Filters containing a silicon carbide separation layer
By using a porous ceramic membrane separation layer made of α-form recrystallized silicon carbide, combined with an intermediate layer and high-temperature sintering technology, the problems of insufficient filter backwashing capacity and low wear resistance in the existing technology are solved, achieving higher Excellent backwash resistance and selectivity, extending the service life of the filter.
Patent Information
- Application Number
- CN202080051938.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-07-10
AI Technical Summary
During the backwash process of existing filters, the membrane's anti-backwash ability is insufficient, resulting in a decrease in filtration performance, and it is difficult to improve the wear resistance and selectivity of the silicon carbide membrane at the same time.
A porous ceramic membrane separation layer made of α-form recrystallized silicon carbide (SiC) is used. By adjusting the porosity, pore size and tortuosity of the membrane, combined with the use of an intermediate layer, the backwash resistance and selectivity of the membrane are improved. And the structure of the membrane is optimized during the high-temperature sintering process.
Significantly improves the filter's backwash resistance and wear resistance, while maintaining high filtrate flow and filtration selectivity, extending the filter's service life.
Smart Images

Figure 67700 
Figure 634697 
Figure 692146DEST_PATH_IMAGE002
Abstract
Description
[0001] The present invention relates to the field of filtering structures made of inorganic materials for filtering liquids, in particular structures coated with membranes for separating particles or molecules from liquids, more particularly from water.
[0002] Filters using ceramic or non-ceramic membranes for filtering various fluids, in particular contaminated water, have long been known. These filters can operate according to the dead-end filtration principle, a technique that involves passing the fluid to be treated through the filter medium (perpendicular to its surface). This technique is limited by the accumulation of particles and the formation of filter cakes on the surface of the filter medium. Therefore, this technique is more particularly suitable for filtering liquids with a low content of pollutants (i.e. suspended liquids or solid particles).
[0003] According to another technology also related to the invention, the use of tangential flow filtration, on the contrary, allows to limit the accumulation of particles due to the longitudinal circulation of the fluid on the membrane surface. The particles are retained in the circulating flow, while the liquid can pass through the membrane under pressure. This technology provides stability in performance and filtration levels.
[0004] The advantages of tangential flow filtration are therefore its ease of use, its reliability (due to the use of organic and / or inorganic membranes), its porosity being adjusted to carry out said filtration, and its continuous operation. Tangential flow filtration uses little or no auxiliary agents and provides two independent fluids, both of which can be added value: a concentrate (also called retentate) and a filtrate (also called permeate); it is considered an environmentally friendly cleaning method. The tangential flow filtration technique is used in particular for microfiltration or ultrafiltration. The tangential flow configuration generally requires the use of at least two pumps, one for pressurization (or boosting), and another for recirculation. The recirculation pump generally has the disadvantage of high energy consumption. The use of a filtration device that guarantees a high flow rate of the filtrate allows limiting energy consumption.
[0005] Therefore, the present invention is applicable to both tangential flow filters and filters with dead-end filtration.
[0006] Thus, various filter structures operating according to the tangential flow filtration or dead-end filtration principle are known from the prior art. They comprise or consist of, for example, a tubular or parallelepiped support made of porous inorganic material, formed by walls defining longitudinal channels parallel to the axis of the support.
[0007] In the case of tangential flow filters, the filtrate passes through the wall and then exits at the surrounding outer surface of the porous support.These filters are more particularly suitable for filtering liquids containing a large number of particles.
[0008] In the case of a dead-end filter, the longitudinal channels are usually plugged at one end, for example alternately plugged, to form inlet and outlet channels separated by channel walls, the inlet and / or outlet channels being coated with a filter membrane through which all liquid passes and particles are retained by the membrane.
[0009] The surface of the channel is most often covered with a membrane, preferably a membrane made of a porous inorganic material, referred to in this specification as a membrane, a membrane layer or a membrane separation layer, whose properties and morphology are suitable for blocking molecules or particles whose size is close to or greater than the median pore size of the membrane when the filtrate diffuses into the pores of the porous support under fluid pressure across the filter. The membrane is usually deposited on the inner surface of the channel by coating with a slurry of porous inorganic material followed by a consolidation heat treatment, in particular drying, most often by sintering of ceramic membranes.
[0010] According to another technology, non-integrated filtering devices are known consisting of a series of perforated plates in a chamber, wherein the liquid to be filtered is most often stirred to promote turbulent conditions. These devices promote shear forces within the liquid in contact with the perforated plates and are more effective for the purification of extremely loaded or very viscous liquids.
[0011] Different forms of plates have been proposed, such as porous, solid or ceramic plates comprising cavities or internal channels (making it possible to drain the filtrate), for example according to FIG. 7 of WO 2009 / 039861 A1 or even as proposed in publication EP 2 543 420 A1. Such plates can have a membrane deposited on the largest face of the filter plate, as described, for example, in DE 20 2010 01 5 318 U1. Some plates have been described as having an inner cavity comprising drainage material, as it is described, for example, by EP 2 910 299 A1.
[0012] Many publications indicate different membrane filter configurations aimed at obtaining a filter with optimal performance for the application, in particular:
[0013] - Low pressure loss,
[0014] - the highest possible outlet permeate flow,
[0015] - high mechanical strength, especially high resistance to abrasion, due to the passage of the liquid to be filtered laden with particles over the membrane surface,
[0016] - high selectivity towards the pollutants to be filtered,
[0017] -Ideally have high chemical resistance, especially acid resistance.
[0018] Previous studies conducted by the applicant company have shown that, according to another complementary approach, in such a filtration structure, it is useful to act on the chemical composition of the separation membrane in order to further improve the filtration performance of the structure and even the service life of the filter. These studies are described in the patent application published under WO2016097661A1.
[0019] Despite the significant improvement in abrasion resistance, there is still much room for improvement in the resistance to backwashing, a step necessary for membrane regeneration. During this step, pressurized water is injected in countercurrent to unclog the contaminants that have accumulated in the pores of the filter. The applicant company found that each backwash exerts strong mechanical stress on the membrane. Finally, the applicant company found that as the backwash operation progressed, the permeability of the membrane separation layer increased, an indicator of its gradual delamination, and therefore its effectiveness decreased.
