0166] When the first principal surface 11 is N-polar, the bulk crystal 10 can be cut along the thickness direction, and the etch density on the Ga-polar cut surface within several hundred μm from the first principal surface can be measured and regarded as the dislocation density of the first principal surface 11 .
[0167] The bulk crystal 10 preferably satisfies one or more conditions selected from the following (a) to (g).
[0168] (a) H concentration is 1×10 17 atoms / cm 3 above.
[0169] (b) O concentration is 1×10 17 atoms / cm 3 above.
[0170] (c) The concentration of at least one of Li, Na and K is less than 1×10 15 atoms / cm 3 .
[0171] (d) The F concentration is 1×10 15 atoms / cm 3 above.
[0172] (e) The concentration of at least one of Cl, Br and I is 1×10 15 atoms / cm 3 above.
[0173] (f) I concentration is 1×10 15 atoms / cm 3 above.
[0174] (g) Si concentration is less than 2×10 15 atoms / cm 3 .
[0175] The conditions (a) to (g) are described below.
[0176] The bulk crystal 10 is grown by the ammonothermal method, so it can be grown at 1×10 17 atoms / cm 3 The above concentrations contain H (hydrogen).
[0177] Due to the raw materials used in the ammonothermal process, the bulk crystal 10 can be 1×10 17 atoms / cm 3 The above concentrations contain O.
[0178] Since the bulk crystal 10 is preferably grown by an ammonothermal method without using a compound containing an alkali metal as a mineralizer, the concentration of at least one of Li (lithium), Na (sodium), and K (potassium) may be less than 1×10 15 atoms / cm 3 .
[0179] Since the bulk crystal 10 preferably uses a compound containing F (fluorine) as a mineralizer and is grown by an ammonothermal method, it can be grown at a rate of 1×10 15 atoms / cm 3 The above concentrations contain F.
[0180] Typical examples of compounds containing F that can be preferably used as mineralizers include HF, NH4F, GaF3, etc. When HF is used, it may react with NH3 added as a solvent and GaN added as a raw material in the growth container to generate NH4F and GaF3.
[0181] Since the bulk crystal 10 is preferably grown by an ammonothermal method using a compound containing a halogen other than F as a mineralizer in addition to a compound containing F, it is also possible to use 1×10 15 atoms / cm 3 The above concentration contains at least one of Cl, Br and I.
[0182] Typical examples of compounds containing halogens other than F that can be preferably used as mineralizers include HCl, NH4Cl, GaCl3, HBr, NH4Br, GaBr3, HI, NH4I, IGaI3, etc. When HX (X = Cl, Br or I) is used, it sometimes reacts with NH3 added as a solvent and GaN added as a raw material in the growth container to generate NH4X and GaX3.
[0183] Since the bulk crystal 10 is preferably grown by an ammonothermal method using a compound containing I (iodine) as a mineralizer in addition to a compound containing F, it is possible to grow the bulk crystal 10 at a rate of 1×10 15 atoms / cm 3 The above concentrations contain I.
[0184] Since the bulk crystal 10 is grown by the ammonothermal method, the concentration of Si can be less than 2×10 15 atoms / cm 3 In the ammonothermal method, when NH4F is used alone as a mineralizer, or when NH4F and HX are used in combination, the concentration of Si can be effectively reduced.
[0185] Since the bulk crystal 10 is grown by the ammonothermal method, it can be found in the infrared absorption spectrum at 3140 to 3200 cm -1 There are peaks attributed to gallium vacancy-hydrogen complexes.
[0186] 2. c-plane GaN wafer
[0187] Another embodiment of the present invention includes a c-plane GaN wafer and a method for manufacturing the same, wherein the c-plane GaN wafer is obtained by a method having at least the following steps: a step of preparing the above-mentioned bulk GaN crystal; and a step of slicing the bulk GaN crystal. In the step of slicing the bulk GaN crystal, it is preferred to slice the crystal approximately parallel to the c-plane of the crystal. However, the c-plane GaN wafer of this other embodiment is not limited to the c-plane GaN wafer obtained from the above-mentioned bulk GaN crystal.
[0188] Figure 4 Shown is a stereoscopic view of an example of a c-plane GaN wafer (also referred to as a "c-plane wafer") according to an embodiment. Referring to the figure, the c-plane wafer 100 is disc-shaped and has two main surfaces facing opposite directions, namely, a third main surface 101 and a fourth main surface 102. One of the third main surface 101 and the fourth main surface 102 is Ga polarity and the other is N polarity. The third main surface 101 and the fourth main surface 102 are parallel to each other, but are not required to be strictly parallel. Here, the disc shape refers to a shape in which the diameter (d) of the circle in the cylindrical shape is larger than the height (l), and the ratio (d / l) is usually greater than 20.
[0189] The shape of the third main surface of the c-plane wafer 100 is not particularly limited, but it is preferable that a virtual line segment of 50 mm or more can be drawn on the main surface. The line segment may be 75 mm or more, 100 mm or more, or 150 mm or more.
[0190] The third main surface of the c-plane wafer 100 is preferably circular. When the shape of the c-plane wafer 100 is a disk shape, the diameter of the circle constituting the disk shape (the upper surface or the lower surface of the disk shape) is not limited, and is usually 50 mm or more, typically 50 mm or more and 55 mm or less (about 2 inches), 75 mm or more and 80 mm or less (about 3 inches), 100 mm or more and 105 mm or less (about 4 inches), 150 mm or more and 155 mm or less (about 6 inches), etc. In addition, the diameter of the c-plane wafer 100 may be outside the above range, that is, it may be less than 50 mm, more than 55 mm and less than 75 mm, more than 80 mm and less than 100 mm, more than 105 mm and less than 150 mm, or more than 155 mm.
