A pigment with easy color adjustment and high near-infrared reflectivity, its preparation method and application

The Zn1-xAxWO4 inorganic pigment, prepared by incorporating transition metal ions, solves the problems of limited color and low near-infrared reflectivity, achieving diverse color representation and high reflectivity, reducing energy consumption, and is suitable for applications such as building exterior wall coatings.

CN114045047BActive Publication Date: 2026-11-17JIANGXI SHANNA NEW MATERIAL TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202111589014.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-11-03
Filing Date
2021-12-23
Publication Date
2026-11-17
Estimated Expiration
2041-12-23

AI Technical Summary

Technical Problem

Existing inorganic pigments have limited color options, low near-infrared reflectivity, high energy consumption in their preparation process, and contain toxic elements, making it difficult to meet architectural aesthetic requirements and energy conservation and emission reduction requirements.

Method used

Zn1-xAxWO4 inorganic pigments were synthesized by solution combustion. By incorporating transition metal ions such as Co, Mn, Fe, Cu, or Cr, pigments with rich colors, high near-infrared reflectivity, and green and non-toxic properties were prepared. The calcination temperature was low and the process was simple.

Benefits of technology

It achieves diverse color representation of pigments, has a near-infrared reflectivity of over 85%, good acid and alkali resistance, a simple process that is easy to industrialize, reduces energy consumption, and improves the thermal insulation performance of buildings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114045047B_ABST
    Figure CN114045047B_ABST
Patent Text Reader

Abstract

A pigment with easily tinted color and high near-infrared reflectivity and its preparation method, characterized in that its general chemical formula is Zn. 1‑x A x WO4, wherein A is one or more of Co, Mn, Fe, Cu, or Cr. The preparation method is as follows: according to Zn... 1‑x A x The stoichiometric ratio and preparation amount of WO4 are determined by weighing out the nitrates of the corresponding transition metal elements; dissolving them in water to prepare a mixed metal ion solution; then weighing out an appropriate amount of ammonium metatungstate and adding it to the mixed metal ion solution to obtain a mixed solution; then weighing out an appropriate amount of organic fuel and dissolving it in the resulting mixed solution, heating the mixed solution to concentrate it to a viscous state, initiating self-propagating combustion, and then calcining the self-propagating combustion products to obtain the pigment. This invention can obtain pigment powders of various colors, high near-infrared reflectivity, and are environmentally friendly, with low equipment requirements, easy industrialization, and wide applications in building roofs and exterior walls, automobiles, containers, and plastics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of functional inorganic pigment technology, and specifically relates to an easily tinted high near-infrared reflectance pigment and its preparation method, claiming priority to application number 2021112931983 filed on November 3, 2021. Technical Background

[0002] In the past decade or so, a large-scale migration of people to cities has led to a decrease in urban green vegetation and an increase in buildings. These buildings absorb a significant amount of solar heat through their exterior walls, which then seeps into interior spaces, raising temperatures and increasing energy consumption for air conditioning, thus contributing to national energy consumption. Inorganic pigments with heat-insulating properties can effectively reduce heat absorption by buildings and also serve a decorative purpose on building exteriors. Based on the heat insulation mechanism of building exterior coatings, they can be divided into three types: barrier, reflective, and radiative. Among these, reflective coatings offer the best heat insulation effect. 5% of solar heat is distributed in the ultraviolet region, 52% in the visible light region, and 43% in the near-infrared region. Different wavelengths of visible light absorption result in different colors. Given a specific color, the reflectivity of the near-infrared band should be maximized to improve the pigment's heat reflection.

