Lightweight warm-keeping functional flocculent sheet and preparation method thereof

By using a three-layer structure of lightweight thermal wadding in winter clothing, using a combination of modified polyester short fiber and nanofiber layers, the problem of heavy clothing is solved, an efficient lightweight thermal effect is achieved, and the problem of ceramic powder is overcome. The problem of narrow absorption spectrum of body functional fibers.

CN114103365BActive Publication Date: 2024-10-22XIAMEN ANTA SPORTS GOODS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111519074.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-13
Publication Date
2024-10-22
Estimated Expiration
2041-12-13

AI Technical Summary

Technical Problem

It is difficult to achieve lightweight warmth in winter clothing with existing technology. Conventional fiber flakes are thick and make clothing bloated. Ceramic powder far-infrared functional fibers have a narrow absorption spectrum and limited warmth retention effect.

Method used

A three-layer structure flake including a heat-storage modified polyester fiber layer, a polyimide nanofiber layer and a polyester fiber layer is used, and electrospinning is used through a combination of modified polyester short fibers and ZrC and TiO2 powders. The process prepares lightweight thermal functional flakes to achieve overall interaction to improve thermal performance.

Benefits of technology

It achieves lightweight and excellent thermal insulation function, with a weight of no more than 100g/m2, high compression rate, good recovery rate, maximum temperature rise value of 7.5℃~7.8℃, average temperature rise value of 4.6℃~4.9℃, and the process is simple and easy to control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114103365B_ABST
    Figure CN114103365B_ABST
Patent Text Reader

Abstract

The present invention provides a lightweight thermal insulation functional flocculent sheet, comprising: a heat storage modified polyester fiber layer; a polyimide nanofiber layer composited on the heat storage modified polyester fiber layer; a polyester fiber layer composited on the polyimide nanofiber layer; the heat storage modified polyester fiber layer is prepared from modified polyester staple fibers; the modified polyester staple fibers are prepared from raw materials including the following components: 100 parts by weight of PET slices; 1 to 5 parts by weight of ZrC powder; 0.1 to 0.9 parts by weight of TiO2 powder. Compared with the prior art, the lightweight thermal insulation functional flocculent sheet provided by the present invention adopts a specific layer structure and connection relationship to achieve better overall interaction. The product has excellent thermal insulation function and is lightweight, solving the problem of bloated and heavy appearance of winter cotton clothing products. Experimental results show that the gram weight of the lightweight thermal insulation functional flocculent sheet provided by the present invention does not exceed 100g / m 2 The compression rate is 83.1~85.3%, the recovery rate is 90.2~90.7%, the Krogh value is 3.13~3.39, the heat storage property is excellent, the maximum temperature rise value is 7.5~7.8℃, and the average temperature rise value is 4.6~4.9℃.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of clothing, and more specifically to a lightweight warm-keeping functional flocculent sheet and a preparation method thereof. Background Art

[0002] Filling cotton batting is a kind of flocculent material formed by stacking short fibers. It has a fluffy structure similar to down, which can lock in still air and keep warm. It is widely used in winter clothing. However, as the wearing time increases, the fiber batting structure is compressed, and the fluffy structure is gradually compressed and loses its warmth-keeping performance. Therefore, in addition to using conventional fibers to make batting, the industry has begun to use the method of adding functionally modified fibers or spraying additives in the batting.

[0003] Studies have shown that zirconium carbide ZrC can absorb the energy of near-infrared rays less than 2μm and convert it into heat energy. The energy in sunlight with a wavelength less than 2μm accounts for more than 95% of its total energy, while the wavelength of thermal radiation emitted by the human body is about 10μm, which is almost completely reflected, indicating that zirconium carbide has ideal heat absorption and heat storage characteristics. At the same time, electrospinning is a special fiber manufacturing process in which a polymer solution or melt is jet-spun in a strong electric field. The polyimide nanofiber layer is a nanofiber layer material formed by jet deposition through an electrospinning process and has an extremely light weight. At the same time, the thermal conductivity of polyimide material is 0.028, which is close to the thermal conductivity of air. It is a poor conductor of heat and is widely used in electronic products, battery compartments and outer protective layers of aerospace vehicles, mainly for heat insulation protection. Therefore, the use of heat storage functional materials and heat insulation functional materials to prepare a lightweight and moderately thick flake material can effectively block the loss of human heat without making the clothing appear bloated and heavy, which will have a wide range of applications in winter clothing products.