[0020] Other studies conducted by the applicant company have shown that it is also possible to improve the performance of membranes essentially consisting of silicon carbide, this time by modifying the intrinsic structural properties of the membrane. Many documents in the art describe different possible compositions for ceramic membranes made of porous inorganic materials, but no causal relationship is established between the composition of the material constituting the membrane and the performance qualities of the filter.
[0021] According to one embodiment, the application published as WO2005005016A1 or the corresponding patent US7699903B2 describes a membrane separation layer made of silicon carbide obtained from a mixture of two SiCk particle powders in the alpha crystalline form sintered together at a temperature of 1750-1950°C.
[0022] Application FR 2 549 736 proposes increasing the flow of filtered liquid by regulating the size of the particles forming the filter layer relative to the particles forming the support. However, the layer disclosed has a flow that is considered low from the point of view of the present invention.
[0023] Other publications, such as patent application EP3009182A1, propose silicon and silicon carbide membranes obtained from a slurry containing three powders having different median sizes (ranging from 2 to 4 microns, 0.5 to 0.9 microns and 0.2 to 0.4 microns respectively before firing at a temperature of 1500 to 1900° C.), preferably one of the powders being silicon powder. The wear resistance of such membranes appears too low to allow obtaining filters with a prolonged lifetime.
[0024] The object of the present invention is to provide a filter comprising a membrane in the form of a separator which is mechanically resistant, whatever the conditions of its use, in particular during the continuous backwashing necessary for its good operation, thereby increasing its service life while maintaining the same or significantly improved filtration performance quality compared to previous embodiments.
[0025] In particular, studies by the applicant company have demonstrated that it is possible to obtain optimum conditions in terms of resistance to backwashing, while maintaining very good selectivity, by suitable choice of the constituent materials of the membrane, obtainable by the process according to the invention, as described below.
[0026] Very particularly, studies by the applicant company as described below have demonstrated that membrane filters made of recrystallized silicon carbide (SiC), in particular silicon carbide in the alpha form, for filtering liquids have advantages which have not yet been described in the prior art.
[0027] According to the invention, it is possible to obtain membranes that are very resistant to wear and in particular very resistant to backwashing, without increasing the size of the pores and therefore without reducing the selectivity of the filter, as is usually observed with non-oxide membranes, in particular membranes made of silicon carbide (SiC) obtained by high-temperature sintering.
[0028] In this specification, the terms separation membrane, separation layer or membrane separation layer are used indifferently to denote such a layer which allows filtration.
[0029] Therefore, according to a first aspect, the present invention relates to a filter structure or filter, which is constructed for filtering a fluid, such as a liquid, comprising or consisting of a support element, which is made of a porous ceramic material and is provided with a membrane separation layer allowing said filtration.
[0030] More specifically, the present invention relates to a filter for filtering fluids such as liquids, which includes a support element made of a porous ceramic material or is composed of it, at least a portion of the surface of the support element is covered with a porous membrane separation layer, the membrane separation layer is basically composed of silicon carbide (SiC), its porosity is 10% to 70% by volume, its median pore size is 50 nanometers to 500 nanometers, its average thickness is 1 micron-30 microns, and its tortuosity is less than 1.7.
[0031] A filter whose membrane has the above-mentioned properties very particularly has a remarkable resistance to backwashing while maintaining a high filtrate flow rate without increasing the size of the pores and thus without reducing the selectivity of the filter.
[0032] The support element may be provided in any known form, in particular in the form of a plate, a disc, a tube or a parallelepiped. At least a portion of the support surface is covered with a layer of material whose structural characteristics make it possible to filter impurities present in a fluid, in particular a liquid, passing through the layer and then through the support.
[0033] For example, the support may be defined by an outer surface and comprise, in its inner part, a set of adjacent channels defining an inner surface, the channels preferably having axes parallel to one another and separated from one another by walls of a porous ceramic material, at least a portion of the outer surface and / or the inner surface of the channels being covered with a porous membrane separation layer. During operation of the filter, as described above, this layer is in contact with the fluid to be filtered, the permeate passing through the porous ceramic material and then discharged by the discharge device. In the particular case of a tubular or parallelepiped filter, the permeate may be discharged from the outer surface according to a tangential flow filtration mode, or from a portion of the channels not covered by the membrane separation layer according to a dead-end filtration mode.
[0034] The support body according to the invention can also be in other forms, for example a plate as described above, optionally with channels in its thickness for draining off the filtrate.
[0035] According to the optional and advantageous additional properties of the membrane separation layer:
[0036] - SiC accounts for more than 95%, preferably more than 97%, or even more than 99% by weight of the material constituting the membrane separation layer.
[0037] - The SiC constituting the particles is essentially in alpha crystalline form, as can be determined by X-ray diffraction analysis.
[0038] The porosity of the membrane separation layer is preferably 30% to 60% by volume, more preferably 35% to 50%, even 35% to 45%.
[0039] The median pore diameter is 60 nm to 450 nm, preferably 75 to 400 nm, in particular 100 to 300 nm.
[0040] The average thickness of the separation layer is 3 to 20 microns, more preferably 4 to 15 microns, even 5 to 10 microns.
[0041] The tortuosity of the layers constituting the porous membrane separation layer is less than 1.6, preferably less than 1.5, even less than or equal to 1.4, even less than 1.3.
[0042] The tortuosity of the layers constituting the porous membrane separation layer is greater than 1, preferably greater than or equal to 1.1.
[0043] The median size of the SiC particles in the membrane separation layer is preferably greater than 60 nm, preferably greater than 80 nm, more preferably greater than 100 nm, even greater than 150 nm.
[0044] The median size of the SiC particles in the membrane separation layer is less than 400 nm, preferably less than 300 nm, more preferably less than 250 nm, even less than 200 nm. This size can be measured by analyzing photographs obtained by scanning electron microscopy (SEM).
[0045] In the material constituting the membrane separation layer according to the invention, oxygen and in particular also nitrogen can be present in the particles and / or partially at the surface of the particles and at the particle joints by insertion into the crystal lattice of SiC. According to a possible and even preferred mode, nitrogen and / or oxygen are present in the separation layer only in the form of unavoidable impurities.