[0003] Traditional near-infrared reflective pigments used for building exteriors are mostly white or light-colored, offering limited color options and failing to meet aesthetic demands. Furthermore, most inorganic pigments with high near-infrared reflectivity are prepared using solid-state methods, which require high calcination temperatures, result in large particles, and consume significant energy. In addition, most inorganic pigments contain large amounts of toxic elements such as Pb, Cd, and Ni, and their low near-infrared reflectivity poses a serious threat to ecological safety with large-scale use. ZnWO4, a common tungstate, has been widely used in heterogeneous catalysts, photocatalytic water degradation, and phosphors due to its excellent ionic conductivity, physicochemical stability, and photogenerated carrier performance. However, research on its use as a high-near-infrared reflective inorganic pigment has not been reported. Zn has similar ionic radii to colored transition metal ions such as Mn, Fe, and Co, making it easily incorporated into the ZnWO4 lattice. Therefore, using ZnWO4 as a matrix and incorporating different transition metal ions to synthesize an inorganic pigment with rich colors, high near-infrared reflectivity, and a simple process is of significant research value. Summary of the Invention

[0004] The purpose of this invention is to address the problems of limited color and low near-infrared reflectance in existing near-infrared reflective inorganic pigments by providing an inorganic pigment with a simple preparation process, high near-infrared reflectance, and that is green and non-toxic.

[0005] A pigment with easy color adjustment and high near-infrared reflectivity, its general chemical formula is Zn. 1-x Ax WO4, where A is one or more of Co, Mn, Fe, Cu, or Cr, 0 <x≤0.2。

[0006] This invention also provides a method for preparing an easily tinted, high near-infrared reflectance pigment, comprising the following steps:

[0007] (1) According to Zn 1-x A x The stoichiometric ratio and preparation amount of WO4 were determined by weighing the nitrates of the corresponding transition metal elements; they were dissolved in water to prepare a mixed metal ion solution.

[0008] (2) According to Zn 1-x A x The stoichiometric ratio of WO4 and its preparation amount are determined. Then, an appropriate amount of ammonium metatungstate is weighed and added to the mixed metal ion solution in step (1) to obtain a mixed solution.

[0009] (3) Weigh out an appropriate amount of organic fuel and dissolve it in the mixed solution obtained in step (2). Heat the mixed solution to concentrate it to a viscous state, initiate self-propagating combustion, and then calcine the self-propagating combustion product to obtain pigment.

[0010] Further preferably, in step (3), the organic fuel is one or more of ethylene glycol, glycine, citric acid or urea, and the number of moles of the added organic fuel is 1-5 times the number of moles of metal ions in the mixed solution.

[0011] Further preferred, in step (3), the self-propagating combustion initiation temperature is 300-500℃, the calcination temperature of the self-propagating combustion products is 600-1000℃, and the calcination time is 1-4 hours.

[0012] This invention also provides an application of an easily tinted, high near-infrared reflectance pigment, used as a colorant in building exterior wall coatings, automotive coatings, and container coatings.

[0013] This invention also provides an application of an easily tinted, high near-infrared reflectance pigment for use in heat-insulating coatings.

[0014] The features of this invention are:

[0015] (1) The inorganic pigments of the present invention are rich in color, including blue, yellow, brown and light green, and have good acid and alkali resistance;

[0016] (2) The calculated reflectance values ​​of the pigments of the present invention in the near-infrared band of 700-2500nm are all above 85%;

[0017] (3) The present invention is synthesized by solution combustion method, which has low calcination temperature, simple process and easy industrialization. Attached Figure Description

[0018] Figure 1 This is the XRD pattern of the pigment.

[0019] Figure 2 This is a high-resolution FE-SEM image of the pigment.

[0020] Figure 3 This is the EDS diagram of the pigment.

[0021] Figure 4 This is the UV-Vis diffuse reflectance spectrum.

[0022] Figure 5 This is the absorption spectrum of the pigment.

[0023] Figure 6 A photograph of pigments.

[0024] Figure 7 The near-infrared reflectance spectrum of the pigment.

[0025] Figure 8 Zn 1-x A x Solar reflectance spectrum of WO4 pigment.

[0026] Figure 9 Zn 0.95 Fe 0.05 Color coordinates and color difference of WO4 pigment after acid and alkali soaking. Detailed Implementation

[0027] A method for preparing an easily tinted pigment with high near-infrared reflectivity is as follows:

[0028] (1) According to Zn 1-x A x The stoichiometric ratio and preparation amount of WO4 were determined by weighing the nitrates of the corresponding transition metal elements; they were dissolved in water to prepare a mixed metal ion solution.