[0004] At present, the existing technology has a technical solution of mixing ceramic powder far-infrared functional fibers with conventional polyester fibers to prepare a multi-layer structure thermal insulation flakes; however, on the one hand, the ceramic powder far-infrared functional fibers mainly absorb far-infrared rays to increase temperature, and the absorbed spectral band is relatively narrow, so the warming effect is limited; on the other hand, the thermal insulation performance of conventional flake materials mainly depends on the thickness and unit area weight of the flake materials. Therefore, in order to achieve higher thermal insulation performance, the flakes need to be made thicker and heavier, and the clothing produced thereby appears bloated and heavy. Summary of the invention

[0005] In view of this, the object of the present invention is to provide a lightweight thermal insulation functional flake and a preparation method thereof. The lightweight thermal insulation functional flake provided by the present invention has excellent thermal insulation function and is lightweight, thereby solving the problem of bulky and heavy appearance of winter cotton clothing products.

[0006] The present invention provides a lightweight warm-keeping functional flocculent sheet, comprising:

[0007] Thermal storage modified polyester fiber layer;

[0008] A polyimide nanofiber layer composited on the thermal storage modified polyester fiber layer;

[0009] A polyester fiber layer composited on the polyimide nanofiber layer;

[0010] The heat storage modified polyester fiber layer is made of modified polyester staple fibers;

[0011] The modified polyester staple fiber is prepared from raw materials including the following components:

[0012] 100 parts by weight of PET slices;

[0013] 1 to 5 parts by weight of ZrC powder;

[0014] TiO2 powder 0.1 to 0.9 parts by weight.

[0015] Preferably, the weight of the thermal storage modified polyester fiber layer is 35 g / m 2 ~50g / m 2 The polyimide nanofiber layer has a gram weight of 10 g / m 2 ~20g / m 2 , thickness is 1mm to 2mm; the weight of the polyester fiber layer is 20g / m 2 ~45g / m 2 .

[0016] Preferably, the modified polyester staple fiber has a breaking strength of 6 cN / dtex to 7 cN / dtex, an elongation at break of 18% to 24%, a fineness of 1.33 dtex to 1.8 dtex, and a length of 35 mm to 45 mm.

[0017] Preferably, the specification of the ZrC powder is 0.5 μm to 2 μm; the average particle size of the TiO2 powder is 0.1 μm to 0.5 μm.

[0018] Preferably, the preparation method of the modified polyester staple fiber is specifically as follows:

[0019] PET chips, ZrC powder and TiO2 powder are melt-blended and then spun to obtain modified polyester staple fibers.

[0020] Preferably, the spinning process is specifically as follows:

[0021] The material extruded after melt blending of PET chips, ZrC powder and TiO2 powder is sequentially subjected to pressurization, metering, spinning, cooling, bundling and oiling, winding, traction, laying, wire guiding, stretching, heat setting, bundle cooling, oiling, folding, curling steam, curling, relaxation and setting, and cutting to obtain modified polyester staple fibers; the spinning box temperature is 270°C to 300°C, and the spinning speed is 1300m / min to 1400m / min.

[0022] Preferably, the polyester fiber layer is made of polyester staple fibers; the polyester staple fibers have a fineness of 1 dtex to 1.5 dtex and a length of 35 mm to 40 mm.

[0023] The present invention also provides a method for preparing the lightweight thermal insulation functional flakes described in the above technical solution, comprising the following steps:

[0024] A parallel laying method is adopted, with modified polyester staple fibers laid on the lower layer, polyester staple fibers laid on the upper layer, and a polyimide nanofiber layer in the middle layer. After gluing, the fibers are compounded and then dried, cooled, wound, and cut in sequence to obtain lightweight, warm-keeping functional flocs.

[0025] Preferably, the glue used for the gluing is acrylic polymer emulsion, and the viscosity at 25°C is 200cP-500cP; the spraying amount of the gluing is 2g / m 2 ~6g / m 2 .

[0026] Preferably, the drying temperature is 100°C to 160°C, and the time is 3 min to 15 min; the cooling temperature is 10°C to 30°C, and the time is 3 min to 15 min.