[0046] With regard to the porous support, the following information is given in relation to a preferred but non-limiting embodiment of the present invention:
[0047] The support element is in the form of a plate, a disk, a tube or a parallelepiped.
[0048] The porosity of the material constituting the porous support element is between 20% and 70%, preferably between 30% and 60%.
[0049] The porous support element is comprised of a material having a median pore size of 5 to 50 micrometers, more preferably 10 to 40 micrometers.
[0050] The tortuosity of the support element is greater than 1, even greater than 1.1, even greater than 1.2, even greater than 1.3, even greater than 1.4 and / or less than 2, even less than 1.9, even less than 1.8, even less than 1.7.
[0051] The porous support element comprises and preferably consists of a ceramic material, preferably a non-oxide ceramic material, preferably selected from silicon carbide SiC, in particular solid-phase or liquid-phase sintered SiC, recrystallized SiC, silicon nitride, in particular Si3N4, silicon oxynitride, in particular Si2ON2, silicon aluminum oxynitride or a combination thereof. Preferably, the support consists essentially of silicon carbide, more preferably still essentially of recrystallized SiC.
[0052] - The base of the tubular or parallelepiped shape is polygonal, preferably square or hexagonal, or circular. The tubular or parallelepiped shape has a longitudinal central axis of symmetry (A).
[0053] - Particularly in the case of filters with dead-end filtration, the channels are blocked at one end, preferably alternately, to define inlet and outlet channels, thereby forcing the liquid to enter through the inlet channel (on the surface of which the membrane is deposited), pass through the membrane, and then be discharged through the outlet channel.
[0054] - If the filter is tangential flow, the ends of the tubular support can be in contact with a plate sealed against the liquid to be filtered and perforated at the location of the channels facing it, thus forming a filter support or a filter system placed in a pipeline. Another possibility consists in introducing the tangential flow filter into the pipeline, providing sealed peripheral joints at each end and around the filter in order to provide a permeate flow independent of the concentrate flow.
[0055] - The element has a hexagonal cross section, and the distance between two opposite sides of the hexagonal cross section is 20-80 mm.
[0056] - The pipe of the filter element is open at both ends.
[0057] The ducts of the filter element are blocked alternately on the surface for introducing the liquid to be filtered and on the opposite surface.
[0058] The ducts of the filter element are open on the side for introducing the liquid and closed on the withdrawal side.
[0059] - Most of the channels, in particular more than 50%, even more than 80%, have a square, circular or oval cross section, preferably a circular cross section, and more preferably have a hydraulic diameter of 0.5 mm to 10 mm, preferably 1 mm to 5 mm. The hydraulic diameter D of the channel h , in any cross section P of the tubular structure, is calculated from the channel cross-sectional surface area S of the channel and its perimeter P, according to the cross section and by applying the following general expression:
[0060] D h =4×S / P.
[0061] As indicated above, in addition to the membrane separation layer, the filter according to the invention preferably also comprises one or more intermediate layers arranged between the material constituting the support element and the material constituting the membrane separation layer. The role of this (these) "intermediate" layer is to promote the adhesion of the separation layer and / or to prevent particles of the separation membrane from passing through the support, in particular during deposition by coating.
[0062] The filter may further include one or more intermediate layers disposed between the material constituting the support element and the material constituting the membrane separation layer.
[0063] Preferably, the intermediate layer or layers consist essentially of SiC.
[0064] Preferably, at least one intermediate layer has a median pore size at least twice, even at least three times, that of the membrane separation layer and preferably has a thickness between 40 and 100 microns.
[0065] Advantageously, each intermediate layer has an average thickness of 5-100 microns, preferably 15-70 microns, preferably 20-80 microns, or even 30-60 microns.
[0066] In particular, according to one possible mode, the filter comprises a first intermediate layer having a median pore size of 0.5-3 microns and / or having a porosity of 30%-50% by volume and / or having a median particle size of 5-15 microns, according to an average thickness of 5-90 microns.
[0067] According to another possible mode, the filter comprises a first intermediate layer deposited on a support, with a median pore size of 0.5 to 3 microns, and / or a porosity of 30% to 60% by volume, and / or a median particle size of 5 to 15 microns, according to an average thickness of 5 to 50 microns. A second intermediate layer is deposited on said first intermediate layer, this layer having a median pore size of 0.4 to 0.8 microns, and / or a porosity of 30% to 60% by volume, and / or a median particle size of 0.5 to 0.9 microns, according to an average thickness of 5 to 90 microns.
[0068] In this specification, unless otherwise specified, all percentages are by weight.
[0069] Without reporting them again here, it is obvious that the present invention also relates to a membrane separation layer satisfying all the preferred features mentioned above and to a filtration structure comprising said layer.
[0070] The filter according to the invention and as described above is used in particular for filtering liquids, in particular aqueous liquids, such as fruit juices, or alcoholic liquids, in particular wine, beer or spirits.
[0071] Finally, the invention relates to a method for preparing a filter as described above, in particular a tangential flow or dead end filter, comprising the following steps:
[0072] - preparing the mortar from a powder of silicon carbide particles having an average size of 0.05-0.4 μm, preferably 0.1-0.3 μm,
[0073] - applying said mortar to at least a part of the surface of the support element under conditions allowing the formation of a thin layer of mortar (preferably 1-50 micrometers),
[0074] - drying and then firing in a non-oxidizing, preferably neutral atmosphere, in particular under argon, at a temperature between 1400° C. and 1600° C. and within this temperature range for a sufficient time, for example 10 to 120 minutes, preferably 15 to 45 minutes, to obtain a membrane separation layer, said layer consisting essentially of silicon carbide.
[0075] This preparation method may further comprise, before the step of depositing said slurry, a step of depositing at least one intermediate layer starting from a slurry containing a powder of silicon carbide particles, at least part of which has a median diameter less than 1 micron and greater than 0.1 micron.
[0076] Also provide the following information:
[0077] The open porosity and the median pore diameter of the porous supports described in this description are determined in a known manner by mercury porosimetry according to Standard ISO 15901-1.2005, Part 1 .