[0029] (2) According to Zn 1-x A x The stoichiometric ratio of WO4 and its preparation amount are determined. Then, an appropriate amount of ammonium metatungstate is weighed and added to the mixed metal ion solution in step (1) to obtain a mixed solution.

[0030] (3) Weigh an appropriate amount of organic fuel and dissolve it in the mixed solution obtained in step (2). The organic fuel is one or more of ethylene glycol, glycine, citric acid or urea. The number of moles of the organic fuel added is 1-5 times the number of moles of metal ions in the mixed solution. Heat the mixed solution to concentrate it to a viscous state and initiate self-propagating combustion. The self-propagating combustion temperature is 300-500℃. Calcinate the self-propagating combustion product in air at a temperature of 600-1000℃ for 1-4 hours to obtain the pigment.

[0031] The present invention will be further illustrated by the following embodiments.

[0032] Example 1

[0033] According to Zn 0.9 Co 0.1 According to the stoichiometric ratio of WO4, weigh 2.0081 g of Zn(NO3)3·6H2O and 0.2183 g of Co(NO3)3·6H2O and dissolve them in 35 ml of water; then weigh 1.9047 g of ammonium metatungstate and dissolve it in a transition metal ion solution to form a mixed solution; then weigh 1.6891 g of glycine and dissolve it in the mixed solution. Continue to heat and concentrate until it reaches a viscous state, and initiate a self-propagating combustion reaction at 500℃. Keep the combustion products at 800℃ in air for 3 hours to obtain pigment powder.

[0034] Example 2

[0035] According to Zn 0.9 Mn 0.1 According to the stoichiometric ratio of WO4, weigh 2.0081 g of Zn(NO3)3·6H2O and 0.2684 g of Mn(NO3)2 and dissolve them in 35 ml of water; then weigh 1.9047 g of ammonium metatungstate and dissolve it in a transition metal ion solution to form a mixed solution; then weigh 1.6891 g of glycine and dissolve it in the mixed solution. Continue to heat and concentrate until it reaches a viscous state, and initiate a self-propagating combustion reaction at 500℃. Keep the combustion products at 800℃ in air for 3 hours to obtain pigment powder.

[0036] Example 3

[0037] According to Zn 0.95 Fe 0.05 According to the stoichiometric ratio of WO4, weigh 2.1196 g of Zn(NO3)3·6H2O and 0.1515 g of Fe(NO3)3·9H2O and dissolve them in 35 ml of water; then weigh 1.9047 g of ammonium metatungstate and dissolve it in a transition metal ion solution to form a mixed solution; then weigh 1.6891 g of glycine and dissolve it in the mixed solution. Continue to heat and concentrate until it reaches a viscous state, and initiate a self-propagating combustion reaction at 500℃. Keep the combustion products at 800℃ in air for 3 hours to obtain pigment powder.

[0038] Example 4

[0039] According to Zn 0.9 Co 0.05 Mn 0.05According to the stoichiometric ratio of WO4, weigh 2.0081 g of Zn(NO3)3·6H2O, 0.1091 g of Co(NO3)3·6H2O, and 0.1342 g of Mn(NO3)2 and dissolve them in 35 ml of water; then weigh 1.9047 g of ammonium metatungstate and dissolve it in a transition metal ion solution to form a mixed solution; then weigh 1.6891 g of glycine and dissolve it in the mixed solution. Continue to heat and concentrate until it reaches a viscous state, and initiate a self-propagating combustion reaction at 500℃. Keep the combustion products at 800℃ in air for 3 hours to obtain pigment powder.

[0040] Example 5

[0041] According to Zn 0.95 Co 0.02 Fe 0.03 According to the stoichiometric ratio of WO4, weigh 2.1196 g of Zn(NO3)3·6H2O, 0.0437 g of Co(NO3)3·6H2O, and 0.0909 g of Fe(NO3)3·9H2O and dissolve them in 35 ml of water; then weigh 1.9047 g of ammonium metatungstate and dissolve it in a transition metal ion solution to form a mixed solution; then weigh 1.6891 g of glycine and dissolve it in the mixed solution. Continue to heat and concentrate until it reaches a viscous state, and initiate a self-propagating combustion reaction at 500℃. Keep the combustion products at 800℃ in air for 3 hours to obtain pigment powder.