[0027] The present invention provides a lightweight thermal insulation functional flocculent sheet, comprising: a heat storage modified polyester fiber layer; a polyimide nanofiber layer composited on the heat storage modified polyester fiber layer; a polyester fiber layer composited on the polyimide nanofiber layer; the heat storage modified polyester fiber layer is prepared from modified polyester staple fibers; the modified polyester staple fibers are prepared from raw materials including the following components: 100 parts by weight of PET slices; 1 to 5 parts by weight of ZrC powder; 0.1 to 0.9 parts by weight of TiO2 powder. Compared with the prior art, the lightweight thermal insulation functional flocculent sheet provided by the present invention adopts a specific layer structure and connection relationship to achieve better overall interaction. The product has excellent thermal insulation function and is lightweight, solving the problem of bloated and heavy appearance of winter cotton clothing products. Experimental results show that the gram weight of the lightweight thermal insulation functional flocculent sheet provided by the present invention does not exceed 100g / m 2The compression rate is 83.1%~85.3%, the recovery rate is 90.2%~90.7%, the Krogh value is 3.13~3.39, and the heat storage property is excellent, the maximum temperature rise value is 7.5℃~7.8℃, and the average temperature rise value is 4.6℃~4.9℃.

[0028] In addition, the preparation method provided by the present invention has simple process, mild conditions, easy control, and broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A schematic structural diagram of a lightweight, warm-keeping functional flocculent provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0030] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] The present invention provides a lightweight warm-keeping functional flocculent sheet, comprising:

[0032] Thermal storage modified polyester fiber layer;

[0033] A polyimide nanofiber layer composited on the thermal storage modified polyester fiber layer;

[0034] A polyester fiber layer composited on the polyimide nanofiber layer;

[0035] The heat storage modified polyester fiber layer is made of modified polyester staple fibers;

[0036] The modified polyester staple fiber is prepared from raw materials including the following components:

[0037] 100 parts by weight of PET slices;

[0038] 1 to 5 parts by weight of ZrC powder;

[0039] TiO2 powder 0.1 to 0.9 parts by weight.

[0040] In the present invention, the lightweight thermal insulation functional flocculent sheet comprises a heat storage modified polyester fiber layer, a polyimide nanofiber layer and a polyester fiber layer, preferably a three-layer structure of a heat storage modified polyester fiber layer, a polyimide nanofiber layer and a polyester fiber layer; the connection relationship between the three can be seen in Figure 1 As shown; Figure 1 A schematic structural diagram of a lightweight, warm-keeping functional flocculent provided in an embodiment of the present invention.

[0041] In the present invention, the weight per unit area of ​​the three-layer structure does not exceed 50g / m 2 ; Wherein, the weight of the thermal storage modified polyester fiber layer is preferably 35g / m 2 ~50g / m 2 , more preferably 40g / m 2 ~50g / m 2 The weight of the polyimide nanofiber layer is preferably 10 g / m 2 ~20g / m 2 , more preferably 14g / m 2 The thickness is preferably 1 mm to 2 mm, more preferably 1.3 mm to 1.4 mm; the weight of the polyester fiber layer is preferably 20 g / m 2 ~45g / m 2 , more preferably 25g / m 2 ~40g / m 2 .

[0042] In the present invention, the polyimide nanofiber layer is a nanofiber layer obtained by an electrospinning process and has an extremely light weight; the present invention has no special limitation on its source, and commercially available products known to those skilled in the art can be used.

[0043] In the present invention, the heat storage modified polyester fiber layer is prepared from modified polyester staple fibers; the modified polyester staple fibers are prepared from raw materials including the following components:

[0044] 100 parts by weight of PET slices;

[0045] 1 to 5 parts by weight of ZrC powder;

[0046] TiO2 powder 0.1-0.9 parts by weight;

[0047] Preferably:

[0048] 100 parts by weight of PET slices;

[0049] 1-2 parts by weight of ZrC powder;

[0050] 0.3-0.5 parts by weight of TiO2 powder.