[0078] The porosity and median pore size of the membrane separation layer (and the one or more intermediate layers) are advantageously determined according to the invention using scanning electron microscopy. Figure 2 As shown, in cross section, a portion of the support wall is produced so as to show the entire thickness of the coating over a cumulative length of at least 1.5 cm. The image is acquired on a sample of at least 10 particles. The area and equivalent diameter of each pore are obtained from the photograph by conventional image analysis techniques, preferably after binarization or segmentation of the image with the goal of increasing its contrast. From this, the distribution of equivalent diameters is derived, from which the median pore size is extracted. Similarly, the median size of the particles constituting the film layer can be determined by this method.
[0079] As an illustration, an embodiment of determining the median pore diameter or median size of particles constituting the membrane separation layer comprises the following sequence of steps conventional in the art:
[0080] A series of SEM photographs (observed along a cross section, ie in the entire thickness of the wall) are taken of the support with its membrane separation layer. For greater clarity, the photographs are taken on a polished section of the material. The images are acquired over a cumulative length of the membrane layer at least equal to 1.5 cm, in order to obtain values representative of the entire sample.
[0081] The photographs are preferably subjected to binarization techniques well known in the art of image processing, in order to increase the contrast of the outlines of the particles or pores.
[0082] - For each particle or each pore constituting the membrane separation layer, a measurement of its area is performed. An equivalent pore size or equivalent particle size is determined, which corresponds to the diameter of a perfect disk of the same area as measured for said particle or said pore (this operation can optionally be carried out using dedicated software, in particular Visilog® sold by Noesis).
[0083] -Thus, a distribution of particle or particle sizes or pore diameters is obtained according to a conventional distribution curve, and the median size of the particles and / or the median pore diameter constituting the membrane layer is determined therefrom, this median size or this median diameter corresponding to dividing the distribution into a first population comprising only particles or pores whose equivalent diameter is greater than or equal to the median size and a second population comprising only particles whose equivalent diameter is less than the median size or this median diameter, respectively.
[0084] Tortuosity is a well-known parameter in the field of porous structures, as described in the publication "Tortuosity in electrochemical devices: a review of calculation approaches", International Materials Reviews, 63, 2, pp. 47-67 (2018).
[0085] It can be measured by image analysis of a series of cross sections of the membrane, according to different planes parallel to each other and perpendicular to the filtration surface of the membrane separation layer, to illustrate the three-dimensional structure of the microstructure of the membrane throughout its thickness. A suitable technique is the use of a scanning electron microscope equipped with a focused ion probe or a FIB (focused ion beam). Another possible technique is nanotomography. The image preferably has a minimum resolution of one million pixels to obtain an image quality suitable for sufficient binarization or segmentation to clearly distinguish the ceramic wall from the porosity of the membrane (throughout its thickness). The use of software such as iMorph© allows the three-dimensional geometric characteristics of the membrane layer to be obtained and the tortuosity to be calculated. The tortuosity is defined as the ratio of the shortest path allowed to pass through the membrane separation layer in the thickness direction of the membrane separation layer and the distance or line segment connecting the departure point and the arrival point (corresponding to the path). The tortuosity of the support can be measured according to the same procedure.
[0086] Within the meaning of the present description and unless otherwise indicated, the median size of the particles or the median pore diameter measured by microscopy denotes the diameter of the particles or pores, respectively, below which 50% by number of the population are present. On the other hand, with regard to the pore diameter measured by mercury porosimetry on a substrate or support, the median diameter corresponds to the threshold value of 50% by volume of the population.
[0087] The term "sintering" generally refers in the ceramics field (that is to say within the meaning indicated in the international standard ISO 836:2001, point 120) to the consolidation of granular agglomerates by heat treatment. Thus, the heat treatment of the particles used as the starting charge for obtaining the film layer according to the invention allows their contact interfaces to connect and grow by atomic movement inside and between said particles.
[0088] The sintering between the SiC particles according to the invention usually takes place substantially in the solid / gas phase, the sintering temperature being close to or even above the vaporization temperature of the finest particles constituting the membrane separation layer deposit.
[0089] The median diameter D of the particle powder used to produce the support or membrane separation layer 50 It is usually given by characterization of the particle size distribution (eg by means of a laser particle size analyzer).
[0090] The SiC content can also be measured according to the protocol defined in standard ANSI B74.15-1992-(R2007) by the difference between total carbon and free carbon, this difference corresponds to the carbon fixed in the form of silicon carbide.
[0091] Below are given non-limiting examples allowing the preparation of a filter according to the invention, it being quite obvious that the method making it possible to obtain such a filter and the method according to the invention are also non-limiting.
[0092] According to a first step, the filter support is obtained by extruding a paste through a die configured according to the geometry of the structure to be produced according to the invention. Extrusion is followed by drying and firing to sinter the inorganic material constituting the support and obtain the porosity and mechanical strength characteristics required for the application.
[0093] For example, when it concerns a SiC support, it can be obtained in particular according to the following preparation steps:
[0094] - kneading a mixture containing silicon carbide particles with a purity greater than 98%, the particle size distribution of the silicon carbide particles is such that 75% by weight of the particles have a diameter greater than 30 microns, the median diameter by weight of this particle size fraction (measured by a laser particle size analyzer) being less than 300 microns. The mixture also contains an organic binder derived from the cellulose type. Water is added and kneading is performed until a homogeneous paste is obtained, the plasticity of which allows extrusion, and the mold is constructed to obtain the monolith according to the invention.
[0095] - The green monolith is dried using microwaves for a sufficient period of time to reduce the content of non-chemically bound water to less than 1% by weight.
[0096] - In the case of a filter support based on liquid phase sintered silicon carbide, silicon nitride, silicon oxynitride, silicon aluminum oxynitride or even BN, firing is carried out until a temperature of at least 1300 ° C and in the case of a filter support based on recrystallized or solid phase sintered SiC, firing is carried out until at least 1900 ° C and less than 2400 ° C. In the case of a filter support made of nitride or oxynitride, the firing atmosphere is preferably based on nitrogen. In the case of a filter support made of recrystallized SiC, the firing atmosphere is preferably neutral, more particularly argon. The temperature is generally maintained in a battery furnace at ambient pressure for at least 1 hour, preferably at least 3 hours. The material obtained has an open porosity of 20% to 60% by volume and a median pore size of the order of 5 to 50 microns.