[0042] Comparative Example

[0043] The comparison sample was ZnWO4.

[0044] The crystal structure of the prepared pigment powders was characterized by X-ray diffraction (XRD) on a powder X-ray diffractometer (Bruker, D8) with Cu Kα (λ = 0.154060 nm, 40 kV, 40 mA) radiation between 10 and 90° (step size 0.02°). Morphological analysis of the pigment powders was performed using a field emission scanning electron microscope (FE-SEM, Quanta 200FEG) at an accelerating voltage of 5 kV. The chemical composition distribution of the pigments was determined by an X-ray energy dispersive spectroscopy (Aztec X-Max 80) instrumented with the FE-SEM. X-ray photoelectron spectroscopy (XPS) was performed to determine the elemental valence states of the pigment powders. Diffuse reflectance spectra of all pigment powders in the range of 300 nm to 2500 nm were measured by a UV-Vis-NIR spectrophotometer. Near-infrared reflectance (R) was calculated in the wavelength range of 700 nm to 2500 nm according to ASTM G173-03 reference. The formula is

[0045]

[0046] Where r(λ) is the experimentally obtained spectral reflectance (W·m).-2 ), i(λ) is the solar spectral irradiance (W·m) obtained according to ASTM standard G173-03. -2 ·nm -1 ).

[0047] The diffuse reflectance data from 300 nm to 800 nm were converted into absorption data using the Kubelka-Munk equation:

[0048] F(R)=(1-R) 2 / 2R=α / S (2)

[0049] Where R is reflectivity, and α and S represent absorption and scattering factors, respectively.

[0050] The color parameters L* (luminosity), a* (green to red axis), and b* (blue to yellow axis) were calculated using spectral data obtained in the range of 380 nm to 780 nm. First, the mathematical processing involved determining the X, Y, and Z tristimulus values ​​as defined by CIE 1964 from integrals. Then, the L*, a*, and b* color parameters were measured by transferring from the XYZ space to the CIE 1976 L*a*b* space. To assess chemical stability and durability, the prepared pigments were immersed in 5% HNO3, HCl, H2SO4, and Na(OH) solutions, respectively, with stirring for 15 min. The treated pigment powders were then washed and dried. The color parameters of the pigments after immersion were tested and calculated using the formula... Calculate the color difference; if the color difference does not exceed 5, the pigment can be considered to have excellent chemical stability.

[0051] Zn 1-x A x The XRD pattern of WO4 pigment is as follows Figure 1 As shown in the figure, detailed analysis reveals that the characteristic peaks of all pigments are very clear and consistent with those of ZnWO4 (JCPDSNO15-0774) with a standard wolframite structure, indicating that the prepared pigment structure was successfully synthesized. The absence of impurity peaks in the XRD pattern indicates that transition metal ions have completely entered the ZnWO4 lattice and replaced Zn. 2+ Without generating any other phases, as long as the doping amount of transition metal ions does not exceed 0.1 (x≤0.1), the monoclinic crystal structure remains unchanged and belongs to the P2 / c(13) space group.

[0052] With doping of different transition metal ions, the lattice parameters and average grain size of the pigments are refined and are given in Table 1. A slight decrease in lattice parameters (a, b, and c) can be observed, which may be attributed to the doping metal ion (Co). 2+ 0.065 nm, Fe 3+ (0.069nm) compared to Zn 2+The radius of Mn is smaller (0.074nm), while Mn 2+ It has a larger radius of 0.080 nm, which leads to lattice distortion and an increase in cell volume.

[0053] Table 1. Zn 1-x A x lattice parameters of WO4 pigment

[0054]

[0055] The crystal structure of ZnWO4 inorganic pigments exhibits characteristics of wolframite structure. 2+ and W 6+ The ions reacted with the six O atoms respectively 2- Ionic bonding forms distorted ZnO6 and WO6 octahedral geometries, which are interconnected by sharing an angle. The corresponding angle-sharing octahedral tilt angles are 47-54°. In addition, there are two equivalent O atoms. 2- Site, one type is O 2- With a W 6+ And two identical Zn 2+ Ionic bonding, another type is O 2- Connect to two equivalent W 6+ and a Zn 2+ When different transition metal ions (A = Co, Mn, Fe) are doped into the ZnWO4 host, severely distorted octahedral Zn / A-O6 chromophores will appear in the compound.