[0051] In the present invention, the modified polyester staple fiber is prepared from raw materials including PET chips, ZrC powder and TiO2 powder, preferably prepared from PET chips, ZrC powder and TiO2 powder. The modified polyester staple fiber prepared by the present invention, with the addition of ZrC and TiO2 functional materials, can convert the energy in visible light into heat energy and has excellent heat storage performance.

[0052] The present invention has no special restrictions on the sources of the PET slices, ZrC powder and TiO2 powder, and commercially available products known to those skilled in the art can be used; wherein the purity of the ZrC powder and the TiO2 powder is above 95%.

[0053] In the present invention, the specification of the ZrC powder is preferably 0.5 μm to 2 μm, more preferably 0.8 μm to 1 μm; the average particle size of the TiO2 powder is preferably 0.1 μm to 0.5 μm, more preferably 0.2 μm to 0.25 μm.

[0054] In the present invention, the preparation method of the modified polyester staple fiber is preferably as follows:

[0055] PET chips, ZrC powder and TiO2 powder are melt-blended and then spun to obtain modified polyester staple fibers.

[0056] In the present invention, before the melt blending, preferably the following steps are further included:

[0057] The mixture of PET slices, ZrC powder and TiO2 powder is dried; the drying temperature is preferably 130°C to 145°C, more preferably 135°C to 140°C.

[0058] In the present invention, the intrinsic viscosity of the melt blend is preferably 0.4 dL / g to 1 dL / g, more preferably 0.6 dL / g to 0.7 dL / g.

[0059] In the present invention, the spinning process is preferably specifically as follows:

[0060] The material extruded after melt blending of PET chips, ZrC powder and TiO2 powder is sequentially subjected to pressurization, metering, spinning, cooling, bundling and oiling, winding, traction, laying, wire guiding, stretching, heat setting, bundle cooling, oiling, folding, curling steam, curling, relaxation and setting, and cutting to obtain modified polyester staple fibers.

[0061] In the present invention, the boost load is preferably 4 t / h to 8 t / h, more preferably 5.5 t / h to 6 t / h.

[0062] The present invention has no special limitation on the metering process, and the technical means in the spinning process well known to those skilled in the art can be adopted.

[0063] In the present invention, the box temperature of the spinning is preferably 270° C. to 300° C., more preferably 280° C. to 290° C.; the spinning speed of the spinning is preferably 1300 m / min to 1400 m / min.

[0064] In the present invention, the main air duct pressure of the cooling is preferably 750Pa-900Pa, more preferably 800Pa-850Pa, and the air temperature is preferably 15°C-25°C, more preferably 20°C-23°C.

[0065] In the present invention, the oil content of the bundled oil is preferably 1 wt% to 2 wt%, more preferably 1.5 wt%.

[0066] The present invention has no special restrictions on the processes of winding, pulling, laying, guiding and subsequent stacking, steam curling, relaxation and shaping, and cutting, and the technical means in the spinning process well known to those skilled in the art can be adopted.

[0067] In the present invention, the stretching ratio is preferably 2 to 4, and more preferably 3 to 3.5.

[0068] In the present invention, the heat setting pressure is preferably 15 MPa to 25 MPa, more preferably 18 MPa to 20 MPa.

[0069] In the present invention, the filament bundle cooling may be performed in the same manner as the cooling in the above technical solution.

[0070] In the present invention, the oil content of the oiling is preferably 0.5wt% to 1wt%, more preferably 0.8wt%.

[0071] In the present invention, the curling temperature is preferably 100°C to 150°C, more preferably 120°C.

[0072] In the present invention, the modified polyester staple fiber preferably has a breaking strength of 6 cN / dtex to 7 cN / dtex, a breaking elongation of 18% to 24%, more preferably 20% to 22%, a fineness of 1.33 dtex to 1.8 dtex, and a length of 35 mm to 45 mm, more preferably 38 mm to 42 mm.

[0073] In the present invention, the heat storage modified polyester fiber layer is prepared from the modified polyester staple fibers having the heat storage function, thereby further obtaining a flake having excellent heat storage and warmth retention function.

[0074] In the present invention, the polyester fiber layer is preferably made of polyester staple fibers; the present invention has no special restrictions on the source of the polyester staple fibers, and commercially available products known to those skilled in the art can be used. In the present invention, the fineness of the polyester staple fibers is preferably 1 dtex to 1.5 dtex, more preferably 1.3 dtex to 1.4 dtex, and the length is preferably 35 mm to 40 mm, more preferably 38 mm.