[0097] The filter support is then coated with a membrane (or membrane separation layer) according to the invention. One or more layers can be deposited to form a membrane according to various techniques known to those skilled in the art: techniques using suspension or slurry deposition, chemical vapor deposition (CVD) techniques or thermal spraying techniques, such as plasma spraying.
[0098] Preferably, the membrane layers are deposited by coating with a slurry or suspension.The first layer, called the intermediate layer, is preferentially deposited in contact with the porous material constituting the substrate, acting as a tie layer.
[0099] A non-limiting example of an inorganic formulation of an intermediate layer comprises 30% to 60%, preferably 35% to 50%, by weight of SiC powder with a median diameter of 2 to 20 microns, the remainder being demineralized or deionized water (except for optional organic additives). According to one possible mode, a second intermediate layer is deposited on the first intermediate layer. The formulation of this second layer comprises 20% to 65%, preferably 35% to 60%, by weight of SiC powder with a median diameter of 0.5 to 0.9 microns, the supplement to 100% being provided by demineralized water (except for organic additives or additives).
[0100] According to another non-limiting example, the intermediate layer is unique and its formulation comprises by weight 15% to 25% of SiC powder with a median diameter of 7 to 15 microns, 5% to 15% of SiC powder with a median diameter of 1.5 to 5 microns and 0.5% to 5% of SiC powder with a median diameter of 0.1 to 1.0 microns, preferably 0.13 to 0.3 microns, the balance to 100%, preferably 60% to 80% is provided by demineralized water or deionized water (excluding organic additives or additions).
[0101] Although preferably present, in certain filter constructions this second intermediate layer may not be present without departing from the scope of the present invention.
[0102] Another layer with a smaller median pore size is then deposited on the last intermediate layer (or directly on the support), which constitutes the membrane or, more precisely, the membrane separation layer. The porosity of this last layer is suitable for giving the filter element its final filtration characteristics, in particular its selectivity, by adjusting the value of its median pore size. A non-limiting example of a separation layer inorganic formulation comprises 2% to 20%, preferably 3% to 10% by weight of SiC powder having a median diameter of 0.05 to 0.5 microns, preferably 0.1 to 0.3 microns, the rest being demineralized water (except for optional organic additives).
[0103] In order to control the rheology of the mortar and maintain a suitable viscosity (usually 0.01 to 1.5 Pa.s, preferably 0.1 to 0.8 Pa.s, which is 1s at 22°C -1 The present invention relates to a kind of SiC powder, which is preferably a cellulose derivative, a binder, preferably a PVA or acrylic acid derivative, and a dispersant, preferably a polymethacrylate ammonium type.
[0104] Organic additives to the mortar, expressed by weight, in particular Dolapix A88 as a deflocculant, for example in a proportion of 0.01% to 0.5%; Tylose, for example type MH4000P, as a thickener, in a proportion of 0.01% to 1%; PVA or acrylic-based resins as tackifiers, in a proportion of 0.1% to 2%, calculated on a dry weight basis; monoethylene glycol as a plasticizer; and 95% by volume of ethanol as a surface tension reducer are more particularly suitable.
[0105] These coating operations generally allow to obtain an intermediate layer having a thickness of about 30 to 80 microns after drying. In a second coating step, a membrane separation layer having a thickness of, for example, about 3 to 20 microns, preferably 5 to 15 microns, even more preferably 5 to 10 microns is obtained after drying, this thickness range being of course in no way limiting.
[0106] The specific steps of the method according to the invention for depositing the membrane separation layer according to the invention on a support, optionally on top of the above-mentioned intermediate layer, are described below:
[0107] According to a first preferred embodiment, as described above, the mortar is prepared from a powder or preferably a plurality of powders having silicon carbide particles of different particle sizes and in the presence of an amount of water which preferably allows the above-mentioned rheological and viscosity conditions to be met, and in the presence of the necessary organic agents, preferably to obtain a mortar having a pH value less than or equal to 10.
[0108] The mortar is then applied to the support element under conditions and in a manner suitable to allow the formation of a thin layer on the internal parts of the channels of the filter, in particular those described above.
[0109] After applying the layer, the support is first dried at ambient temperature, usually for at least 10 minutes, and then heated at 60°C for at least 12 hours. Finally, the porous membrane separation layer on the surface of the support channel is obtained by sintering in a furnace in a non-oxidizing atmosphere, preferably in an atmosphere that is very mainly or only contains argon (Ar), at atmospheric pressure (1 bar). The firing temperature is usually at least 1400°C, preferably at least 1500°C, and preferably below 1600°C for a sufficiently long time, especially at least 1 hour, to obtain the membrane according to the present invention as described above.
[0110] The thickness of the membrane separation layer obtained is preferably 5-15 micrometers. Diffraction analyses performed by electron microscopy and X-ray fluorescence show that the material thus obtained consists essentially of α-SiC particles.
[0111] In order to obtain the desired properties according to the invention in an essential manner, the silicon carbide powder initially selected in the method for preparing the membrane separation layer is selected according to the following criteria:
[0112] the initial SiC powder has a metallic Si content of less than 1.0% by weight, preferably less than 0.5% by weight, or even less than 0.2% by weight,
[0113] the initial SiC powder has an elemental oxygen content of less than 2.0% by weight, preferably less than 1.5%, even less than 1.0%,
[0114] - the initial SiC powder has a SiC content of more than 97% by weight,
[0115] The median diameter of the initial SiC powder is less than 400 nm, preferably less than 300 nm, more preferably less than 250 nm, even less than 200 nm.
[0116] If the filter is constructed for tangential flow filtration applications, it can be fixed in a sealed manner to a perforated plate at the channel opening for installation in a pipeline or filter system. The heat treatment for fixing the perforated plate to the filter support must be carried out at a temperature below the decomposition temperature of the composite membrane.
[0117] If the filter has alternately plugged channels to obtain a membrane filter operating according to the dead-end filtration principle, and if the plugging is performed on at least one side of the filter after membrane deposition, either on the inlet channel side or on the outlet side, the plugging can be performed with a SiC slurry and the plugs are sintered at a temperature below the decomposition temperature of the composite membrane, preferably simultaneously with the membrane.