[0056] High-resolution FE-SEM images of the pigments obtained in Examples 1-4 are shown below. Figure 2 As shown. Zn was detected by EDS analysis. 0.9 Co 0.1 The chemical composition of WO4 pigments was determined by EDS spectroscopy, which showed that all expected elements, including Zn, Co, W, and O, were detected in the pigments, and the stoichiometry calculated by EDS analysis was very close to the theoretical values.

[0057] Zn 1-x A x The UV-Vis diffuse reflectance and corresponding absorption spectra of WO4 (A=Co,Mn,Fe) are as follows: Figure 4 , 5 As shown. In Figure 4 In the analysis, it can be detected that ZnWO4 reflects almost all sunlight in the visible light spectrum, indicating that ZnWO4 is white. After doping different chromophores into the ZnWO4 lattice, distinct spectral valleys appear, indicating that some visible light has been absorbed, resulting in different colors in the prepared pigments. For example... Figure 5 As shown, Zn 2+There are no dd transitions because of its fully filled d orbitals, and the weak absorption peak in the UV region can be attributed to ligand-to-metal charge transfer transitions. For Zn 0.9 Co 0.1 WO4, Zn 0.9 Co 0.05 Mn 0.05 WO4 and Zn 0.95 Co 0.02 Fe 0.03 WO4 compounds, due to 4 T1g→ 4 During the T2g transition, the blue CoO6 twisted octahedral chromophore exhibits a slight absorption around 1 eV, with the absorption spanning from 2 to 2.5 eV. This is due to... 4 T1g→ 4 T2g(p) and 4 T1g→ 4 This is caused by the A2g transition. Due to the Mn... 2+ and Fe 3+ The d orbitals have the same 5 electrons and the dd transition is spin-forbidden. The transfer of charge from the partially filled Mn3d orbitals to the W5d orbitals brings about extensive absorption in the ultraviolet region.

[0058] The color coordinates of the pigments and ZnWO4 obtained in Examples 1-5 were characterized using the CIE 1976 L*a*b* color space, as shown in Table 2. The L* axis represents lightness from 0 to 100; the smaller the L* value, the darker the pigment color. The a* axis represents colors from green (-) to red (+), and the b* axis represents colors from blue (-) to yellow (+). The color coordinates of the ZnWO4 pigment are L* = 98.68, a* = -0.95, and b* = 3.14, determining the color to be white. Figure 6 The color of ZnWO4 is uniform. However, through transition metal ion doping, the color of ZnWO4 changes significantly. 0.9 Co 0.1 The b* value of WO4 pigment is -22.19, indicating a shift towards blue. This can be determined by using Mn... 2+ Ions fully replace Zn 2+ The b* value increased from 3.14 to 31.36, which corresponds to the yellow color. Meanwhile, Fe... 3+ Replace Zn 2+ This results in the a* axis being slightly closer to green, the b* axis closer to yellow, and the final color being brown. Due to Co... 2+ &Mn 2+ Co-doping with ZnWO4 dramatically increases the b* value to 6.18, ultimately resulting in a bright green color. Furthermore, although Co... 2+ and Fe 3+All of them have been incorporated into the ZnWO4 lattice, but the values ​​of a* and b* have not changed significantly and remain brown. Therefore, the color values ​​of these high near-infrared pigments are consistent with the color of the pigment powder.