[0075] The lightweight thermal insulation functional flakes provided by the present invention adopts a three-layer structure, the inner (lower) layer adopts a specific heat storage material, and the middle layer adopts an extremely lightweight polyimide nanofiber layer with low thermal conductivity, so that the inner layer can store heat and the middle layer can be heat-insulated. The prepared flake material has a lightweight and excellent thermal insulation performance. In addition, the polyimide nanofiber layer is composed of nanofiber layers, so the tear resistance of the entire fiber layer is poor. Using it as an intermediate layer and sandwiching it between the polyester fiber layers can protect the nanolayer and reduce damage during use, thereby utilizing its advantages and avoiding its disadvantages.

[0076] The present invention also provides a method for preparing the lightweight thermal insulation functional flakes described in the above technical solution, comprising the following steps:

[0077] A parallel laying method is adopted, with modified polyester staple fibers laid on the lower layer, polyester staple fibers laid on the upper layer, and a polyimide nanofiber layer in the middle layer. After gluing, the fibers are compounded and then dried, cooled, wound, and cut in sequence to obtain lightweight, warm-keeping functional flocs.

[0078] In the present invention, the parallel web laying form is realized by using two parallel web laying machines, one web laying machine lays the upper layer, and the other web laying machine lays the lower layer.

[0079] In the present invention, before laying the web, it is preferred to further include the processes of weighing and feeding, opening, feeding and combing, the purpose of which is to pretreat the raw material fibers, and the present invention has no special limitation on this.

[0080] The present invention adopts a parallel laying form, with modified polyester staple fibers laid on the lower layer, polyester staple fibers laid on the upper layer, and the middle layer being a polyimide nanofiber layer; in the present invention, the modified polyester staple fibers, ester staple fibers, and polyimide nanofiber layers are the same as those in the above technical solution and will not be repeated here.

[0081] After feeding, the present invention performs gluing to achieve overall compounding; the glue used for the gluing is preferably an acrylic polymer emulsion, and its viscosity at 25° C. is preferably 200 cP to 500 cP; the present invention has no special restrictions on the source of the acrylic polymer emulsion, and commercial products well known to those skilled in the art can be used.

[0082] In the present invention, the spraying amount of the glue is preferably 2g / m 2 ~6g / m 2 , more preferably 4g / m 2 .

[0083] In the present invention, the drying temperature is preferably 100°C to 160°C, more preferably 145°C, and the time is preferably 3min to 15min, more preferably 5min; the cooling temperature is preferably 10°C to 30°C, more preferably 18°C ​​to 23°C, and the time is preferably 3min to 15min, more preferably 5min.

[0084] Finally, the flakes are wound and cut to obtain finished products.

[0085] The preparation method provided by the invention has simple process, mild conditions, easy control and broad application prospects.

[0086] The present invention provides a lightweight thermal insulation functional flocculent sheet, comprising: a heat storage modified polyester fiber layer; a polyimide nanofiber layer composited on the heat storage modified polyester fiber layer; a polyester fiber layer composited on the polyimide nanofiber layer; the heat storage modified polyester fiber layer is prepared from modified polyester staple fibers; the modified polyester staple fibers are prepared from raw materials including the following components: 100 parts by weight of PET slices; 1 to 5 parts by weight of ZrC powder; 0.1 to 0.9 parts by weight of TiO2 powder. Compared with the prior art, the lightweight thermal insulation functional flocculent sheet provided by the present invention adopts a specific layer structure and connection relationship to achieve better overall interaction. The product has excellent thermal insulation function and is lightweight, solving the problem of bloated and heavy appearance of winter cotton clothing products. Experimental results show that the gram weight of the lightweight thermal insulation functional flocculent sheet provided by the present invention does not exceed 100g / m 2 The compression rate is 83.1%~85.3%, the recovery rate is 90.2%~90.7%, the Krogh value is 3.13~3.39, and the heat storage property is excellent, the maximum temperature rise value is 7.5℃~7.8℃, and the average temperature rise value is 4.6℃~4.9℃.

[0087] In addition, the preparation method provided by the present invention has simple process, mild conditions, easy control, and broad application prospects.