[0191] The c-plane wafer 100 is required to have a strength that does not hinder processing, and therefore its thickness is generally 250 μm or more, and may be further increased depending on the diameter.
[0192] When the diameter of the c-plane wafer 100 is about 2 inches, the thickness is preferably 250 μm or more, more preferably 300 μm or more, and is preferably 450 μm or less, more preferably 400 μm or less.
[0193] When the diameter of the c-plane wafer 100 is about 4 inches, the thickness is preferably 350 μm or more, more preferably 400 μm or more, and is preferably 750 μm or less, more preferably 650 μm or less.
[0194] When the diameter of the c-plane wafer 100 is about 6 inches, the thickness is preferably 400 μm or more, more preferably 450 μm or more, further preferably 550 μm or more, and preferably 800 μm or less, more preferably 700 μm or less.
[0195] In this specification, with respect to the diameter of the c-plane wafer 100, “approximately” means within a range of ±20%, or within a range of ±10%, or within a range of ±0 to +20%, or ±0 to +10%.
[0196] The c-plane wafer 100 may have an off angle of 10 degrees or less.
[0197] The off-angle of the c-plane wafer 100 can be decomposed into an m-axis component and an a-axis component. Figure 5For explanation, when the normal vector of the third main surface 101 is vector N, the off-angle of the c-plane wafer 100 refers to the inclination θ of vector N with respect to the c-axis. This vector N can be decomposed into vector N as the a-axis direction component a , and vector N as the m-axis component m The orthographic projection of vector N on the m plane is vector N a , the orthographic projection of vector N on plane a is vector N m .
[0198] When vector N is decomposed in this way, vector N a The a-axis component θ is tilted at an angle θ relative to the c-axis. a , vector N m The m-axis component θ is tilted at an angle θ relative to the c-axis. m .
[0199] Since the c-plane wafer 100 is sliced from the bulk crystal 10 of the embodiment, the variation of the off angle within the third main surface 101 is reduced.
[0200] Specifically, for the c-plane wafer 100, except for the portion less than 5 mm from the periphery when viewed from above, the variation range of the m-axis component of the deflection angle in the third main surface 101 and the variation range of the a-axis component are both within 0.05 degrees. The variation range of the m-axis component of the deflection angle and the variation range of the a-axis component are independently preferably less than 0.05 degrees, preferably within 0.04 degrees, more preferably within 0.03 degrees, and further preferably within 0.02 degrees. This preferred range may also satisfy only one of the above two variation ranges, but preferably all variation ranges are satisfied.
[0201] In addition, for the c-plane wafer 100, it can also be interpreted alternatively as: except for the portion less than 5 mm from the periphery when viewed from above, the variation range of any first-axis direction component corresponding to the diameter in the third main surface 101 and the variation range of the second-axis direction component corresponding to the diameter in the direction orthogonal to the first axis are both within 0.05 degrees. The variation range of the first-axis direction component and the variation range of the second-axis direction component of the deflection angle are independently preferably less than 0.05 degrees, preferably within 0.04 degrees, more preferably within 0.03 degrees, and further preferably within 0.02 degrees. This preferred range may also satisfy only one of the above two variation ranges, or both variation ranges may satisfy them.
[0202] The third main surface 101 of the c-plane wafer 100 is a “surface”. When a semiconductor device is manufactured using the c-plane wafer 100 , a semiconductor layer is epitaxially grown on the third main surface 101 .
[0203] The processing performed to planarize the third main surface 101 may include one or more selected from grinding, polishing, and CMP. In addition to these processing, etching may be performed for the purpose of removing a damaged layer.
[0204] The root mean square (RMS) roughness of the third main surface 101 measured by AFM is preferably less than 5 nm, more preferably less than 2 nm, further preferably less than 1 nm, and may be less than 0.5 nm within a measurement range of 2 μm×2 μm.
[0205] The fourth main surface 102 of the c-plane wafer 100 is the “back surface” and may be mirror-polished, roughened, or etched.
[0206] Although in Figure 4 Although not shown, the edge of the c-plane wafer 100 may also be chamfered. In addition, the c-plane wafer 100 may be provided with various marks as required, such as an orientation flat or notch indicating the orientation of the crystal, an index flat for facilitating identification of the front and back surfaces, etc.
[0207] The c-plane wafer 100 can be preferably used for manufacturing a nitride semiconductor device.
[0208] As a method for manufacturing a nitride semiconductor device, for example, there can be cited a method having the following steps: a step of preparing the above-mentioned c-plane GaN wafer; and a step of epitaxially growing one or more nitride semiconductor layers on the c-plane GaN wafer. This manufacturing method can also be applied to the case of manufacturing epitaxial wafers, specifically, epitaxially growing one or more nitride semiconductor layers on the third main surface of the c-plane wafer 100 to form an epitaxial wafer. As epitaxial growth methods, preferably used are: MOVPE (Metal Organic Vapor Phase Epitaxy), MBE (Molecular Beam Epitaxy), PXD (Pulsed Excitation Deposition), sputtering, HVPE (Hydride Vapor Phase Epitaxy) and other vapor phase methods.
[0209] The epitaxially grown nitride semiconductor layer can be made to have n-type conductivity, p-type conductivity, or semi-insulating properties by doping.
[0210] Examples of nitride semiconductor devices that can be manufactured using the c-plane wafer 100 include: light-emitting diodes (LEDs), laser diodes (LDs) and other light-emitting devices, rectifiers, bipolar transistors, field effect transistors, HEMTs (High Electron Mobility Transistors) and other electronic devices, temperature sensors, pressure sensors, radiation sensors, visible-ultraviolet light detectors and other semiconductor sensors, solar cells, etc.