[0118] The drawings related to the following examples are provided to illustrate the invention and its advantages, although, of course, the embodiments thus described are not to be considered limiting of the invention.
[0119] In the attached picture:
[0120] - Figure 1 A conventional construction of a tubular filter along a cross section P according to the prior art is shown.
[0121] - Figure 2 is a micrograph of a filter within the meaning of the present invention showing a membrane separation layer.
[0122] Figure 1 A tangential flow filter 1 according to the prior art and according to the invention is shown for filtering a fluid, such as a liquid. Figure 1 Schematic diagram showing a cross section P. The filter comprises or most often consists of a support element 1 made of a porous, preferably non-oxide, inorganic material. This element is generally in the shape of a tube with a longitudinal central axis A, delimited by an outer surface 2. It comprises in its inner part 3 a set of adjacent channels 4 with mutually parallel axes and separated from each other by walls 8. Said walls are formed of a porous inorganic material, allowing the filtrate to flow from the inner part 3 to the outer surface 2. As Figure 2 As shown in the electron micrograph, the channel 4 is covered on its inner surface with a membrane separation layer 5 deposited on a connection intermediate. This membrane separation layer 5 (or membrane) is in contact with the fluid circulating in the channel and allows its filtration.
[0123] exist Figure 2 In Figure 1 Electron microscope photograph taken on channel 4 of FIG. In this figure, a porous support 100 with high porosity, a first intermediate layer 101, and a second intermediate layer 102 are observed, which allow the membrane separation layer 103 with finer porosity to be adhered.
[0124] According to another configuration of another filter of the present invention (not shown), the latter is configured so that the fluid to be treated initially passes through the outer wall and the permeate is collected by the receiving device. According to this configuration, the membrane filtration layer is advantageously deposited on the outer surface of the filter and covers at least a portion thereof.
[0125] This construction is often referred to as FSM (Flat Membrane). See the publications on the website:
[0126] http: / / www.liqtech.com / img / user / file / FSM_Sheet_F_4_260214V2.pdf.
[0127] The following examples are provided by way of illustration only. They are not limiting and allow for a better understanding of the technical advantages associated with the implementation of the present invention.
[0128] The supports according to all examples were identical and were obtained following the same experimental protocol.
[0129] Mix the following in a kneader:
[0130] - 3000 g of a mixture of two powders of silicon carbide particles with a purity greater than 98% in the following proportions: 75% by weight of a first powder of particles having a median diameter of about 60 microns and 25% by weight of a second powder of particles having a median diameter of about 2 microns (within the meaning of this specification, the median diameter d 50 represents a particle size below which 50% by weight of the particle population is below).
[0131] - 300 g of organic binder of cellulose derivative type.
[0132] Water, about 20% by weight of the total weight of SiC and organic additives, is added and kneaded until a homogeneous paste is obtained, the plasticity of which allows the extrusion of tubular structures, and the die is constructed to obtain a monolith, the channels and the outer wall of which have a structure according to the desired configuration, as in the attached Figure 1 As shown above.
[0133] More specifically, the fired monolith has circular channels with a hydraulic diameter of 2 mm, and the peripheral half-moon channels shown in the figure have a hydraulic diameter of 1.25 mm. The average thickness of the outer wall is 1.1 mm, and the OFA (open frontal area) of the filter inlet face is 37%. OFA or open frontal area is obtained by calculating the percentage of open area (the sum of the channel cross-sections relative to the total area of the corresponding cross-section of the porous support).
[0134] Therefore, 5-10 pristine supports with a diameter of 25 mm and a length of 30 cm were synthesized for each configuration.
[0135] The green monolith thus obtained is dried by microwaves for a sufficient time to bring the content of non-chemically bound water to less than 1% by weight.
[0136] The monolith was subsequently fired to a temperature of at least 2100° C. and maintained for 5 hours. The material obtained had an open porosity of 43% and an average pore distribution diameter of about 25 micrometers, measured by mercury porosimetry.
[0137] The particles had a median size of approximately 20 microns.
[0138] Example 1 (comparative example according to WO2016097661A1):
[0139] According to this embodiment, a membrane separation layer made of silicon carbide is then deposited on the inner walls of the channels of the support structure obtained above according to the procedure described below:
[0140] As a first step, the adhesive intermediate layer of the separating layer is formed from a mortar whose inorganic formulation contains 30% by weight of SiC particle powder (SIKA DPF-C) with a mean diameter D 50 The average diameter D 50 is approximately 2.5 microns, and 50% deionized water.
[0141] A material slurry constituting the membrane filtration layer was also prepared, the formulation of which contained 40 wt % of SiC particles (d 50 about 0.6 microns) and 60% deionized water.
[0142] The rheological properties of the mortar were determined by -1 The organic additive is added to adjust the shear gradient to 0.5-0.7 Pa.s, which is measured at 22°C according to standard DINC33-53019.
[0143] The two layers are deposited successively according to the same method described below: The slurry is introduced into the container under stirring (20 rpm). After a degassing step under a gentle vacuum (typically 25 mbar) while maintaining stirring, the container is placed under an overpressure of about 0.7 bar in order to be able to coat the interior of the support from the bottom to its upper end. For a support with a length of 30 cm, this operation takes only a few seconds. After the slurry has been applied to the inner walls of the channels of the support, the excess is immediately drained by gravity.
[0144] The support was subsequently dried at ambient temperature for 10 minutes and then for 12 hours at 60° C. The support thus dried was subsequently fired under nitrogen at a temperature of 1600° C. at ambient pressure for 2 hours.
[0145] A cross section was produced on the filter thus obtained. The structure of the membrane was observed and studied using a scanning electron microscope according to the following method.
[0146] Embodiment 2 (comparison):
[0147] According to this example, the process is carried out in the same manner as in Example 1, but the firing of the coated support is carried out at 1600° C. under argon, with a time length of 30 minutes between 1400 and 1600° C.
[0148] Embodiment 3 (comparison):
[0149] According to this example, the same process as in Example 1 was carried out, but the firing of the coated support was carried out at 1550° C. under argon and the length of time between 1400-1550° C. was 30 minutes.