[0059] Table 2. CIE 1976 L*a*b* values ​​of pigments

[0060]

[0061] To reduce energy consumption caused by buildings absorbing solar radiation, the use of high near-infrared reflectance pigments in coatings is essential. Near-infrared reflectance and spectral irradiance in the 700-2500 nm range are as follows: Figure 7-8 As shown, Figure 7 It can be clearly seen that the ZnWO4 pigment has the highest near-infrared reflectance, at 96.66%. When chromophores replace Zn... 2+ After ionization, the near-infrared reflectance in the 1300-2100 nm wavelength range decreased slightly, but compared with the generally reported near-infrared spectra, the synthesized pigment still maintained a high near-infrared reflectance (R) for reflective pigments, such as Ce. 0.8 Bi 0.2 O2 yellow pigment (R = 87.31%), Sr 0.6 Eu 0.4 CuSi4O 10+σ Blue pigments (R = 57.07%), etc. Furthermore, these pigments represent a significant portion of solar irradiance. This indicates that these pigments used in coatings can reflect a large amount of heat, and all of them are promising candidates for cool pigments to save energy.

[0062] Excellent stability of pigments plays a crucial role in coating applications; therefore, pigments with high near-infrared reflectance need to withstand harsh operating conditions. The calcination temperature of the pigment is 800℃, meaning that the prepared pigment can withstand high temperatures without affecting its color or near-infrared reflectance. Furthermore, typical Zn is selected... 0.95 Fe 0.05 WO4 pigments were shaken in a 5% acid-base solution for 15 minutes to assess their chemical stability. Treated Zn... 0.95 Fe 0.05 The chromaticity values ​​of WO4 pigments are summarized in Figure 9 The pigment does not show significant color change when immersed in either acidic or alkaline solutions. When calculating the color difference ΔE* using the formula, the result is far less than the allowable limit (ΔE*≤5), indicating that it is a pigment with high near-infrared reflectance. Therefore, the above results reveal that Zn... 1-x A x WO4 (A = Co, Mn, Fe) inorganic pigments have good thermal and chemical stability.

[0063] The above embodiments are only for illustrating the technical concept and features of the present invention, and are intended to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be construed as limiting the scope of protection of the present invention. All equivalent changes or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.

Claims

1. The application of an easily tinted, high near-infrared reflectance pigment, characterized in that, Used in heat insulation coatings; The general chemical composition formula of the easily tonable high near-infrared reflectivity pigment is Zn 1-x A x WO4, wherein A is one or more of Co, Mn and Fe, and 0<x≤0.2; the preparation steps thereof are as follows: (1) According to Zn 1-x A x The stoichiometric ratio and preparation amount of WO4 were determined by weighing the nitrates of the corresponding transition metal elements; they were dissolved in water to prepare a mixed metal ion solution. (2) According to Zn 1-x A x The stoichiometric ratio of WO4 and its preparation amount, then weigh an appropriate amount of ammonium metatungstate and add it to the mixed metal ion solution in step (1) to obtain a mixed solution; (3) Weigh out an appropriate amount of one or more organic fuels from ethylene glycol, glycine, citric acid, or urea and dissolve them in the mixed solution obtained in step (2). Heat the mixed solution to concentrate it to a viscous state, initiate self-propagating combustion at 300-500℃, and then calcine the self-propagating combustion product at 600-1000℃ for 1-4 hours to obtain a pigment. The pigment has the crystal structure characteristics of wolframite. Zn 2+ and W 6+ The ions reacted with the six O atoms respectively 2- Ionic bonding forms distorted ZnO6 and WO6 octahedral geometries, which are interconnected by sharing an angle. The corresponding angle-sharing octahedral tilt angles are 47-54°. In addition, there are two equivalent O atoms. 2- Site, one type is O 2- With a W 6+ And two identical Zn 2+ Ionic bonding, another type is O 2- Connect to two equivalent W 6+ and a Zn 2+ When different transition metal ions are doped into the ZnWO4 matrix, distorted octahedral Zn / A-O6 chromophores appear in the compound.

Citation Information

Patent Citations

  • Tungstate upconversion luminescence temperature sensitive material doped with rare-earth elements Er and Yb and preparation method thereof

    CN105131950A

  • Amorphous stabilized nano composite anticorrosive pigment

    CN109836872A

  • Metal oxide particle and its use

    CN1922104A

  • LED conversion phosphors in the form of ceramic dodies

    US20100187976A1

  • Nanocomposite scintillator, detector, and method

    WO2007075983A2