[0211] Other uses of the c-plane wafer 100 are as seeds for growing bulk GaN crystals by HVPE, THVPE (Tri-Halide Vapor Phase Epitaxy), OVPE (Oxide Vapor Phase Epitaxy), the ammonothermal method, the Na flux method, and other various methods.
[0212] Another embodiment of the c-plane GaN wafer relates to a c-plane GaN wafer having a main surface selected from a surface inclined at least 0 degrees and least 10 degrees relative to the (0001) crystal plane, and a surface inclined at least 0 degrees and least 10 degrees relative to the (000-1) crystal plane, wherein the main surface is a specific main surface B that satisfies the following condition (iii).
[0213] (iii) The specific main surface B can draw an imaginary line segment of more than 50 mm, and the variation range of the m-axis component and the a-axis component of the deflection angle are both less than 0.05 degrees, except for the portion less than 5 mm from the periphery when viewed from above.
[0214] In this embodiment, from the viewpoint of being able to obtain the effect of the present invention, as long as the main surface is selected from a surface inclined at least 0 degrees and not more than 10 degrees relative to the (0001) crystal plane, and a surface inclined at least 0 degrees and not more than 10 degrees relative to the (000-1) crystal plane, there is no particular restriction on the morphology of the surface on the opposite side of the main surface, and it may be parallel to the main surface or not parallel to the main surface. In addition, it may be a crystal plane other than the (0001) crystal plane and the (000-1) crystal plane.
[0215] In the c-plane GaN wafer in the above-mentioned method (referred to as the "second method of the c-plane GaN wafer"), when one of the surfaces selected from the surface inclined at 0 degrees or more and 10 degrees or less relative to the (0001) crystal plane and the surface inclined at 0 degrees or more and 10 degrees or less relative to the (000-1) crystal plane is a specific principal surface B, and there is a principal surface on the opposite side of the specific principal surface B, and the principal surface on the opposite side is a surface not selected as the specific principal surface B of the above-mentioned two surfaces, the above-mentioned bulk GaN crystal becomes the same method as the above-mentioned method having the third principal surface and the fourth principal surface (referred to as the "first method of the c-plane GaN wafer"). In this case, the specific principal surface B of the c-plane GaN wafer in the second method is the third principal surface in the first method.
[0216] The configuration, characteristics, uses, and the like of the various elements of the c-plane GaN wafer in the first embodiment of the c-plane GaN wafer can also be similarly applied to the c-plane GaN wafer in the second embodiment of the c-plane GaN wafer.
[0217] 3. Manufacturing method of bulk GaN crystal
[0218] The manufacturing method of the bulk GaN crystal is not limited, and for example, the bulk GaN crystal can be obtained by the following manufacturing method: a manufacturing method including the steps of preparing the c-plane GaN wafer and epitaxially growing GaN crystal from the gas phase on the c-plane GaN wafer; a manufacturing method including the step of growing GaN crystal on a seed assembly including a plurality of c-plane GaN wafers by an ammonothermal method. With regard to the above-mentioned epitaxial growth embodiment, the embodiment described in the above-mentioned c-plane GaN wafer can be applied.
[0219] Hereinafter, a method for producing bulk GaN crystal using a seed crystal assembly will be described in detail.
[0220] The notable feature of the seed assembly is that metal wires are used to fix the c-plane GaN wafers that constitute it. Specifically, all c-plane GaN wafers are perforated with small through holes, and all c-plane GaN wafers are tied together with other c-plane GaN wafers by metal wires passing through their through holes.
[0221] The metal wire can be used as long as it can withstand the ammonothermic environment to which the GaN crystal is exposed during growth. When a halogen-containing compound is used as a mineralizer in the process of growing GaN crystals by the ammonothermic method, the metal wire that can be preferably used is at least one metal wire selected from Pt wire and Au wire, more preferably Pt wire, but it can also be W wire, Mo wire, Ag wire, etc. In addition, as long as the material can withstand the ammonothermic environment and can fix the c-plane GaN wafers to each other, it is not limited to metal wires.
[0222] In one embodiment of the seed assembly, the seed assembly is further characterized in that the orientations of the c-axis, a-axis, and m-axis of all c-plane GaN wafers constituting the seed assembly are consistent. Therefore, in the crystal growth process, the GaN crystals grown from the surfaces of different c-plane GaN wafers are smoothly integrated (coreless). It can be inferred that this helps prevent the generation of harmful stress. It should be noted that the consistent orientations of the c-axis, a-axis, and m-axis of the c-plane GaN wafer indicate that the direction of the polarity of the c-plane GaN wafer is also consistent.
[0223] For the c-plane GaN wafer constituting the seed assembly, when the front and back sides of the seed assembly are defined by setting the main surface on the N-polar side to face the material on the surface side of the seed assembly, two or more c-plane GaN wafers each having a rectangular or substantially rectangular main surface are adjacently arranged on the surface side of the seed assembly. The GaN wafer can also be expressed as follows: when the direction of the N-polar side of the main surface of the c-plane GaN wafer constituting the seed assembly is set as the surface direction, two or more c-plane GaN wafers each having a rectangular or substantially rectangular main surface are arranged on the surface direction side of the seed assembly.
[0224] Preferably, there is no gap between two or more adjacent c-plane GaN wafers. Here, the gap refers to a gap that can be observed with the naked eye, and more preferably, the c-plane GaN wafers are adjacent to each other so that there is no gap at the level observed with an optical microscope.
[0225] The two or more c-plane GaN wafers are preferably obtained by slicing in parallel from the same bulk GaN crystal. Specifically, one or more c-plane GaN wafers obtained by slicing from a bulk GaN crystal can be cut out in parallel, or two or more c-plane GaN wafers can be cut out in parallel from different slices. In the case of cutting c-plane GaN wafers from different slices, it is preferred to cut out two or more wafers along parallel directions in the original bulk GaN crystal. For example, it is also preferred to cut out two or more different wafers along the thickness direction at the same position in the original bulk GaN crystal and combine them to form a seed assembly. In this case, even if the positions are not exactly the same, they can be cut out and used in a manner that there are overlapping positions at least in the thickness direction.