[0088] In order to further illustrate the present invention, the following examples are used for detailed description. The raw materials used in the following examples of the present invention are all commercially available; among them, PET slices: Yizheng Chemical Fiber, white, intrinsic viscosity 0.66, melting point 260°C; ZrC powder: Zhongnuo New Materials, black, purity 99.8%, specification 0.8μm~1μm, item number Zr52206; TiO2 powder: DuPont Ti-Pure R-103, TiO2 content 96%, average particle size 0.23μm, specific gravity 4.1;

[0089] The heat storage fiber used is modified polyester staple fiber, and the production process steps are as follows:

[0090] PET slices and powder additives (based on the weight of the PET slices, the powder additives include 1.5wt% zirconium carbide ZrC, 0.4wt% titanium dioxide TiO2) are added to the spinning equipment, and the production process is as follows: drying (temperature 135°C-140°C) → screw melt extrusion (melt intrinsic viscosity 0.63dL / g) → pressurization (load 5.85t / h) → metering → spinning (box temperature 285°C, spinning speed 1350m / min) → cooling (main air duct pressure 830Pa, wind temperature 20°C-23°C) → bundling oiling (oil content 1.5wt%) → winding → traction → laying → wire guiding → stretching (stretching ratio 3.16) → heat setting (pressure 18MPa-20MPa) → tow cooling → oiling (oil content 0.8wt%) → stacking → crimping steam → crimping (temperature 120°C) → relaxation and setting → cutting → packaging → PET staple fibers;

[0091] The performance parameters of the obtained heat storage fiber are as follows:

[0092] Breaking strength: 6.2cN / dtex;

[0093] Elongation at break: 21%;

[0094] Fineness: 1.33dtex~1.8dtex;

[0095] Length: 38mm~42mm.

[0096] Example 1

[0097] The production process steps of lightweight thermal insulation flakes are as follows:

[0098] Weighing and feeding → opening → feeding → combing → laying the net → feeding → gluing → compounding → drying → cooling → winding → cutting → flakes are finished;

[0099] Two parallel laying machines are used, one laying machine lays the upper layer, and the other laying machine lays the lower layer;

[0100] The weight of the upper flakes is 25-30g / m 2 , using conventional polyester staple fiber, Yizheng chemical fiber, brand YL720, fineness 1.33dtex, length 38mm;

[0101] The weight of the lower layer flakes is 40~45g / m 2 , using the heat storage fiber (modified polyester staple fiber) prepared above, with a fineness of 1.33-1.8 dtex and a length of 38-42 mm;

[0102] The middle layer is a polyimide nanofiber layer, Jiangxi Xiancai Nanofiber Technology Co., Ltd., with a gram weight of 14g / m 2 , thickness 1.34mm;

[0103] The glue used is acrylic polymer emulsion, milky white liquid, Dibang Nanotechnology, model PA-512, solid content 48%, anionic, viscosity (25℃) 200~500cP; spraying amount 4g / m 2 ;

[0104] Drying temperature: 145°C, time 5min;

[0105] Cooling temperature: 18℃~23℃, time 5min.

[0106] After testing, the weight of the lightweight thermal insulation flakes is 80g / m 2 .

[0107] Example 2

[0108] The production process steps of lightweight thermal insulation flakes are as follows:

[0109] Weighing and feeding → opening → feeding → combing → laying the net → feeding → gluing → compounding → drying → cooling → winding → cutting → flakes are finished;

[0110] Two parallel laying machines are used, one laying machine lays the upper layer, and the other laying machine lays the lower layer;

[0111] Upper layer flake weight 35~40g / m 2 , using conventional polyester staple fiber, Yizheng chemical fiber, brand YL720, fineness 1.33dtex, length 38mm;

[0112] The weight of the lower layer flakes is 45~50g / m 2 , using the heat storage fiber (modified polyester staple fiber) prepared above, with a fineness of 1.33-1.8 dtex and a length of 38-42 mm;

[0113] The middle layer is a polyimide nanofiber layer, Jiangxi Xiancai Nanofiber Technology Co., Ltd., with a gram weight of 14g / m 2 , thickness 1.34mm;

[0114] The glue used is acrylic polymer emulsion, milky white liquid, Dibang Nanotechnology, model PA-512, solid content 48%, anionic, viscosity (25℃) 200~500cP; spraying amount 4g / m 2 ;

[0115] Drying temperature: 145°C, time 5min;

[0116] Cooling temperature: 18℃~23℃, time 5min.