[0150] Example 4 (according to the present invention):
[0151] According to this example, the process is carried out in the same way as in Example 3, but the coated support is fired under argon at 1650° C. instead of 1550° C., with a time length of 30 minutes between 1400 and 1650° C. A third layer, which becomes the separation layer, is then deposited. This layer is obtained by depositing a slurry whose recipe corresponds to 7% by weight of a powder of green SiC particles, the median diameter D 50 It is about 0.18 microns, corresponding to a specific surface area of 50 square meters / gram, and the rest is deionized. In particular, for the mortar of the separation layer, the pH value is adjusted to 9-10 by adding sodium hydroxide solution. In order to thicken the mortar, control the sedimentation, and obtain a film-forming effect (for a good surface appearance after drying), 0.01-0.03 TyloseMH4000P2 is added relative to the amount of water. By monitoring the weight of the mortar fixed on the substrate, the average thickness of the deposition is 7 microns.
[0152] The support body coated in this way was fired again to 1550° C. under argon and ambient pressure, the length of time between 1400 and 1550° C. being 30 minutes.
[0153] Example 5 (according to the present invention):
[0154] According to this embodiment, the implementation is carried out in the same manner as in Embodiment 3, but:
[0155] -Median particle diameter D 50 A separate layer of particles of about 0.18 micrometers was deposited directly on a single intermediate bonding layer formed by a mortar whose inorganic formulation contained 18% by weight of particles with a median diameter D 50 SiC particle powder (SIKA DPF-C) of about 11 microns, with a median diameter D of 9% by weight 50 SiC particle powder (SIKA 1500F) of about 2 microns, 3 wt% median diameter D 50 Silicon carbide powder of approximately 0.18 micron particles, the remainder being 70% deionized water, and
[0156] - The separation layer is obtained by depositing a mortar whose formulation has a median diameter D of 7% by weight 50 A green SiC particle powder of approximately 0.18 microns was prepared as in Example 4. The average thickness of the deposit was 7 microns as monitored by the weight of the slurry fixed on the substrate.
[0157] The support body thus coated was fired again under argon at ambient pressure at 1550° C. for a period of 30 minutes between 1400 and 1550° C.
[0158] Embodiment 6 (comparison):
[0159] Unlike the previous examples, the intermediate layer is formed from a mortar whose inorganic formulation contains 30% by weight of particles with a median diameter D 50 SiC particle powder (SIKA DPF-C) of about 11 microns, 20% by weight with a median diameter D 50 It is SiC particle powder (SIKA FCP-07) of about 2.5 microns and 50% distilled water.
[0160] The same separation layer as in the previous example was deposited on the intermediate layer by monitoring the weight of the mortar fixed on the substrate.
[0161] Example 7 (comparison):
[0162] In contrast to Example 3, the final firing of the support body coated in this way was carried out at a temperature of 1100° C. for 2 hours under pure nitrogen.
[0163] This example therefore appears to be in compliance with the teaching of the application published under FR 2 587 026 A1 for the production of membrane filters made of silicon carbide.
[0164] Embodiment 8 (comparison):
[0165] In contrast to the previous examples, the final firing of the coated support was carried out this time according to the teaching of EP 2 559 470 A1 at a temperature of 1700° C. for 2 hours under argon for producing a membrane made of silicon carbide.
[0166] Embodiment 9 (comparison):
[0167] In contrast to Example 6, the separation layer was obtained from a mortar having the following inorganic composition: 20% by weight of median diameter d 50 The α-SiC powder particles are about 0.6 microns, with a median diameter d of 53% by weight. 50 Metallic silicon particle powder of about 4 microns, with a median diameter D of 27% 50 Amorphous carbon powder of approximately 1 micron.
[0168] The support dried as described above was finally fired under argon at ambient pressure at a temperature of 1470° C. for 4 hours.
[0169] The characteristics and properties of the filters thus obtained were measured as follows:
[0170] For each embodiment, the membrane sample on its support is placed in a scanning electron microscope equipped with a focused ion probe (FIB or focused ion beam). Slices are made in the thickness of the membrane layer along parallel planes (allowing observation of different cross sections to represent the cross section of the membrane layer). In order to obtain very good resolution between the porosity of the ceramic wall and the membrane (over the entire thickness), an electron microscope is used to take photos of at least one million pixels according to a mode (SE mode) using secondary electrons. The magnification used makes the width of the image between ten times and one hundred times the average size of the particles of the membrane separation layer, which is about 50 times according to the embodiment. On the basis of these photos, ImageJ software is used to segment to distinguish the porosity of the particles (by noting the depth of field). For each photo, the surface ratio of the porosity of the membrane layer is determined. The average ratio of the photos taken along different planes in the membrane is a value representing the pore volume of the membrane.
[0171] The tortuosity of Examples 3 to 6 was determined using iMorph© software.
[0172] The results are given in Table 1 and the following features of the experimental protocol followed are described below:
[0173] a) Measure the specific flow or flow rate (relative water flow) of the filter according to the following method:
[0174] At a temperature of 25°C, the -3 The filter to be evaluated is fed with a fluid consisting of demineralized water with 1 mol / l KCl at a transmembrane pressure of 0.5 bar and a circulation velocity in the channel of 2 m / s. The permeate (water) is recovered at the periphery of the filter. The measured values of the characteristic flow of the filter are expressed in l / min per m² of filtration surface area after 20 hours of filtration. The flow results in the table are expressed with reference to the data recorded for comparative example 3. More precisely, values greater than 100% indicate an increase in the flow velocity relative to the reference sample (Example 3), and thus an increase in the filtration capacity.
[0175] b) Abrasion resistance is measured by subjecting the filter produced according to the previous example to a slurry (containing 2 g / l of SiC powder with a median diameter of 250 μm) passing through the filter channels at a speed of 2 m / s. The permeability loss is measured after 20 hours of testing (provided standard). Example 3 is considered as reference (100). Values below 100, such as 80, mean a relative loss in permeability that is 20% lower than the reference value and therefore have a better abrasion resistance.