[0226] Here, in the case of obtaining a c-plane GaN wafer by any of the above methods, it is particularly important that the crystal orientations of the c-plane GaN wafers are consistent with each other. Specifically, the a-axis direction and m-axis direction of the c-plane GaN wafer are independently offset by usually less than 0.05°, preferably less than 0.02°, more preferably less than 0.01°, and further preferably less than 0.005° to form a seed assembly. It should be noted that the direction of the crystal axis of the c-plane GaN wafer can be determined by XRD.
[0227] A c-plane GaN wafer serving as a connecting plate may be disposed on the back side of the seed crystal assembly (the direction opposite to the above-mentioned surface direction).
[0228] In the past, a method commonly used in vapor phase growth such as HVPE is to arrange multiple wafers in parallel as a seed assembly and manufacture GaN crystals on its surface. This is because, in the case of manufacturing methods such as HVPE, the seed assembly can be firmly fixed to the base. In contrast, in the case of the ammonothermal method, the seed assembly is in a state of being suspended by a wire in a liquid such as ammonia. Even if you want to arrange multiple wafers in parallel and integrate them into a seed assembly, it is difficult to fix them to each other. Due to this problem, the side-by-side method has not been used in the ammonothermal method in the past. As mentioned above, this problem can be solved by fixing with a wire.
[0229] The growth of GaN crystals based on the ammonothermal method can preferably be performed using Figure 6 The crystal growth apparatus shown.
[0230] Reference Figure 6 The crystal growth device has an autoclave and a sealed container (capsule) disposed therein. A dissolution zone and a growth zone separated from each other by a baffle are disposed inside the sealed container. When growing GaN crystals, the raw materials together with the mineralizer (not shown) are placed in the dissolution zone, and in the growth zone, the seed crystal is suspended by a wire.
[0231] Gas pipelines connected to the vacuum pump, the ammonia cylinder and the nitrogen cylinder are connected to the autoclave and the sealed container via valves.
[0232] When adding NH3 (ammonia) to a sealed container, the amount of NH3 supplied from the ammonia cylinder can be confirmed by a mass flow meter.
[0233] The pressure inside the sealed container when the sealed container is heated to a given temperature depends on the free volume of the sealed container and the amount of NH3 introduced into the sealed container.
[0234] When growing GaN, seed crystals, raw materials, mineralizers, and NH3 are added to a sealed container. The sealed container is sealed and heated from the outside of the autoclave using a heater (not shown) in such a way that the inside reaches a supercritical state. At this time, in order to balance the pressure inside and outside the sealed container, NH3 is sealed not only in the sealed container but also in the space between the autoclave and the sealed container.
[0235] In order to set a temperature gradient between the dissolution zone and the growth zone, multiple heaters are used to heat the upper and lower parts of the autoclave respectively.
[0236] When a halogen-containing compound such as HX, NH4X, GaX3 (where X=F, Cl, Br or I) is used as a mineralizer, the sealed container, the baffle and the clamp provided in the sealed container, and the wire for suspending the seed crystal are preferably made of Pt (platinum) or an alloy containing Pt as a main component. It is particularly preferred that the sealed container be formed of a Pt-Ir alloy.
[0237] 4. Experimental Results
[0238] 4.1. Fabrication of large-area bulk GaN crystals
[0239] By executing Figure 7 A large-area bulk GaN crystal is produced by following steps 1 to 4 shown in the figure. Here, the "large area" is not limited to a specific area, but specifically has a size that allows two imaginary line segments perpendicular to each other and each with a length of 80 mm to be drawn on the main surface. The outline of each step is as follows.
[0240] In step 1, a seed assembly is prepared.
[0241] In step 2, a first generation GaN crystal is grown on the seed crystal assembly.
[0242] In step 3, a c-plane GaN wafer is sliced out from the portion of the first generation GaN crystal grown on the surface side of the seed crystal assembly.
[0243] In step 4, a second generation GaN crystal is grown on the c-plane GaN wafer sliced in step 3.
[0244] In the experiments described here, the growth of GaN crystals based on the ammonothermal method was performed using Figure 6 Crystal growing apparatus of the type shown.
[0245] Hereinafter, each step will be described in detail.
[0246] [Step 1]
[0247] In step 1, a seed crystal assembly is prepared in the following order.
[0248] a. Growth of GaN crystals for seed crystals
[0249] A 4-inch diameter c-plane GaN wafer (hereinafter referred to as "HVPE wafer") formed of GaN crystal grown on a sapphire substrate by HVPE and having an N-polar surface finished to be mirror-flat was prepared. The N-polar surface refers to the main surface on the [000-1] side.
[0250] On the N-pole surface of the HVPE wafer, a stripe-patterned selective growth mask was formed by a lift-off method. The stripe-patterned selective growth mask was formed by a sputtered film having a double-layer structure of a 100 nm thick TiW base layer and a 100 nm thick Pt surface layer stacked on top of the base layer.
[0251] The line width of the linear openings provided in the selective growth mask was 50 μm, and the spacing between the linear openings was 4 mm. The stripe direction was parallel to the a-plane of the GaN crystal used to form the HVPE wafer.
[0252] After the selective growth mask is formed, GaN crystals are grown on the HVPE wafer by the ammonothermal method. The raw material used is polycrystalline GaN produced by a method in which HCl gas is brought into contact with Ga single substance under heating to generate gaseous GaCl and the gaseous GaCl is reacted with NH3 gas. NH4F and NH4I are used as mineralizers. NH4I is synthesized by reacting HI (hydrogen iodide) gas and NH3 in a sealed container.