[0117] After testing, the weight of the lightweight thermal insulation flakes is 100g / m 2 .

[0118] Comparative Example 1

[0119] Weight: 80g / m 2 Ordinary flake sample.

[0120] Comparative Example 2

[0121] Weight: 100g / m 2 Ordinary flake sample.

[0122] The various properties of the lightweight thermal insulation functional flakes provided in Examples 1 to 2 and the ordinary flake samples provided in Comparative Examples 1 to 2 were tested, wherein the compression resilience test method: FZ / T 64003-2011 spray-bonded cotton flakes; the Crowe value test method: GB / T 35762-2017 Textile heat transfer performance test method flat plate method; the heat storage test method: G / T 18319-2019 Textile light heat storage performance test method; the test results are shown in Table 1.

[0123] Table 1 Performance data of lightweight warm-keeping functional flakes provided in Examples 1 to 2 and ordinary flakes provided in Comparative Examples 1 to 2

[0124]

[0125] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A lightweight thermal insulation functional flocculent sheet, which is composed of a three-layer structure of a heat storage modified polyester fiber layer, a polyimide nanofiber layer composited on the heat storage modified polyester fiber layer, and a polyester fiber layer composited on the polyimide nanofiber layer; The heat storage modified polyester fiber layer is made of modified polyester staple fibers; The modified polyester staple fiber is prepared from the following raw materials: 100 parts by weight of PET slices; 1 to 5 parts by weight of ZrC powder; TiO2 powder 0.1-0.9 parts by weight; The weight of the thermal storage modified polyester fiber layer is 35 g / m 2 ~50g / m 2 The polyimide nanofiber layer has a gram weight of 10 g / m 2 ~20g / m 2 , thickness is 1mm to 2mm; the weight of the polyester fiber layer is 20g / m 2 ~45g / m 2 ; The modified polyester staple fiber has a breaking strength of 6 cN / dtex to 7 cN / dtex, a breaking elongation of 18% to 24%, a fineness of 1.33 dtex to 1.8 dtex, and a length of 35 mm to 45 mm.

2. The lightweight thermal insulation functional flakes according to claim 1, characterized in that: The specification of the ZrC powder is 0.5 μm to 2 μm; the average particle size of the TiO2 powder is 0.1 μm to 0.5 μm.

3. The lightweight thermal insulation functional flocculent sheet according to claim 1, characterized in that: The preparation method of the modified polyester staple fiber is specifically as follows: PET chips, ZrC powder and TiO2 powder are melt-blended and then spun to obtain modified polyester staple fibers.

4. The lightweight thermal insulation functional flocculent sheet according to claim 3, characterized in that: The spinning process is specifically as follows: The material extruded after melt blending of PET chips, ZrC powder and TiO2 powder is sequentially subjected to pressurization, metering, spinning, cooling, bundling and oiling, winding, traction, laying, wire guiding, stretching, heat setting, bundle cooling, oiling, folding, curling steam, curling, relaxation and setting, and cutting to obtain modified polyester staple fibers; the spinning box temperature is 270°C to 300°C, and the spinning speed is 1300m / min to 1400m / min.

5. The lightweight thermal insulation functional flocculent sheet according to claim 1, characterized in that: The polyester fiber layer is made of polyester staple fibers; the polyester staple fibers have a fineness of 1 dtex to 1.5 dtex and a length of 35 mm to 40 mm.

6. A method for preparing the lightweight thermal insulation functional flakes according to any one of claims 1 to 5, comprising the following steps: A parallel laying method is adopted, with modified polyester staple fibers laid on the lower layer, polyester staple fibers laid on the upper layer, and a polyimide nanofiber layer in the middle layer. After gluing, the fibers are compounded and then dried, cooled, wound, and cut in sequence to obtain lightweight, warm-keeping functional flocs.

7. The preparation method according to claim 6, characterized in that: The glue used for the gluing is acrylic polymer emulsion with a viscosity of 200cP to 500cP at 25°C. The spraying amount of the gluing is 2g / m 2 ~6g / m 2 .