[0176] c) The test of resistance to strong backwashing consists in subjecting the filter to 1000 water pulses at a pressure of 3 bar / s / min, so that the liquid flows in reverse through the porous wall. The increase in permeability due to membrane degradation is measured. Example 3 is used as reference (100). Values below 100, for example 80, mean a relative loss in permeability, which is 20% lower than the reference value (thus better resistance to the mechanical stresses of backwashing).
[0177] d) Turbidity test:
[0178] The following method is used: synthetic dirty water containing clay, salt, oil and surfactant is used, according to the content of 100ppm, 4000ppm, 300ppm and 2ppm respectively. At a constant temperature of 25°C, the dirty water is supplied to the filter to be evaluated at a transmembrane pressure of 0.5 bar and a circulation speed in the channel of 3m / s. The filtrate (purified water) is recovered at the periphery of the filter. In order to evaluate the filtering performance of the filter, after 10 filtering cycles, the turbidity of the filtrate is continuously measured by the Beam-Turbidy Meter SeriesLAT N1 type turbidity meter provided by Kobold Instrumentation. Example 3 is regarded as a reference (100). Therefore, higher values after the turbidity test correspond to poorer liquid filtration quality.
[0179] Table 1 below gives the characteristics and properties of the filters and membrane separation layers (designated by membrane in the table below) obtained according to Examples 1 to 9:
[0180]
[0181]
[0182] The results collated in the previous Table 1 show that Examples 4 and 5 according to the invention have the best combined performance qualities in the different tests and measurements performed. The membrane filters of these examples have in particular a better resistance to backwashing, while having a very high wear resistance and a very high specific flow rate without reducing their selectivity.
[0183] Finally, the results collated in the table show that the material for producing the membrane separation layer according to the invention can only be obtained under certain process conditions which have not yet been described in the prior art.
Claims
1. A filter for filtering a fluid, comprising or consisting of a support element made of a porous ceramic material, at least a portion of the surface of the support element being covered with a membrane separation layer, the filter being characterized in that: - the membrane separation layer consists essentially of silicon carbide (SiC), - The porosity of the membrane separation layer is 10-70% by volume, - the median pore size in the membrane separation layer is 50 nm to 500 nm, - The average thickness of the membrane separation layer is 1 micron to 30 microns, -The tortuosity of the membrane separation layer is less than 1.
7.
2. The filter according to claim 1, wherein the median size of particles constituting the membrane separation layer is less than 400 nanometers and greater than 80 nanometers.
3. The filter according to claim 2, wherein the median size of the particles constituting the membrane separation layer is less than 300 nanometers.
4. The filter according to any one of claims 1-2, wherein the average thickness of the separation layer is 4-15 microns.
5. The filter according to any one of claims 1-2, wherein the median pore size in the separation layer is 100-300 nanometers.
6. The filter according to any one of claims 1-2, wherein SiC accounts for more than 95% by weight of the material constituting the membrane separation layer.
7. The filter according to any one of claims 1 to 2, further comprising one or more intermediate layers between the material constituting the support element and the material constituting the membrane separation layer.
8. The filter of claim 7, wherein one or more intermediate layers consist essentially of SiC.
9. The filter of claim 7, wherein the median pore size of at least one intermediate layer is at least twice the median pore size of the membrane separation layer.
10. The filter of claim 7, wherein the one or more intermediate layers have an average thickness of 5-100 microns.
11. The filter according to any one of claims 1 to 2, wherein the support element is in the form of a plate, a disk, a tube or a parallelepiped.
12. The filter according to any one of claims 1-2, wherein the porous support element comprises or consists of a material selected from silicon carbide, SiC, silicon nitride, silicon oxynitride, silicon aluminum oxynitride, or a combination thereof.
13. The filter according to any one of claims 1 to 2, wherein the material constituting the support element has an open porosity of 20% to 70% and the material constituting the porous support element has a median pore size of 5 to 50 microns.
14. The filter according to any one of claims 1-2, wherein the tortuosity of the support element is greater than 1 and / or less than 2.
15. The filter according to any one of claims 1-2, wherein the fluid is a liquid, and the tortuosity of the membrane separation layer is less than 1.
5.
16. The filter according to any one of claims 1-2, wherein the separation layer has an average thickness of 5-10 microns.
17. The filter according to claim 12, wherein the SiC is liquid phase or solid phase sintered SiC or recrystallized SiC, and the silicon nitride is Si 3 N 4 and the silicon oxynitride is Si 2 ON 2 .
18. A method for preparing a filter according to any one of claims 1 to 17, The following steps are involved: - preparing the mortar from a powder of silicon carbide particles having an average size of 0.05-0.4 micrometers, - applying the mortar to the support element under conditions allowing a mortar layer to form on at least a portion of the outer surface of the support element, - drying and then firing in a non-oxidizing atmosphere at a temperature between 1400° C. and 1600° C. for a sufficient time within this temperature range to obtain a membrane separation layer, said layer consisting essentially of silicon carbide.
19. The method according to claim 18, The following steps are involved: - preparing the mortar from a powder of silicon carbide particles having an average size of 0.1-0.3 micrometers, - applying the mortar to the support element under conditions allowing a mortar layer to form on at least a portion of the outer surface of the support element, - drying and then firing in a neutral atmosphere at a temperature of 1400° C. to 1600° C. for 10 to 120 minutes in this temperature range to obtain a membrane separation layer, said layer consisting essentially of silicon carbide.
20. The method for preparing a filter according to any one of claims 18-19, further comprising, before the step of depositing the slurry, a step of depositing at least one intermediate layer from a slurry comprising a powder of silicon carbide particles, at least a portion of the particles of the powder having a median diameter less than 1 micron and greater than 0.1 micron.
21. Use of a filter according to any one of claims 1 to 17 for filtering a liquid.
22. The use according to claim 21, wherein the liquid is an aqueous liquid or an alcoholic liquid.
Citation Information
Patent Citations
Porous ceramic filter
DE202010015318U1
Porous ceramic filter
EP2543420A1
Exhaust gas purification filter, and method for manufacturing exhaust gas purification filter
EP2559470A1
Plate-shaped or disk type filter device
EP2910299A1
Method for producing a porous ceramic body and a porous ceramic body obtained from said method
EP3009182A1