[0253] The molar ratios of F and I contained in the mineralizer to NH 3 used as a solvent were 0.5% and 4.0%, respectively.
[0254] Growth conditions are: temperature T in the dissolution zone D The temperature T of the growth zone G The average value is 600℃, and the temperature difference between the two zones is T D -T G About 5℃(T D >T G ), the pressure is about 220MPa.
[0255] On the N-polar surface of the HVPE wafer, GaN crystal is grown in layers through the above-mentioned selective growth mask. A c-plane GaN wafer is sliced from the GaN crystal, and the c-plane GaN wafer is used as a seed crystal to grow new GaN crystal by the ammonothermal method.
[0256] When a c-plane GaN wafer grown by the ammonothermal method was used as a seed crystal, no selective growth mask was used, and the molar ratios of F and I contained in the mineralizer to NH 3 were set to 5.0% and 3.5%, respectively.
[0257] The growth conditions when the c-plane GaN wafer grown by the ammonothermal method is used as the seed crystal are: the temperature of the dissolution zone is T D The temperature T of the growth zone G The average value is 605~615℃, and the temperature difference between the two zones is T D -T G About 15~20℃(T D >T G), the pressure is about 210~220MPa.
[0258] b. Assembly of the Seed Module
[0259] Using a multi-wire saw, a plurality of c-plane wafers were sliced in parallel from a bulk GaN crystal grown in the order described in item a. above, and three wafers were selected from them. After the crystal orientation of the selected three wafers was confirmed by an X-ray diffraction device, a portion of the edge was cut off by a dicing saw in such a way that the main surface became rectangular or approximately rectangular. Thus, wafers A to C shown in Table 1 below were prepared.
[0260] [Table 1]
[0261]
[0262] During the production process of wafer A, dicing saw processing was performed so that one of the long sides of the substantially rectangular main surface was within ±0.005 degrees with respect to the m-axis direction.
[0263] The same dicing saw process is also performed during the production of wafer B.
[0264] Next, using wax as an adhesive, wafer A, wafer B, and wafer C are fixed to each other, thereby assembling Figure 8 A temporary seed assembly is shown.
[0265] Figure 8 (a) is a top view of the temporary seed crystal assembly as viewed from the surface side, Figure 8 (b) is a side view of the temporary seed assembly observed from a direction parallel to the long side of wafer A. In this experiment, the side of the main surface of wafers A to C facing the N polarity side is called the surface side of the temporary seed assembly. The directions of the c-axis, a-axis, and m-axis of the three wafers A to C are consistent, including polarity.
[0266] Wafer A and wafer B are adjacent to each other on the surface side of the temporary seed crystal assembly so that the long sides processed in a manner within ±0.005 degrees relative to the m-axis direction are adjacent to each other, and are arranged in parallel so that there is no gap when observed with the naked eye. Wafer C is arranged on the back side of the temporary seed crystal assembly so that half of it overlaps with wafer A and half overlaps with wafer B.
[0267] Next, use an ultrasonic drill with a diameter of 0.7 mm, such as Fig. 9 As shown, a plurality of through holes are formed through the temporary seed assembly.
[0268] The plurality of through holes penetrate both wafers. That is, the through holes formed at the overlapping portion of wafer A and wafer C penetrate both wafer A and wafer C, and the through holes formed at the overlapping portion of wafer B and wafer C penetrate both wafer B and wafer C.
[0269] The plurality of through holes are arranged in pairs with other through holes, and the distance between the central axes of the two through holes in the pair is set to 2 mm in the through hole pair of type I and 4 mm in the through hole pair of type II.
[0270] Here, a type I through-hole pair refers to a pair of through-holes in which both of the two through-holes pass through chip A and chip C, or both of the through-holes pass through chip B and chip C, and a type II through-hole pair refers to a pair of through-holes in which one of the two through-holes passes through chip A and chip C, and the other passes through chip B and chip C.
[0271] When looking down at the temporary seed crystal assembly, the straight line connecting the central axes of the two through holes forming the type I through hole pair is parallel to the <10-10> crystal axis, and the straight line connecting the central axes of the two through holes forming the type II through hole pair is perpendicular to the boundary between chip A and chip B.
[0272] It should be noted that in this process, in addition to the above-mentioned through holes, a through hole necessary for suspending the permanent seed assembly to be formed later in the sealed container is also formed. Fig. 9 The illustration is omitted.
[0273] After forming the through-holes, the temporary seed assembly was disassembled by heating and melting the wax used for bonding. After wiping off the attached wax, wafers A, B, and C were etched with a 48% KOH aqueous solution heated to 100° C. to remove the damaged layer.
[0274] Next, a permanent seed crystal assembly was assembled by fixing wafer A, wafer B, and wafer C to each other in the same arrangement as the temporary seed crystal assembly.
[0275] In the assembly of the permanent seed assembly, one end and the other end of a Pt wire with a diameter of 0.2 mm are passed through one and the other of the paired through holes from the surface side, respectively, and twisted on the back side. Here, the side of the main surface of wafers A to C facing the N polarity side is referred to as the surface side of the permanent seed assembly.
[0276] Fig.10 It is shown as an example, and is a cross-sectional view showing a state in which, in a pair of I-type through holes provided in the overlapping portion of chip A and chip C, one end and the other end of the Pt wire pass through one and the other through holes from the surface side as described above and then merge on the back side.
[0277] Fig.11 This is a top view of the completed permanent seed assembly from the surface side. Fig.11 In FIG. 1 , the wafer C whose outline is drawn with a dotted line is arranged on the back side of the seed crystal assembly and serves as a connecting plate for connecting the wafer A and the wafer B.
[0278] [Step 2]
[0279] In step 2, a first generation GaN crystal is grown on a permanent seed assembly (hereinafter referred to as "seed assembly") by an ammonothermal method as described below.
[0280] The raw material used was polycrystalline GaN produced by the following method: HCl gas was brought into contact with Ga single substance under heating to generate gas GaCl, and the gas GaCl was reacted with NH3 gas. NH4F and NH4I were used as mineralizers. NH4I was synthesized by reacting HI (hydrogen iodide) gas with NH3 in a Pt-Ir sealed container.
[0281] The molar ratios of F and I contained in the mineralizer to NH 3 used as a solvent were 5.0% and 3.5%, respectively.
[0282] The growth conditions of the first generation of GaN crystals are: the temperature of the melting zone T D The temperature T of the growth zone G The average value is about 605-615℃, and the temperature difference between the two zones is T D -T G About 15~20℃(T D >T G ), the pressure inside the sealed container is about 210~220MPa.
[0283] The first-generation GaN crystal grown encloses the entire seed crystal assembly, but because the whole is transparent, it can be confirmed by naked eye that there is no sign of abnormal growth caused by the through hole formed in the c-plane GaN wafer that constitutes the seed crystal, or the Pt wire passing through the through hole.
[0284] [Step 3]
[0285] As described above, the first generation GaN crystal grown in step 2 encloses the entire seed crystal assembly, and a plurality of c-plane wafers are sliced from the portion grown on the surface side of the seed crystal assembly using a wire saw.
[0286] [Step 4]
[0287] In step 4, a piece of the c-plane GaN wafer sliced in step 3 is used as a seed crystal, and a second-generation GaN crystal is grown by an ammonothermal method, thereby producing a large-area bulk GaN crystal containing the seed crystal.
[0288] In the growth of the second generation GaN crystal, the raw materials used and the molar ratio of F and I contained in the mineralizer to NH3 used as a solvent are the same as those used in the growth of the first generation GaN crystal. In addition, the growth conditions used are also the same as those used in the growth of the first generation GaN crystal.
[0289] The appearance of the obtained large-area bulk GaN crystal observed from the N-polar side is shown in Fig.12 The crystal is a plate-like crystal with a main face oriented along the c-axis, and the thickness including the seed crystal contained inside is 2.93 mm. The main face has a shape obtained by cutting off four corners from a square with two sides roughly parallel to the m-axis and the other two sides roughly parallel to the a-axis. In terms of the total width of the crystal, Fig.12 The direction shown as the m-axis is 8.8 cm. Fig.12 The main surface has a diameter of 9.1 cm and a diameter of 7.5 cm (area of about 44 cm). 2 ) area.
[0290] 4.2. Evaluation of Large Area Bulk GaN Crystals
[0291] In order to evaluate the curvature of the c-plane of the large-area bulk GaN crystal obtained in 4.1. above, XRD rocking curves were measured with the (002) crystal plane as the reflection plane at intervals of 5 mm along a line passing through the approximate center of the main surface on the N-polar side of the crystal. Therefore, the number of measurement points on one line was 17.
[0292] The X-ray diffraction apparatus used for the measurement was Panalytical X'Part PRO manufactured by Spectris Corporation. The CuKα ray source of the apparatus was operated at 30 kV and 10 mA, and a Ge (220) hybrid monochromator was used to obtain CuKα1 rays.
[0293] Measure the lines perpendicular to the a-axis and Fig.12 In the figure, the first line is an imaginary line segment which is substantially parallel to the m-axis direction, and the second line is an imaginary line segment which is perpendicular to the first line.
[0294] In the measurement on the first line, the ω axis is perpendicular to the first line and the X-ray incident plane is parallel to the first line. In the measurement on the second line, the ω axis is perpendicular to the second line and the X-ray incident plane is parallel to the second line.
[0295] The measurement results on the first line are shown in Fig.13 (a), and the measurement results on the second line are shown in Fig.13 (b).
[0296] exist Fig.13 (a) and Fig.13 In each graph of (b), the horizontal axis represents the relative position of each measuring point when the central measuring point is taken as the origin, that is, the distance from the origin, and the vertical axis represents the peak angle ω of the rocking curve of each measuring point and the average value ω of the peak angle among all 17 measuring points. AVE The difference Δω(=ω-ω AVE ).
[0297] Whether on the first line or the second line, the variation range of Δω is very small, and the difference between the maximum and minimum values of Δω between the 17 measurement points on all lines is 0.012 degrees. It should be noted that, according to the definition of Δω, it can be understood that the difference between the maximum and minimum values of Δω is the same as the difference between the maximum and minimum values of the peak angle ω of the rocking curve.
[0298] In addition, there is no portion where the peak angle difference of the rocking curve between two adjacent measurement points is greater than 0.01 degrees in absolute value on either the first line or the second line. The maximum value (absolute value) of the peak angle difference of the rocking curve between two adjacent measurement points is 0.007 degrees on the first line and 0.004 degrees on the second line.
[0299] like Fig.13 As shown in (a) and (b), no tendency of monotonous increase or decrease of Δω was confirmed on either the first line or the second line, and the curvature radius of the c-plane calculated based on the rate of change of Δω obtained by linear fitting using the least squares method was 1050m on the first line and 450m on the second line.
[0300] If the large-area bulk GaN crystal produced in the above 4.1. is sliced along the c-plane, a c-plane GaN wafer with a diameter of about 2 inches (50-55 mm) or about 3 inches (75-80 mm) can be obtained, and the variation range of the m-axis direction component and the a-axis direction component of the off-angle is less than 0.012 degrees in the main plane.
[0301] It should be noted that, according to the results obtained by measuring GaN crystals grown by similar or equivalent methods, on the main surface of the large-area bulk GaN crystal produced in 4.1. above, in all 100μm×100μm regions, the dislocation density calculated based on the number of dislocations in the region and the area of the region is less than 1×10 6 cm -2In addition, in all 2 mm × 2 mm regions, the dislocation density calculated based on the number of dislocations in the region and the area of the region is less than 1 × 10 5 cm -2 .
[0302] As shown in the evaluation results, the large-area bulk GaN crystal produced in 4.1. above has a significantly improved c-plane curvature even with a large area of about 9 cm in both length and width. This shows that the seed assembly involved in the technical idea of the present inventors is useful as a method for increasing the area without applying stress to the GaN crystal grown thereon.
[0303] In addition, although two c-plane GaN wafers are arranged side by side on the surface side of the seed crystal assembly, no obvious difference in the inclination of the c-axis is found in the large-area bulk GaN crystal containing the GaN crystal grown thereon, which can be said to be a result that deserves special mention.
[0304] The detailed mechanism for obtaining such a result is not yet clear, but it is possible that the grown GaN crystals spontaneously align neatly. For example, it is possible that the surface of the seed assembly dissolves before the growth zone reaches a supersaturated state during the ammonothermal process, and the Pt wire relaxes due to the widening of the through hole, thereby spontaneously deforming the seed assembly and minimizing the stress of the grown GaN crystal.
[0305] Reasonably considering, it can be considered that even if the area of the GaN wafer constituting the seed assembly increases, or the number of GaN wafers constituting the seed assembly increases, the preferred effect obtained based on the use of the seed assembly will not be significantly hindered. Therefore, by expanding the area of the GaN wafer constituting the seed assembly and / or increasing the number of wafers, it is also possible to manufacture a large-area bulk GaN crystal with a vertical and horizontal size of about 4 inches (100-105 mm) and further about 6 inches (150-155 mm) of the same quality as the crystal manufactured in the above experiment.
[0306] The present invention has been described above in conjunction with specific embodiments, but each embodiment is merely an example and does not limit the scope of the present invention. Various modifications may be made to each embodiment described in this specification without departing from the gist of the invention, and may be combined with features described in other embodiments within the scope of implementation.
Claims
1. A bulk GaN crystal having a primary surface selected from a surface inclined at 0 to 10 degrees relative to a (0001) crystal plane and a surface inclined at 0 to 10 degrees relative to a (000-1) crystal plane, wherein the primary surface is a specific primary surface A satisfying the following conditions (i) and (ii): (i) a first line having a length of 80 mm and extending along a first direction can be drawn on the specific principal surface A, and the difference between the maximum value and the minimum value of the peak angle of the (002) XRD rocking curve of the GaN crystal measured at 17 measurement points arranged at intervals of 5 mm on the first line with the ω axis perpendicular to the first direction is 0.05 degrees or less; (ii) a second line having a length of 80 mm and extending along a second direction perpendicular to the first direction can be drawn on the specific principal surface A, and the difference between the maximum value and the minimum value of the peak angle of the (002) XRD rocking curve of the GaN crystal measured with the ω axis perpendicular to the second direction at 17 measurement points arranged on the second line at intervals of 5 mm is 0.05 degrees or less, in, In all 2 mm×2 mm virtual regions that can be arbitrarily set in the specific main surface A except for the portion less than 5 mm from the outer periphery in a plan view, the dislocation density is less than 1×10 5 cm -2 .
2. A bulk GaN crystal having a first principal surface and a second principal surface facing in opposite directions, wherein one of the first principal surface and the second principal surface is a surface inclined at a degree of not less than 0 and not more than 10 with respect to a (0001) crystal plane, and the other surface is a surface inclined at a degree of not less than 0 and not more than 10 with respect to a (000-1) crystal plane, and the bulk GaN crystal satisfies the following conditions (i) and (ii): (i) a first line having a length of 80 mm and extending along a first direction can be drawn on the first principal surface, and the difference between the maximum and minimum values of the peak angle of the (002) XRD rocking curve of the GaN crystal measured at 17 measurement points arranged at intervals of 5 mm on the first line with the ω axis perpendicular to the first direction is 0.05 degrees or less; (ii) a second line having a length of 80 mm and extending along a second direction perpendicular to the first direction can be drawn on the first principal surface, and the difference between the maximum value and the minimum value of the peak angle of the (002) XRD rocking curve of the GaN crystal measured with the ω axis perpendicular to the second direction between 17 measurement points arranged at intervals of 5 mm on the second line is 0.05 degrees or less, in, In all 2 mm×2 mm imaginary regions that can be arbitrarily set in the first main surface except for the portion that is less than 5 mm from the periphery when viewed from above, the dislocation density calculated based on the number of dislocations in the region and the area of the region is less than 1×10 5 cm -2 .
3. The bulk GaN crystal according to claim 1 or 2, wherein: The difference between the maximum value and the minimum value of the peak angle in the condition (i) and the difference between the maximum value and the minimum value of the peak angle in the condition (ii) are both 0.02 degrees or less.
4. The bulk GaN crystal according to claim 1 or 2, wherein: The 17 measurement points in the condition (i) and the 17 measurement points in the condition (ii) do not include a measurement point whose peak angle differs from an adjacent measurement point by 0.01 degrees or more.
5. The bulk GaN crystal according to claim 1 or 2, wherein: The radius of curvature of the surface along the first direction calculated based on the rate of change of the peak angle in the condition (i) and the radius of curvature of the surface along the second direction calculated based on the rate of change of the peak angle in the condition (ii) are both greater than 300 m.
6. The bulk GaN crystal according to claim 1 or 2, which satisfies one or more conditions selected from the following (a) to (g): (a) H concentration is 1×10 17 atoms / cm 3 above; (b) O concentration is 1×10 17 atoms / cm 3 above; (c) The concentration of at least one of Li, Na and K is less than 1×10 15 atoms / cm 3 ; (d) The F concentration is 1×10 15 atoms / cm 3 above; (e) The concentration of at least one of Cl, Br and I is 1×10 15 atoms / cm 3 above; (f) I concentration is 1×10 15 atoms / cm 3 above; (g) Si concentration is less than 2×10 15 atoms / cm 3 .
7. The bulk GaN crystal according to claim 2 has a wavelength of 3140-3200 cm in the infrared absorption spectrum. -1 There are peaks attributed to gallium vacancy-hydrogen complexes.
8. A c-plane GaN wafer having a main surface selected from a surface inclined at 0 to 10 degrees relative to a (0001) crystal plane and a surface inclined at 0 to 10 degrees relative to a (000-1) crystal plane, wherein the main surface is a specific main surface B satisfying the following condition (iii): (iii) the specific main surface B can be drawn with an imaginary line segment of 75 mm or more, and the variation range of the m-axis component and the variation range of the a-axis component of the deflection angle are both less than 0.05 degrees, except for a portion less than 5 mm from the outer periphery when viewed from above, in, In all 2 mm×2 mm virtual regions that can be arbitrarily set except for the portion less than 5 mm from the periphery in a plan view of the specific main surface B, the dislocation density is less than 1×10 5 cm -2 .
9. A c-plane GaN wafer having a third main surface and a fourth main surface facing in opposite directions, wherein one of the third main surface and the fourth main surface is a surface inclined at 0 degrees or more and 10 degrees or less relative to a (0001) crystal plane, and the other surface is a surface inclined at 0 degrees or more and 10 degrees or less relative to a (000-1) crystal plane, The third main surface can draw an imaginary line segment of more than 75 mm, and the variation range of the m-axis component and the a-axis component of the deflection angle are both within 0.05 degrees, except for the portion less than 5 mm from the outer periphery when viewed from above. in, The dislocation density is less than 1×10 5 cm -2 .
10. The c-plane GaN wafer according to claim 8 or 9, wherein: The variation range of the m-axis component of the off-angle and the variation range of the a-axis component are both within 0.02 degrees. 11 . The c-plane GaN wafer according to claim 8 , having any diameter selected from 50 mm to 55 mm, 75 mm to 80 mm, 100 mm to 105 mm, and 150 mm to 155 mm.
12. The c-plane GaN wafer according to claim 8 or 9, which satisfies one or more conditions selected from the following (a) to (g): (a) H concentration is 1×10 17 atoms / cm 3 above; (b) O concentration is 1×10 17 atoms / cm 3 above; (c) The concentration of at least one of Li, Na and K is less than 1×10 15 atoms / cm 3 ; (d) The F concentration is 1×10 15 atoms / cm 3 above; (e) The concentration of at least one of Cl, Br and I is 1×10 15 atoms / cm 3 above; (f) I concentration is 1×10 15 atoms / cm 3 above; (g) Si concentration is less than 2×10 15 atoms / cm 3 .
13. The c-plane GaN wafer according to claim 12, wherein the GaN wafer has a wavelength of 3140 to 3200 cm-1 in the infrared absorption spectrum. -1 There are peaks attributed to gallium vacancy-hydrogen complexes.
14. An epitaxial wafer comprising: The c-plane GaN wafer according to any one of claims 8 to 13, and One or more nitride semiconductor layers are epitaxially grown on the c-plane GaN wafer.
15. A method for manufacturing an epitaxial wafer, the method comprising: The step of preparing a c-plane GaN wafer according to any one of claims 8 to 13; and A step of epitaxially growing one or more nitride semiconductor layers on the c-plane GaN wafer.
16. A method for manufacturing a nitride semiconductor device, the method comprising: The step of preparing a c-plane GaN wafer according to any one of claims 8 to 13; and A step of epitaxially growing one or more nitride semiconductor layers on the c-plane GaN wafer.
17. A method for manufacturing a bulk GaN crystal, the method comprising: The step of preparing a c-plane GaN wafer according to any one of claims 8 to 13; and A step of epitaxially growing GaN crystal from a gas phase on the c-plane GaN wafer.
18. A method for manufacturing a bulk GaN crystal, the method comprising: The step of growing GaN crystal on the seed crystal assembly by ammonothermal method, The seed crystal assembly includes a plurality of c-plane GaN wafers, and the plurality of c-plane GaN wafers are fixed to each other using metal wires. The c-axis, a-axis and m-axis of all c-plane GaN wafers constituting the seed crystal assembly are oriented in the same direction. When the direction of the N-polarity side of the main surface of the c-plane GaN chip constituting the seed crystal component is set as the surface direction, the seed crystal component has two or more c-plane GaN chips each having a rectangular or substantially rectangular main surface arranged adjacently and side by side on the surface direction side of the seed crystal component, and a c-plane GaN chip is arranged on the opposite direction side of the surface direction of the seed crystal component.
19. The method for manufacturing bulk GaN crystal according to claim 18, wherein: In the step of growing the GaN crystal by the ammonothermal method, a mineralizer including a halogen-containing compound is used, and as the metal wire, at least any one metal wire selected from the group consisting of an Ag wire, a Pt wire, and an Au wire is used.
20. A method for manufacturing a c-plane GaN wafer, the method comprising at least: A step of preparing a bulk GaN crystal by the method for producing a bulk GaN crystal according to claim 18 or 19; and The step of slicing the GaN crystal.
21. The manufacturing method according to claim 20, wherein: The c-plane GaN wafer has a disk shape, and a diameter of a circle constituting the disk shape is 50 mm or more.